Method for leaching nickel element and method for preparing nickel sulfate
By using nickel cobalt hydroxide and nickel sulfonium raw materials for collaborative leaching under acidic conditions, the problems of large reducing agent consumption and high equipment requirements in the leaching process of nickel elements in the prior art are solved, and low-cost and high-efficiency nickel leaching is achieved Effect.
Patent Information
- Application Number
- CN202310560609.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-22
AI Technical Summary
The existing nickel leaching process and nickel sulfate preparation methods have high cost, high equipment requirements and large capital investment, resulting in high cost and low efficiency.
The nickel hydroxide raw material and nickel sulfonium raw material are used to synergize leaching under acidic conditions, and the elemental nickel in nickel sulfonium raw material is used as a reducing agent and tetravalent manganese in nickel hydroxide is used as an oxidant to avoid additional reducing agents or oxidants, so as to achieve Coordinated leaching of nickel.
It significantly reduces the cost of auxiliary materials, reduces the introduction of impurities and ions, and increases the production capacity of the nickel sulfonium raw material leaching system, short reaction time, high safety, and improves efficiency by 100-200%.
Smart Images

Figure BDA0004234829670000061 
Figure BDA0004234829670000062 
Figure BDA0004234829670000071
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of hydrometallurgy, and in particular to a method for leaching nickel elements and a method for preparing nickel sulfate. Background Art
[0002] With the rapid development of the new energy industry, lithium-ion batteries are widely used in electric vehicle battery components due to their high energy density and other characteristics. As the main component of electric vehicle batteries, positive electrode materials play a core role in the internal charging and discharging of batteries. Among them, nickel metal, as the main core element of positive electrode materials, plays a role in improving the energy density of batteries, and nickel sulfate is the raw material for preparing positive electrode materials.
[0003] At present, the mainstream raw materials for preparing battery-grade nickel sulfate are electrolytic nickel, nickel cobalt hydroxide raw materials (abbreviated as: MHP) and high matte nickel. Among them, the mainstream process for preparing battery-grade nickel sulfate from electrolytic nickel is the leaching-iron removal process. This method has a short process flow and small equipment investment. It is the main method for preparing battery-grade nickel sulfate in the past. However, with the rapid development of new energy, the price of electrolytic nickel has risen sharply, resulting in the problem of high cost of this process. The mainstream process for preparing battery-grade nickel sulfate from MHP is the leaching-iron removal-extraction and impurity removal process. This method has stable raw materials and short reaction time. It is an important method for preparing battery-grade nickel sulfate at present. However, the leaching process of this method consumes a large amount of reducing agent, and there is a risk of introducing sodium into the system, resulting in increased crystallization costs. The mainstream process for preparing battery-grade nickel sulfate from high matte nickel is the atmospheric pressure oxygen leaching-pressure leaching-extraction and impurity removal process. This method has a high nickel content in the raw materials, low transportation cost per ton of nickel and low slag volume. It is also an important method for preparing battery-grade nickel sulfate at present, but this method has high equipment requirements and large initial capital investment. Summary of the invention
[0004] The purpose of the present application is to provide a method for leaching nickel and a method for preparing nickel sulfate, aiming to solve the problems of large reducing agent consumption, high equipment requirements and large capital investment in the existing nickel leaching process and nickel sulfate preparation method.
[0005] To achieve the above objectives, the present application provides a method for leaching nickel, comprising:
[0006] Primary leaching: The nickel cobalt hydroxide raw material and the nickel matte raw material are synergistically leached under acidic conditions to obtain a leached solution.
[0007] The nickel-cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide and manganese dioxide; the nickel matte raw material contains nickel element.
[0008] Nickel cobalt hydroxide raw material (also referred to as nickel cobalt hydroxide by technicians in the field; English abbreviation: MHP) is a nickel smelting intermediate, belonging to nickel hydrometallurgy intermediate, and the production method is mainly laterite nickel ore pressure leaching-magnesium oxide nickel precipitation process. The main elements of the prepared nickel intermediate are nickel, cobalt, manganese and magnesium, among which nickel, cobalt and manganese mainly exist in the form of hydroxide and oxide. Copper may be contained in some laterite nickel ores.
[0009] Nickel matte raw material is also called nickel matte, which is a mixture of nickel, cobalt, iron and other metals and their sulfides, and is a kind of nickel pyrometallurgical intermediate product. Nickel matte raw materials with higher nickel content are usually called high nickel matte. The nickel content (dry basis) of high nickel matte is usually more than 50%, such as 50%-80%, preferably 55%-80%, more preferably 60%-80%, and can also be 65%-70%, 70%-75%, 65%-75%, etc.
[0010] In certain embodiments, the high nickel matte production process is to obtain low nickel matte with high iron and sulfur contents by smelting laterite nickel ore raw material through pyrometallurgical method, and the low nickel matte is blown in a converter to obtain high nickel matte with high nickel content and low iron and sulfur contents.
[0011] In the prior art, in the nickel leaching system of nickel cobalt hydroxide raw materials, additional reducing agents need to be added, which makes the auxiliary material cost high, and also introduces other impurity ions, increasing the subsequent impurity removal cost. In the prior art high-matte nickel leaching system, an oxygen pressure leaching process is usually used, which requires a large amount of oxygen as an oxidant, and hydrogen is generated during the leaching process.
[0012] The present application scheme uses nickel-cobalt hydroxide raw material and nickel matte raw material as leaching raw materials, so that when the nickel-cobalt hydroxide raw material is leached, the elemental nickel in the nickel matte raw material can be used as a reducing agent, and when the nickel matte raw material is leached, the tetravalent manganese in the nickel-cobalt hydroxide raw material can be used as an oxidant, thereby eliminating the need to add additional reducing agents or oxidizing agents as auxiliary materials, and nickel can be directly leached in a coordinated manner.
[0013] Preferably, the dry basis content of Mn in the nickel cobalt hydroxide raw material is 1% to 10%, preferably 1.5% to 8%; for example, it can be 1.5% to 4%, or 4% to 6%, or 5% to 10%, preferably, the dry basis content of Mn in nickel cobalt hydroxide is 5% to 10%; the dry basis content of elemental nickel in the nickel matte raw material is 5% to 25%, for example, it can be 5% to 10%, or 10% to 15%, or 15% to 20%, or 20% to 25%, or 15% to 25%; preferably, the dry basis content of elemental nickel in the nickel matte raw material is 15% to 25%. Preferably, the nickel matte raw material is high matte nickel.
[0014] In some embodiments, the dry basis content of Co in nickel cobalt hydroxide is 2% to 3%, for example, 2% to 2.4%, or 2.4% to 2.6%, or 2.6% to 3%; the dry basis content of Ni in nickel cobalt hydroxide is 30% to 40%, for example, 30% to 35%, or 35% to 37%, or 37% to 40%.
[0015] In some embodiments, the dry basis content of iron in the nickel matte raw material is 2% to 5%, for example, 2% to 3%, or 3% to 4%, or 4% to 5%; the dry basis content of Co in the nickel matte raw material is 0.5% to 2%, for example, 0.5% to 0.7%, or 0.7% to 0.8%, or 0.8% to 1%, or 1% to 1.5%, or 1.5% to 2%.
[0016] Preferably, the mass ratio of the nickel cobalt hydroxide raw material to the nickel matte raw material is 1:(0.01-0.09); for example, it can be 1:(0.015, 0.02, 0.025, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08 or 0.09), preferably 1:0.015-0.05, and more preferably 1:0.015-0.03.
[0017] Preferably, a certain amount of water needs to be added during the primary leaching, and the amount of water added during the primary leaching is appropriate to ensure that the leached nickel element (such as nickel sulfate) is not precipitated. The solid-liquid ratio of the nickel cobalt hydroxide and water is 1g: (1.5-3)mL, for example, 1g: 1.5mL, or 1g: 2mL, or 1g: 3mL.
[0018] Those skilled in the art may conceive of first diluting a mixture of water and sulfuric acid and then performing leaching; or directly using a diluted acid solution.
[0019] The application scheme only requires the mixed leaching of MHP and nickel matte raw materials, without other complicated operations, and is highly feasible.
[0020] Preferably, the temperature of the primary leaching is 85-100°C, for example, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C or 100°C.
[0021] Preferably, the pH of the primary leaching is 1.0-2.0, for example, 1.0, 1.5 or 2.0, and the leaching time is 2-6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.
[0022] Preferably, before obtaining the post-leaching liquid, the process also includes: solid-liquid separation to obtain the post-leaching liquid and leaching residue; the method also includes adjusting the pH of the leaching residue with acid solution and pouring it into a pressure autoclave for pressure leaching to obtain a pressurized leaching liquid, and returning the pressurized leaching liquid for use in a first leaching. Further pressurizing the leaching residue after stirring leaching can increase the leaching rate of nickel. The leaching residue is used as the raw material for the pressurized leaching process of the nickel matte raw material system. The nickel content of the leaching residue is lower, which can significantly reduce the pressurized leaching reaction time and increase the production capacity of the nickel matte raw material system.
[0023] Preferably, the leached residue is adjusted to pH 1.5-2.0 with acid solution and then poured into a pressure autoclave for pressure leaching. Usually, the pressure leaching is performed after the pH is stabilized in the above range for 0.5-1.5 hours.
[0024] Preferably, the pressure leaching temperature is 160-180°C, for example, 160°C, 165°C, 170°C, 175°C or 180°C, the oxygen partial pressure is 0.6-1.0Mpa, for example, 0.6Mpa, 0.7Mpa, 0.8Mpa, 0.9Mpa or 1.0Mpa, and the time is 4-7h, for example, 4h, 5h, 6h or 7h.
[0025] Usually, the oxygen partial pressure during oxygen pressure leaching is relatively high, reaching more than 1.0 MPa. The leached residue after one leaching of the present invention can be leached at a lower oxygen partial pressure, and the oxygen partial pressure is preferably 0.6-0.9 MPa, and more preferably 0.6-0.8 MPa.
[0026] Compared with the leaching and iron removal process of the nickel matte raw material system, the single leaching process of the present application has a shorter reaction time and an efficiency improvement of 100-200%. In addition, the reaction process of this scheme is milder, does not require the introduction of oxygen, does not produce hydrogen, and is safer.
[0027] The present application also provides a method for preparing nickel sulfate, including the above-mentioned method for leaching nickel elements.
[0028] Preferably, the method further comprises:
[0029] Iron removal: hydrogen peroxide is added to the leached liquid to remove iron, and the solid-liquid separation is performed to obtain iron-removed liquid and iron-removed slag. The iron-removed liquid can also enter the subsequent extraction system for further impurity removal.
[0030] Preferably, the molar ratio of the ferrous iron content in the leached liquid to the hydrogen peroxide content in the added hydrogen peroxide is controlled to be 1:(1.5-3.0), for example, it can be 1:1.5, or 1:2.0, or 1:2.5, or 1:3.0.
[0031] Preferably, after stirring, the pH is adjusted to 3.5-4.5, for example, 3.5, 4.0 or 4.5, and then solid-liquid separation is performed to obtain deironing liquid and deironing slag. Preferably, the pH is stabilized at 3.5-4.5 for 1-2 hours, and then solid-liquid separation is performed.
[0032] Compared with the prior art, the beneficial effects of this application include:
[0033] The method for leaching nickel element provided by the present application uses nickel cobalt hydroxide raw material and nickel matte raw material as leaching raw materials, so that when the nickel cobalt hydroxide raw material is leached, the elemental nickel in the nickel matte raw material is used as a reducing agent, and when the nickel matte raw material is leached, the manganese in the nickel cobalt hydroxide raw material is used as an oxidant, so that no additional reducing agent or oxidant is required, which significantly reduces the auxiliary material cost of the MHP leaching process. Compared with other processes, the introduction of impurity ions (such as sodium ions) in the system is reduced, and the evaporation cost is reduced; and the oxygen and equipment investment costs of the nickel matte raw material leaching process are also reduced. The leaching process time is short, which greatly improves the production capacity of the nickel matte raw material leaching system, and the reaction process does not require the introduction of oxygen, and the reaction process does not produce hydrogen, and the reaction is more gentle and safe.
[0034] This method not only solves the problems of large reductant consumption and high sodium introduction in the MHP leaching process in the prior art, but also solves the problems of long leaching time and low leaching efficiency in the atmospheric pressure leaching process of high-grade nickel matte, and reduces oxygen consumption. This method does not require the addition of reductant and oxidant auxiliary materials, and the auxiliary material cost is extremely low; it is simple to operate, the reaction process is mild, and the safety and feasibility are higher; compared with the leaching and iron removal process of the high-grade nickel matte system, this scheme has a shorter reaction time for one leaching, an efficiency increase of 100% to 200%, and an excellent overall effect. DETAILED DESCRIPTION
[0035] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0036] In the present invention, "and / or" is used to indicate that one or both of the described situations may occur. For example, A and / or B includes (A and B) and (A or B).
[0037] In the present invention, "nickel cobalt hydroxide raw material" is sometimes referred to as nickel cobalt hydroxide or MHP, which have the same meaning. In the present invention, unless otherwise specified, the percentage content refers to the mass percentage content.
[0038] In the present invention, "natural basis" refers to the natural state of the material (containing water), and "dry basis" refers to the state of the material after water is removed. For example, in material A in Table 1, the water content is 46.51%, which refers to the water content in the natural basis of material A; after drying material A, a dry basis is obtained, and the content of Ni element in the dry basis is 38.57%. Unless otherwise specified, the content of elements or components in the present invention refers to the dry basis content, that is, the content of elements or components after water is removed.
[0039] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0040] The elemental composition of the MHP raw material used in the present application is shown in Table 1, and further analysis of the chemical composition of the MHP raw material is shown in Table 2. The elemental composition of the high nickel matte raw material used is shown in Table 3, and further analysis of the chemical composition of the high nickel matte raw material is shown in Table 4.
[0041] Table 1 Elemental composition of MHP
[0042]
[0043] Note: Water content is natural basis content, and other ingredients in the table are dry basis content.
[0044] Table 2 Chemical composition of MHP
[0045]
[0046] Note: Water content is natural basis content, and other ingredients in the table are dry basis content.
[0047] Table 3 Element composition of nickel matte
[0048]
[0049] Note: Water content is natural basis content, and other ingredients in the table are dry basis content.
[0050] Table 4 Chemical composition of nickel matte
[0051]
[0052] Note: Water content is natural basis content, and other ingredients in the table are dry basis content.
[0053] Example 1
[0054] (1) First, take 600 g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0055] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker, add 800mL of pure water at a liquid-to-solid ratio of 2:1 and start stirring, set the temperature to 95°C, and add 10g of sample 3 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours; after the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high nickel matte nickel leaching rate is greater than 65%, the slag rate is 4.51%, and the Ni, Co and Mn contents in the leached liquid are 125.45g / L, 4.89g / L and 5.743g / L respectively, and the Fe, Al and Si contents are 245mg / L, 125mg / L and 114mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leached slag are 37.74%, 0.15%, 0.04%, 2.41% and 20.82% respectively.
[0056] (3) Take 1L of the leached liquid obtained in step (2) and put it in a 2L beaker, set the temperature to room temperature; add 0.36mL of hydrogen peroxide (the molar coefficient ratio of divalent iron to hydrogen peroxide in the leached liquid is 1:2.0) and mix and stir for 10 minutes. After the stirring is completed, add a certain amount of calcium powder to adjust the pH to 4.5. After the pH is stable for 1 to 2 hours, separate the solid and liquid to obtain the iron-removing liquid and iron-removing slag. The iron-removing liquid enters the subsequent extraction system, and the iron-removing slag is washed and scrapped. The Fe and Al in the iron-removing liquid are reduced to less than 1 mg / L.
[0057] (4) Take 24g of the leached residue obtained in step (2) in a 1L beaker, add a certain amount of sulfuric acid to adjust the pH to 2.0, and pour it into a pressure autoclave after stabilization for 1h. The temperature is set to 160°C, the oxygen partial pressure is set to 0.8Mpa, and after reacting for 6h, solid-liquid separation is performed to obtain a pressurized leaching liquid and a pressurized leaching residue. The pressurized leaching liquid enters the previous process step (2) as a solution, and the pressurized leaching residue is treated in the hematite leaching treatment method. The Ni and Fe in the pressurized leaching liquid are 117g / L and 0.12g / L, respectively, and the dry basis contents of nickel and iron in the pressurized leaching residue are 4.32% and 49.44%, respectively.
[0058] Example 2
[0059] (1) First, take 600 g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0060] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker, add 800mL of pure water at a liquid-to-solid ratio of 2:1 and start stirring, set the temperature to 95°C, and add 10g of sample 3 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours; after the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high nickel matte nickel leaching rate is greater than 68%, the slag rate is 3.15%, and the Ni, Co and Mn contents in the leached liquid are 131.24g / L, 3.94g / L and 9.147g / L respectively, and the Fe, Al and Si contents are 382mg / L, 119mg / L and 130mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leached slag are 35.45%, 0.24%, 0.08%, 2.05% and 21.42% respectively.
[0061] (3) Take 1L of the leached liquid obtained in step (2) and put it in a 2L beaker, set the temperature to room temperature; add 0.36mL of hydrogen peroxide (the molar coefficient ratio of divalent iron to hydrogen peroxide in the leached liquid is 1:1.5) and mix and stir for 10 minutes. After the stirring is completed, add a certain amount of calcium powder to adjust the pH to 4.5. After the pH is stable for 1 to 2 hours, separate the solid and liquid to obtain the iron-removing liquid and iron-removing slag. The iron-removing liquid enters the subsequent extraction system, and the iron-removing slag is washed and scrapped. The Fe and Al in the iron-removing liquid are reduced to less than 1 mg / L.
[0062] (4) Take 24g of the leached residue obtained in step (2) in a 1L beaker, add a certain amount of sulfuric acid to adjust the pH to 2.0, and pour it into a pressure autoclave after stabilization for 1h. The temperature is set to 160°C, the oxygen partial pressure is set to 0.8Mpa, and after reacting for 6h, solid-liquid separation is performed to obtain a pressurized leaching liquid and a pressurized leaching residue. The pressurized leaching liquid enters the previous process step (2) as a solution, and the pressurized leaching residue is treated in the hematite leaching treatment method. The Ni and Fe in the pressurized leaching liquid are 117g / L and 0.12g / L, respectively, and the dry basis contents of nickel and Fe in the pressurized leaching residue are 4.32% and 49.44%, respectively.
[0063] Example 3
[0064] (1) First, take 600 g of MHP powder of material C into a crusher and start stirring and crushing for 10 minutes to obtain MHP powder.
[0065] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker, add 800mL of pure water at a liquid-to-solid ratio of 2:1 and start stirring, set the temperature to 95°C, and add 10g of sample 3 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours; after the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high nickel matte nickel leaching rate is greater than 70%, the slag rate is 2.94%, and the Ni, Co and Mn contents in the leached liquid are 134.11g / L, 4.86g / L and 11.52g / L respectively, and the Fe, Al and Si contents are 308.86mg / L, 162.24mg / L and 237.35mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leached slag are 41.33%, 0.03%, 0.04%, 2.68% and 15.54% respectively.
[0066] (3) Take 1L of the leached liquid obtained in step (2) and put it in a 2L beaker, set the temperature to room temperature; add 0.48mL of hydrogen peroxide (the molar coefficient ratio of divalent iron to hydrogen peroxide in the leached liquid is 1:2.6) and mix and stir for 10 minutes. After the stirring is completed, add a certain amount of calcium powder to adjust the pH to 4.5. After the pH is stable for 1 to 2 hours, separate the solid and liquid to obtain the iron-removing liquid and iron-removing slag. The iron-removing liquid enters the subsequent extraction system, and the iron-removing slag is washed and scrapped. The Fe and Al in the iron-removing liquid are reduced to less than 1 mg / L.
[0067] (4) Take 20g of the leached residue obtained in step (2) in a 1L beaker, add a certain amount of sulfuric acid to adjust the pH to 2.0, and pour it into a pressure autoclave after stabilization for 1h. The temperature is set to 180°C, the oxygen partial pressure is set to 0.7Mpa, and after reacting for 6h, solid-liquid separation is performed to obtain a pressurized leaching solution and a pressurized leaching residue. The pressurized leaching solution enters the previous process step (2) as a solution, and the pressurized leaching residue is treated in the same manner as hematite leaching. The Ni and Fe in the pressurized leaching solution are 123.06g / L and 0.26g / L, respectively, and the dry basis contents of nickel and iron in the leached residue are 3.38% and 58.87%, respectively.
[0068] Example 4
[0069] (1) First, take 600 g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0070] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker, add 800mL of pure water at a liquid-to-solid ratio of 2:1 and start stirring, set the temperature to 95°C, and add 32g of sample 1 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours; after the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high nickel matte nickel leaching rate is greater than 55%, the slag rate is 10.17%, and the Ni, Co and Mn contents in the leached liquid are 101.09g / L, 3.57g / L and 8.693g / L respectively, and the Fe, Al and Si contents are 396.7mg / L, 250.66mg / L and 270.7mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leached slag are 48.33%, 0.07%, 0.05%, 3.68% and 20.54% respectively.
[0071] Example 5
[0072] (1) First, take 600 g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0073] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker, add 800mL of pure water at a liquid-to-solid ratio of 2:1 and start stirring, set the temperature to 95°C, and add 15.2g of sample 2 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours; after the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high nickel matte nickel leaching rate is greater than 60%, the slag rate is 8.71%, the Ni, Co and Mn contents in the leachate are 112.79g / L, 1.77g / L and 8.347g / L respectively, and the Fe, Al and Si contents are 276.7mg / L, 140.6mg / L and 230.9mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leaching slag are 42.73%, 0.07%, 0.05%, 2.96% and 18.54% respectively.
[0074] Example 6
[0075] (1) First, take 600 g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0076] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker, add 800mL of pure water at a liquid-to-solid ratio of 2:1 and start stirring, set the temperature to 95°C, and add 7.75g of sample 4 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours; after the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high matte nickel leaching rate is greater than 70%, the slag rate is 3.47%, the Ni, Co and Mn contents in the leachate are 128.47g / L, 2.44g / L and 8.783g / L respectively, and the Fe, Al and Si contents are 206.7mg / L, 140.6mg / L and 360.7mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leaching slag are 25.77%, 0.07%, 0.04%, 2.08% and 18.94% respectively.
[0077] Comparative Example 1
[0078] (1) First, take 600 g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0079] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1 and stirring was started. The temperature was set to 95 ° C. After reaching the reaction temperature, 317 mL of hydrogen peroxide and a certain amount of sulfuric acid were slowly added to maintain the pH at 1.5. The addition time was 3 h and the pH stabilization time was 2 h. After the time was reached, solid-liquid separation was performed to obtain the leached liquid and leached residue. The MHP nickel leaching rate is 99%, the slag rate is 1.04%, the Ni, Co and Mn contents in the leaching solution are 102g / L, 1.02g / L and 5.52g / L respectively, and the Fe, Al and Si contents are 115.3mg / L, 104.6mg / L and 65.12mg / L respectively; the dry basis contents of Ni, Co, Mn and Fe in the leached slag are 2.65%, 0.04%, 0.025% and 0.59% respectively, among which the hydrogen peroxide consumption is about 7.21 times of the theoretical amount, and the cost of auxiliary materials is high.
[0080] Comparative Example 2
[0081] (1) First, take 600 g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0082] (2) Take 400g of the MHP powder obtained in step (1) in a 1L beaker, add 1000mL of pure water at a liquid-solid ratio of 2.5:1 and start stirring, set the temperature to 95°C, and after reaching the reaction temperature, slowly add 31.86g of sodium pyrosulfite and a certain amount of sulfuric acid to maintain the pH at 1.5, the addition time is 3h, and the pH stabilization time is 2h; after reaching the time, solid-liquid separation is performed to obtain the leached liquid and leached residue. The MHP nickel leaching rate is 99%, the residue rate is 1.14%, the Ni, Co, and Mn contents in the leaching liquid are 104g / L, 1.12g / L, and 4.89g / L, respectively, and the Fe, Al, Si, and Na contents are 125.2mg / L, 126.6mg / L, 61.12mg / L, and 7712mg / L, respectively; the dry basis contents of Ni, Co, Mn, and Fe in the leached residue are 2.65%, 0.04%, 0.025%, and 0.59%, respectively. The sodium content in the leachate is high, and the subsequent evaporation and crystallization pressure is high.
[0083] Comparative Example 3
[0084] (1) First, take 600 g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0085] (2) Take 400g of the MHP powder obtained in step (1) in a 1L beaker, add 1000mL of pure water at a liquid-solid ratio of 2.5:1 and start stirring, set the temperature to 95°C, and after reaching the reaction temperature, add 22g of nickel sulfide powder and a certain amount of sulfuric acid to maintain the pH at 1.5, and the reaction time is 4h; after reaching the time, solid-liquid separation is performed to obtain a leachate and a leach residue. The MHP nickel leaching rate is only 92%, the slag rate is 22.45%, the Ni, Co, and Mn contents in the leachate are 98.21g / L, 0.82g / L, and 1.19g / L, respectively, and the Fe, Al, and Si contents are 109.2mg / L, 229.6mg / L, and 54.12mg / L, respectively; the dry basis contents of Ni, Co, Mn, Fe, and S in the leach residue are 11.54%, 0.18%, 6.5%, 1.59%, and 34.47%, respectively. Nickel sulfide powder is not very effective as a reducing agent and has a low leaching rate.
[0086] Comparative Example 4
[0087] (1) First, take 600 g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0088] (2) Take 400g of the MHP powder obtained in step (1) in a 1L beaker, add 1000mL of pure water at a liquid-solid ratio of 2.5:1 and start stirring, set the temperature to 95°C, and after reaching the reaction temperature, add 23g of nickel cobalt sulfide powder and a certain amount of sulfuric acid to maintain the pH at 1.5, and the reaction time is 4h; after reaching the time, solid-liquid separation is performed to obtain leached liquid and leached residue. The MHP nickel leaching rate is only 92%, the residue rate is 22.85%, the Ni, Co, and Mn contents in the leaching liquid are 99.21g / L, 0.92g / L, and 1.39g / L, respectively, and the Fe, Al, and Si contents are 165.2mg / L, 119.6mg / L, and 65.12mg / L, respectively; the dry basis contents of Ni, Co, Mn, Fe, and S in the leached residue are 7.47%, 4.81%, 6.25%, 1.78%, and 36.47%, respectively. The effect of nickel cobalt sulfide powder as a reducing agent is not obvious and the leaching rate is low.
[0089] Comparative Example 5
[0090] (1) First, take 600 g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0091] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1 and stirring was started. The temperature was set to 95 ° C. and 8 g of metal nickel powder was added. After reaching the reaction temperature, a certain amount of sulfuric acid was added to maintain the pH at 1.5. The reaction time was 4 h. After the reaction time was reached, solid-liquid separation was performed to obtain a leached liquid and a leached residue. The MHP nickel leaching rate is greater than 99%, the metal nickel leaching rate is greater than 98%, and the slag rate is only 0.85%. The contents of Ni, Co, and Mn in the leaching solution are 128g / L, 3.58g / L, and 4.35g / L, respectively, and the contents of Fe, Al, and Si are 109.8mg / L, 124.87mg / L, and 48.16mg / L, respectively; the dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 31.42%, 0.034%, 0.0422%, 0.54%, and 0.004%, respectively. Metal nickel has good leaching effect and high efficiency as a reducing agent, but the cost of metal nickel powder is extremely high.
[0092] Comparative Example 6
[0093] (1) First, take 600 g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.
[0094] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1 and stirring was started. The temperature was set to 95 ° C. and 12 g of nickel-iron alloy powder was added. After reaching the reaction temperature, a certain amount of sulfuric acid was added to maintain the pH at 1.5. The reaction time was 4 h. After the reaction time was reached, solid-liquid separation was performed to obtain a leached liquid and a leached residue. The nickel leaching rate of MHP is greater than 99%, the nickel leaching rate of nickel-iron alloy is greater than 75%, the slag rate is 2.85%, the Ni, Co, and Mn contents in the leachate are 123g / L, 3.23g / L, and 4.62g / L, respectively, and the Fe, Al, and Si contents are 4587mg / L, 104.78mg / L, and 55.34mg / L, respectively; the dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 35.32%, 0.004%, 0.02%, 45.45%, and 0.004%, respectively. Nickel-iron alloy has a certain leaching effect as a reducing agent, but it will increase the iron content in the leachate.
[0095] Comparative Example 7
[0096] (1) First, take 1000g of sample 3 high-grade nickel matte in a 10L beaker, add 5L of water at a liquid-solid mass ratio of 5:1, set the temperature to 65°C, and after reaching the reaction temperature, add 333mL of sulfuric acid, and continue to introduce oxygen. After the reaction reaches a pH value of 5.0, solid-liquid separation begins and atmospheric pressure leaching residue and atmospheric pressure leaching liquid are obtained. The process reaction time is 10h, the high-grade nickel matte leaching rate is 45%, and the Ni content in the atmospheric pressure leaching liquid is 90.58g / L.
[0097] (2) Take the atmospheric leaching residue in a 3L pressure autoclave, add 2L water and 50mL sulfuric acid and stir. After stirring for 1 hour, seal the autoclave and set the temperature in the autoclave to 200°C. After reaching the set temperature, introduce oxygen into the autoclave until the oxygen partial pressure is 1.0Mpa and react for 6 hours. After the reaction, pressure leaching residue and pressure leaching liquid are obtained. The residue rate is about 3.5%. The main components of the residue are iron and nickel, with dry basis contents of 52.1% and 3.2%, respectively, and the contents of various impurities are all less than 0.01%. In the conventional leaching process of high-matte nickel, the atmospheric pressure oxygen leaching stage has a long reaction time, a large oxygen consumption, and high requirements for leaching conditions in the pressure leaching stage.
[0098] The schemes and leaching results of the various embodiments and comparative examples are shown in Table 5. According to Table 5, it can be seen that Examples 1 to 6 of the scheme of the present application use both nickel cobalt hydroxide and nickel matte as leaching raw materials, which can improve the nickel leaching rate of nickel cobalt hydroxide and the nickel leaching rate of nickel matte, and the method is low in cost and does not introduce other impurities. It not only solves the problems of large reducing agent consumption and high sodium introduction in the MHP leaching process in the prior art, but also solves the problems of long leaching time and low leaching efficiency in the atmospheric pressure leaching process of nickel matte, and reduces oxygen consumption. In addition, according to Examples 2 and Examples 4-6, the higher the elemental nickel content of the nickel matte, the higher the nickel leaching rate of the nickel matte, and the higher the liquid nickel content after leaching.
[0099] Table 5 Schemes and leaching results of various embodiments and comparative examples
[0100]
[0101] Note: In Table 5, when both the oxidant and the reductant contain nickel, the nickel leaching rates of MHP and high-grade nickel matte are estimated values, because there are great differences in the morphology of the leached residues of MHP and high-grade nickel matte. The MHP leaching rate greater than 99% means that MHP has been completely dissolved and there is no leached residue.
[0102] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0103] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for leaching nickel, It is characterized in that include: Primary leaching: co-leaching of nickel cobalt hydroxide raw material and nickel matte raw material under acidic conditions to obtain leached liquid; The nickel-cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide and manganese dioxide; the nickel matte raw material contains nickel element.
2. The method for leaching nickel according to claim 1, It is characterized in that The dry content of manganese dioxide in the nickel-cobalt hydroxide raw material is 1% to 10%; and / or the dry content of elemental nickel in the nickel matte raw material is 5% to 25%; Preferably, the nickel matte raw material is high-grade nickel matte.
3. The method for leaching nickel according to claim 1 or 2, It is characterized in that The mass ratio of the nickel cobalt hydroxide raw material to the nickel matte raw material is 1:(0.01-0.09); Preferably, water is added during the primary leaching, and the solid-liquid ratio of the nickel cobalt hydroxide raw material to water is 1 g: (1.5-3) mL; Preferably, the acidic conditions of the primary leaching are: pH is controlled at 1.0 to 2.0; Preferably, the primary leaching temperature is 85-100° C. and the time is 2-6 hours.
4. The method for leaching nickel according to claim 1, It is characterized in that Before the primary leaching to obtain the leached liquid, the method further comprises: solid-liquid separation to obtain the leached liquid and leached residue; The method further comprises: Pressure leaching: The leaching residue is adjusted to pH with acid solution and then subjected to pressure leaching to obtain a pressure leaching solution.
5. The method for leaching nickel according to claim 4, It is characterized in that The leached residue is adjusted to pH 1.5-2.0 with acid solution and then leached under pressure.
6. The method for leaching nickel according to claim 4, It is characterized in that The pressure leaching temperature is 160-180° C., the oxygen partial pressure is 0.6-1.0 MPa, and the time is 4-7 hours.
7. A method for preparing nickel sulfate, It is characterized in that A method for leaching nickel elements comprising the method described in any one of claims 1 to 6.
8. The method for preparing nickel sulfate according to claim 7, It is characterized in that The method further comprises: Iron removal: adding hydrogen peroxide to the leached liquid to remove iron by stirring, and separating the solid and liquid to obtain iron-removed liquid and iron-removed slag.
9. The method for preparing nickel sulfate according to claim 8, It is characterized in that The molar ratio of the ferrous iron content in the leached solution to the hydrogen peroxide content in the added hydrogen peroxide is controlled to be 1:(1.5-3.0).
10. The method for preparing nickel sulfate according to claim 8, It is characterized in that After stirring, the pH is adjusted to 3.5-4.5, and then the solid-liquid separation is performed to obtain the iron-removed liquid and the iron-removed slag.
Citation Information
Cited By
Method for recovering nickel from nickel matte in sulfide form
JP2025542052A
Method for recovering nickel from nickel matte in sulfide form
JP7925977B2