Two-dimensional heterojunction transistor device capable of enhancing image contrast and preparation method thereof
By introducing gallium sulfide material into the tungsten sulfide field effect transistor to build a two-dimensional heterojunction structure, the problem of single function of the photoelectric field effect transistor device and difficulty in controlling defects is solved, and the modulation of the storage window size and image contrast are improved. It demonstrates nonvolatile storage characteristics and significant regulation of charge traps.
Patent Information
- Application Number
- CN202411229552.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
The existing photoelectric field effect transistor devices have single functions and lack effective control of field effect transistor defects, which limits its versatility and performance improvement in optoelectronics applications.
By introducing gallium sulfide material into tungsten sulfide field effect transistors, the interface performance is improved and the impact of carrier traps in silicon oxide is shielded, thereby expanding the storage window and using a two-dimensional heterostructure to build devices, including substrates and GaS thin layer, WS2 thin layer and gold electrode realize modulation of storage window size.
It effectively enhances image contrast, demonstrates non-volatile storage characteristics and significant charge trap regulation capabilities, and expands the application prospects of the device.
Smart Images

Figure CN119008762A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of photoelectric detectors, and in particular to a device of a two-dimensional heterojunction transistor capable of enhancing image contrast and a preparation method thereof, wherein gallium sulfide material is introduced into a tungsten sulfide field effect transistor to improve interface performance and shield the influence of carrier traps in silicon oxide, thereby expanding its storage window. Background Art
[0002] Field effect transistors use electric fields to control the transport of charge, and their basic structure includes source, gate and drain. By applying voltage to the gate, field effect transistors can control the flow of current, thereby changing the conductivity between the drain and source. This voltage control characteristic makes it widely used in electronic devices, especially at low frequencies, and its high input impedance characteristic makes it an ideal signal processing element. As an external field regulation, photoelectric field coupling regulation field effect transistors are cutting-edge technologies in modern optoelectronics and microelectronics, and are widely used in military and civilian products. Traditional photoelectric field effect tubes are large in size, have strong interface effects, and require external cooling devices. Various factors limit their performance improvement. Currently, photoelectric field effect transistors are gradually developing towards lightweight, integrated, low power consumption, and low cost. Single-layer two-dimensional materials have atomic-level thickness, and their ultra-high specific surface area provides them with a strong quantum confinement effect, enhances multi-field coupling, and provides high light absorption efficiency. Moreover, the weak van der Waals force between the layers of two-dimensional materials facilitates the construction of homojunction / heterojunction, stacking of multi-dimensional materials, charge transport within the layer, and charge transfer between layers, ensuring the smooth progress of the whole chain research and development process of heterojunction photoelectric field effect transistors based on two-dimensional materials from material preparation to device characterization and performance optimization. Taking new two-dimensional semiconductor materials such as gallium-based and tungsten-based as examples, their band gaps cover the ultra-wide band of near-ultraviolet-visible-near-infrared, and can achieve different photoelectric responses under different wavelength conditions. However, the heterojunction photoelectric field effect transistor devices based on them have a single function, and current research lacks the regulation of the number of defects in field effect transistors, and has not achieved signal detection, identification, denoising and other multifunctionality on a single device, which seriously limits its application prospects in the next generation of optoelectronics. Designing a photoelectric field effect transistor that expands the scanning window of the transfer curve is of great significance and application value. Summary of the invention
[0003] The purpose of the present invention is to solve the above problems and provide a device of a two-dimensional heterojunction transistor that can realize storage window size modulation and enhance image contrast and a preparation method thereof;
[0004] A device of a two-dimensional heterojunction transistor capable of enhancing image contrast, comprising, from bottom to top, a substrate, a GaS thin layer, a WS2 thin layer, and a gold electrode;
[0005] The GaS thin layer is smaller in area than the WS2 thin layer;
[0006] The gold electrode comprises: a source electrode and a drain electrode;
[0007] The gold electrode channel size is 6 μm; the deposited layer is 50-80 nm;
[0008] The substrate is a silicon dioxide substrate.
[0009] A method for preparing a device of a two-dimensional heterojunction transistor capable of enhancing image contrast, comprising:
[0010] 1) Prepare two-dimensional GaS thin layers and WS2 thin layers by repeated pasting method;
[0011] 2) Transfer the GaS thin layer to the substrate, and then transfer the WS2 thin layer to the GaS thin layer;
[0012] 3) Use electron beam evaporation of gold electrodes on the GaS thin layer.
[0013] The device of the two-dimensional heterojunction transistor capable of enhancing image contrast is used in preparing field effect transistors.
[0014] A device of a two-dimensional heterojunction transistor capable of enhancing image contrast and a preparation method thereof, which comprises a substrate, a GaS thin layer, a WS2 thin layer, and a gold electrode from bottom to top. By introducing gallium sulfide material into a tungsten sulfide field effect transistor, the interface performance is improved, the influence of carrier traps in silicon oxide is shielded, and thus its storage window is expanded. Compared with WS2 FET, the storage window reduction phenomenon of WS2 / GaS FET shows a cumulative effect, indicating that the defect has non-volatile characteristics. After negative gate voltage treatment, the storage window area of WS2 / GaS FET will not return to the original state in a short time, indicating that the number of carriers has been accumulated, showing non-volatile storage characteristics. In a field effect transistor constructed with a heterostructure of tungsten sulfide (WS2) and gallium sulfide (GaS), the gate has a particularly significant effect on the regulation of the storage window size. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 is a flow chart of a method for preparing the device structure of the present invention;
[0016] Figure 2 The transfer curve of the thin-layer WS2 FET of the present invention after being treated with a 532 nm laser and a gate voltage of 40 V for a period of time and tested in a dark environment with a bias voltage of 0.5 V;
[0017] Figure 3The transfer curve of the thin-layer WS2 FET of the present invention after being treated with a 532 nm laser and a gate voltage of -40 V for a period of time and tested in a dark environment with a bias voltage of 0.5 V;
[0018] Figure 4 The time current (It) characteristic curve of the thin-layer WS2FET described in the present invention under a 532 nm laser with an optical power of 400 μW and a frequency of 0.5 Hz, with a fixed bias voltage of 0.1 V and a change in the gate voltage polarity, is found to have little difference;
[0019] Figure 5 The transfer curve of the WS2 / GaS FET of the present invention after being treated with a 532 nm laser and a gate voltage of 40 V for a period of time and tested in a dark environment with a bias voltage of 0.5 V;
[0020] Figure 6 The transfer curve of the thin-layer WS2 / GaS FET of the present invention after being treated with a 532 nm laser and a gate voltage of -40 V for a period of time and tested in a dark environment with a bias voltage of 0.5 V;
[0021] Figure 7 The time current (It) characteristic curve of the thin-layer WS2 / GaS FET described in the present invention under a 532 nm laser with an optical power of 400 μW and a frequency of 0.5 Hz, with a fixed bias voltage of 0.5 V and a variable gate voltage;
[0022] Figure 8 A comparison diagram of the transfer curve separation mechanism of the device of the present invention;
[0023] Fig. 9 Image detection in a 15×15 imaging array of WS2FET (left) and WS2 / GaS FET (right). DETAILED DESCRIPTION
[0024] Example 1 WS2 FET preparation and testing
[0025] 1. Please see Figure 1 , the preparation method of WS2 FET detector is as follows:
[0026] (1) Stripping of tungsten sulfide material: clamp the bulk material on the blue film tape, and gradually thin it by repeated sticking. Then remove the PDMS film protective film and directly stick it on the thinned material. Use the surface viscoelasticity of the PDMS film to remove the material. Repeat the above process and apply mechanical force multiple times to obtain a thinner layered structure. This process requires careful operation to avoid damaging the sample. Observe under a microscope and expect to obtain a thin layer of WS2;
[0027] (2) Transfer tungsten sulfide to the substrate: At this time, the material WS2 to be transferred adheres to PDMS (polydimethylsiloxane). Align the carrier with the material to the target substrate to ensure that the material is in the correct position. Use a mechanical device (such as a clamp) to apply pressure to transfer the material from the carrier to the target substrate. Once the material is transferred to the target substrate, use hot pressing to gradually increase the temperature from room temperature to 90°C (slowly heat every 10°C), then keep it at 90°C for 10 minutes to fix the position of the material on the substrate, and finally slowly lift the upper layer of PDMS glue to successfully transfer it to the substrate;
[0028] (3) Fabrication of gold electrodes: The pattern corresponding to the metal electrode is obtained by processes including spin coating of photoresist, UV exposure, and development. The channel size of the gold electrode is 6 μm. Electron beam evaporation is used to prepare a 50-80 nm gold electrode deposition layer. The excess gold is washed away with acetone and allowed to stand for 5 min, leaving only the preset gold electrode pattern on the silicon wafer. The residual acetone is then washed away with anhydrous ethanol. Finally, the treated electrode is soaked in deionized water and blown dry.
[0029] (4) Use PVA solution to spin-coat the metal electrode on the silicon wafer; use PDMS to adhere the gold electrode pattern on the PVA, soak it in deionized water for 20 min, wash off the residual PVA glue, and blow dry it with nitrogen.
[0030] 2. Performance test of WS2 FET detector
[0031] 1. Reduced defect window detection for WS2 FET
[0032] The device was subjected to voltage scanning test using MetaTest ScanPro 100 high-resolution, high-speed, multi-field coupled photoelectric scanning test system. During the test, the source-drain voltage (V ds ) is fixed at 0.5V, the gate voltage (Vg) is gradually increased from -40V to +50V, and then back to -40V, while recording the source-drain current (I ds ) change curve. Storage window (ΔV M ) through the maximum current and minimum current corresponding to the V on the transfer characteristic curve g A +40 V positive gate voltage was applied for 6 minutes to extract electrons from the WS2 channel and reduce the conductivity.
[0033] Attached Figure 2 The thin-film WS2 FET was shown to be able to withstand 532 nm laser light and 40 V gate voltage for 6 minutes. ds =0.5 V dark environment test transfer curve. The curve shows that after positive gate voltage treatment, the storage window ΔV MHowever, when tested for the second time 2 seconds later, the storage window quickly returned to its initial state.
[0034] 2. Expanded defect window detection for WS2 FET
[0035] The device is subjected to voltage scanning test by the same photoelectric scanning test system, where the source-drain voltage (V ds ) is fixed at 0.5V. During the test, the gate voltage (V g ) is gradually increased from -40 V to +50 V and then back to -40 V, while recording the source-drain current (I ds ). A negative gate voltage of -40V was applied for 6 minutes to inject electrons into the WS2 channel, increase conductivity, and allow electrons to be captured by vacancies in silicon oxide. The results showed that after 6 minutes of 532 nm laser treatment and -40V gate voltage treatment, the transfer curve of the WS2 FET in a dark state with a bias of 0.5 V showed an increase in the storage window.
[0036] Attached Figure 3 It is demonstrated that after a negative gate voltage treatment of -40 V, the memory window shows a trend of returning to the initial state in the second test 2 seconds later.
[0037] By analyzing Figure 2 and Figure 3 From the data, we observed that the memory window of the WS2 FET device was significantly reduced after being treated with a +40 V positive gate voltage and a 532 nm, 400 μW laser. On the contrary, when the device was simultaneously treated with a -40 V negative gate voltage and a 532 nm, 400 μW laser, the memory window showed an increasing trend. In addition, we also noticed a clockwise hysteresis loop in the transfer characteristic curve, which indicates the capture and release process of charge in the surface trap state, resulting in changes in device performance. The memory window (ΔV hys ) is defined as I ds = 1nA when the gate voltage (V g ) can be used to calculate the charge trap density (N) based on the hysteresis voltage window. t ):
[0038] ;
[0039] Among them C ox =1.18×10 −4 Fm –2 is the oxide (silicon oxide) capacitance per unit area between the channel and the bottom gate; ε0 is the vacuum dielectric constant, ε ox is the gate insulator dielectric constant, t ox is the gate insulator thickness and q is the electron charge.
[0040] .
[0041] 3. Image detection of WS2 FET time photocurrent function with changing gate voltage polarity
[0042] The device is tested using an optoelectronic scanning test system, where the source-drain voltage (V ds ) is fixed at 0.1V and pulse light is applied. By changing the gate voltage (V g ) polarity (±50 V) to monitor the photocurrent over time. A 532 nm laser light source with a pulse width of 0.5 Hz and an incident light power of 400 μW was used in the experiment. The device was exposed to the laser for testing, and the recorded photocurrent data was plotted against time to observe the trend of the photocurrent over time.
[0043] according to Figure 4 The results shown in the figure, the source-drain current time function curve of the WS2 FET under 532 nm laser irradiation, show that although the bias voltage remains unchanged at 0.1 V, the photocurrent differentiation is not significant after changing the gate voltage polarity. Although the gate voltage changes from -50 V to +50 V, a difference of 100 V, the difference in photocurrent is not obvious.
[0044] Example 2 WS2 / GaS FET preparation and performance testing
[0045] 1. Please refer to Figure 1 , the preparation method of WS2 / GaS FET detector is as follows:
[0046] (1) Substrate cleaning: Clean the silicon substrate with an in-situ thermal oxide layer of silicon dioxide on the surface with trichloroethylene, acetone, ethanol, deionized water, etc.;
[0047] (2) Stripping of gallium sulfide materials: clamp the bulk material on the blue film tape, and gradually thin it by repeated sticking. Then remove the PDMS film protective film and directly stick it on the thinned material. Use the surface viscoelasticity of the PDMS film to remove the material. Repeat the above process and apply mechanical force multiple times to obtain a thinner layered structure. This process requires careful operation to avoid damaging the sample. Observe under a microscope and expect to obtain a thin layer of GaS. The thin layer of GaS selected under the microscope is smaller in area than the thin layer of WS2.
[0048] (3) Transfer gallium sulfide to the substrate: At this time, the material GaS to be transferred adheres to PDMS (polydimethylsiloxane). Align the carrier with the material to the target substrate to ensure that the material is in the correct position. Use a mechanical device (such as a clamp) to apply pressure to transfer the material from the carrier to the target substrate. Once the material is transferred to the target substrate, use hot pressing to gradually increase the temperature from room temperature to 90°C (slowly heat every 10°C), then keep it at 90°C for 10 minutes to fix the position of the material on the substrate, and finally slowly lift the upper layer of PDMS glue to successfully transfer GaS to the substrate;
[0049] (4) Stripping and transfer of tungsten sulfide material: A thin layer of WS2 is obtained by the same method, and the above-mentioned transfer method is used to stack it in situ on a silicon substrate, and the thin layer of WS2 is placed vertically on the thin layer of GaS; and a second two-dimensional semiconductor top-gate transistor structure photoelectric detection device, a tungsten sulfide field effect transistor, is prepared, and WS2 is placed on a silicon substrate to facilitate comparison between the two.
[0050] (5) Fabrication of gold electrodes: The pattern corresponding to the metal electrode is obtained by processes including spin coating of photoresist, UV exposure, and development. The channel size of the gold electrode is 6 μm. Electron beam evaporation is used to prepare a 50-80 nm gold electrode deposition layer. The excess gold is washed away with acetone and allowed to stand for 5 min, leaving only the preset gold electrode pattern on the silicon wafer. The residual acetone is then washed away with anhydrous ethanol. Finally, the treated electrode is soaked in deionized water and blown dry.
[0051] (6) Preparation of polyvinyl alcohol (PVA) glue: Use an electronic balance to weigh 4 g of PVA and pour it into a sample bottle equipped with a stirrer. Then weigh 46 mL of secondary deionized water, mix the two and seal them. Heat on a hot plate at 100°C and 800 r / s for 5 h, then put it in an oven and heat it at 100°C for 1 h. Finally, heat it on the hot plate for another 1 h to make the solution uniform and transparent. The purpose of putting it in an oven here is to evenly heat the PVA solution so that the PVA is fully dissolved, and finally heat it on the hot plate again. The purpose is to make the solution concentration uniform.
[0052] (7) Use PVA solution to spin-coat the metal electrode on the silicon wafer; use PDMS to adhere the gold electrode pattern on the PVA, and then use the same transfer method to transfer the gold electrode on the PDMS to the WS2 / GaS vertical structure, soak it in deionized water for 20 min, wash off the residual PVA glue, and blow dry it with nitrogen.
[0053] 2. WS2 / GaS FET preparation and performance testing
[0054] 1. WS2 / GaS FET reduced storage window detection
[0055] The device is subjected to voltage scanning test by the photoelectric scanning test system, where the source-drain voltage (V ds ) is fixed at 0.5V. During the test, the gate voltage (V g ) was gradually increased from -40 V to +50 V, and then decreased back to -40 V, while recording the source-drain current (I ds ) versus Vg. During the test, a positive gate voltage of +40 V was applied to the device for a period of time to extract electrons from the WS2 channel, which then filled the vacancies in the bottom GaS material. As electrons are extracted, the number of free carriers in the WS2 channel decreases, resulting in a decrease in conductivity.
[0056] according to Figure 5 The results shown in the figure show that the WS2 / GaS FET was exposed to a 532 nm laser and subjected to a gate voltage of +40 V for 1 minute, 3 minutes, and 5 minutes. ds =0.5 V in a dark environment. The bias scan range in the test was from -40 V to +50 V, and then from +50 V back to -40 V. The results show that the storage window area decreases significantly with the increase of the positive gate voltage treatment time. Compared with WS2 FET, the storage window reduction phenomenon of WS2 / GaS FET shows an additive effect, indicating that the defect has non-volatile characteristics.
[0057] 2. WS2 / GaS FET Expanded Storage Window Detection
[0058] The device was subjected to voltage sweep test using the same test system as before, maintaining the source-drain voltage (V ds ) is constant at 0.5 V. During the test, the gate voltage (V g ) is gradually increased from -40 V to +50 V, and then reduced back to -40 V, while recording the source-drain current (I ds )With V g The curve of the change. During the application of a continuous negative gate voltage of -40 V, electrons in GaS are injected into the WS2 channel, increasing the number of free carriers and thus improving the conductivity. These injected electrons are captured and stored by vacancies in GaS. Even after the negative gate voltage is removed, the vacancies can still retain the captured electrons, thereby maintaining the high conductivity state of the WS2 channel.
[0059] according to Figure 6 The results shown in the figure show that the WS2 / GaS FET was exposed to a 532 nm laser and subjected to a -40 V gate voltage for 1 minute, 3 minutes, and 5 minutes, respectively. ds=0.5 V in a dark environment. The bias scan range in the test was from -40 V to +50 V, and then from +50 V back to -40 V. The results show that the defect window area increases significantly with the increase of negative gate voltage treatment time. Compared with WS2 FET, the storage window area of WS2 / GaS FET will not return to its original state in a short time after negative gate voltage treatment, indicating that the number of carriers has been accumulated, showing non-volatile storage characteristics.
[0060] Table 2: Comparison of charge trap density generated by two treatment methods in WS2 / GaS FET .
[0061] Based on the above experimental results, the following conclusions can be drawn: Through the analysis of Table 1 and Table 2, we have verified a rule that applying a positive gate voltage can reduce the density of charge traps, thereby reducing the storage window area; on the contrary, applying a negative gate voltage will introduce more charge traps and expand the storage window area. In addition, we also observed that by changing the polarity of the gate voltage, the number of charge traps can be effectively controlled. Especially in field effect transistors built with tungsten sulfide (WS2) and gallium sulfide (GaS) heterostructures, the gate has a particularly significant effect on the size of the storage window.
[0062] 3. Image detection of WS2 / GaS FET time photocurrent function with changing gate voltage polarity
[0063] The device is tested using an optoelectronic scanning test system, where the source-drain voltage (V ds ) is fixed at 0.1 V and pulse light is applied. g ) to monitor the photocurrent over time. The test uses a 532 nm laser light source with a pulse width of 0.5 Hz and an incident light power of 400 μW, and only the thin layer of the channel material WS2 of the device is exposed to the light source. The relationship between the photocurrent and time is recorded, and a graph is drawn to observe the trend of the photocurrent over time.
[0064] according to Figure 7 The results shown in the figure show that the photocurrent (It) characteristic curve of WS2 / GaS FET at a frequency of 0.5 Hz under 532 nm laser irradiation with an optical power of 400 μW shows that significant differences in photocurrent can be observed by changing the gate voltage under the condition of a fixed bias voltage of 0.1 V. This finding shows that compared with WS2 FET, the effect of gate regulation in WS2 / GaS heterojunction is more obvious, thus proving the significant effect of gate regulation in the heterojunction constructed by tungsten sulfide and gallium sulfide.
[0065] Table 3 Combination Figure 2 , Figure 3 , Figure 5 , Figure 6 Conclusion
[0066] Table 3: Comparison of WS2 FET and GaS / WS2 FET device parameters .
[0067] In this experiment, we first set the source-drain bias voltage (V ds ) was fixed at 0.5 V. Subsequently, a laser light source with a wavelength of 532 nm and an optical power of 400 μW was used to apply a fixed positive gate voltage (+40 V) and a negative gate voltage (-40 V) to the device, and each gate voltage condition was maintained for a certain period of time to fully affect the charge state of the device. After the treatment cycle, to ensure data accuracy, we scanned the transfer curve of the device in a completely dark environment. The scanning process covers the voltage range from -40 V to +50 V, and reverses from +50 V back to -40 V to accurately characterize the characteristics of the transfer window.
[0068] While scanning the transfer curve, we paid special attention to the situation when the gate voltage was +20 V, and recorded the dark current values obtained by forward scanning and reverse scanning at this voltage. In order to quantify the change in dark current, we obtained the change in dark current by accurately calculating the difference between the dark current values in the two scanning directions. This step not only ensures the repeatability of the data, but also provides an important basis for analyzing the charge dynamic behavior of the device under gate voltage regulation.
[0069] WS2 / GaS FET and WS2 FET with fixed gate voltage (V g = 20 V) Photocurrent detection
[0070] exist Figure 2 In the process, the gate voltage (V g ) from -40 V to 50 V. Select the circled line marked (40 V 6 min) and g =20 V, the photocurrent value is recorded, which represents the change in dark current under positive gate voltage treatment under 532 nm laser irradiation. Since the transfer curve is circular, there are two intersections at Vg=20 V, and the difference is the change, which is calculated to be 3.37×10 -9 A.
[0071] Likewise, in Figure 5 In the WS2 / GaS FET, the gate voltage (V g) from -40 V to 50 V. Read the circle marked (40 V 5 min) and g = 20 V, which reflects the change in dark current under positive gate voltage treatment under 532 nm laser irradiation. The ring feature of the curve is at V g =20 V, and the difference between them is taken as the variation. The calculated result is 1.30×10 -8 A. WS2 / GaS FET and WS2 FET with fixed gate voltage (V g = 20 V) photocurrent detection.
[0072] exist Figure 3 In the process, the gate voltage (V g ) from -40 V to 40 V. Select the circled line marked (-40 V 6 min) and record V g =20 V, which represents the change in dark current under negative gate voltage treatment under 532 nm laser irradiation. Since the transfer curve is circular, V g =20 V, there are two intersection points, and the difference is the change, which is calculated to be 4.1×10 -8 A.
[0073] Figure 6 Demonstrated WS2 / GaS FET performance in gate voltage (V g ) from -40 V to 50 V. Read the circle marked (-40 V 5 min) and g = 20 V, the photocurrent value is recorded, which reflects the change of dark current under negative gate voltage treatment under 532 nm laser irradiation. The ring feature of the curve is at V g =20 V, and the difference between them is taken as the variation. The calculated result is 6.59×10 -7 A.
[0074] Results Figure 8 :By introducing GaS, the interface performance is improved, the carrier traps in SiO2 are effectively shielded, the carrier mobility is increased and the hysteresis behavior is reduced. The existence of stable defect states in the middle band gap of GaS provides a good platform for studying the photoinduced doping effect. Under 532 nm laser irradiation, the carriers in WS2 are excited to achieve doping, and in the WS2 / GaS heterojunction, the photoinduced doping shows non-volatile characteristics.
[0075] Fig. 9 : Combined Figure 3 and Figure 6 Draw the application image
[0076] In the first figure, the WS2 FETs are arranged in a 15×15 array, with 19 cells directly exposed to light and the remaining 206 cells opaque to light. After the device was treated with a -50 V gate voltage, a 532 nm laser with a power of 400 μW was used to illuminate the device through a mask for five minutes. The dark current value obtained by the subsequent test in the dark state showed that the black cell current was 5.81×10 -9 A, the light gray part is 9.18×10 -9 A. The difference between the two is small, and the depth of color is used to reflect the difference in electrical current. Due to the small current difference, the color distinction is not obvious.
[0077] The second image shows a 15×15 array of WS2 / GaS FETs, again with 19 cells directly illuminated and 206 cells opaque. The device was also treated with a -50 V gate voltage and 400 μW 532nm laser irradiation for five minutes. The dark current value obtained in the dark state test shows that the black cell current is 8.91×10 -8 A, and the white part is 1.55×10 -6 A, there is a significant difference between the two, and the colors are clearly distinguished.
[0078] Example 3: Construction of bottom gate of field effect transistor
[0079] (1) Paste the copper conductive tape on a clean glass slide, and use conductive silver glue A to bond the device to the copper conductive glue tape B. Mix the conductive silver glue in a mass ratio of 10:1 (the mixing amount is not less than 0.55 g), and stir with a stirring rod for two to three minutes (including the colloid remaining on the stirring rod) until it is mixed evenly.
[0080] (2) Heat the entire device on a hot plate. The heating process is also an annealing process. Treat it at 90°C for one hour until the conductive silver glue is completely cured.
[0081] Field Effect Transistor Bottom Gate Testing Photoelectric characterization and data logging using WS2 FETs and WS2 / GaS FETs.
Claims
1. A two-dimensional heterojunction transistor device capable of enhancing image contrast, characterized in that: From bottom to top: substrate, GaS thin layer, WS2 thin layer, gold electrode.
2. The device of a two-dimensional heterojunction transistor capable of enhancing image contrast according to claim 1, characterized in that: The GaS thin layer has a smaller area than the WS2 thin layer.
3. The device of a two-dimensional heterojunction transistor capable of enhancing image contrast according to claim 2, characterized in that: The gold electrode comprises a source electrode and a drain electrode.
4. The device of a two-dimensional heterojunction transistor capable of enhancing image contrast according to claim 3, characterized in that: The gold electrode channel size is 6 μm; the deposition layer is 50-80 nm.
5. The device of a two-dimensional heterojunction transistor capable of enhancing image contrast according to claim 4, characterized in that: The substrate is a silicon dioxide substrate.
6. A method for preparing a two-dimensional heterojunction transistor device capable of enhancing image contrast, characterized in that : 1) Prepare two-dimensional GaS thin layers and WS2 thin layers by repeated pasting method; 2) Transfer the GaS thin layer to the substrate, and then transfer the WS2 thin layer to the GaS thin layer; 3) Use electron beam evaporation of gold electrodes on the GaS thin layer.
7. Use of the two-dimensional heterojunction transistor device capable of enhancing image contrast as claimed in claim 1 in the preparation of a field effect transistor.