Preparation method of high-conductivity positive electrode material and lithium battery
By using titanium and strontium element coatings and doped aluminum or zirconium elements in high nickel positive electrode materials, combined with gradient stirring and multi-stage calcining technology, the problems of conductivity and cycling performance of high nickel positive electrode materials are solved, and the lithium battery is significantly improved electrochemical properties and stability.
Patent Information
- Application Number
- CN202411192005.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-22
AI Technical Summary
The current high-nickel cathode materials have reduced conductivity and poor circulation performance, which affects the electrochemical performance of lithium batteries.
Titanium and strontium elements are used as coating materials and mixed with the positive electrode material and calcined. Combined with doped aluminum or zirconium elements, the conductive properties and cyclic stability of the positive electrode material are improved through gradient stirring and multi-stage calcination process.
It significantly improves the migration rate and electron transport performance of lithium ions, reduces the DC resistance, enhances the cyclic performance and structural stability of the positive electrode material, and reduces the possibility of cation mixing and side reactions.
Smart Images

Figure CN119008833A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials, and in particular to a preparation method of a highly conductive positive electrode material and a lithium battery. Background Art
[0002] With the proposal of the carbon neutrality goal, the new energy industry has developed rapidly. As an energy storage device in the new energy industry, lithium-ion batteries are widely used in new energy vehicles, power tools, energy storage power stations and other fields. In recent years, lithium-ion battery technology has undergone rapid innovation, including the diversification of positive and negative electrode materials, the improvement of electrolyte systems and the optimization of battery management systems, which have effectively improved the energy density, cycle life and safety of new energy batteries. Among them, the positive electrode material is an important factor in determining battery performance. At present, high-nickel positive electrode materials with strong thermal stability and high energy density have attracted widespread attention because of their larger specific capacity, but the cycle performance of high-nickel materials is poor.
[0003] The existing technology uses materials such as phosphates and borates to coat high-nickel positive electrode materials to improve their cycle performance. However, after the high-nickel materials are coated with the above materials, the conductivity of the positive electrode materials decreases, affecting the electrochemical performance of the battery formed by the positive electrode materials. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defect of reduced conductivity of high-nickel positive electrode materials in the prior art, thereby providing a method for preparing a high-conductivity positive electrode material and a lithium battery.
[0005] Another technical problem to be solved by the present invention is to overcome the defect of poor cycle performance of high-nickel positive electrode materials in the prior art, thereby providing a method for preparing a highly conductive positive electrode material and a lithium battery.
[0006] To this end, on one hand, the present invention provides a method for preparing a highly conductive positive electrode material, comprising the steps of mixing the positive electrode material with a coating material, and calcining the mixture, wherein the coating material comprises a titanium-containing compound and a strontium-containing compound.
[0007] In some of the embodiments, the doping amount of the titanium element in the highly conductive positive electrode material is 300-2000 ppm, and the doping amount of the strontium element is 300-2000 ppm.
[0008] In some embodiments, the titanium-containing compound is at least one of titanium dioxide, titanium tetrachloride, and barium titanate.
[0009] In some embodiments, the strontium-containing compound is at least one of strontium oxide, strontium carbonate, strontium nitrate, strontium chloride, and strontium hydroxide.
[0010] Preferably, the doping amount of the titanium element is 500-800 ppm, and the doping amount of the strontium element is 500-800 ppm.
[0011] In some of the embodiments, the calcination temperature is 400-600° C., the calcination time is 5-8 h, and the heating rate during calcination is 2° C. / min.
[0012] In some of the embodiments, the positive electrode material and the coating material are mixed under gradient stirring, and the gradient stirring process is that the positive electrode material and the coating material are mixed at a rotation speed of 800-1200 rpm for 1-3 min, at a rotation speed of 1800-2200 rpm for 2-4 min, and at a rotation speed of 3200-3800 rpm for 12-18 min.
[0013] In some of the embodiments, the positive electrode material is prepared by mixing and calcining a lithium source, a nickel-cobalt precursor and a doping material.
[0014] Preferably, the doping material is at least one of an aluminum-containing compound or a zirconium-containing compound.
[0015] In some of the embodiments, the nickel-cobalt precursor includes first grains and second grains, and the mass ratio of the first grains to the second grains is (6-8):(2-4), wherein the median particle size of the first grains is 13 to 16 μm, and the median particle size of the second grains is 2 to 4 μm.
[0016] In some of the embodiments, the molar amount of lithium element in the lithium source is n, the total molar ratio of nickel and cobalt elements in the nickel and cobalt precursor and the metal element in the doping material is N, and n:N=(1.0-1.1):1.
[0017] In some embodiments, the molar ratio of aluminum to lithium in the aluminum-containing compound is (0.01-0.02): (0.95-1.05). Preferably, the aluminum-containing compound is at least one of aluminum oxide, aluminum hydroxide, aluminum chloride, and aluminum sulfate.
[0018] In some embodiments, the molar ratio of zirconium to lithium in the zirconium-containing compound is (0.001-0.002): (0.95-1.05). Preferably, the zirconium-containing compound is at least one of zirconium oxide, zirconium sulfate, zirconium nitrate or zirconium fluoride.
[0019] In some embodiments, the specific surface area of the nickel-cobalt precursor is 5-10 m 2 / g, the tap density of the nickel-cobalt precursor is 1-3g / cm 3 .
[0020] In some of the embodiments, in the preparation of the positive electrode material, the calcination process is as follows: calcination at 400-600° C. for 3-5 h, and then calcination at 710-750° C. for 8-12 h.
[0021] In some embodiments, the lithium source includes at least one of lithium hydroxide, lithium carbonate or lithium acetate.
[0022] In some embodiments, the chemical formula of the positive electrode material is Li 1+y (Ni a Co b Al 1-a-b-c Zr c ) 1-y O2, where 0≤y≤0.2, 0.7≤a≤0.95, 0.01≤b≤0.1, 0≤c≤0.05.
[0023] In another aspect, the present invention provides a lithium battery, comprising a high-conductivity positive electrode material, wherein the high-conductivity positive electrode material is prepared by the above-mentioned method for preparing the high-conductivity positive electrode material.
[0024] The technical solution of the present invention has the following advantages:
[0025] 1. The present invention provides a method for preparing a highly conductive positive electrode material, comprising the steps of mixing and calcining a positive electrode material with a coating material, wherein the coating material contains titanium and strontium. The present invention uses titanium and strontium elements to coat the positive electrode material, which can, on the one hand, isolate the positive electrode material from contact with the electrolyte and improve the cycle performance of the positive electrode material; on the other hand, through the synergistic effect of titanium and strontium elements, increase the migration rate of lithium ions, improve the electronic transmission performance of the positive electrode material, reduce the DC resistance of the positive electrode material, improve the conductivity of the positive electrode material, and at the same time inhibit the growth of DC resistance during the cycle.
[0026] 2. The present invention provides a method for preparing a highly conductive positive electrode material, wherein the positive electrode material is prepared by mixing and calcining a lithium source, a nickel-cobalt precursor and a doping element. The present invention adds a doping element to the positive electrode material to modify the positive electrode material.
[0027] The doping element includes at least one of aluminum or zirconium. The present invention dopes a small amount of aluminum or zirconium into the positive electrode material, which will not significantly reduce the nickel content in the high-nickel material, nor change the stable structure of the positive electrode material. Therefore, it has little effect on the capacity of the positive electrode material, and can also reduce the cation mixing phenomenon of the positive electrode material, further improve the stability of the structure, improve the cycle performance, and reduce the DC resistance of the positive electrode material and the possibility of side reactions inside the positive electrode material, and improve the deintercalation rate of lithium ions.
[0028] 3. The present invention provides a method for preparing a highly conductive positive electrode material, wherein the nickel-cobalt precursor comprises a first crystal grain and a second crystal grain, wherein the mass ratio of the first crystal grain to the second crystal grain is (6-8):(2-4), wherein the median particle size of the first crystal grain is 13-16 μm, and the median particle size of the second crystal grain is 2-4 μm. The present invention utilizes a reasonable combination of large-sized crystal grains and small-sized crystal grains to reduce the DC resistance of the positive electrode material, improve the conductivity of the positive electrode material, reduce the ion insertion and extraction transmission distance, and significantly improve the electron and ion transport, storage and reaction kinetics rates. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a scanning electron microscope image of the highly conductive positive electrode material in Example 2 of the present invention;
[0031] Figure 2 It is a cycle performance diagram of Example 1 and Comparative Example 1 in the experimental examples of the present invention. DETAILED DESCRIPTION
[0032] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0033] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0034] Example 1
[0035] This embodiment provides a method for preparing a highly conductive positive electrode material, and the specific steps and parameters are as follows:
[0036] (1) According to the molar ratio of lithium element to nickel and cobalt element in the precursor being 1.02:1, the molar ratio of aluminum element to lithium element being 0.015:1.02, and the molar ratio of zirconium element to lithium element being 0.001:1.02, lithium hydroxide, nickel-cobalt-manganese precursor, aluminum oxide, and zirconium oxide are prepared. The chemical formula of the nickel-cobalt-manganese precursor is Ni 0.90 Co0.10 (OH)2, there are two specifications of grains in the nickel-cobalt-manganese precursor. The total weight of the first grain is 10.624 mol / kg, and the specific surface area of the first grain is 9.08m 2 / g, tap density is 2.15g / cm 3 The median particle size D50 is 14.58 μm, the total weight of the second crystal is 10.603 mol / kg, and the specific surface area is 7.58 m 2 / g, tap density is 1.90g / cm 3 The median particle size D50 is 2.86 μm, the mass ratio of the first grain to the second grain is 7:3, and the above raw materials are mixed evenly with a high-speed mixer, the speed is set to 1000 r / min for mixing for 2 minutes, then the speed is set to 2000 r / min for mixing for 3 minutes, and the speed is set to 3500 r / min for mixing for 15 minutes, without setting a waiting time in between, to obtain a first mixture.
[0037] (2) The first mixed material obtained in step (1) is heated to 500° C. at a heating rate of 2° C. / min in a box furnace, kept at 500° C. for 4 h, then heated to 730° C. at a heating rate of 2° C. / min, kept at 730° C. for 10 h, the sintering atmosphere is oxygen at a flow rate of 2 L / min, naturally cooled to room temperature, and crushed to obtain a sintered material of a nickel cobalt aluminum oxide positive electrode material.
[0038] (3) The crushed nickel cobalt aluminum oxide positive electrode material is sieved through a filter with a pore size of 45 microns. The sieved sintered material is taken, and titanium oxide is weighed according to a titanium element doping amount of 500ppm, and strontium oxide is weighed according to a strontium element doping amount of 500ppm. The sintered material, titanium oxide and strontium oxide are mixed in a high-speed mixer, and the speed is set to 1000r / min for mixing for 2min, then set the speed to 2000r / min for mixing for 3min, and set the speed to 3500r / min for mixing for 15min, without setting a waiting time in between, to obtain a second mixed material.
[0039] (4) The second mixed material is calcined in a box furnace with oxygen as the atmosphere. The temperature is raised to 500°C at a heating rate of 2°C / min and kept at that temperature for 6 hours. After natural cooling and screening, a highly conductive positive electrode material is obtained.
[0040] Example 2
[0041] This embodiment provides a method for preparing a highly conductive positive electrode material, and the specific steps and parameters are as follows:
[0042] (1) Weigh 700g of the first grain and 300g of the small grain Ni 0.90 Co 0.10(OH)2 precursor, 456.6g lithium hydroxide, 8.329g Al2O3 and 1.435g ZrO2, of which the lithium hydroxide content is 57.68, and the content of aluminum oxide and zirconium oxide is above 99.9%. There are also two specifications of grains in the nickel-cobalt-manganese precursor. The total weight of the first grain is 10.624mol / kg, and the specific surface area is 9.08m 2 / g, tap density is 2.15g / cm 3 The median particle size D50 is 14.58 μm, the total weight of the second crystal is 10.603 mol / kg, and the specific surface area is 7.58 m 2 / g, tap density is 1.90g / cm 3 The median particle size D50 is 2.86 μm, the mass ratio of the first grain to the second grain is 7:3, and the above raw materials are mixed evenly with a high-speed mixer, the speed is set to 1000 r / min for mixing for 2 minutes, then the speed is set to 2000 r / min for mixing for 3 minutes, and the speed is set to 3500 r / min for mixing for 15 minutes, without setting a waiting time in between, to obtain a first mixture.
[0043] (2) The first mixed material obtained in step (1) is heated to 500° C. at a heating rate of 2° C. / min in a box furnace, kept at 500° C. for 4 h, then heated to 730° C. at a heating rate of 2° C. / min, kept at 730° C. for 10 h, the sintering atmosphere is oxygen at a flow rate of 2 L / min, naturally cooled to room temperature, and crushed to obtain a sintered material of a nickel cobalt aluminum oxide positive electrode material.
[0044] The chemical formula of the burnt material prepared in this embodiment was tested by the analytical method of the standard "YS / T·1006.2-2014", and the obtained molecular formula was: Li 1.02 Ni 0.88 Co 0.104 Al 0.015 Zr 0.001 O2.
[0045] (3) The crushed nickel cobalt aluminum oxide positive electrode material was sieved through a filter with a pore size of 45 microns. 500 g of the sieved sintered material, 0.417 g of titanium oxide and 0.296 g of strontium oxide were mixed in a high-speed mixer, and the speed was set to 1000 r / min for 2 min, then the speed was set to 2000 r / min for 3 min, and the speed was set to 3500 r / min for 15 min, without setting a waiting time in between, to obtain a second mixture.
[0046] (4) The second mixed material is calcined in a box furnace with oxygen as the atmosphere. The temperature is raised to 500°C at a heating rate of 2°C / min and kept at that temperature for 6 hours. After natural cooling and screening, a highly conductive positive electrode material is obtained.
[0047] The chemical formula of the highly conductive positive electrode material obtained in this embodiment was tested by the analytical method of the standard "YS / T·1006.2-2014", and the obtained molecular formula was: Li 1.02 Ni 0.88 Co 0.104 Al 0.015 Zr 0.001 O2.
[0048] The obtained high conductive cathode material was scanned by electron scanning electron microscope. Figure 1 .
[0049] Example 3
[0050] This embodiment provides a method for preparing a highly conductive positive electrode material, and the specific steps and parameters are as follows:
[0051] (1) According to the molar ratio of lithium element to nickel and cobalt element in the precursor being 1:1, the molar ratio of aluminum element to lithium element being 0.01:1, and the molar ratio of zirconium element to lithium element being 0.002:1, lithium carbonate, nickel-cobalt-manganese precursor, aluminum hydroxide, and zirconium sulfate are prepared. The chemical formula of the nickel-cobalt-manganese precursor is Ni 0.95 Co 0.01 (OH)2, there are two specifications of grains in the nickel-cobalt-manganese precursor. The total weight of the first grain is 10.582 mol / kg, and the specific surface area of the first grain is 9.85m 2 / g, tap density is 2.23g / cm 3 The median particle size D50 is 13.25 μm, the total weight of the second crystal is 10.630 mol / kg, and the specific surface area is 6.98 m 2 / g, tap density is 1.95g / cm 3 The median particle size D50 is 3.86 μm, the mass ratio of the first crystal grain to the second crystal grain is 7:3, and the above raw materials are mixed evenly with a high-speed mixer, the speed is set to 1200 r / min for mixing for 1 min, then the speed is set to 2200 r / min for mixing for 2 min, and the speed is set to 3200 r / min for mixing for 18 min, without setting a waiting time in between, to obtain a first mixture.
[0052] (2) The first mixed material obtained in step (1) is heated to 400° C. at a heating rate of 2° C. / min in a box furnace, kept at 400° C. for 6 h, then heated to 750° C. at a heating rate of 2° C. / min, kept at 750° C. for 8 h, the sintering atmosphere is oxygen at a flow rate of 2 L / min, naturally cooled to room temperature, and crushed to obtain a sintered material of a nickel cobalt aluminum oxide positive electrode material.
[0053] (3) The crushed nickel cobalt aluminum oxide positive electrode material is sieved through a filter with a pore size of 45 microns. The sieved sintered material is taken, and titanium tetrachloride is weighed according to a titanium element doping amount of 500ppm, and strontium carbonate is weighed according to a strontium element doping amount of 500ppm. The sintered material, titanium oxide and strontium oxide are mixed in a high-speed mixer, and the speed is set to 800r / min for 3min, then the speed is set to 1800r / min for 4min, and the speed is set to 3800r / min for 12min, without setting a waiting time in between, to obtain a second mixture.
[0054] (4) The second mixed material is calcined in a box furnace with oxygen as the atmosphere. The temperature is raised to 600°C at a heating rate of 2°C / min and kept at this temperature for 5 hours. After natural cooling and screening, a highly conductive positive electrode material is obtained.
[0055] Example 4
[0056] This embodiment provides a method for preparing a highly conductive positive electrode material, and the specific steps and parameters are as follows:
[0057] (1) According to the molar ratio of lithium element to nickel and cobalt element in the precursor of 1.1:1, the molar ratio of aluminum element to lithium element of 0.02:0.95, and the molar ratio of zirconium element to lithium element of 0.001:1.05, lithium acetate, nickel cobalt manganese precursor, aluminum chloride, and zirconium nitrate are taken, wherein the chemical formula of the nickel cobalt manganese precursor is Ni 0.7 Co 0.05 (OH)2, there are two specifications of grains in the nickel-cobalt-manganese precursor. The total weight of the first grain is 10.721 mol / kg, and the specific surface area of the first grain is 8.25m 2 / g, tap density is 2.02g / cm 3 The median particle size D50 is 15.87 μm, the total weight of the second crystal is 10.612 mol / kg, and the specific surface area is 6.53 m 2 / g, tap density is 1.35g / cm 3 The median particle size D50 is 2.14 μm, the mass ratio of the first grain to the second grain is 7:3, and the above raw materials are mixed evenly with a high-speed mixer, the speed is set to 1200 r / min for mixing for 1 min, then the speed is set to 2000 r / min for mixing for 2 min, and the speed is set to 3300 r / min for mixing for 16 min, without setting a waiting time in between, to obtain a first mixture.
[0058] (2) The first mixed material obtained in step (1) is heated to 600° C. at a heating rate of 2° C. / min in a box furnace, kept at 600° C. for 3 h, then heated to 710° C. at a heating rate of 2° C. / min, kept at 710° C. for 12 h, the sintering atmosphere is oxygen at a flow rate of 2 L / min, naturally cooled to room temperature, and crushed to obtain a sintered material of a nickel cobalt aluminum oxide positive electrode material.
[0059] (3) The crushed nickel cobalt aluminum oxide positive electrode material is sieved through a filter with a pore size of 45 microns. The sieved sintered material is taken, and titanium oxide is weighed according to a titanium element doping amount of 500ppm, and strontium oxide is weighed according to a strontium element doping amount of 500ppm. The sintered material, titanium oxide and strontium oxide are mixed in a high-speed mixer, and the speed is set to 1200r / min for 1min, then the speed is set to 2200r / min for 2min, and the speed is set to 3200r / min for 18min, without setting a waiting time in between, to obtain a second mixture.
[0060] (4) The second mixed material is calcined in a box furnace with oxygen as the atmosphere. The temperature is raised to 400°C at a heating rate of 2°C / min and kept at this temperature for 8 hours. After natural cooling and screening, a highly conductive positive electrode material is obtained.
[0061] Example 5
[0062] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those of Embodiment 1, except that in step (1), the mass ratio of the first crystal grain to the second crystal grain is 8:2.
[0063] Example 6
[0064] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those of Embodiment 1, except that in step (1), the mass ratio of the first crystal grain to the second crystal grain is 6:4.
[0065] Example 7
[0066] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those in Embodiment 1, except that step (1) does not contain aluminum oxide.
[0067] Example 8
[0068] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those in Embodiment 1, except that step (1) does not contain zirconium oxide.
[0069] Example 9
[0070] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those in Embodiment 1, except that step (2) does not contain zirconium oxide or aluminum oxide, that is, the raw materials are only lithium hydroxide and nickel-cobalt precursors.
[0071] Example 10
[0072] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those in Embodiment 1, except that the doping amount of strontium element and the doping amount of titanium element in step (1) are both 800 ppm.
[0073] Embodiment 11
[0074] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those in Embodiment 1, except that the doping amount of strontium element and the doping amount of titanium element in step (3) are both 2000 ppm.
[0075] Example 12
[0076] This embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those in Embodiment 1, except that the doping amount of strontium element and the doping amount of titanium element in step (3) are both 300 ppm.
[0077] Comparative Example 1
[0078] The present embodiment provides a method for preparing a highly conductive positive electrode material. The specific steps and parameters are the same as those of Embodiment 1, except that step (3) is not included, that is, the first-burnt material obtained in step (2) is second-burned in a box furnace, oxygen is selected as the atmosphere, and the temperature is increased to 500° C. at a heating rate of 2° C. / min, and the temperature is kept for 6 hours. The highly conductive positive electrode material is obtained after natural cooling and sieving.
[0079] Comparative Example 2
[0080] The present embodiment provides a method for preparing a highly conductive positive electrode material, wherein the specific steps and parameters are the same as those of the embodiment 1, except that step (3) does not contain titanium oxide, that is, a sifted burnt material is taken, strontium oxide is weighed according to a strontium element doping amount of 1000 ppm, the burnt material and strontium oxide are mixed in a high-speed mixer, the speed is set to 1000 r / min for mixing for 2 min, then the speed is set to 2000 r / min for mixing for 3 min, and the speed is set to 3500 r / min for mixing for 15 min, without setting a waiting time in between, to obtain a second mixture.
[0081] Comparative Example 3
[0082] The present embodiment provides a method for preparing a highly conductive positive electrode material, wherein the specific steps and parameters are the same as those of the embodiment 1, except that step (3) does not contain strontium oxide, that is, a sifted burnt material is taken, titanium oxide is weighed according to a titanium element doping amount of 1000 ppm, the burnt material and titanium oxide are mixed in a high-speed mixer, the speed is set to 1000 r / min for mixing for 2 min, then the speed is set to 2000 r / min for mixing for 3 min, and the speed is set to 3500 r / min for mixing for 15 min, without setting a waiting time in between, to obtain a second mixture.
[0083] Experimental example
[0084] The highly conductive positive electrode materials prepared in Examples 1-12 and Comparative Examples 1-3 were respectively subjected to electrical performance tests according to the following methods: the positive electrode material: polyvinylidene fluoride: conductive carbon black were homogenized in a mass ratio of 95:3:2, and then the aluminum foil was spread flat on a coating machine for coating (surface density 13.3-13.5 mg / cm 2 , compacted density 3.4-3.6mg / cm 2 ), put it into an 80℃ forced air drying oven and dry it for 3h; then punch, weigh, bake the electrode and make it into a button battery.
[0085] When the cut-off voltage is in the range of 2.5V-4.25V, the charging and discharging process is the first cycle (0.2C / 0.2C), the second cycle (0.2C / 1C), the third cycle (0.2C / 1C), and the fourth to the 53rd cycle (1C / 1C), and the electrical performance test is carried out using the blue electric test system.
[0086] At the same time, the voltage of 10-second 1C discharge is increased in the 53rd cycle, and the DC resistance (DCR) value of the button battery is obtained by using the voltage / current.
[0087] The results are shown in Table 1.
[0088] The capacity retention rates of Example 1 and Comparative Example 1 obtained from each cycle test within 50 cycles are plotted as shown in FIG. Figure 2 .
[0089] Table 1 Test results
[0090]
[0091] According to Table 1 and Figure 2It can be seen that compared with Comparative Example 1, the high-conductivity positive electrode material provided by the present invention has greatly improved conductivity. Compared with Comparative Examples 2-3, the high-conductivity positive electrode material provided by the present invention has greatly improved performance stability and capacity. It can be seen from the embodiments that in the nickel-cobalt precursor, different grading ratios have a certain influence on the conductivity, cycle stability or capacity. When the mass ratio of large-sized grains to small-sized grains is 7:3, all performances are best. It can be seen from the measurement results of Examples 1 and 8 that doping with metal zirconium elements plays an important role in improving the performance of the positive electrode material. This may be because as the charge and discharge proceed, a certain amount of doping ions Zr 4+ It may also migrate to the electrode surface and form a solid solution, preventing the structural collapse caused by the anisotropic structural change during charge and discharge. At the same time, the solid solution also acts as a protective coating to prevent cobalt from dissolving into the electrolyte. Therefore, the material structure becomes very stable during the phase change of the cycle process, and the cycle stability is enhanced. At the same time, the particle size of the material becomes smaller after ZrO2 doping. After the particle size becomes smaller, the material is easier to deintercalate during the charge and discharge process, so the discharge specific capacity of the doped material increases.
[0092] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a highly conductive positive electrode material, It is characterized in that The following steps are included: The positive electrode material is mixed with a coating material, and calcined. The coating material comprises a titanium-containing compound and a strontium-containing compound.
2. The method for preparing the highly conductive positive electrode material according to claim 1, It is characterized in that The doping amount of titanium element in the highly conductive positive electrode material is 300-2000ppm; and / or, The doping amount of strontium element is 300-2000ppm.
3. The method for preparing a highly conductive positive electrode material according to claim 2, It is characterized in that The titanium-containing compound is at least one of titanium dioxide, titanium tetrachloride and barium titanate; and / or, The strontium-containing compound includes at least one of strontium oxide, strontium carbonate, strontium nitrate, strontium chloride and strontium hydroxide; and / or, The doping amount of the titanium element is 500-800 ppm; and / or, The doping amount of strontium element is 500-800ppm.
4. The method for preparing a highly conductive positive electrode material according to any one of claims 1 to 3, It is characterized in that The calcination temperature is 400-600°C and the calcination time is 5-8h; The positive electrode material and the coating material are mixed under gradient stirring, and the gradient stirring process is as follows: the positive electrode material and the coating material are mixed at a rotation speed of 800-1200 rpm for 1-3 min, at a rotation speed of 1800-2200 rpm for 2-4 min, and at a rotation speed of 3200-3800 rpm for 12-18 min.
5. The method for preparing a highly conductive positive electrode material according to claim 4, It is characterized in that The positive electrode material is prepared by mixing and calcining a lithium source, a nickel-cobalt precursor and a doping material.
6. The method for preparing the highly conductive positive electrode material according to claim 5, It is characterized in that The doping material is at least one of an aluminum-containing compound and a zirconium-containing compound; and / or, The nickel-cobalt precursor includes first crystal grains and second crystal grains, and the mass ratio of the first crystal grains to the second crystal grains is (6-8):(2-4), wherein the median particle size of the first crystal grains is 13 to 16 μm, and the median particle size of the second crystal grains is 2 to 4 μm.
7. The method for preparing a highly conductive positive electrode material according to claim 6, It is characterized in that The molar amount of lithium in the lithium source is n, the total molar ratio of nickel and cobalt in the nickel-cobalt precursor and the metal element in the doping material is N, n:N=(1.0-1.1):1; and / or, The molar ratio of aluminum element to lithium element in the aluminum-containing compound is (0.01-0.02): (0.95-1.05); and / or, The molar ratio of zirconium element to lithium element in the zirconium-containing compound is (0.001-0.002): (0.95-1.05); and / or, The specific surface area of the nickel-cobalt precursor is 5-10m 2 / g; and / or, The tap density of the nickel-cobalt precursor is 1-3 g / cm 3 .
8. The method for preparing a highly conductive positive electrode material according to claim 7, It is characterized in that In the preparation of the positive electrode material, the calcination process is: calcining at 400-600° C. for 3-5 hours, and then calcining at 710-750° C. for 8-12 hours; and / or, The lithium source includes at least one of lithium hydroxide, lithium carbonate or lithium acetate.
9. The method for preparing a highly conductive positive electrode material according to claim 8, It is characterized in that The chemical formula of the positive electrode material is Li 1+y (Ni a Co b Al 1-a-b-c Zr c ) 1-y O 2 , where 0≤y≤0.2, 0.7≤a≤0.95, 0.01≤b≤0.1, 0≤c≤0.05; The aluminum-containing compound is at least one of aluminum oxide, aluminum hydroxide, aluminum chloride, and aluminum sulfate; The zirconium-containing compound is at least one of zirconium oxide, zirconium sulfate, zirconium nitrate or zirconium fluoride.
10. A lithium battery, It is characterized in that It comprises a high-conductivity positive electrode material, and the high-conductivity positive electrode material is prepared by the preparation method of the high-conductivity positive electrode material according to any one of claims 1 to 9.
Citation Information
Cited By
Surface modification method of positive electrode
CN119673972A