Strong stray light absorption and anti-halation photoelectric glass and its preparation method and application

By optimizing the composition and process of glass composition, a high-efficiency light absorption layer is formed, which solves the problem of insufficient absorption of stray light performance of anti-halo photoelectric glass in the prior art, and achieves a balance of high transmittance and high cathode sensitivity, and has good results. chemical and mechanical properties.

CN118221350BActive Publication Date: 2024-11-22CNBM PHOTONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410409330.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-11-22
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

The existing anti-halo photoelectric glasses are difficult to meet the dual requirements of high transmittance and low light absorption layer transmission when absorbing stray light, and are prone to reduce cathode sensitivity and toxicity, affecting equipment performance.

Method used

The glass composition using SiO2, B2O3, Al2O3, alkali metal oxide, alkaline earth metal oxide, Bi2O3, PbO, CeO2 and Yb2O3 is formed by adjusting the component ratio and process processing to form an efficient light absorption layer to improve optical transmission. rate and cathode sensitivity while ensuring chemical stability and mechanical strength.

Benefits of technology

It has achieved transmittance in the wavelength range of 350-400nm, transmittance in the wavelength range of 400-1000nm, thickness of black light absorbing layer ≥0.6mm, average cathode sensitivity ≥850μA/lm, and good Chemical stability, thermal stability and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118221350B_ABST
    Figure CN118221350B_ABST
Patent Text Reader

Abstract

The present application provides a strong stray light absorption anti-halation photoelectric glass and its preparation method and application. The strong stray light absorption anti-halation photoelectric glass comprises a light-transmitting effective area, and the composition of the light-transmitting effective area is calculated by mass percentage, including: SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, alkali metal oxide 5.4-9%, alkaline earth metal oxide 2.3-5.2%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0-0.2%, CeO2 0.1-0.2% and Yb2O3 0-0.2%. The effective area of ​​the strong stray light absorption anti-halation photoelectric glass has excellent optical transmittance, and the light absorption area has good stray light elimination performance and high cathode sensitivity performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to optical glass materials, and in particular to a strong stray light absorption and anti-halation photoelectric glass, and a preparation method and application thereof. Background Art

[0002] Any discussion of the prior art throughout the specification should not be considered as an admission that such prior art is widely known or forms part of the common general knowledge in the field.

[0003] The anti-halation cathode glass window (AVG), as a key input window component of the second and third generation low-light night vision devices, undertakes the important task of improving the performance of the equipment. This glass window uses its high transmittance in the ultraviolet, visible and near-infrared spectrum to achieve wide-spectrum detection and observation capabilities. More importantly, through the self-substrate generation technology, a high-efficiency absorption layer is formed around the effective area of ​​the cathode glass window. This absorption layer can absorb more than 99.5% of the incident stray light, effectively eliminating the halo problem in low-light imaging, thereby greatly improving the cathode sensitivity, clarity and observation distance of the night vision device.

[0004] However, in the manufacturing process of anti-halation photoelectric glass, a major challenge is how to make a glass material that can effectively absorb stray light without damaging the performance of the device. Traditional methods, such as using Corning 7056 glass and some borosilicate glass, produce a black glass layer on the surface by heating it in a hydrogen environment. Although it can absorb stray light to a certain extent, the absorption effect produced by trace amounts of arsenic trioxide, antimony trioxide, halogen ions, and a small amount of heavy metal or precious metal element ions in these glass materials is often insufficient to meet actual requirements. This is because in order to fully absorb stray light and meet the requirements of use, not only a higher concentration of ions that can produce color centers or can be reduced is required, but the thickness of the black glass layer cannot be too thin.

[0005] Current solutions include the introduction of environmentally friendly oxides such as bismuth oxide, and the exploration of the use of precious metal elements such as palladium, tellurium, and rhodium. These methods aim to increase the thickness of the black glass layer on the surface after hydrogen treatment and reduce the light transmittance at a wavelength of 900nm to less than 5%. Nevertheless, the ions in the anti-halation input window glass are of various types and are easily poisoned by the multi-alkali photocathode reaction, which not only reduces the central transmittance, but also reduces the cathode sensitivity, which is usually only less than 800μA / lm. Therefore, although higher cathode sensitivity can be obtained to a certain extent by introducing variable valence environmentally friendly oxides, these solutions still find it difficult to meet the dual requirements of high effective area transmittance and low light absorption layer transmittance. Summary of the invention

[0006] Therefore, the purpose of this application is to provide an anti-halo photoelectric glass that can efficiently absorb stray light without damaging cathode sensitivity and equipment performance, and at the same time has good optical transmittance. The effective area of ​​the anti-halo photoelectric glass provided by the present invention has a transmittance of ≥90.2% in the wavelength range of 350-400nm, and a transmittance of ≥92.4% in the wavelength range of 400-1000nm; the thickness of the black light absorption layer is ≥0.6mm, the transmittance is 0 in the wavelength range of 350-800nm, and the transmittance is ≤1.8% in the wavelength range of 800-1000nm. The cathode sensitivity average is ≥850μA / lm, and it can also have good chemical stability, thermal stability and mechanical strength, good molding and processing performance, and excellent comprehensive performance.

[0007] Specifically, the present invention provides the following technical features, and the combination of one or more of the following technical features constitutes the technical solution of the present invention.

[0008] In a first aspect of the present invention, a glass composition is provided, which comprises, in terms of mass percentage, 71-80% SiO2, 5-9% B2O3, 3-8% Al2O3, 5.4-9% alkali metal oxides, 2.3-5.2% alkaline earth metal oxides, 0.2-0.4% Bi2O3, 0.2%-0.4% PbO, 0-0.2% BeO, 0.1-0.2% CeO2 and 0-0.2% Yb2O3.

[0009] In the present invention, SiO2 is a glass-forming oxide, the main body of the glass-forming skeleton, and the component that plays a major role in the glass skeleton. The silicon dioxide content can reduce the thermal expansion coefficient of the glass, improve the thermal stability, chemical stability, softening temperature, heat resistance, hardness and mechanical strength of the glass, but too high a content will also increase the melting point of the glass, increase the viscosity of the glass at high temperature, and cause melting difficulties. In an embodiment of the present invention, the content of SiO2 is 71-80% by mass percentage. In some embodiments of the present invention, the content of SiO2 is further selected from the following content range or any value in the following content range by mass percentage: 74.1-80%, 76-80%, 71-76%, 74.1-76%, 71-74.1%, 71-72%, 71-73%, etc. In some preferred embodiments of the present invention, the content of SiO2 is preferably 71-76% by mass percentage.

[0010] In the present invention, B2O3 is not only a glass-forming oxide, but also has boron-oxygen triangles [BO3] and boron-oxygen tetrahedrons [BO4] as structural units, and together with silicon-oxygen tetrahedrons in borosilicate glass, it forms a structural network. It can also be used as a network regulator to change the structure of glass, thereby adjusting the physical and chemical properties of glass. B2O3 can reduce the expansion coefficient of glass, improve the thermal stability and chemical stability of glass, increase the refractive index of glass, improve the gloss of glass, and improve the mechanical properties of glass. When the amount of B2O3 added is too high, due to the increase in boron-oxygen triangles, the expansion coefficient of glass increases instead, and boron anomaly occurs. In an embodiment of the present invention, the content of B2O3 is 5-9% by mass percentage. In some embodiments of the present invention, the content of B2O3, by mass percentage, can be further selected from the following content ranges or any value in the following content ranges: 6.75-9%, 7.85-9%, 5-7.85%, 6.75-7.85%, 5-6.75%, and so on. In some preferred embodiments of the present invention, the content of B2O3 is 6.75-9% by mass.

[0011] In the present invention, Al2O3 is an intermediate oxide. When the molar ratio of Na2O to Al2O3 in the glass is greater than 1, aluminum-oxygen tetrahedrons are formed and form a continuous structural network with silicon-oxygen tetrahedrons. When the molar ratio of Na2O to Al2O3 is less than 1, octahedrons are formed, which are network exosomes and are in the cavities of the silicon-oxygen structural network. Al2O3 can reduce the crystallization tendency of glass, improve the chemical stability, thermal stability, mechanical strength, hardness and refractive index of glass, but adding too much will significantly increase the viscosity of glass and increase the difficulty of melting. In an embodiment of the present invention, the content of Al2O3 is 3-8% by mass percentage. In some embodiments of the present invention, the content of Al2O3 is measured by mass percentage, and can be further selected from the following content range or any value in the following content range: 5-8%, 6-8%, 7-8%, 3-6%, 5-6%, 3-5%, etc. In some preferred embodiments of the present invention, the content of Al2O3 is 5-8% by mass percentage.

[0012] In some embodiments of the present invention, the sum of the contents of SiO2, B2O3 and Al2O3 is not less than 87%, preferably not less than 88%, more preferably 87-89%, more preferably 87.7-88.2%.

[0013] In some embodiments of the present invention, the alkali metal oxide includes Na2O, K2O and Li2O. In the present invention, Na2O, K2O and Li2O are network oxides of glass. Alkali metal ions are easy to move and diffuse in the glass body, which can reduce the viscosity of glass during high-temperature melting and make the glass easy to melt. They are good fluxing agents, but the amount of introduction should not be too much. Excessive introduction will increase the thermal expansion coefficient of the glass and reduce the chemical stability, thermal stability and mechanical strength of the glass.

[0014] In some embodiments of the present invention, the alkaline earth metal oxides include CaO, BaO and MgO. In the present invention, CaO, BaO and MgO are all network exosome oxides, and the main role of CaO in glass is a stabilizer, that is, to increase the chemical stability and mechanical strength of the glass. However, improper use will increase the crystallization tendency of the glass and easily make the glass brittle. BaO can increase the refractive index, density, gloss and chemical stability of the glass, and a small amount of BaO can accelerate the melting of the glass. The present invention replaces part of the CaO with no more than 0.1wt% of MgO to slow down the hardening speed of the glass and improve the forming properties of the glass. MgO can also reduce the crystallization tendency and crystallization speed, increase the high temperature viscosity of the glass, and improve the chemical stability and mechanical strength of the glass.

[0015] In some embodiments of the present invention, the content ratio of alkali metal oxide to alkaline earth metal oxide is less than 2.5, preferably less than 2, and more preferably less than 1.4. For example, in some embodiments, the content ratio of alkali metal oxide to alkaline earth metal oxide is 1-4, preferably 1-1.5, and more preferably 1-1.2.

[0016] In some embodiments of the present invention, the content of Na2O is greater than 70% of the total amount of alkali metal oxides, and the proportion may be further greater than 75%, greater than 78%, greater than 80%, or greater than 81%. In some preferred embodiments of the present invention, the content of Na2O accounts for 75%-81.5% of the total amount of alkali metal oxides, preferably 80-81.5%.

[0017] In some embodiments of the present invention, the content of Na2O is 4.4-7% by mass percentage. In some embodiments of the present invention, the content of Na2O is further selected from the following content ranges or any value in the following content ranges by mass percentage: 5-7%, 6-7%, 4.4-6%, 5-6%, 4.4-5%, etc. In some preferred embodiments of the present invention, the content of Na2O is 4.4-6% by mass percentage.

[0018] In some embodiments of the present invention, the content of K2O is 0.5-1% by mass. In some embodiments of the present invention, the content of K2O is further selected from the following content ranges or any value in the following content ranges by mass: 0.7-1%, 0.8-1%, 0.5-0.8%, 0.7-0.8%, 0.5-0.7%, etc. In some preferred embodiments of the present invention, the content of K2O is 0.5-0.8% by mass.

[0019] In some embodiments of the present invention, the content of Li2O is 0.5-1% by weight. In some embodiments of the present invention, the content of Li2O is 0.5-1% by weight, and can be further selected from the following content ranges or any value in the following content ranges: 0.7-1%, 0.5-0.7%, 0.5-0.8%, 0.5-0.6%, and the like.

[0020] In some embodiments of the present invention, the content of BaO is greater than 65% of the total amount of alkaline earth metal oxides, and the proportion may be further greater than 69%, greater than 71%, or greater than 78%. In some preferred embodiments of the present invention, the content of BaO accounts for 69-78.5% of the total amount of alkaline earth metal oxides, and more preferably 69-71%.

[0021] In some embodiments of the present invention, the content of CaO is 0.49-1.5% by mass percentage. In some embodiments of the present invention, the content of CaO is further selected from the following content ranges or any value in the following content ranges by mass percentage: 1.07-1.5%, 1.3-1.5%, 0.49-1.3%, 1.07-1.3%, 0.49-1.07%, etc. In some preferred embodiments of the present invention, the content of CaO is 1.07-1.5% by mass percentage.

[0022] In some embodiments of the present invention, the content of BaO is 1.8-3.6% by mass percentage. In some embodiments of the present invention, the content of BaO is further selected from the following content ranges or any value in the following content ranges, 2.5-3.6%, 3.3-3.6%, 1.8-3.3%, 2.5-3.3%, 1.8-2.5%, etc. In some preferred embodiments of the present invention, the content of BaO is 2.5-3.6% by mass percentage.

[0023] In some embodiments of the present invention, the content of MgO is 0.01-0.1% by mass. In some embodiments of the present invention, the content of MgO is 0.01-0.1% by mass, and can be further selected from the following content ranges or any value in the following content ranges: 0.03-0.1%, 0.07-0.1%, 0.01-0.07, 0.03-0.07%, 0.01-0.03%, etc. In some preferred embodiments of the present invention, the content of MgO is 0.03-0.1% by mass.

[0024] In the present invention, the addition of Bi2O3 and PbO plays a very important role in improving the performance of glass. PbO, as a network exogenous oxide, not only increases the thermal expansion coefficient of glass, but also reduces the melting temperature by taking away oxygen ions in the Si-O network and causing Si-O network disconnection to form non-bridging oxygen. Bi2O3, which has similar effects to PbO, can significantly reduce the viscosity of glass and increase the refractive index, so that Bi2O3 and PbO can enhance each other's effects when they coexist. In an embodiment of the present invention, the content of PbO is 0.2-0.4% by mass percentage. In some embodiments of the present invention, the content of PbO is calculated by mass percentage, and can be further selected from the following content ranges or any value in the following content ranges 0.24-0.4%, 0.3-0.4%, 0.2-0.3%, 0.24-0.3%, 0.2-0.24%, and the like. In some preferred embodiments of the present invention, the content of PbO is 0.24-0.4% by mass.

[0025] In addition, Bi2O3 can also help improve the thermal stability of glass and enhance its light absorption capacity. In particular, the reducing properties of the Bi element in a high-temperature hydrogen atmosphere can be used to optimize the anti-halation effect, which provides new possibilities for the application of glass materials. However, the amount of Bi2O3 introduced needs to be precisely controlled to avoid reduced chemical stability of the glass and severe corrosion of the melting container due to excessive addition. Too much Bi2O3 may also promote crystallization of the glass, affecting its transparency and optical uniformity, while insufficient Bi2O3 content will make it difficult to fully play its role in improving optical properties.

[0026] In an embodiment of the present invention, the content of Bi2O3 is 0.2-0.4% by mass percentage. In some embodiments of the present invention, the content of Bi2O3 is further selected from the following content ranges or any value in the following content ranges, 0.24-0.4%, 0.3-0.4%, 0.2-0.3%, 0.24-0.3%, 0.2-0.24%, etc. In some preferred embodiments of the present invention, the content of Bi2O3 is 0.24-0.4% by mass percentage.

[0027] In the present invention, the main purpose of introducing CeO2 is to improve the glass's ability to absorb ultraviolet rays so that the glass can maintain color stability under strong radiation. In addition, CeO2 can decompose and release oxygen at the melting temperature, which can be used as a clarifier to effectively improve the light transmittance of the glass. In an embodiment of the present invention, the content of CeO2 is 0.1-0.2% by mass percentage. In some embodiments of the present invention, the content of CeO2 is measured by mass percentage, and can also be further selected from the following content range or any value in the following content range 0.12-0.2%, 0.15-0.2%, 0.1-0.15%, 0.12-0.15%, 0.1-0.12%, and so on. In some preferred embodiments of the present invention, the content of CeO2 is 0.12-0.2% by mass percentage.

[0028] In the embodiments of the present invention, the synergistic effect of PbO, Bi2O3 and CeO2 not only optimizes the physical and chemical properties of the glass, but also improves the optoelectronic performance by forming a light absorbing layer in the glass.

[0029] In some embodiments of the present invention, the sum of the contents of Bi2O3, PbO and CeO2 is not less than 0.5% by mass percentage, and the value may be further not less than 0.6%, not less than 0.65%, not less than 0.7%, not less than 0.75%, not less than 0.8%, not less than 0.9%, not less than 1.0%. In some preferred embodiments of the present invention, the sum of the contents of Bi2O3, PbO and CeO2 may be 0.5-1%, 0.6-1%, 0.65-1%, 0.7-1%, 0.75-1%, 0.8-1%, 0.9-1%.

[0030] In some embodiments of the present invention, the content ratio of Bi2O3, PbO and CeO2 is 2:2:1 in terms of mass percentage.

[0031] In some embodiments of the present invention, the content ratio of Bi2O3 to PbO is 1:1 in terms of mass percentage.

[0032] In some embodiments of the present invention, the sum of the contents of Bi2O3 and PbO is 0.4-0.8%, preferably 0.45-0.8%, and more preferably 0.6-0.8%, in terms of mass percentage.

[0033] In the present invention, the Yb element in Yb2O3 is a variable valence element, and its absorption peak and emission peak are both located in the near-infrared region, which will not affect the visible light transmittance of the glass. At the same time, the addition of Yb can reduce the thermal expansion coefficient of the glass and improve its mechanical properties by densifying the glass microstructure. However, it should be noted that in the embodiments of the present invention, the amount of Yb2O3 should be controlled to not exceed 0.2wt% to avoid crystallization. In some embodiments of the present invention, the content of Yb2O3 is 0-0.2% by mass percentage. In some embodiments of the present invention, the content of Yb2O3 is measured by mass percentage, and can be further selected from the following content ranges or any value in the following content ranges: 0, 0-0.05%, 0-0.1%, 0-0.16%, 0-0.2%, 0.1-0.2%, 0.16-0.2%, 0.05-0.16%, 0.1-0.16%, 0.05-0.1%, and the like. In some preferred embodiments of the present invention, the content of Yb2O3 is 0 or 0.16-0.2% by mass.

[0034] In some embodiments of the present invention, the content of CeO2 is not less than the content of Yb2O3.

[0035] And, in the present invention, the variable valence metal oxide BeO can be added in an amount not higher than 0.2%. BeO has a high thermal conductivity, which can help the glass to dissipate the heat generated during processing or use more effectively, which is beneficial to improve the performance of the glass in high-temperature applications. At the same time, BeO can improve the mechanical strength and hardness of the material, making the glass more durable and more wear-resistant. In an embodiment of the present invention, the content of BeO is 0-0.2% by mass percentage. In some embodiments of the present invention, the content of BeO is further selected from the following content ranges or any value in the following content ranges by mass percentage: 0, 0-0.1%, 0-0.12%, 0-0.15%, 0.12-0.2%, 0.15-0.2%, 0.1-0.15%, 0.12-0.15%, 0.1-0.12%, and so on. In some preferred embodiments of the present invention, the content of BeO is 0 or 0.12-0.2% by mass percentage.

[0036] In some embodiments of the present invention, the sum of the contents of PbO, Bi2O3, BeO and CeO2 is not less than 0.5% by mass percentage, and the ratio may be further not less than 0.6%, not less than 0.72%, not less than 0.8%, not less than 0.9%, not less than 1.0%, not less than 1.2%. In some preferred embodiments of the present invention, the sum of the contents of PbO, Bi2O3, BeO and CeO2 is 0.5-1.2%, 0.6-1.2%, preferably 0.72-1.2%, and more preferably 1-1.2%. In some embodiments of the present invention, the ratio of the contents of Bi2O3, PbO, BeO and CeO2 is 2:2:1:1 by mass percentage.

[0037] In some embodiments of the present invention, the glass composition comprises, by mass percentage, SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0-0.2%, CeO2 0.1-0.2% and Yb2O3 0-0.2%.

[0038] In some embodiments of the present invention, the glass composition comprises, by mass percentage, SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0.1-0.2%, CeO2 0.1-0.2% and Yb2O3 0-0.2%.

[0039] In some embodiments of the present invention, the glass composition comprises, by mass percentage, SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0-0.2%, CeO2 0.1-0.2% and Yb2O3 0.05-0.2%.

[0040] In some embodiments of the present invention, the glass composition comprises, by mass percentage, SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0.1-0.2%, CeO2 0.1-0.2% and Yb2O3 0.05-0.2%.

[0041] In some embodiments of the present invention, the glass composition comprises, by mass percentage, SiO2 71-76%, B2O3 6-9%, Al2O3 5-8%, Na2O 4.4-6%, K2O 0.5-0.8%, Li2O 0.5-1%, CaO 1.07-1.5%, BaO 2.5-3.6%, MgO 0.03-0.1%, Bi2O3 0.24-0.4%, PbO 0.24%-0.4%, BeO0.12-0.2%, CeO20.12-0.2% and Yb2O3 0.05-0.2%.

[0042] In some embodiments of the present invention, the glass prepared according to the glass composition of the present invention has good transmittance, and its transmittance in the wavelength range of 350-400nm is ≥90.0%, and its transmittance in the wavelength range of 400-1000nm is ≥92.4%. For example, in some embodiments, the minimum transmittance of the glass in the wavelength range of 350-400nm is ≥90.2%, ≥90.3%, ≥90.4%, ≥90.5%, ≥90.6%, ≥90.7%, ≥90.8%, ≥90.69%, ≥91%, ≥91.5%, and the minimum transmittance of the glass in the wavelength range of 400-1000nm is ≥92.4%, ≥92.5%, ≥92.6%, ≥92.7%, ≥92.8%, ≥92.9%, ≥93%, ≥93.5%. Specifically, in some embodiments, the minimum transmittance of the glass in the wavelength range of 350-400nm is 90.2-91.5%, further 90.5-91.5%, further 90.8-91.5%, preferably 91-91.5%, and the minimum transmittance of the glass in the wavelength range of 400-1000nm is 92.4-93.6%, further 92.9-93.6%, further 93-93.6%.

[0043] In some embodiments of the present invention, the glass prepared according to the glass composition of the present invention has a good thermal expansion coefficient, and its thermal expansion coefficient at 30°C-300°C can be stabilized at (55±2)×10 -7 / ℃, its glass transition temperature T g ≥555℃, relaxation temperature T s ≥650℃. This indicates that the glass has good thermal processing properties, chemical stability, thermal stability and mechanical strength.

[0044] In some embodiments of the present invention, the glass prepared according to the glass composition of the present invention can form a light absorption layer after reduction treatment, the thickness of the light absorption layer is ≥0.6mm, further ≥0.7mm, further ≥0.8mm, the light absorption layer has a transmittance of 0 in the wavelength range of 350-800nm, and a transmittance of ≤1.8%, further ≤1.4%, ≤1.3%, ≤1.2%, ≤1.0% in the wavelength range of 800-1000nm. Specifically, in some embodiments, the transmittance of the light absorption layer in the wavelength range of 800-1000nm is 1.0-1.8%, further 1.0-1.4%, further 1.0-1.3%.

[0045] In some embodiments of the present invention, the glass prepared according to the glass composition of the present invention has an average cathode sensitivity of ≥850 μA / lm, further ≥860 μA / lm, ≥870 μA / lm, and particularly ≥875 μA / lm. For example, in some embodiments, the average cathode sensitivity is 864-876 μA / lm, further 870-876 μA / lm, and further 872-876 μA / lm.

[0046] In a second aspect of the present invention, a glass blank is provided, which is prepared from the glass composition described in the first aspect.

[0047] In some embodiments of the present invention, the method for preparing the glass blank comprises: mixing raw materials, melting the mixture at 1350-1400° C., stirring, clarifying, and molding at 1150-1250° C. to obtain the glass blank.

[0048] The stirring can be mechanical stirring, which can accelerate the homogenization process of the glass liquid. Stirring can continuously divide the uneven areas and thick stripes in the glass liquid into very thin and short stripes, thereby increasing the contact surface, facilitating the mutual dissolution and diffusion between the glass liquid and the stripes, thereby causing the stripes to gradually disappear or decrease.

[0049] In some embodiments of the present invention, the melting time is 20-30 hours, which is helpful for clarifying the glass liquid.

[0050] In some embodiments of the present invention, the molding time is 10-15 minutes, and the generation of secondary bubbles and impurities can be reduced by shortening the molding time.

[0051] In some embodiments of the present invention, the transmittance of the glass blank in the wavelength range of 350-400nm is ≥90.2%, and the transmittance in the wavelength range of 400-1000nm is ≥92.4%. In some embodiments of the present invention, the minimum optical transmittance of the glass blank in the wavelength range of 350-400nm is ≥90.5%, and the minimum optical transmittance in the wavelength range of 400-1000nm is ≥92.5%. For example, in some embodiments, the minimum transmittance of the glass blank in the wavelength range of 350-400nm is ≥90.2%, ≥90.3%, ≥90.4%, ≥90.5%, ≥90.6%, ≥90.7%, ≥90.8%, ≥90.69%, ≥91%, ≥91.5%; the minimum transmittance of the glass blank in the wavelength range of 400-1000nm is ≥92.4%, ≥92.5%, ≥92.6%, ≥92.7%, ≥92.8%, ≥92.9%, ≥93%, ≥93.5%. Specifically, in some embodiments, the minimum transmittance of the glass blank in the wavelength range of 350-400nm is 90.2-91.5%, further 90.5-91.5%, further 90.8-91.5%, preferably 91-91.5%, and the minimum transmittance of the glass blank in the wavelength range of 400-1000nm is 92.4-93.6%, further 92.9-93.6%, further 93-93.6%.

[0052] In some embodiments of the present invention, the glass blank has a good thermal expansion coefficient, and its thermal expansion coefficient at 30°C-300°C can be stabilized at (55±2)×10 -7 / ℃.

[0053] In some embodiments of the present invention, the glass blank has good thermal processing performance, chemical stability, thermal stability and mechanical strength, and its glass transition temperature T g ≥555℃, relaxation temperature T s ≥650℃.

[0054] The method of the present invention has process stability, and the glass material prepared by the process method can show stable characteristics, and will not cause significant fluctuations in glass performance due to the increase or decrease of the process within the range. Of course, it can be understood that within the process range, some higher temperatures can shorten the preparation process compared to lower temperatures. If it is necessary to shorten the time cost as much as possible, those skilled in the art can choose a relatively higher temperature within the temperature range disclosed in the present invention when operating.

[0055] In the third aspect of the present invention, there is provided a strong stray light absorption and anti-halation photoelectric glass, which comprises a light-transmitting effective area, wherein the glass composition of the light-transmitting effective area is the same as the glass composition described in the first aspect, or is made of the glass blank described in the second aspect.

[0056] In some embodiments of the present invention, the strong stray light absorption and anti-halation photoelectric glass further comprises a light absorption layer, and the light absorption layer is obtained by reducing the light-transmitting effective area.

[0057] In some embodiments of the present invention, the reduction treatment is carried out in a reducing atmosphere, the temperature of the reduction treatment is 550-650°C, the pressure is 0.01-0.5MPa, and the time is 3000-15000min. For example, in some embodiments of the present invention, the reduction treatment is: the glass blank is processed into a step shape and placed in a closed container and heated to 600°C, and a reducing atmosphere (such as hydrogen) is introduced, the hydrogen pressure is 0.20MPa, the hydrogen treatment time is 60h, and the hydrogen in the closed container is replaced every 15h.

[0058] In some embodiments of the present invention, the transmittance of the effective light transmission area of ​​the strong stray light absorption anti-halation photoelectric glass in the wavelength range of 350-400nm is ≥90.0%, and the transmittance in the wavelength range of 400-1000nm is ≥92.4%. For example, in some embodiments, the minimum transmittance of the glass in the wavelength range of 350-400nm is ≥90.2%, ≥90.3%, ≥90.4%, ≥90.5%, ≥90.6%, ≥90.7%, ≥90.8%, ≥90.69%, ≥91%, ≥91.5%, and the minimum transmittance of the glass in the wavelength range of 400-1000nm is ≥92.4%, ≥92.5%, ≥92.6%, ≥92.7%, ≥92.8%, ≥92.9%, ≥93%, ≥93.5%. Specifically, in some embodiments, the minimum transmittance of the glass in the wavelength range of 350-400 nm is 90.2-91.5%, further 90.5-91.5%, and the minimum transmittance of the glass in the wavelength range of 400-1000 nm is 92.4-93.6%, further 92.9-93.6%, and further 93-93.6%.

[0059] In some embodiments of the present invention, the thickness of the light absorption layer of the strong stray light absorption anti-halation photoelectric glass is ≥0.6mm, further ≥0.7mm, further ≥0.8mm, and the light absorption layer has a transmittance of 0 in the wavelength range of 350-800nm, and a transmittance of ≤1.8%, further ≤1.4%, ≤1.3%, ≤1.2%, ≤1.0% in the wavelength range of 800-1000nm. Specifically, in some embodiments, the transmittance of the light absorption layer in the wavelength range of 800-1000nm is 1.0-1.8%, further 1.0-1.4%, further 1.0-1.3%.

[0060] In some embodiments of the present invention, the cathode sensitivity of the strong stray light absorption anti-halation photoelectric glass has an average value of ≥850μA / lm, further ≥860μA / lm, ≥870μA / lm, and in particular ≥875μA / lm. For example, in some embodiments, the cathode sensitivity has an average value of 864-876μA / lm, further 870-876μA / lm, and further 872-876μA / lm.

[0061] In a fourth aspect of the present invention, a method for preparing the strong stray light absorption and anti-halation photoelectric glass according to the third aspect is provided, which comprises:

[0062] The raw materials are mixed, the mixture is melted at 1350-1400°C, stirred, clarified, and formed at 1150-1250°C to obtain a glass blank;

[0063] After the glass blank is annealed, it is cold-worked, then reduced to form a light-absorbing layer on the surface of the glass blank, and finally surface-treated to obtain a strong stray light-absorbing and anti-halation photoelectric glass.

[0064] In an embodiment of the present invention, the method for preparing the glass blank may be as described in the second aspect above.

[0065] In an embodiment of the present invention, annealing is performed to eliminate internal stress of the glass to meet the requirements of subsequent cold working, and the annealing temperature is 500-620°C.

[0066] In the embodiments of the present invention, the purpose of the cold working is mainly to accurately modify the shape, size and surface state of the glass blank to meet specific application requirements. Such operations include but are not limited to cutting and edge grinding. A suitable processing method can be selected according to the needs. For example, in some embodiments of the present invention, the glass blank is rounded, rolled, sliced ​​and stepped to obtain a stepped glass blank. Then, the stepped glass blank is reduced.

[0067] In an embodiment of the present invention, the surface treatment includes but is not limited to grinding, polishing and cutting, polishing, etc., to adjust the surface state of the glass, such as flatness and smoothness, etc. Appropriate treatment methods can be selected according to needs. For example, in some embodiments of the present invention, the step-type glass blank obtained after cold working is subjected to reduction treatment to form a light absorption layer on the surface of the step-type glass blank, and then the light absorption layer on the upper and lower surfaces of the step-type glass blank is ground and removed and polished to expose the transparent glass part, while retaining the light absorption layer on the remaining surface (step surface), to obtain the step-type strong stray light absorption anti-halo photoelectric glass. The glass can be used as an anti-halo glass input window, such as an example such as Figure 3 As shown, the upper surface and the lower surface expose the light-transmitting effective area, and the remaining surfaces have a black light-absorbing layer.

[0068] In the fifth aspect of the present invention, an optical element is provided, which is made of the glass composition described in the first aspect or the glass blank described in the second aspect, or includes the strong stray light absorption and anti-halation photoelectric glass described in the third aspect.

[0069] In some embodiments of the present invention, the optical element is an optical window, preferably an anti-halation glass input window.

[0070] In a sixth aspect of the present invention, the present invention provides a low-light-level image intensifier, which includes the optical element described in the fifth aspect.

[0071] In some embodiments of the present invention, the optical element is an anti-halation glass input window.

[0072] In the seventh aspect of the present invention, there is provided an application of the glass composition described in the first aspect, or the glass blank described in the second aspect, or the strong stray light absorption and anti-halation photoelectric glass described in the third aspect, or the optical element described in the fifth aspect, or the low-light image intensifier described in the sixth aspect in the optical field or the application field of intelligent technology.

[0073] In some embodiments of the present invention, the application is use as an optical window.

[0074] In some embodiments of the present invention, the application is for preparing an anti-halation glass input window for a low-light image intensifier.

[0075] In some embodiments of the present invention, the application is for preparing optical system components for low-light-level night vision devices.

[0076] The specific technical features described in all the embodiments of the above-mentioned various aspects of the present invention can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further explain various possible combinations.

[0077] Unless otherwise specified, the numerical range described in the present invention includes all the numerical values ​​within this range, and includes the range value composed of any two numerical values ​​within this range. For example, 0.1-0.2%, this numerical range includes all the numerical values ​​between 0.1-0.2%, and includes the range value (0.11-0.19%) composed of any two numerical values ​​within this range (for example: 0.11%, 0.19%); different numerical values ​​of the same indicator appearing in all embodiments of the present invention can be arbitrarily combined to form a range value.

[0078] Through one or more of the above technical means, the following beneficial effects can be achieved:

[0079] The present invention provides a glass composition and a strong stray light absorption anti-halo photoelectric glass prepared from the composition. The strong stray light absorption anti-halo photoelectric glass provided by the present invention has good transmittance, and its transmittance in the effective light transmission area is ≥90.0% in the wavelength range of 350-400nm, and the transmittance in the wavelength range of 400-1000nm is ≥92.4%; the thickness of the black light absorption layer is ≥0.6mm, the transmittance in the wavelength range of 350-800nm ​​is 0, and the transmittance in the wavelength range of 800-1000nm is ≤1.8%. The cathode sensitivity average of the anti-halo glass is ≥850μA / lm. The high transmittance, strong stray light absorption anti-halo photoelectric glass of the present invention has an edge stray light absorption layer, which can effectively eliminate the halo formed by a strong light source and improve the image contrast.

[0080] The strong stray light absorption and anti-halation photoelectric glass provided by the present invention has a thermal expansion coefficient that can be stabilized at (55±2)×10 -7 / ℃, transition temperature T g ≥555℃, sag temperature T s ≥650℃, with good chemical stability, thermal stability and mechanical strength, and good molding and processing properties.

[0081] The existing anti-halo photoelectric glass has a low average transmittance in the wavelength range of 400-1000nm, and it is difficult to improve the stray light absorption performance. The present invention selects and adjusts the types and ratios of raw materials and clarifiers, as well as the synergistic effect produced by the introduction of variable valence ion components, so that the anti-halo glass has higher optical transmittance, excellent stray light elimination performance and high cathode sensitivity performance, which can meet the use requirements of advanced image intensifiers and other anti-halo glass materials that require high performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0082] The drawings constituting part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. The implementation scheme of the present application is described in detail below in conjunction with the drawings, wherein:

[0083] Figure 1 It is a comparison chart of the transmittance of the glass of Example 1 and Comparative Example 5 in the light transmission effective area within the range of 350-1000nm.

[0084] Figure 2 It is a comparison chart of the transmittance of the light absorption layer of the glass of Example 1 and Comparative Example 5 in the range of 350-1000nm.

[0085] Figure 3 This is a physical picture of the anti-halation input window (step type). DETAILED DESCRIPTION

[0086] The present application is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or according to the conditions recommended by the manufacturer.

[0087] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in this application can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in this application are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the content described herein can be applied to the method of this application. The preferred implementation methods and materials described in the text are for demonstration purposes only.

[0088] Example 1

[0089] The glass composition and physical properties of this example are shown in Table 1.

[0090] The preparation method is as follows: quartz sand, boric acid, aluminum hydroxide, sodium nitrate, potassium nitrate, lithium carbonate, barium nitrate, calcium carbonate, basic magnesium carbonate, bismuth trioxide, lead silicate, beryllium oxide, cerium oxide and titanium oxide are used as raw materials, after being fully mixed, they are melted at 1350°C for 30 hours, mechanically stirred (10 r / min, 15 hours), assisted by high-temperature clarification (compressed air is introduced into the bottom of the glass liquid at a pressure of 0.20 MPa for 10 hours), and leak-formed at 1250°C (forming time is 10 minutes) to obtain a plate glass blank.

[0091] The plate glass blank is placed in an annealing furnace that has been preheated to 550°C for annealing to eliminate the stress inside the glass and meet the requirements of subsequent cold processing.

[0092] The plate-shaped glass blank after annealing is subjected to cold processing steps of rounding, rolling, slicing and stepping, and then the step-shaped blank is placed in a sealed container and heated to 600°C, and hydrogen is introduced with a hydrogen pressure of 0.20MPa. The hydrogen treatment time is 60h, and the hydrogen in the sealed container is replaced every 15h. After the reduction treatment, a light absorption layer is generated on the surface of the glass blank, and the light absorption layer on the upper and lower surfaces of the blank is ground and removed and polished to expose the transparent glass part, while retaining the light absorption layer on the step surface to obtain the anti-halo photoelectric glass. The glass can be used as an anti-halo input window, such as Figure 3 shown.

[0093] The transmittance test was carried out using a UV-visible-infrared spectrophotometer.

[0094] The thickness of the light absorbing layer (black layer) formed after the glass reduction was measured using an optical microscope.

[0095] The thermal expansion coefficient of the glass sample was tested using the NETZSCH DIL 402 thermal expansion coefficient tester. Sample preparation: The glass sample was polished into a cylindrical glass strip of Φ6mm×50mm, and the two end faces were parallel. The heating rate was set to 5℃ / min, and the data acquisition cycle was 20ms. The data was plotted against the temperature and linear expansion curve, and the glass linear expansion coefficient (α), transition temperature (T) were obtained by the tangent method. g ) and relaxation temperature (T s ). (GB / T 7962.16~2010)

[0096] The cathode sensitivity of the anti-halation input window is measured on a super-second-generation image intensifier tube (the image intensifier tube is the core component of the night vision device). A specified voltage is applied to the super-second-generation image intensifier tube, and a tungsten filament lamp with a color temperature of 2856K±50K is used as the light source. The specified luminous flux is evenly distributed in the specified area of ​​the photocathode parallel to the input optical axis. When using a dimmer, the spectral characteristics of the input light radiation should not be changed. Measure the cathode current at this time; after cutting off the light source, measure the cathode current when there is no light radiation input to the photocathode. The light sensitivity is calculated according to the following formula:

[0097]

[0098] In the formula, s is the light sensitivity, in μA / lm; I1 is the cathode current when there is light radiation input, which is the sum of the photocurrent caused by light radiation and I2, in μA; I2 is the cathode current when there is no light radiation input, which is the sum of the photocathode dark current and the internal and external leakage currents, in μA; Φ is the input luminous flux, in lm. (GJB 7351-2011)

[0099] Example 2

[0100] The glass composition and physical properties of this example are shown in Table 1.

[0101] The melting temperature in the preparation method is 1400°C, the melting time is 20h, mechanical stirring (15r / min, 10h), the molding temperature is 1150°C, and the molding time is 15min. The other preparation steps, parameters and test process are the same as those in Example 1.

[0102] Example 3

[0103] The glass composition and physical properties of this example are shown in Table 1.

[0104] The melting temperature in the preparation method is 1380°C, the melting time is 25h, mechanical stirring (25r / min, 12h), the molding temperature is 1200°C, and the molding time is 12min. The other preparation steps, parameters and test process are the same as those in Example 1.

[0105] Example 4

[0106] The glass composition and physical properties of this example are shown in Table 1.

[0107] The melting temperature in the preparation method is 1360°C, the melting time is 21h, mechanical stirring (40r / min, 11h), the molding temperature is 1170°C, and the molding time is 14min. The other preparation steps, parameters and test process are the same as those in Example 1.

[0108] Example 5

[0109] The glass composition and physical properties of this example are shown in Table 1.

[0110] The melting temperature in the preparation method is 1370°C, the melting time is 22h, mechanical stirring (40r / min, 11.5h), the molding temperature is 1190°C, and the molding time is 13min. The other preparation steps, parameters and test process are the same as those in Example 1.

[0111] Example 6

[0112] The glass composition and physical properties of this example are shown in Table 1.

[0113] The preparation method is the same as that in Example 1.

[0114] Example 7

[0115] The glass composition and physical properties of this example are shown in Table 1.

[0116] The preparation method is the same as that in Example 1.

[0117] Example 8

[0118] The glass composition and physical properties of this example are shown in Table 1.

[0119] The preparation method is the same as that in Example 1.

[0120] Example 9

[0121] The glass composition and physical properties of this example are shown in Table 1.

[0122] The preparation method is the same as that in Example 1.

[0123] Comparative Examples 1-11

[0124] The glass composition and physical properties are shown in Table 2. The introduction of other components, glass preparation steps, parameters and testing process are the same as those in Example 1.

[0125] Table 1 Composition, content and physical properties of the anti-halation glass of Examples 1-9 of the present invention

[0126]

[0127]

[0128]

[0129] Table 2 Components, contents and physical properties of comparative examples of the present invention

[0130]

[0131]

[0132]

[0133] Embodiments 1-9, by reasonably adding corresponding components and controlling the proportion of each component in the raw material, ensure that the anti-halo photoelectric glass has a higher optical transmittance in the effective area and a lower optical transmittance in the black light absorption area while ensuring a high cathode sensitivity. As can be seen from Table 1, the optical transmittance of the high-transmittance, strong stray light absorption anti-halo photoelectric glass made from the glass components of embodiments 1-9 of the present invention is as follows: the transmittance of the anti-halo glass effective area in the wavelength range of 350-400nm is ≥90.2%, and the transmittance in the wavelength range of 400-1000nm is ≥92.4%; the thickness of the black light absorption layer is ≥0.6mm, the transmittance in the wavelength range of 350-800nm ​​is 0, and the transmittance in the wavelength range of 800-1000nm is ≤1.8%. The cathode sensitivity average is ≥850μA / lm, and the comprehensive performance is excellent.

[0134] The high transmittance, strong stray light absorption and anti-halation photoelectric glass provided by the present invention has a thermal expansion coefficient of (55±2)×10 -7 / ℃, transition temperature T g ≥555℃, relaxation temperature T s ≥650℃, with good chemical stability, thermal stability and mechanical strength, and good molding and processing properties.

[0135] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. Although the present application is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A glass composition, comprising the following components in percentage by mass: SiO271-80%, B2O35-9%, Al2O33-8%, alkali metal oxides 5.4-9%, alkaline earth metal oxides 2.3-5.2%, Bi2O3 0.2-0.4%, PbO0.2%-0.4%, BeO 0-0.2%, CeO20.1-0.2% and Yb2O30-0.2%; Wherein, the alkali metal oxides include Na2O, K2O and Li2O; the alkaline earth metal oxides include CaO, BaO and MgO.

2. The glass composition according to claim 1, characterized in that In terms of mass percentage, it contains: SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0-0.2%, CeO2 0.1-0.2% and Yb2O3 0-0.2%.

3. The glass composition according to claim 1, characterized in that In terms of mass percentage, it contains: SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0.1-0.2%, CeO2 0.1-0.2% and Yb2O3 0-0.2%.

4. The glass composition according to claim 1, characterized in that In terms of mass percentage, it contains: SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0-0.2%, CeO2 0.1-0.2% and Yb2O3 0.05-0.2%.

5. The glass composition according to claim 1, characterized in that In terms of mass percentage, it contains: SiO2 71-80%, B2O3 5-9%, Al2O3 3-8%, Na2O 4.4-7%, K2O 0.5-1%, Li2O 0.5-1%, CaO 0.49-1.5%, BaO 1.8-3.6%, MgO 0.01-0.1%, Bi2O3 0.2-0.4%, PbO 0.2%-0.4%, BeO 0.1-0.2%, CeO2 0.1-0.2% and Yb2O3 0.05-0.2%.

6. The glass composition according to claim 1, characterized in that In terms of mass percentage, it contains: SiO2 71-76%, B2O3 6-9%, Al2O3 5-8%, Na2O 4.4-6%, K2O 0.5-0.8%, Li2O 0.5-1%, CaO 1.07-1.5%, BaO 2.5-3.6%, MgO 0.03-0.1%, Bi2O3 0.24-0.4%, PbO 0.24-0.4%, BeO 0.12-0.2%, CeO2 0.12-0.2% and Yb2O3 0.05-0.2%.

7. The glass composition according to any one of claims 1 to 5, characterized in that Calculated by mass percentage, the content of SiO2 is 71-76%.

8. The glass composition according to any one of claims 1 to 6, characterized in that In terms of mass percentage, the content of B2O3 is 6.75-9%.

9. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the content of Al2O3 is 5-8%.

10. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the content of Na2O is 4.4-6%.

11. The glass composition according to any one of claims 1 to 5, characterized in that Calculated by mass percentage, the content of K2O is 0.5-0.8%.

12. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the content of Li2O is 0.5-0.8%.

13. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the CaO content is 1.07-1.5%.

14. The glass composition according to any one of claims 1 to 5, characterized in that Calculated by mass percentage, the BaO content is 2.5-3.6%.

15. The glass composition according to any one of claims 1 to 5, characterized in that Calculated by mass percentage, the content of MgO is 0.03-0.1%.

16. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the content of PbO is 0.24-0.4%.

17. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the content of Bi2O3 is 0.24-0.4%.

18. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the content of CeO2 is 0.12-0.2%.

19. The glass composition according to any one of claims 1 to 3, characterized in that Calculated in percentage by mass, the content of Yb2O3 is 0.

20. The glass composition according to any one of claims 1 to 6, characterized in that In terms of mass percentage, the content of Yb2O3 is 0.16-0.2%.

21. The glass composition according to any one of claims 1, 2 or 4, characterized in that Calculated by mass percentage, the BeO content is 0.

22. The glass composition according to any one of claims 1 to 5, characterized in that In terms of mass percentage, the BeO content is 0.12-0.2%.

23. The glass composition according to any one of claims 1 to 6, characterized in that The content ratio of the alkali metal oxide to the alkaline earth metal oxide is less than 2.

5.

24. The glass composition according to any one of claims 1 to 6, characterized in that The content of Na2O is greater than 70% of the total amount of alkali metal oxides.

25. The glass composition according to any one of claims 1 to 6, characterized in that The content of BaO is greater than 65% of the total amount of alkaline earth metal oxides.

26. The glass composition according to any one of claims 1 to 6, characterized in that The sum of the contents of SiO2, B2O3 and Al2O3 shall not be less than 87%.

27. The glass composition according to any one of claims 1 to 6, characterized in that The content of CeO2 is not less than the content of Yb2O3.

28. The glass composition according to any one of claims 1 to 6, characterized in that The content ratio of Bi2O3 and PbO is 1:

1.

29. The glass composition according to any one of claims 1 to 6, characterized in that The sum of the contents of PbO, Bi2O3, BeO and CeO2 shall not be less than 0.5%.

30. The glass composition according to any one of claims 1 to 6, characterized in that The content ratio of Bi2O3, PbO, BeO and CeO2 is 2:2:1:

1.

31. A glass blank prepared from the glass composition according to any one of claims 1 to 30.

32. The glass blank according to claim 31, characterized in that The preparation method comprises: mixing raw materials, melting the mixture at 1350-1400 DEG C, stirring, clarifying, and molding at 1150-1250 DEG C to obtain glass blank.

33. A strong stray light absorption and anti-halation photoelectric glass, comprising a light-transmitting effective area, wherein the glass composition of the light-transmitting effective area is as described in any one of claims 1 to 30, or is made of the glass blank as described in claim 31 or 32.

34. The strong stray light absorbing and anti-halation photoelectric glass according to claim 33, characterized in that: It also comprises a light absorbing layer, wherein the light absorbing layer is obtained by reducing the light-transmitting effective area glass.

35. The strong stray light absorbing and anti-halation photoelectric glass according to claim 34, characterized in that: The reduction treatment is carried out in a reducing atmosphere, the temperature of the reduction treatment is 550-650°C, the pressure is 0.01-0.5 MPa, and the time is 3000-15000 min.

36. The strong stray light absorbing and anti-halation photoelectric glass according to any one of claims 33 to 35, characterized in that: The transmittance of the light-transmitting effective area in the wavelength range of 350-400 nm is ≥90.2%, and the transmittance in the wavelength range of 400-1000 nm is ≥92.4%.

37. The strong stray light absorbing and anti-halation photoelectric glass according to claim 34 or 35, characterized in that: The thickness of the light absorbing layer is ≥0.6 mm, the transmittance of the light absorbing layer is 0 in the wavelength range of 350-800 nm, and the transmittance in the wavelength range of 800-1000 nm is ≤1.8%.

38. The strong stray light absorbing and anti-halation photoelectric glass according to claim 34 or 35, characterized in that: The average cathode sensitivity of the strong stray light absorption and anti-halation photoelectric glass is ≥850 μA / lm.

39. A method for preparing the strong stray light absorption and anti-halation photoelectric glass according to any one of claims 33 to 38, comprising: The raw materials are mixed, the mixture is melted at 1350-1400°C, stirred, clarified, and formed at 1150-1250°C to obtain a glass blank; The glass blank is annealed at 500-620°C and then cold worked; After the cold working treatment, a reduction treatment is performed to form a light absorbing layer on the surface of the glass blank; The glass blank with a light absorbing layer on the surface is subjected to surface treatment to obtain a photoelectric glass with strong stray light absorption and anti-halation.

40. The method according to claim 39, characterized in that The method comprises: mixing raw materials, melting the mixture at 1350-1400°C, stirring, clarifying, and molding at 1150-1250°C to obtain glass blank; The glass blank is annealed at 500-620 ℃, and then rounded, rolled, sliced ​​and stepped to obtain a step-type glass blank; the step-type glass blank is then reduced to form a light absorption layer on the surface of the step-type glass blank after the reduction treatment, and the light absorption layers on the upper and lower surfaces of the step-type glass blank are ground and removed and polished to expose the transparent glass part while retaining the light absorption layer on the step surface to obtain a strong stray light absorption and anti-halation photoelectric glass.

41. An optical element, which is made of the glass composition according to any one of claims 1 to 30 or the glass blank according to claim 31 or 32, or comprises the strong stray light absorbing anti-halation photoelectric glass according to any one of claims 33 to 38.

42. The optical element according to claim 41, characterized in that The optical element is an optical window.

43. The optical element according to claim 41, characterized in that The optical element is an anti-halation glass input window.

44. A low-light image intensifier, characterized in that: The low-light level image intensifier comprises the optical element described in any one of claims 41 to 43.

45. The low-light level image intensifier according to claim 44, characterized in that: The optical element is an anti-halation glass input window.

46. ​​Use of the glass composition according to any one of claims 1 to 30, or the glass blank according to claim 31 or 32, or the strong stray light absorbing anti-halation photoelectric glass according to any one of claims 33 to 38, or the optical element according to any one of claims 41 to 43, or the low-light image intensifier according to claim 44 or 45 in the optical field or the application field of intelligent technology.

47. The use according to claim 46, characterized in that The application is use as an optical window.

48. The use according to claim 46, characterized in that The application is to prepare the anti-halation glass input window of the low-light image intensifier.

49. The use according to claim 46, characterized in that The application is to prepare optical system components for low-light-level night vision devices.