High-entropy titanate negative electrode material, preparation method and application

Through high entropy titanate material (Li0.2La0.2X0.2Y0.2Z0.2)TiO3, the problem of poor safety and rate performance of the negative electrode material of lithium-ion battery is solved, and high lithium storage capacity and stability are achieved. It is suitable for Large-scale energy storage system.

CN118983430APending Publication Date: 2024-11-19YIBIN VOCATIONAL & TECH COLLEGE
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411278903.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials such as graphite have problems such as low safety, poor rate performance and lithium dendrites during high load and circulation, which are difficult to meet the requirements of large-scale energy storage systems.

Method used

High entropy titanate material (Li0.2La0.2X0.2Y0.2Z0.2)TiO3 is prepared by co-precipitation method, combined with doping of different metal elements, a perovskite type material with a tetragonal phase structure is formed to optimize lithium storage Capacity and stability.

Benefits of technology

It achieves high lithium storage specific capacity, good rate performance and cycling performance, improves the electrochemical stability and energy density of lithium-ion batteries, and has excellent fast charging and discharging performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983430A_ABST
    Figure CN118983430A_ABST
Patent Text Reader

Abstract

The invention discloses a high-entropy titanate negative electrode material as well as a preparation method and application thereof, the intrinsic structure is a classical perovskite type structure (ABO3), and the chemical structural formula of the high-entropy titanate negative electrode material is (Li < 0.2 > La < 0.2 > X < 0.2 > Y < 0.2 > Z < 0.2 >) TiO3, and the A site is occupied by Li, La and other three types of atoms from different main groups and subgroups in an equal molar ratio. X is selected from alkali metal elements (Na, K, Rb and Cs), Y is selected from transition metal elements (Mn, Fe, Co, Ni and Zr), and Z is selected from rare earth metal elements (Sc, Y, Pr, Nd, Gd and Sm). The invention relates to a method for preparing the high-entropy titanate (Li < 0.2 > La < 0.2 > X < 0.2 > Y < 0.2 > Z < 0.2 >) TiO < 3 > negative electrode material by adopting a coprecipitation method and a lithium ion battery based on the high-entropy negative electrode. The high-entropy titanate negative electrode is high in lithium storage specific capacity, moderate in charge and discharge potential, good in electrochemical lithium intercalation stability and relatively high in lithium ion diffusion rate. The lithium ion battery assembled by the high-entropy negative electrode is good in cyclic charging and discharging stability, high in energy density and excellent in rapid charging and discharging performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of negative electrode materials for lithium-ion batteries, and in particular, relates to a high-entropy titanate negative electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are the most popular electrochemical energy storage technology currently being studied and have been widely used in portable electronic devices, electric vehicles and other fields. However, lithium-ion batteries still have many shortcomings, such as poor battery life, low power density, and safety that needs to be improved, which greatly limits their further application in large-scale energy storage / conversion fields. In order to overcome these problems and improve the performance indicators of lithium-ion batteries, the development of negative electrode materials with excellent comprehensive electrochemical properties is an effective and conventional approach. Graphite is the most mature commercial lithium-ion battery negative electrode currently. However, due to its lithium insertion and extraction potential being lower than 0.2 V (vs. Li / Li + ), close to the lithium deposition potential, under overcharge or high current charge and discharge conditions, lithium dendrites will form on the surface of the graphite negative electrode, and the transitional growth of lithium dendrites will penetrate the diaphragm, which will cause the battery to short-circuit; Obviously, the graphite negative electrode has poor rate performance and low safety, and it is difficult to meet the requirements of large-scale energy storage systems. Therefore, it is urgent to develop new high-performance negative electrode materials with the advantages of low cost, high power density, cycle stability, and safety to replace traditional graphite negative electrodes.

[0003] Li s La 2 / 3-s / 3 TiO3 is a fast ion conductor (room temperature lithium ion conductivity σ ≈ 10 -3 Ω -1 cm -1 ), with a typical perovskite oxide crystal structure (chemical formula is ABO3). Studies have shown that when the lithium element / lanthanum element has an equal molar ratio (s=0.5) occupying Li s La 2 / 3-s / 3 When the TiO3 crystal structure is in the A position, its crystal is a tetragonal phase structure. 0.5 La 0.5 TiO3 is an intrinsic embedded pseudocapacitor electrode material with a high lithium storage capacity (225 mA hg -1 On the other hand, density functional theory calculations speculate that the diffusion potential of lithium ions along the a, b, and c axes of its crystal structure is much lower than that of other titanium-based oxide negative electrodes. Its structure can provide a three-dimensional lithium diffusion path, so the diffusion properties are close to isotropic, and the average working potential is reduced by 0.3 ~ 0.5 V; in addition, lithium ions are embedded in Li 0.5 La 0.5 TiO3 does not cause structural phase change, so it has good stability and the electrode capacity is not easy to decay. 0.5 La0.5 As a new type of titanate negative electrode material, TiO3 has demonstrated its application potential. Further optimization of its structure and lithium storage performance will enable it to meet the various requirements of current high-performance lithium-ion batteries for negative electrodes. It is expected to become a new research hotspot in the field of lithium-ion battery negative electrodes.

[0004] Recently, high entropy oxide solid solution materials have attracted close attention from researchers due to their unique structural characteristics and excellent electrical, magnetic, thermal and other physical and chemical properties. The concept of this type of material is derived from high entropy alloys, which generally refers to oxides with a single stable phase (mixed configuration entropy ΔS) formed by solid solution of 5 or more elements in an equiatomic ratio or near equiatomic ratio. mix >1.5R, R is the gas constant). Compared with traditional low-entropy oxide electrode materials, known high-entropy oxide electrodes show obvious differences in composition, structure or performance. 0.5 La 0.5 The TiO3 negative electrode, from the perspective of its perovskite crystal intrinsic structure, has a "gene" rich in doping positions, which is conducive to the incorporation of a variety of metal elements. Especially at the A position of the crystal structure, alkali metals, alkaline earth metals, transition metals and other rare earth metal elements can replace Li and La, thereby achieving the high entropy effect of the titanate lithium storage negative electrode. Summary of the invention

[0005] The purpose of the present invention is to provide a high entropy titanate negative electrode material for lithium ion batteries and a preparation method thereof. By controlling the element type, element ratio, preparation method, reaction time, temperature and other process parameters, a high entropy titanate negative electrode material (Li 0.2 La 0.2 X 0.2 Y 0.2 Z 0.2 )TiO3 high entropy titanate anode. The high entropy titanate anode exhibits high lithium storage capacity, good rate performance and cycle performance.

[0006] To achieve the above purpose, the specific technical solutions provided by the present invention are as follows: A high entropy titanate for lithium-ion batteries 0.2 La 0.2 X 0.2 Y 0.2 Z 0.2 )TiO3 negative electrode material, the chemical composition is a perovskite type material (ABO3). The high entropy titanate negative electrode is a single-phase structure; the single-phase structure is a tetragonal phase structure; and the single-phase structure exists stably during the charging and discharging process of the lithium-ion battery.

[0007] A high entropy titanate negative electrode material for lithium-ion batteries, characterized in that the A position of the molecular structure is occupied by Li, La and three other types of atoms from different main groups and subgroups in an equal molar ratio. X is limited to be selected from the alkali metal element sequence (Na, K, Rb and Cs), Y is limited to be selected from the transition metal element sequence (Mn, Fe, Co, Ni, and Zr), and Z is limited to be selected from the rare earth metal element sequence (Sc, Y, Pr, Nd, Gd and Sm). In the single-phase structure, different metal elements Li, La, X, Y and Z are uniformly mixed.

[0008] To prepare the high entropy titanate negative electrode material, a coprecipitation method is used, which specifically includes the following steps: (1) First, dissolve the titanium precursor in ethanol. Then add lithium acetate, lanthanum acetate, and acetates containing metal elements of X / Y / Z. Stir and dissolve them first, then form a precipitate. Filter the emulsion and dry it.

[0009] (2) The precipitate obtained by filtration is placed in a crucible and sintered in a muffle furnace. After rapid cooling, a high-entropy titanate material is obtained.

[0010] Preferably, the titanium precursor in step (1) is a mixture of one or more of tetrabutyl titanate, titanium isopropoxide, titanyl sulfate and titanium tetrachloride.

[0011] Preferably, in step (1), the mass ratio of the titanium precursor to the solvent ethanol is 0.1 to 1.

[0012] Preferably, the acetate containing X / Y / Z metal elements in step (1) is a metal acetate containing one of Na, K, Rb and Cs, a metal acetate containing Mn, Fe, Co, Ni and Zr, and a metal acetate containing Sc, Y, Pr, Nd, Gd and Sm.

[0013] Preferably, in step (2), the sintering temperature is 700-1200° C., and the sintering holding time is 3-12 hours.

[0014] The present invention also provides the use of a high entropy titanate negative electrode in a lithium ion battery. The high entropy titanate negative electrode of the present invention is made into a lithium ion battery negative electrode according to the following steps: the high entropy titanate negative electrode material and the conductive carbon black Super-P are dispersed in ethanol at a mass ratio of 8:1, ultrasonic mixing and dispersion are performed, and then vacuum filtration is performed to collect the powder. A polyvinylidene fluoride / N-methylpyrrolidone solution (3 wt %) is prepared and added to the high entropy titanate negative electrode / conductive carbon black powder at a mass ratio of 1 (polyvinylidene fluoride): 9 (high entropy titanate negative electrode), and the mixture is fully stirred to form a slurry. The mixed slurry is evenly coated on the surface of the copper foil and placed in a vacuum drying oven at 80°C for vacuum drying for 12 hours. After taking out, the copper foil is cut into a small disc negative electrode with a diameter of 12 mm using a round hole punching machine, and assembled into a button battery in a glove box for electrochemical performance testing.

[0015] The present invention has the following innovations and features: Based on the fast ion conductor Li s La 2 / 3-s / 3 TiO3 constructs high entropy titanate negative electrode materials, realizes high entropy effect, and further optimizes the lithium storage capacity and stability of fast ion conductors.

[0016] Compared with the prior art, the beneficial effects of the present invention are as follows: Compared with the traditional single electrode material, constructing a high entropy component in the crystal structure can, on the one hand, greatly increase the disordered structure and multi-scale defects in the lattice, and optimize the lithium storage capacity and stability of the material; on the other hand, the increase in entropy can make the crystal structure achieve a balance between local characteristic disorder and macroscopic long-range order, synergistically optimize the lithium ion diffusion performance and material electronic conductivity, and improve the electrode rate performance. The emergence of high entropy design ideas has broken through the design limitations of simple component components, opened up ideas and provided guidance for the research and development of new electrode material systems and the optimization of lithium storage performance; and the diversification of components can also alleviate the dependence of the industrial field on scarce metal elements. Exploring the optimization mechanism of lithium storage performance of electrode materials based on high entropy design strategies has become a new hot spot in the field of electrochemical energy storage.

[0017] The high entropy titanate negative electrode of the present invention has high specific lithium storage capacity, moderate charge and discharge potential, good electrochemical lithium insertion stability, and high lithium ion diffusion rate. The lithium ion battery assembled with this high entropy negative electrode has good cycle charge and discharge stability, high energy density, and excellent rapid charge and discharge performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 The high entropy titanate (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 )Scanning electron microscope photo of TiO3 powder; Figure 2 The high entropy titanate (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 ) XRD pattern of TiO3 powder; Figure 3 The high entropy titanate (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 ) The cycle charge and discharge performance diagram of lithium-ion battery assembled with TiO3 negative electrode; Figure 4 The high entropy titanate (Li 0.2 La 0.2 K 0.2 Mn 0.2 Sr 0.2 )Charge and discharge performance diagram of lithium-ion battery assembled with TiO3 negative electrode. DETAILED DESCRIPTION

[0020] The present invention is further described below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention, and those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention.

[0021] Example 1 This embodiment provides a high entropy titanate negative electrode material, the high entropy titanate negative electrode material is a perovskite type material (ABO3), the chemical composition is (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 )TiO3; the high entropy titanate negative electrode material has a single-phase structure, and the single-phase structure is a tetragonal phase structure.

[0022] In the single-phase structure, different metal elements Li, La, Na, Fe and Y are evenly mixed, the A position of the molecular structure is occupied by Li, La, Na, Fe and Y in an equal molar ratio, and the microstructure of the high-entropy titanate negative electrode material is regular tetragonal particles, and the size of a single crystal is 3 μm to 5 μm.

[0023] The preparation method of the high entropy titanate negative electrode material in this embodiment is as follows: (1) Weigh 2 mmol of tetrabutyl titanate and dissolve it in 10 mmol of ethanol. Then add 2 mmol of lithium acetate, 2 mmol of lanthanum acetate, 2 mmol of sodium acetate, 2 mmol of iron acetate and 2 mmol of yttrium acetate. Stir and dissolve to form a homogeneous transparent solution. Then, due to the gradual hydrolysis of the titanium precursor, an emulsion is formed. After stirring for 12 hours, filter and dry the collected powder in an oven at 80°C for 12 hours.

[0024] (2) The precipitate obtained by filtration was placed in a crucible and sintered in a muffle furnace at a sintering temperature of 1000°C, a heating rate of 3°C / min, and a temperature preservation period of 10 hours. The temperature was then rapidly cooled to room temperature at a cooling rate of 20°C / min to obtain a high entropy titanate (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 )TiO3.

[0025] The (Li prepared in Example 1 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 )TiO3 is used as the negative electrode material of lithium-ion batteries and assembled into lithium-ion half-cells. Its electrochemical lithium storage stability is tested under constant current: when the charge and discharge current density is 200 mA g -1 The first reversible capacity is 230 mA hg -1 After 10 cycles, the specific capacity of the battery only dropped to 216 mA h g -1 , the capacity decay is less than 10%.

[0026] Figure 1 The high entropy titanate (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 )Scanning electron microscope photo of TiO3 powder; Figure 2 The high entropy titanate (Li 0.2 La 0.2 Na 0.2 Fe0.2 Y 0.2 ) XRD pattern of TiO3 powder; Figure 1 It can be seen that (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 )TiO3 has a regular square particle appearance. Figure 2 It can be seen that the prepared (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Y 0.2 )TiO3 crystals have a single phase structure without obvious impurity phases.

[0027] Example 2 This embodiment provides a high entropy titanate negative electrode material (Li 0.2 La 0.2 K 0.2 Mn 0.2 Sr 0.2 )TiO3, the preparation method thereof is as follows: (1) Weigh 1 mmol of tetrabutyl titanate and dissolve it in 10 mmol of ethanol. Then add 1 mmol of lithium acetate, 1 mmol of lanthanum acetate, 1 mmol of potassium acetate, 1 mmol of manganese acetate and 1 mmol of strontium acetate. Stir and dissolve to form a homogeneous transparent solution. Then, due to the gradual hydrolysis of the titanium precursor, an emulsion is formed. After stirring for 12 hours, filter and dry the collected powder in an oven at 80°C for 12 hours.

[0028] (2) The precipitate obtained by filtration was placed in a crucible and sintered in a muffle furnace at a temperature of 900°C, a heating rate of 3°C / min, and a temperature preservation period of 11 hours. The temperature was then rapidly cooled to room temperature at a cooling rate of 20°C / min to obtain high entropy titanate (Li 0.2 La 0.2 K 0.2 Mn 0.2 Sr 0.2 )TiO3.

[0029] The (Li prepared in Example 2 0.2 La 0.2 K 0.2 Mn 0.2 Sr 0.2 )TiO3 is used as the negative electrode material of lithium-ion batteries and assembled into lithium-ion half-cells. Its electrochemical lithium storage stability is tested under constant current: when the charge and discharge current density is 200 mA g -1 The first reversible capacity is 211 mA h g -1After 10 cycles, the specific capacity of the battery dropped to only 210 mA h g -1 , the capacity remains stable.

[0030] Example 3 This embodiment provides a high entropy titanate negative electrode material (Li 0.2 La 0.2 Na 0.2 Co 0.2 Sm 0.2 )TiO3, the preparation method thereof is as follows: (1) Weigh 3 mmol of tetrabutyl titanate and dissolve it in 10 mmol of ethanol. Then add 3 mmol of lithium acetate, 3 mmol of lanthanum acetate, 3 mmol of sodium acetate, 3 mmol of cobalt acetate and 3 mmol of samarium acetate. Stir and dissolve to form a homogeneous transparent solution. Then, due to the gradual hydrolysis of the titanium precursor, an emulsion is formed. After stirring for 12 hours, filter and dry the collected powder in an oven at 80°C for 12 hours.

[0031] (2) The precipitate obtained by filtration was placed in a crucible and sintered in a muffle furnace at a sintering temperature of 1000°C, a heating rate of 3°C / min, and a temperature preservation period of 10 hours. The temperature was then rapidly cooled to room temperature at a cooling rate of 20°C / min to obtain a high entropy titanate (Li 0.2 La 0.2 Na 0.2 Co 0.2 Sm 0.2 )TiO3.

[0032] The (Li prepared in Example 3 0.2 La 0.2 Na 0.2 Co 0.2 Sm 0.2 )TiO3 is used as the negative electrode material of lithium-ion batteries and assembled into lithium-ion half-cells. Its electrochemical lithium storage stability is tested under constant current: when the charge and discharge current density is 200 mA g -1 The first reversible capacity is 224 mA hg -1 After 10 cycles, the specific capacity of the battery dropped to only 215 mA h g -1 , the capacity decay is less than 5%.

[0033] Example 4 This embodiment provides a high entropy titanate negative electrode material (Li 0.2 La 0.2 K 0.2 Ni 0.2 Sm 0.2 )TiO3, the preparation method thereof is as follows: (1) Weigh 1.5 mmol of tetrabutyl titanate and dissolve it in 10 mmol of ethanol. Then add 1.5 mmol of lithium acetate, 1.5 mmol of lanthanum acetate, 1.5 mmol of potassium acetate, 1.5 mmol of nickel acetate and 1.5 mmol of samarium acetate. Stir and dissolve to form a homogeneous transparent solution. Then, due to the gradual hydrolysis of the titanium precursor, an emulsion is formed. After stirring for 12 hours, filter and dry the collected powder in an oven at 80°C for 12 hours.

[0034] (2) The precipitate obtained by filtration was placed in a crucible and sintered in a muffle furnace at a sintering temperature of 1100°C, a heating rate of 3°C / min, and a heat preservation time of 6 hours. The temperature was then rapidly cooled to room temperature at a cooling rate of 20°C / min to obtain a high entropy titanate (Li 0.2 La 0.2 K 0.2 Ni 0.2 Sm 0.2 )TiO3.

[0035] The (Li prepared in Example 4 0.2 La 0.2 K 0.2 Ni 0.2 Sm 0.2 )TiO3 is used as the negative electrode material of lithium-ion batteries and assembled into lithium-ion half-cells. Its electrochemical lithium storage stability is tested under constant current: when the charge and discharge current density is 200 mA g -1 The first reversible capacity is 211 mA h g -1 After 10 cycles, the specific capacity of the battery dropped to only 200 mA h g -1 , the capacity decay is less than 10%.

[0036] Example 5 This embodiment provides a high entropy titanate negative electrode material (Li 0.2 La 0.2 Na 0.2 Ni 0.2 Sm 0.2 )TiO3, the preparation method thereof is as follows: (1) Weigh 1.3 mmol of tetrabutyl titanate and dissolve it in 10 mmol of ethanol. Then add 1.3 mmol of lithium acetate, 1.3 mmol of lanthanum acetate, 1.3 mmol of sodium acetate, 1.3 mmol of nickel acetate and 1.5 mmol of samarium acetate. Stir and dissolve to form a homogeneous transparent solution. Then, due to the gradual hydrolysis of the titanium precursor, an emulsion is formed. After stirring for 12 hours, filter and dry the collected powder in an oven at 80°C for 12 hours.

[0037] (2) The precipitate obtained by filtration was placed in a crucible and sintered in a muffle furnace at a temperature of 900°C, a heating rate of 3°C / min, and kept at this temperature for 8 hours. The temperature was then rapidly cooled to room temperature at a cooling rate of 20°C / min to obtain high entropy titanate (Li 0.2 La 0.2 Na 0.2 Ni 0.2 Sm 0.2 )TiO3.

[0038] The (Li prepared in Example 5 0.2 La 0.2 Na 0.2 Ni 0.2 Sm 0.2 )TiO3 is used as the negative electrode material of lithium-ion batteries and assembled into lithium-ion half-cells. Its electrochemical lithium storage stability is tested under constant current: when the charge and discharge current density is 200 mA g -1 The first reversible capacity is 217 mA h g -1 After 10 cycles, the specific capacity of the battery dropped to only 205 mA h g -1 , the capacity decay is less than 10%.

[0039] Example 6 This embodiment provides a high entropy titanate negative electrode material (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Sr 0.2 )TiO3, the preparation method thereof is as follows: (1) Weigh 2 mmol of tetrabutyl titanate and dissolve it in 10 mmol of ethanol. Then add 2 mmol of lithium acetate, 2 mmol of lanthanum acetate, 2 mmol of sodium acetate, 2 mmol of iron acetate and 2 mmol of strontium acetate. Stir and dissolve to form a homogeneous transparent solution. Then, due to the gradual hydrolysis of the titanium precursor, an emulsion is formed. After stirring for 12 hours, filter and dry the collected powder in an oven at 80°C for 12 hours.

[0040] (2) The precipitate obtained by filtration was placed in a crucible and sintered in a muffle furnace at a sintering temperature of 1100°C, a heating rate of 3°C / min, and a temperature preservation period of 7 hours. The temperature was then rapidly cooled to room temperature at a cooling rate of 20°C / min to obtain a high entropy titanate (Li 0.2 La 0.2 Na 0.2 Fe 0.2 Sr 0.2 )TiO3.

[0041] The (Li prepared in Example 6 0.2 La0.2 Na 0.2 Fe 0.2 Sr 0.2 )TiO3 is used as the negative electrode material of lithium-ion batteries and assembled into lithium-ion half-cells. Its electrochemical lithium storage stability is tested under constant current: when the charge and discharge current density is 200 mA g -1 The first reversible capacity is 225 mA hg -1 After 10 cycles, the specific capacity of the battery only dropped to 208 mA h g -1 , the capacity decay is less than 10%.

[0042] Example 7 This embodiment provides a high entropy titanate negative electrode material (Li 0.2 La 0.2 Na 0.2 Ni 0.2 Sr 0.2 )TiO3, the preparation method thereof is as follows: (1) Weigh 3 mmol of tetrabutyl titanate and dissolve it in 10 mmol of ethanol. Then add 3 mmol of lithium acetate, 3 mmol of lanthanum acetate, 3 mmol of sodium acetate, 3 mmol of nickel acetate and 3 mmol of strontium acetate. Stir and dissolve to form a homogeneous transparent solution. Then, due to the gradual hydrolysis of the titanium precursor, an emulsion is formed. After stirring for 12 hours, filter and dry the collected powder in an oven at 80°C for 12 hours. (2) The precipitate obtained by filtration was placed in a crucible and sintered in a muffle furnace at a sintering temperature of 1000°C, a heating rate of 3°C / min, and a temperature preservation period of 7 hours. The temperature was then rapidly cooled to room temperature at a cooling rate of 20°C / min to obtain a high entropy titanate (Li 0.2 La 0.2 Na 0.2 Ni 0.2 Sr 0.2 )TiO3.

[0043] The (Li prepared in Example 7 0.2 La 0.2 Na 0.2 Ni 0.2 Sr 0.2 )TiO3 is used as the negative electrode material of lithium-ion batteries and assembled into lithium-ion half-cells. Its electrochemical lithium storage stability is tested under constant current: when the charge and discharge current density is 200 mA g -1 The first reversible capacity is 231 mA h g -1 After 10 cycles, the specific capacity of the battery dropped to only 211 mA h g -1 , the capacity decay is less than 10%.

[0044] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A high entropy titanate negative electrode material, characterized in that: The high entropy titanate negative electrode material is a perovskite type material (ABO3) with a chemical composition of (Li 0.2 La 0.2 X 0.2 Y 0.2 Z 0.2 )TiO3; the high entropy titanate negative electrode material has a single-phase structure, and the single-phase structure is a tetragonal phase structure.

2. The high entropy titanate negative electrode material according to claim 1, characterized in that: In the single-phase structure, different metal elements Li, La, X, Y and Z are uniformly mixed, and the A position of the molecular structure is occupied by Li, La and other three types of atoms from different main groups and sub-groups in an equal molar ratio, wherein X is limited to one selected from the alkali metal elements Na, K, Rb and Cs, Y is limited to one selected from the transition metal elements Mn, Fe, Co, Ni, and Zr, and Z is limited to one selected from the rare earth metal elements Sc, Y, Pr, Nd, Gd and Sm.

3. The high entropy titanate negative electrode material according to claim 1, characterized in that: The microstructure of the high entropy titanate negative electrode material is regular tetragonal particles, and the size of a single crystal is between 3 μm and 5 μm.

4. A method for preparing a high entropy titanate negative electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) The titanium precursor is first dissolved and dispersed in ethanol, and then lithium acetate, lanthanum acetate, and acetates containing metal elements of type X, Y, and Z are added, stirred and dissolved, and then a precipitate is formed. The emulsion is filtered and dried; (2) The precipitate obtained by filtration is placed in a crucible and sintered in a muffle furnace. After rapidly cooling to room temperature, a high entropy titanate material is obtained.

5. The method for preparing a high entropy titanate negative electrode material according to claim 4, characterized in that: The titanium precursor in step (1) is a mixture of one or more of tetrabutyl titanate, titanium isopropoxide, titanyl sulfate and titanium tetrachloride.

6. The method for preparing a high entropy titanate negative electrode material according to claim 4, characterized in that: The molar ratio of the titanium precursor to ethanol in step (1) is (0.1 ~ 1):

1.

7. The method for preparing a high entropy titanate negative electrode material according to claim 4, characterized in that: The acetate containing the X-type metal element in step (1) is a metal acetate containing Na, K, Rb or Cs, the acetate containing the Y-type metal element is a metal acetate containing Mn, Fe, Co, Ni or Zr, and the acetate containing the Z-type metal element is a metal acetate containing Sc, Y, Pr, Nd, Gd or Sm.

8. The method for preparing a high entropy titanate negative electrode material according to claim 4, characterized in that: In step (1), the drying temperature is 80°C and the drying time is 24 h.

9. The method for preparing a high entropy titanate negative electrode material for a lithium ion battery according to claim 4, characterized in that: In step (2), the sintering temperature is 700-1200°C, the heating rate is 3°C / min, the sintering holding time is 3-12 hours, and the cooling rate is 20°C / min.

10. Use of the high entropy titanate negative electrode material according to any one of claims 1 to 3 in a lithium ion battery.

Citation Information

Cited By

  • Negative electrode material and preparation method and application thereof

    CN122338043A

  • A negative electrode material, a preparation method therefor, and an application thereof

    CN122338043B

  • Titanium-based active material and preparation method and application thereof

    CN122338048A

  • Titanium-based active material, and preparation method and application thereof

    CN122338048B