High MFR polypropylene for meltblown nonwoven applications
By using Ziegler-Natta catalyst to prepare high melt flow rate polypropylene polymers, the problems of low efficiency of metallocene catalysts and expensive peroxide cracking in the prior art are solved, and higher melt flow rate and Wide operating temperature window, improving productivity and polymer stability.
Patent Information
- Application Number
- CN202380033429.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-11
- Filing Date
- 2023-02-10
- Publication Date
- 2024-11-22
AI Technical Summary
Prior Art When producing high melt flow rate polypropylene polymers, the use of metallocene catalysts has low efficiency, time-consuming and expensive equipment conversion, and is susceptible to reactor operability, while peroxide cracking technology is expensive and requires careful control. , and unreacted peroxides may cause degradation problems.
The Ziegler-Natta catalyst is used to prepare high melt flow rate polypropylene polymers. By adjusting the catalyst composition and reaction conditions, a polymer with a wide operating temperature window and molecular weight distribution is prepared, avoiding the use of peroxides and improving production efficiency .
A higher melt flow rate and wide operating temperature window are achieved, which reduces production costs and equipment conversion time, avoids degradation problems caused by peroxides, and improves the stability and processing convenience of polymers.
Smart Images

Figure CN119013320A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 309,378, filed on February 11, 2022, which is incorporated herein by reference in its entirety for any and all purposes. Technical Field
[0003] The present technology generally relates to polyolefin polymers, such as polypropylene polymers. More specifically, the technology relates to high melt flow rate (MFR) polypropylene polymers that can be used in meltblown nonwoven applications. Background Art
[0004] Polyolefin polymers are used in many different applications and fields. For example, polyolefin polymers are thermoplastic polymers that can be easily processed. Polyolefin polymers can also be recycled and reused. Polyolefin polymers are formed from hydrocarbons such as ethylene and alpha-olefins, which are obtained from petrochemicals and are produced in abundance.
[0005] Polypropylene polymer is a polyolefin polymer, usually having a linear structure based on propylene monomer. Polypropylene polymer can have various stereospecific configurations. For example, polypropylene polymer can be isotactic, syndiotactic and atactic. Isotactic polypropylene may be the most common form and can be highly crystalline. Polypropylene polymers that can be produced include homopolymers, modified polypropylene polymers and polypropylene copolymers including polypropylene terpolymers. By modifying polypropylene or copolymerizing propylene with other monomers, various polymers with desired properties for specific applications can be manufactured.
[0006] At present, there is a special demand and need for polypropylene polymers with very high melt flow rates. The melt flow rate of a polymer generally represents the amount of molten polymer that flows over a period of time at a specific temperature and load. A higher melt flow rate can indicate that the polymer can be easily processed, especially in extrusion, injection molding processes, and in the formation of fibers and films. High melt flow rate polypropylene polymers are particularly suitable for making meltblown webs. Meltblown nonwoven webs are generally formed by molten thermoplastic polymers, which are extruded in the form of molten fibers through a plurality of thin, usually circular spinning holes (dye capillaries). When the fibers are formed, the fibers contact a high-speed gas, such as air, which thins the fibers to reduce their diameter. The meltblown fibers are subsequently deposited onto a collecting surface, which forms a web of randomly dispersed meltblown fibers. The meltblown fibers can be continuous or discontinuous. Meltblown webs are particularly suitable for filtration applications.
[0007] For example, meltblown webs can be incorporated into masks designed to cover the nose and mouth of the wearer. When incorporated into masks, meltblown webs are well suited to protect the wearer by preventing the passage of microorganisms (such as viruses) and other contaminants. Due to the coronavirus pandemic, masks are now worn not only by medical professionals, but also by office workers, industrial workers, students, and consumers in almost all public places.
[0008] In the past, in order to produce polypropylene polymers with high melt flow rate for the manufacture of melt-blown webs, metallocene catalysts were used to form polymers, or peroxide cracking was imposed on polymers. When using metallocene catalysts (which are also referred to as single-site catalysts), polymerization may be relatively slow, and inefficient due to low raw material utilization. In addition, it may be time-consuming and expensive to convert equipment to produce polymers using Ziegler-Natta catalysts and metallocene catalysts. In addition, metallocene catalysts may be susceptible to the impact of reactor operability problems, and are incompatible with any known activity limiting agents. Metallocene catalysts may also be sensitive to raw material impurities.
[0009] The peroxide cracking technology of producing high melt flow rate polypropylene polymer also has various disadvantages.For example, peroxide may be expensive.In addition, the peroxide feeding during this process must be carefully controlled so that enough peroxide of feeding is to realize the stable production of high melt flow rate polymer.In addition, unreacted peroxide may remain in the final material, which causes degradation over time, causing undesirable taste, smell and volatile components.Finally, peroxide cracking may cause unwanted volatiles, which may need to be removed by thermal oxidation process to meet environmental regulations.
[0010] In view of the above, there is a need for a more efficient process for producing high melt flow rate polypropylene polymers. There is also a need for polypropylene polymer compositions containing high melt flow rate polypropylene polymers that can be used to produce all different types of articles, including meltblown webs.
[0011] The high melt flow rate polypropylene polymers described herein may have the following advantages in the case of multilayer spun-melt-spun (SMS) fabrics. Compared to reactor-grade meltblown polypropylene polymers produced with metallocene catalysts, the reactor-grade ultra-high MFR polypropylene polymers described herein produced with Ziegler-Natta catalysts can provide a wider operating temperature window in the multilayer spunbond-meltblown-spunbond (SMS) fabric (SBNW-MB-SBNW layer; SBNW = spunbond nonwoven, MB = meltblown) calendering / bonding step. Because most SBNW layers are produced with polypropylene polymers based on cracking-grade Ziegler-Natta catalysts, the reactor-grade polypropylene polymers used in the present invention for meltblowing (MB) applications have a wider molecular weight distribution (MWD) than the metallocene polypropylene polymer counterparts, which contributes to a wider bonding temperature window. SUMMARY OF THE INVENTION
[0013] The present disclosure generally relates to methods for producing high melt flow rate polyolefin polymers, and to polymers produced by the method. The high melt flow rate polyolefin polymers can be used for many different applications. For example, the high melt flow rate polypropylene polymers described herein prepared with Ziegler-Natta catalysts have a wider molecular weight distribution than polypropylene polymers prepared using metallocene catalysts. This is particularly useful for producing multi-layer spunbond-meltblown-spunbond (SMS) fabrics, wherein the meltblown layer comprises the high melt flow rate polypropylene polymers described herein and therefore provides a wider operating temperature window in the bonding step.
[0014] In one aspect, a polymer composition is provided comprising a polypropylene polymer having the following characteristics: exhibiting a melt flow rate greater than about 900 g / 10 mmin; having a molecular weight distribution (MDR) greater than about 4.5 or 6 w / M n ); having an M of less than about 8 z+1 / M w and having a xylene soluble content of less than about 4.0 wt %.
[0015] In some embodiments, the polypropylene polymer exhibits a melt flow rate greater than about 1300 g / 10 min. In some embodiments, the polypropylene polymer exhibits a melt flow rate of about 1300 g / 10 min to about 4000 g / 10 min.
[0016] In some embodiments, the polypropylene polymer has an M greater than about 6. w / M n In some embodiments, the polypropylene polymer has an M greater than about 7. w / M nIn some embodiments, the polypropylene polymer has an M of about 6.0 to about 10.0. w / M n .
[0017] In some embodiments, the polypropylene polymer has an M of less than about 7. z+1 / M w In some embodiments, the polypropylene polymer has an M of about 6.0 to about 8.0. z+1 / M w Compare.
[0018] In some embodiments, the polypropylene polymer has a xylene soluble content of about 1.5 wt% to about 4 wt%. In some embodiments, the polypropylene polymer exhibits a melting temperature greater than about 155°C. In some embodiments, the polypropylene polymer exhibits a melting temperature of about 155°C to about 168°C.
[0019] In some embodiments, the polypropylene polymer has a weight average molecular weight of less than about 80,000 g / mol. In some embodiments, the polypropylene polymer has a weight average molecular weight of about 55,000 to about 70,000 g / mol as measured by gel permeation chromatography (GPC).
[0020] In some embodiments, the polypropylene polymer has a number average molecular weight of less than about 8500 g / mol. In some embodiments, the polypropylene polymer has a number average molecular weight of about 7,000 to about 8,000 g / mol.
[0021] In some embodiments, the polypropylene polymer is a polypropylene homopolymer. In some embodiments, the polypropylene polymer has been Ziegler-Natta catalyzed. In some embodiments, the polypropylene polymer has been catalyzed in the presence of a Ziegler-Natta catalyst comprising an internal electron donor comprising a substituted phenylene diester or phthalate compound.
[0022] In some embodiments, the polypropylene polymer comprises a processing aid in combination with at least one other polymer exhibiting a lower melt flow rate, the polypropylene polymer being included in the composition in an amount less than about 50 wt %. In some embodiments, the polypropylene polymer comprises a wax, a lubricant, a mold release agent, or a flow aid.
[0023] In some embodiments, the polypropylene polymer has been catalyzed in the presence of a Ziegler-Natta catalyst, the Ziegler-Natta catalyst comprising a solid catalyst component, a magnesium portion, a titanium portion and an internal electron donor, a selectivity control agent and an optional activity limiting agent. In some embodiments, the solid catalyst component further comprises an organosilicon compound and an epoxy compound. In some embodiments, the selectivity control agent comprises an organosilicon compound. In some embodiments, the selectivity control agent comprises propyltriethoxysilane, diisobutyldimethoxysilane, n-propyltrimethoxysilane or a mixture thereof, and is used in combination with an activity limiting agent.
[0024] In some embodiments, the polypropylene polymer does not contain any peroxide.In some embodiments, the composition is suitable for meltblown nonwoven applications.
[0025] In one aspect, a meltblown web comprised of nonwoven meltblown fibers made from any of the polymer compositions described herein is provided.
[0026] In one aspect, meltblown fibers made from any of the polymer compositions described herein are provided, the meltblown fibers having a diameter of less than about 5 microns.
[0027] In some embodiments, the meltblown fibers have a diameter of less than about 3 microns. In some embodiments, the meltblown fibers have a diameter of about 1.5 to about 3.0 microns.
[0028] In one aspect, a nonwoven web is provided that includes a multi-layer structure, the multi-layer structure including: one or more meltblown layers, the meltblown layers comprising any one of the meltblown fibers described herein.
[0029] In some embodiments, the nonwoven web comprises a meltblown layer. In some embodiments, the nonwoven web comprises two or more meltblown layers. In some embodiments, two or more meltblown layers comprise the same meltblown layer. In some embodiments, two or more meltblown layers comprise different meltblown layers.
[0030] In some embodiments, the nonwoven web further comprises two or more spunbond layers comprising spunbond fibers. In some embodiments, the spunbond fibers are prepared from a polymer composition comprising a polypropylene polymer having one or more of the following characteristics: exhibiting a melt flow rate of about 20 g / 10 min to about 70 g / 10 min; having a molecular weight distribution (M) of less than about 4; w / M n ); and having a xylene soluble content of about 1.5 wt % to about 4 wt %.
[0031] In some embodiments, the polypropylene polymer has an M of about 3.0 to about 4.0. w / M n . In some embodiments, the polypropylene polymer has a weight average molecular weight of less than about 300,000 g / mol. In some embodiments, the polypropylene polymer has a weight average molecular weight of about 150,000 to about 250,000 g / mol. In some embodiments, the polypropylene polymer has a number average molecular weight of less than about 60,000 g / mol. In some embodiments, the polypropylene polymer has a number average molecular weight of about 40,000 to about 55,000 g / mol. In some embodiments, the polypropylene polymer exhibits a melting temperature greater than 155°C. In some embodiments, the polypropylene polymer can be made with a metallocene catalyst and exhibit a melting temperature of about 155°C or less.
[0032] In some embodiments, the nonwoven web comprises two or more spunblown layers. In some embodiments, the two or more spunblown layers comprise the same spunblown layer. In some embodiments, the two or more spunblown layers comprise different spunblown layers.
[0033] In some embodiments, the nonwoven web has a multilayer structure including a first spunbond layer, a meltblown layer, and a second spunbond layer. In some embodiments, the first spunbond layer and the second spunbond layer are the same. In some embodiments, the first spunbond layer and the second spunbond layer are different.
[0034] In some embodiments, the nonwoven web has a density of less than about 100 1 / m 2 / s air permeability. In some embodiments, the nonwoven web has an air permeability of about 40 to about 80 l / m 2 / s air permeability. In some embodiments, the nonwoven web has a machine direction (MD) tensile strength of about 2500 g / inch to about 3500 g / inch.
[0035] In another aspect, a method for producing any of the nonwoven webs disclosed herein is provided, comprising contacting one or more meltblown layers with two or more spunbond layers at a bonding temperature of about 130°C to about 140°C.
[0036] In some embodiments, the bonding temperature is about 135°C.
[0037] In one aspect, a process for producing a polypropylene polymer is provided, comprising: polymerizing propylene monomer in the presence of a Ziegler-Natta catalyst comprising a solid catalyst component comprising a magnesium moiety, a titanium moiety, and an internal electron donor, a selectivity control agent, and optionally an activity limiting agent, the solid catalyst component comprising a magnesium moiety, a titanium moiety, and an internal electron donor, the selectivity control agent comprising an organosilicon compound, and wherein a polypropylene polymer is formed that exhibits a melt flow rate greater than about 900 g / 10 min, and wherein no peroxide is used during the process of forming the polypropylene polymer.
[0038] In some embodiments, the solid catalyst component further comprises an organosilicon compound and an epoxy compound. In some embodiments, the internal electron donor comprises a substituted phenylene diester or phthalate compound. In some embodiments, the selectivity control agent comprises an organosilicon compound, and wherein a polypropylene polymer exhibiting a melt flow rate greater than about 1000 g / 10 min is formed.
[0039] In some embodiments, the H2 / C3 molar ratio during the polymerization is from about 0.1 to about 0.3. In some embodiments, the cocatalyst and the external electron donor are fed to the polymerization reactor at a molar ratio of from about 1.5 to about 15. In some embodiments, the reactor temperature during the polymerization is from about 65° C. to about 95° C. In some embodiments, the temperature is increased to increase the melt flow rate. In some embodiments, the propylene partial pressure is reduced to increase the melt flow rate of the polypropylene polymer.
[0040] BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 is a perspective view of a mask that can be made from the polymer composition of the present disclosure.
[0042] Figure 2 is a graphical representation of some of the results obtained in the following examples and shows the relationship between melt flow rate and H2 / C3 molar ratio.
[0043] Figure 3 is a graphical representation of some of the results obtained in the following examples and shows the relationship between melt flow rate and xylene solubles; and
[0044] Figure 4 is a graphical representation of some of the results obtained in the following examples and shows the relationship between fines and melt flow rate.
[0045] Figure 5 is a depiction of the tensile test template used in the machine direction (MD) tensile strength testing described in the Examples. DETAILED DESCRIPTION OF THE INVENTION
[0047] Various embodiments are described below. It should be noted that the specific embodiments are not intended as an exhaustive description or as a limitation to the broader aspects discussed herein. An aspect described in conjunction with a specific embodiment is not necessarily limited to that embodiment and can be practiced with any other one or more embodiments.
[0048] As used herein, "about" will be understood by one of ordinary skill in the art and will vary to some extent depending on the context in which it is used. If the use of the term is unclear to one of ordinary skill in the art, "about" means up to + or - 10% of the particular item, given the context in which it is used.
[0049] Unless otherwise specified herein or obviously contradicted with the context, the terms "one" and "a kind of" and "the" and similar indicators used in the text describing the elements (especially in the text of the following claims) should be interpreted as covering the singular and plural. Unless otherwise specified herein, the enumeration of the numerical ranges herein is only intended to serve as a shorthand for referring to each individual numerical value falling within the range one by one, and each individual numerical value is incorporated into this specification as if it is enumerated one by one in this article. Unless otherwise specified herein or obviously contradicted with the context, all methods described herein can be carried out in any suitable order. Unless otherwise specified, the use of any and all examples or exemplary wordings (such as "such as") provided herein is only intended to better illustrate the embodiments, rather than to limit the scope of the claims. The wording in the specification should not be interpreted as indicating that any unclaimed element is essential.
[0050] Typically, "substituted" refers to an alkyl, alkenyl, aryl or ether group (e.g., alkyl) as defined below, wherein one or more bonds to the hydrogen atoms contained therein are replaced by bonds to non-hydrogen or non-carbon atoms. Substituent groups also include groups in which one or more bonds to one or more carbon or hydrogen atoms are replaced by one or more bonds to heteroatoms (including double bonds or triple bonds). Thus, unless otherwise stated, a substituted group is replaced by one or more substituents. In some embodiments, a substituted group is replaced by 1, 2, 3, 4, 5 or 6 substituents. Examples of substituents include: halogen (i.e., F, Cl, Br, and I); hydroxy; alkoxy, alkenyloxy, alkynyloxy, aryloxy, aralkyloxy, heterocyclooxy, and heterocycloalkoxy; carbonyl (oxo); carboxyl; ester; carbamate; oxime; hydroxylamine; alkoxyamine; aralkyloxyamine; thiol; sulfide; sulfoxide; sulfone; sulfonyl; sulfonamide; amine; N-oxide; hydrazine; hydrazide; hydrazone; azide; amide; urea; amidine; guanidine; enamine; imide; isocyanate; isothiocyanate; cyanate; thiocyanate; imine; nitro; nitrile (i.e., CN); and the like.
[0051] As used herein, "alkyl" includes straight and branched chain alkyl groups having 1 to about 20 carbon atoms, typically 1 to 12 carbon atoms, or in some embodiments 1 to 8 carbon atoms. As used herein, "alkyl" includes cycloalkyl groups as defined below. Alkyl groups may be substituted or unsubstituted. Alkyl groups may be substituted once or multiple times. Alkyl groups may be substituted twice or more. Examples of straight chain alkyl groups include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, and n-octyl. Examples of branched chain alkyl groups include, but are not limited to, isopropyl, sec-butyl, tert-butyl, neopentyl, isopentyl, and 1-cyclopentyl-4-methylpentyl. Representative substituted alkyl groups may be substituted once or multiple times by, for example, amino, thio, hydroxyl, cyano, alkoxy, and / or halogen groups such as F, Cl, Br, and I groups. The term haloalkyl group as used herein is an alkyl group having one or more halogen groups. In some embodiments, haloalkyl refers to a perhaloalkyl group.
[0052] Cycloalkyl is a cyclic alkyl group, such as but not limited to cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl and cyclooctyl. In some embodiments, cycloalkyl has 3 to 8 ring members, and in other embodiments, the number of ring carbon atoms is 3 to 5, 6 or 7. Cycloalkyl can be substituted or unsubstituted. Cycloalkyl further includes polycyclic cycloalkyl, such as but not limited to norbornyl, adamantyl, bornyl, camphenyl, isocamphenyl and carenyl, and condensed ring, such as but not limited to decalinyl etc. Cycloalkyl also includes the ring substituted by straight or branched alkyl as defined above. Representative substituted cycloalkyl groups can be monosubstituted or substituted more than once, such as, but not limited to, 2,2-; 2,3-; 2,4-; 2,5-; or 2,6-disubstituted cyclohexyl groups or mono-, di- or trisubstituted norbornyl or cycloheptyl groups, which can be substituted, for example, with alkyl, alkoxy, amino, thio, hydroxy, cyano and / or halo groups.
[0053] Alkenyl is a straight chain, branched or cyclic hydrocarbon group having 2 to about 20 carbon atoms and further comprising at least one double bond. In some embodiments, the alkenyl has 1 to 12 carbon atoms, or generally 1 to 8 carbon atoms. The alkenyl group may be substituted or unsubstituted. Alkenyl includes, for example, vinyl, propenyl, 2-butenyl, 3-butenyl, isobutenyl, cyclohexenyl, cyclopentenyl, cyclohexadienyl, butadienyl, pentadienyl and hexadienyl, etc. The alkenyl group may be substituted similarly to the alkyl group. A divalent alkenyl group, i.e., an alkenyl group having two points of attachment, includes but is not limited to CH-CH=CH 2 、C=CH 2 or C=CHCH 3 .
[0054] As used herein, "aryl" or "aromatic" groups are cyclic aromatic hydrocarbons that do not contain heteroatoms. Aryl includes monocyclic, bicyclic and polycyclic systems. Thus, aryl includes, but is not limited to, phenyl, azulenyl, heptalenyl, biphenylene, indacenyl, fluorenyl, phenanthrenyl, triphenylene, pyrenyl, naphthyl, chrysene, biphenyl, anthracenyl, indenyl, indanyl, pentalenyl and naphthyl. Aryl with one or more alkyl groups may also be referred to as alkaryl. In some embodiments, aryl contains 6-14 carbons in the ring portion of the group, and in other embodiments contains 6 to 12 or even 6-10 carbon atoms. The phrase "aryl" includes groups containing fused rings, such as fused aromatic-aliphatic ring systems (e.g., indanyl, tetrahydronaphthyl, etc.). Aryl can be substituted or unsubstituted.
[0055] Heterocyclyl or heterocycle refers to aromatic and non-aromatic ring compounds, including monocyclic, bicyclic and polycyclic compounds containing 3 or more ring members, one or more of which is a heteroatom such as, but not limited to, N, O and S. Examples of heterocyclic groups include, but are not limited to, unsaturated 3- to 8-membered rings containing 1 to 4 nitrogen atoms, such as, but not limited to, pyrrolyl, pyrrolinyl, imidazolyl, pyrazolyl, pyridyl, dihydropyridyl, pyrimidinyl, pyrazinyl, pyridazinyl, triazolyl (e.g., 4H-1,2,4-triazolyl, 1H-1,2,3-triazolyl, 2H-1,2,3-triazolyl, etc.), tetrazolyl (e.g., 1H-tetrazolyl, 2H-tetrazolyl, etc.); saturated 3- to 8-membered rings containing 1 to 4 nitrogen atoms, such as, but not limited to, pyrrolidinyl, imidazolidinyl, piperidinyl, piperazinyl; fused unsaturated heterocyclic groups containing 1 to 4 nitrogen atoms, such as, but not limited to, indolyl, isoindolyl, dihydroindolyl, indolizinyl , benzimidazolyl, quinolyl, isoquinolyl, indazolyl, benzotriazolyl; unsaturated 3 to 8 membered rings containing 1 to 2 oxygen atoms and 1 to 3 nitrogen atoms, such as but not limited to oxazolyl, isoxazolyl, oxadiazolyl (e.g., 1,2,4-oxadiazolyl, 1,3,4-oxadiazolyl, 1,2,5-oxadiazolyl, etc.); saturated 3 to 8 membered rings containing 1 to 2 oxygen atoms and 1 to 3 nitrogen atoms, such as but not limited to morpholinyl; unsaturated fused heterocyclic groups containing 1 to 2 oxygen atoms and 1 to 3 nitrogen atoms, such as benzoxazolyl, benzoxadiazolyl, benzoxazinyl (e.g., 2H-1,4-benzoxazinyl, etc.); unsaturated 3 to 8 membered rings containing 1 to 2 oxygen atoms and 1 to 3 nitrogen atoms, such as but not limited to morpholinyl; 3 to 8 membered rings, such as but not limited to thiazolyl, isothiazolyl, thiadiazolyl (e.g. 1,2,3-thiadiazolyl, 1,2,4-thiadiazolyl, 1,3,4-thiadiazolyl, 1,2,5-thiadiazolyl, etc.); saturated 3 to 8 membered rings containing 1 to 2 sulfur atoms and 1 to 3 nitrogen atoms, such as but not limited to thiazolodinyl; saturated and unsaturated 3 to 8 membered rings containing 1 to 2 sulfur atoms, such as but not limited to thienyl, dihydrodithiinyl, dihydrodisulfinyl, tetrahydrothiophene, tetrahydrothiopyran; unsaturated fused heterocyclic rings containing 1 to 2 sulfur atoms and 1 to 3 nitrogen atoms, such as but not limited to in benzothiazolyl, benzothiadiazolyl, benzothiazinyl (e.g., 2H-1,4-benzothiazinyl, etc.), dihydrobenzothiazinyl (e.g., 2H-3,4-dihydrobenzothiazinyl, etc.); unsaturated 3 to 8-membered rings containing oxygen atoms, such as, but not limited to, furanyl; unsaturated fused heterocyclic rings containing 1 to 2 oxygen atoms, such as benzodioxolyl (e.g., 1,3-benzodioxolyl, etc.); unsaturated 3 to 8-membered rings containing oxygen atoms and 1 to 2 sulfur atoms, such as, but not limited to, dihydrooxathiinyl; saturated 3 to 8-membered rings containing 1 to 2 oxygen atoms and 1 to 2 sulfur atoms, such as 1,4-oxathiinane;Unsaturated fused rings containing 1 to 2 sulfur atoms, such as benzothienyl, benzodithiinyl; and unsaturated fused heterocycles containing one oxygen atom and 1 to 2 oxygen atoms, such as benzoxathiinyl. Heterocyclic groups also include those described above (sulfoxides and sulfones) in which one or more S atoms in the ring are double-bonded to one or two oxygen atoms. For example, heterocyclic groups include tetrahydrothiophene oxide and tetrahydrothiophene 1,1-dioxide. Typical heterocyclic groups contain 5 or 6 ring members. Thus, for example, heterocyclic groups include morpholinyl, piperazinyl, piperidinyl, pyrrolidinyl, imidazolyl, pyrazolyl, 1,2,3-triazolyl, 1,2,4-triazolyl, tetrazolyl, thienyl, thiomorpholinyl, thiomorpholinyl in which the S atom of the thiomorpholinyl is bonded to one or more O atoms, pyrrolyl, pyridinyl, homopiperazinyl, oxazolidin-2-onyl, pyrrolidin-2-onyl, oxazolyl, quinuclidinyl, thiazolyl, isoxazolyl, furanyl, dibenzylfuranyl and tetrahydrofuranyl. The heterocyclic group or heterocycle may be substituted. ;
[0056] Heteroaryl groups are aromatic ring compounds containing 5 or more ring members, one or more of which are heteroatoms such as, but not limited to, N, O, and S. Heteroaryl groups include, but are not limited to, groups such as pyrrolyl, pyrazolyl, triazolyl, tetrazolyl, oxazolyl, isoxazolyl, thiazolyl, pyridinyl, pyridazinyl, pyrimidinyl, pyrazinyl, thienyl, benzothienyl, furanyl, benzofuranyl, dibenzofuranyl, indolyl, azaindolyl (pyrrolopyridinyl), indazolyl, benzimidazolyl, imidazopyridinyl (azabenzimidazolyl), pyrazolopyridinyl, triazolopyridinyl, benzotriazolyl, benzoxazolyl, benzothiazolyl, benzothiadiazolyl, imidazopyridinyl, isoxazolopyridinyl, thiazolyl, purinyl, xanthinyl, adeninyl, guaninyl, quinolinyl, isoquinolinyl, tetrahydroquinolinyl, quinoxalinyl, and quinazolinyl. Heteroaryl includes fused ring compounds in which all rings are aromatic, such as indolyl, and includes fused ring compounds in which only one ring is aromatic, such as 2,3-dihydroindole. Although the phrase "heteroaryl group" includes fused ring compounds, the phrase does not include heteroaryl groups having other groups (such as alkyl) bonded to one of the ring members. Heteroaryl groups having such substitutions are referred to as "substituted heteroaryl groups." Representative substituted heteroaryl groups can be substituted one or more times with various substituents, such as those listed above.
[0057] As used herein, the prefix "halo" refers to a halogen (ie, F, Cl, Br, or I) attached to the group modified by the "halo" prefix. For example, haloaryl is a halogenated aryl group.
[0058] Groups having two or more points of attachment (i.e., divalent, trivalent, or multivalent) in the compounds of the present technology described herein are indicated by the use of the suffix "sub". For example, a divalent alkyl group is an alkylene group, a divalent aryl group is an arylene group, a divalent heteroaryl group is a divalent heteroarylene group, and so on.
[0059] Testing Procedure
[0060] As used herein, melt flow rate (MFR) is measured according to ASTM D 1238 test method at 230°C with a 2.16 kg weight for propylene-based polymers. The melt flow rate can be measured in pellet form or on reactor powder. When measuring reactor powder, a stabilizer package can be added containing 2000 ppm of CYANOX 2246 antioxidant (methylene bis(4-methyl-6-tert-butylphenol)), 2000 ppm of IRGAFOS 168 antioxidant (tris(2,4-di-tert-butylphenyl)phosphite), and 1000 ppm of acid scavenger ZnO.
[0061] For high melt flow rate polymers, the test die orifice can be smaller as shown below:
[0062]
[0063]
[0064] Calculations for Polypropylene Polymer:
[0065]
[0066]
[0067] Particle size can be measured using a sieving test. The sieving test is performed on a GRADEX particle size analyzer available from Rotex Global. The average particle size based on weight fraction is determined from the particle size distribution obtained from the GRADEX particle size analyzer.
[0068] Fines are defined as the weight fraction of polymer particles that pass through a GRADEX 120 mesh (125 microns).
[0069] Xylene solubles (XS) are defined as the weight percent of the polypropylene random copolymer resin that remains in solution after dissolving a sample of the resin in hot xylene and allowing the solution to cool to 25° C. Using a 60 minute settling time according to ASTM D5492-06, this is also known as the gravimetric XS method and is also referred to herein as the “wet method.”
[0070] As described below, the above ASTM D5492-06 method can be adapted to determine the xylene soluble portion. Typically, the procedure involves weighing 2 g of sample and dissolving the sample in 200 ml of o-xylene in a 400 ml flask with a 24 / 40 joint. The flask is connected to a water-cooled condenser and the contents are stirred and condensed under nitrogen (N 2 ) was heated to reflux at 25 ° C and then kept at reflux for another 30 minutes. The solution was then cooled in a temperature controlled water bath at 25 ° C for 60 minutes to crystallize the xylene insoluble portion. Once the solution has cooled and the insoluble portion has precipitated from the solution, the xylene soluble portion (XS) was separated from the xylene insoluble portion (XI) by filtering through a 25 micron filter paper. 100 ml of the filtrate was collected in a pre-weighed aluminum pan, and o-xylene was evaporated from the 100 ml of the filtrate under a nitrogen stream. Once the solvent evaporates, the pan and contents are placed in a 100 ° C vacuum oven for 30 minutes or until dry. The pan is then cooled to room temperature and weighed. The xylene soluble portion is calculated as XS (wt %) = [(m3-m2)*2 / m 1]*100, where m1 is the original weight of the sample used, m2 is the weight of the empty aluminum pan, and m3 is the weight of the pan with the residue (the asterisk * here and elsewhere in the present disclosure indicates that the term or value of the logo is multiplied).
[0071] XS can also be measured according to the Viscotek method as follows: 0.4 g of polymer is dissolved in 20 ml of xylene at 130°C under stirring for 60 minutes. The solution is then cooled to 25°C and after 60 minutes the insoluble polymer fraction is filtered off using a 0.2 μm syringe filter. The resulting filtrate is analyzed by flow injection polymer analysis using a Viscotek ViscoGEL H-100-3078 column with a THF mobile phase flowing at 1.0 ml / min. The column is coupled to a Viscotek Model 302 triple detector array with light scattering, viscometer and refractometer detectors operating at 45°C. The Viscotek PolyCAL TM Polystyrene standards maintain instrument calibration. Polypropylene (PP) homopolymers, such as Dow 5D98 grade biaxially oriented polypropylene (BOPP), are used as reference materials to ensure that the Viscotek instrument and sample preparation procedures provide consistent results. Values for reference polypropylene homopolymers such as 5D98 were originally obtained from testing using the ASTM method described above.
[0072] Weight average molecular weight (M w), number average molecular weight (Mn), molecular weight distribution (Mw / Mn) (also called "MWD") and higher average molecular weights (Mz and Mz+1) were measured by GPC according to the gel permeation chromatography (GPC) analytical method for polypropylene. The polymer was analyzed on a Polymer Char high temperature GPC with an IR5MCT (mercury cadmium telluride-high sensitivity thermoelectric cooled IR detector), a Polymer Char four-capillary viscometer, a Wyatt 8-angle MALLS and three Agilent Plgel Olexis (13μm). The oven temperature was set at 150°C. The solvent was nitrogen-purged 1,2,4-trichlorobenzene (TCB) containing approximately 200ppm of 2,6-di-tert-butyl-4-methylphenol (BHT). The flow rate was 1.0mL / min and the injection volume was 200μl. The sample was injected at N 2 Sample concentrations of 2 mg / mL were prepared by dissolving in purged and preheated TCB (containing 200 ppm BHT) at 160°C with gentle stirring for 2 hours.
[0073] The GPC column set is calibrated by running 20 narrow molecular weight distribution polystyrene standards. The molecular weight (MW) of the standards is 266 to 12,000,000 g / mol, and the standards are included in 6 kinds of "mixed liquid" mixtures. Each standard mixture has at least ten times of intervals between each molecular weight. For molecular weights equal to or greater than 1,000,000 g / mol, polystyrene standards are prepared with 0.005 g / 20 mL solvent, and for molecular weights less than 1,000,000 g / mol, polystyrene standards are prepared with 0.001 g / 20 mL solvent. Under stirring, the polystyrene standards are dissolved at 160 ° C for 60 minutes. First run the narrow standard mixture, and run in the order of decreasing the highest molecular weight component to minimize the degradation effect. Use the fourth-order polynomial fit as a function of elution volume to produce logarithmic molecular weight calibration. The equivalent polypropylene molecular weight is calculated by using the following equation and the Mark-Houwink coefficients reported for polypropylene (Th. G. Scholte, NLJ Meijerink, HM Schoffeleers and AMG Brands, J. Appl. Polym. Sci., 29, 3763-3782 (1984)) and polystyrene (EP Ortocka, RJ Roe, NY Hellman, PMMuglia, Macromolecules, 4, 507 (1971)):
[0074]
[0075] Where Mpp is the PP equivalent MW, MPS is the PS equivalent MW, and the log K and a values of the Mark-Houwink coefficients for PP and PS are shown below (GPC data were processed using a procedure modified from ISO 16014-1 with a lower integration limit set at 3500 Daltons to exclude interference from additives).
[0076]
[0077] Melting point or melting temperature and crystallization temperature are determined using differential scanning calorimetry (DSC). The term "crystallinity" refers to the regularity of the arrangement of atoms or molecules that form a crystal structure. DSC can be used to examine polymer crystallinity. me It refers to the temperature at the end of melting, T max refers to the peak melting temperature, both of which are determined by DSC analysis by one of ordinary skill in the art using data from the final heating step. One suitable method for DSC analysis uses a Model Q 1000 from TA Instruments, Inc. TM DSC. The calibration of DSC is carried out in the following manner. First, a baseline is obtained by heating the cell from -90°C to 290°C without any sample in the aluminum DSC pan. A 7 mg fresh indium sample is then analyzed by heating the sample to 180°C, cooling the sample to 140°C at a cooling rate of 10°C / min, then isothermally holding the sample at 140°C for 1 minute, then heating the sample from 140°C to 180°C at a heating rate of 10°C / min. The heat of fusion and the onset of melting of the indium sample are determined and checked, with the onset of melting within 0.5°C of 156.6°C and the heat of fusion within 0.5J / g of 28.71J / g. Deionized water is then analyzed by cooling a small drop of fresh sample in the DSC pan from 25°C to -30°C at a cooling rate of 10°C / min. The sample is isothermally held at -30°C for 2 minutes and heated to 30°C at a heating rate of 10°C / min. The onset of melting was determined and checked to be within 0.5°C of 0°C.
[0078] One method of measuring crystallinity in high crystalline polypropylene polymers is by differential scanning calorimetry (DSC). A small sample (milligram level) of propylene polymer is sealed into an aluminum DSC pan. The sample is placed in a DSC cell with a 25 cm / min nitrogen purge and cooled to approximately -80°C. A standard thermal history of the sample is established by heating to 225°C at 10°C / min. The sample is subsequently cooled to approximately -80°C and reheated to 225°C at 10°C / min. The heat of fusion (ΔH) observed for the second scan is recorded. 观察 The observed heat of fusion is related to the crystallinity in weight percent based on the weight of the polypropylene sample by the following equation:
[0079]
[0080] The heat of fusion (ΔH) of isotactic polypropylene reported in B. Wunderlich, Macromolecular Physics, Vol. 3, Crystal Melting, Academic Press, New Your, 1980, p. 48 is: 全同立构PP ) is 164.92 joules / gram (J / g) of polymer.
[0081] Alternatively, crystallinity can also be determined using the heat of crystallization (HCH) method when heated. In the HCH method, the sample is equilibrated at 200°C and held at this temperature for 3 minutes. After the isothermal step, the data storage is turned on and the sample is dropped to -80°C at 10°C / minute. When -80°C is reached, the data sampling is turned off and the sample is held at this temperature for 3 minutes. After the second isothermal step, the data storage is turned on and the sample is raised to 200°C at 10°C / minute.
[0082] The average fiber diameter can be determined by taking the average of 50 measurements from five SEM images at different locations on the fabric. SEM images were collected on a desktop microscope TM3030Plus (HITACHI). The imaging conditions are listed below: The observation conditions are at a voltage of 5 kV in the standard observation mode, and the image signal is collected from secondary electrons. All images were collected at a magnification of ×2500.
[0083] The tensile strength of the SMS nonwoven fabrics described herein can be determined by the following test method. Figure 5 The SMS fabric is cut in the tensile test template (in inches) as shown, and the length direction is the machine direction (MD) of the fabric. The tensile test was conducted on a Check-Line test station (model: FGS-50PVL) at room temperature (23°C). During the test, the extension rate was set to 100 mm / min, and the maximum breaking strength (peak tension in grams) was recorded as "MD tensile strength" and the elongation at break was recorded as "MD elongation".
[0084] The air permeability of the SMS nonwoven fabrics described herein was determined by the NWSP 70.1 method, wherein the differential pressure was set to 200 Pa and the fabric was cut into pieces with an area of 20 cm 2 The test was carried out at 23°C and 50% RH.
[0085] Polypropylene polymer
[0086] Polyolefin polymers with very high melt flow rates (MFR) are described herein, such as polypropylene polymers (e.g., homopolymers). These ultra-high MFR polypropylene polymers are prepared with Ziegler-Natta catalysts and under peroxide-free conditions. Such high melt flow rate polypropylene polymers are particularly suitable for producing meltblown webs and nonwoven applications.
[0087] The polypropylene polymers described herein may have one or more of the following advantages over polypropylene polymers produced by peroxide cleavage technology: less odor; no harmful volatiles (e.g., butanol) produced by decomposition of peroxide byproducts (e.g., Trigonox 101); and less MFR variation due to the absence of residual peroxide. In addition, the polypropylene polymers described herein are also suitable for preparing multi-layer spunbond-meltblown-spunbond (SMS) fabrics, wherein the meltblown layer is prepared from meltblown fibers comprising the ultra-high MFR polypropylene polymer described herein.
[0088] In one aspect, a polymer composition is provided comprising a polypropylene polymer having the following properties:
[0089] exhibiting a melt flow rate greater than about 900 g / 10 min;
[0090] Having a molecular weight distribution (M) greater than about 4.5 or 6 w / M n );
[0091] Having an M of less than about 8 z+1 / M w than; and
[0092] Having a xylene solubles content of less than about 4.0 weight percent.
[0093] Generally, the present disclosure relates to methods for producing high melt flow rate polyolefin polymers, particularly polypropylene polymers, including polypropylene homopolymers, polypropylene random copolymers, and polypropylene block copolymers. By the methods of the present disclosure, polypropylene polymers having a melt flow rate of greater than about 900 g / 10 min, such as greater than about 1200 g / 10 min, such as greater than about 1500 g / 10 min, such as greater than about 1800 g / 10 min, such as greater than about 2200 g / 10 min, and such as greater than about 4000 g / 10 min can be produced without the use of a single site catalyst and / or without the use of any peroxide. The polypropylene polymer can exhibit a g / 10 min of greater than about 1300 g / 10 min, such as greater than about 1400 g / 10 min, greater than about 1500 g / 10 min, greater than about 1600 g / 10 min, greater than about 1700 g / 10 min, greater than about 1800 g / 10 min, greater than about 1900 g / 10 min, greater than about 2000 g / 10 min, greater than about 2100 g / 10 min, greater than about 2200 g / 10 min, greater than about 2300 g / 10 min, greater than about 2400 g / 10 min, greater than about 2500 g / 10 min, greater than about 2600 g / 10 min, in, greater than about 2700 g / 10 min, greater than about 2800 g / 10 min, greater than about 2900 g / 10 min, greater than about 3000 g / 10 min, greater than about 3100 g / 10 min, greater than about 3200 g / 10 min, greater than about 3300 g / 10 min, greater than about 3400 g / 10 min, greater than about 3500 g / 10 min, greater than about 3600 g / 10 min, greater than about 3700 g / 10 min, greater than about 3800 g / 10 min, greater than about 3900 g / 10 min, and greater than about 4000 g / 10 min.In some embodiments, the polypropylene polymer exhibits a polypropylene polymer of about 1300 g / 10 min to about 2200 g / 10 min, including about 1300 g / 10 min, about 1400 g / 10 min, about 1500 g / 10 min, about 1600 g / 10 min, about 1700 g / 10 min, about 1800 g / 10 min, about 1900 g / 10 min, about 2000 g / 10 min, about 2100 g / 10 min, about 2200 g / 10 min, about 2300 g / 10 min, about 2400 g / 10 min, about 2500 g / 10 min. In some embodiments, the present invention relates to a polypropylene polymer having a melt flow rate (MFR) of about 2000 g / 10min, about 2600 g / 10min, about 2700 g / 10min, about 2800 g / 10min, about 2900 g / 10min, about 3000 g / 10min, about 3100 g / 10min, about 3200 g / 10min, about 3300 g / 10min, about 3400 g / 10min, about 3500 g / 10min, about 3600 g / 10min, about 3700 g / 10min, about 3800 g / 10min, about 3900 g / 10min and about 4000 g / 10min. The MFR can be up to about 7000 g / 10min. Thus, the method of the present invention can produce the polypropylene polymer of very high MFR in a very effective manner. The present disclosure also relates to the polyolefin polymer made by the method.
[0094] The polypropylene polymer (which may be a polypropylene homopolymer) disclosed herein is manufactured using a Ziegler-Natta catalyst. The catalyst generally comprises a solid catalyst component in combination with a selectivity control agent. Optionally, the catalyst may also include an activity limiting agent. A cocatalyst is used to activate the catalyst during polymerization. The solid catalyst component may vary according to a specific application. In some embodiments, the polypropylene polymer has been catalyzed in the presence of a Ziegler-Natta catalyst, the Ziegler-Natta catalyst comprising a solid catalyst component, a selectivity control agent and an optional activity limiting agent, the solid catalyst component comprising a magnesium portion, a titanium portion and an internal electron donor. Typically, the solid catalyst component contains a magnesium portion, a titanium portion and an internal electron donor. On the one hand, the solid catalyst component may optionally include an organophosphorus compound, an organosilicon compound and an epoxy compound. In some embodiments, the solid catalyst component further includes an organosilicon compound and an epoxy compound. In some embodiments, the internal electron donor includes an aromatic diester, a diether, a succinate, an organic acid ester, a polycarboxylic acid ester, a polyhydroxy ester, a heterocyclic polycarboxylic acid ester, a compound having at least one ether group and at least one keto group, or a mixture of any two or more thereof. In some embodiments, at least one additional internal electron donor comprises an aryl diester, an acylated catechol, a carbonated catechol, or an alkoxyalkyl ether. In some embodiments, at least one additional internal electron donor comprises an aryl diester. The internal electron donor may comprise a phthalate compound or a substituted phenylene diester.
[0095] The selectivity control agent used according to the present disclosure is an organosilicon compound. Examples of suitable organosilicon compounds include, but are not limited to, propyltriethoxysilane, diisobutyldimethoxysilane, n-propyltrimethoxysilane, or mixtures thereof. It is believed that the use of a selectivity control agent helps produce polymers with very high melt flow rates while also producing polymer products with high bulk density, low fines, and good operability. On the one hand, the organosilicon compound can be used in combination with an activity limiting agent such as amyl valerate. In some embodiments, the selectivity control agent comprises propyltriethoxysilane, diisobutyldimethoxysilane, n-propyltrimethoxysilane, or mixtures thereof, and is used in combination with an activity limiting agent. Both the selectivity control agent and the activity limiting agent can be considered as external electron donors, forming a mixed external electron donor. The molar ratio of the activity limiting agent to the selectivity control agent can be from about 40:60 to about 80:20, such as from about 50:50 to about 70:30. The mixed external electron donor can be used to control the xylene soluble content by adding larger amounts of the mixed external electron donor, especially at higher hydrogen ratios in the reactor.
[0096] In one aspect, the method of making a polymer can be carried out in a gas phase reactor. It has been found that the catalyst used according to the method produces a high melt flow rate polymer compared to past methods while still operating at a relatively low hydrogen partial pressure. For example, in one aspect, the hydrogen partial pressure in the reactor can be maintained below 60 psi, such as less than about 58 psi. Likewise, reducing the propylene partial pressure during the method can increase the melt flow rate of the polymer produced.
[0097] The reactor temperature can also be controlled and manipulated to optimize the production of polymers. For example, on the one hand, the reactor temperature can be from about 68°C to about 75°C. Alternatively, a higher temperature can be used. For example, in an alternative embodiment, the reactor temperature can be greater than about 75°C, such as greater than about 80°C, such as greater than about 85°C, such as greater than about 90°C and generally less than about 95°C. In some embodiments, the reactor temperature is from about 65°C to about 95°C, including about 65°C, about 70°C, about 75°C, about 80°C, about 85°C, about 90°C and about 95°C. The reactor temperature can be about 72°C or higher, such as about 80°C to about 90°C. Compared with operating the reactor at a lower temperature, a higher reactor temperature can increase the hydrogen response, and thus can produce a polymer with a higher melt flow rate at a lower hydrogen concentration. Higher reactor temperatures can also reduce the weight average molecular weight and reduce the molecular weight distribution, which is beneficial to the fiber blowing process in the meltblown web production process.
[0098] On the one hand, the ratio of hydrogen to other components in the reactor can be relatively high. In some embodiments, the H2 / C3 molar ratio during polymerization is about 0.1 to about 0.3, including about 0.1, about 0.2 and about 0.3. As mentioned above, the xylene solubles are controlled by changing the amount of the external electron donor present, and the amount of the external electron donor is the amount of both the selectivity control agent and the activity limiting agent. For higher melt flow with low xylene solubles, more external electron donors can be fed into the reactor. On the one hand, the external electron donor mixture can include a mixture of amyl valerate and propyltriethoxysilane in a molar ratio of about 50:50 to about 70:30. It has been found that combining high hydrogen concentrations in the presence of external electron donors and using a specific catalyst system as described below produces a polymer with an ultra-high melt flow rate.
[0099] By the method of the present disclosure, it is possible to manufacture a polypropylene polymer with a melt flow rate generally greater than about 900g / 10min. For example, the melt flow rate of the polymer can be from about 900g / 10min to about 9000g / 10min, such as from about 900g / 10min to about 7000g / 10min, including all increments of 5g / 10min therebetween. In some aspects, the melt flow rate of the polypropylene polymer can be from about 1000g / 10min to about 7000g / 10min. In some aspects, the melt flow rate of the polypropylene polymer can be greater than about 1000g / 10min, such as greater than about 1200g / 10min, such as greater than about 1400g / 10min, such as greater than about 1800g / 10min, such as greater than about 2200g / 10min and such as greater than about 4000g / 10min. In certain aspects, the melt flow rate of the polypropylene polymer can be greater than about 1400 g / 10 min, such as greater than about 1800 g / 10 min, such as greater than about 2200 g / 10 min. In some embodiments, the melt flow rate of the polypropylene polymer can be less than about 9000 g / 10 min, such as less than about 7000 g / 10 min, such as less than about 4000 g / 10 min. In some embodiments, the melt flow rate of the polypropylene polymer is greater than about 1300 g / 10 min, such as greater than about 1400 g / 10 min, greater than about 1500 g / 10 min, greater than about 1600 g / 10 min, greater than about 1700 g / 10 min, greater than about 1800 g / 10 min, greater than about 1900 g / 10 min, greater than about 2000 g / 10 min, greater than about 2100 g / 10 min, greater than about 2200 g / 10 min, greater than about 2300 g / 10 min, greater than about 2400 g / 10 min, greater than about 2500 g / 10 min, greater than about g / 10min, greater than about 3500 g / 10min, greater than about 3600 g / 10min, greater than about 3700 g / 10min, greater than about 3800 g / 10min, greater than about 3900 g / 10min, and greater than about 4000 g / 10min.In some embodiments, the melt flow rate of the polypropylene polymer is from about 1300 g / 10 min to about 2200 g / 10 min, including about 1300 g / 10 min, about 1400 g / 10 min, about 1500 g / 10 min, about 1600 g / 10 min, about 1700 g / 10 min, about 1800 g / 10 min, about 1900 g / 10 min, about 2000 g / 10 min, about 2100 g / 10 min, about 2200 g / 10 min, about 2300 g / 10 min, about 2400 g / 10 min, about 2500 g / 10 min, about 2600 g / 10 min, about 2700 g / 10 min, about 2800 g / 10 min, about 2900 g / 10 min, about 3000 g / 10 min, about 3100 g / 10 min, about 3200 g / 10 min, about 3300 g / 10 min, about 3400 g / 10 min, about 3500 g / 10 min, about 3600 g / 10 min, about 3700 g / 10 min, about 3800 g / 10 min, about 3900 g / 10 min, about 4000 g / 10 min, about 4100 g / 10 min, about 4200 g / 10 min, about 4300 g / 10 min, about 4400 g / 10 min, about 4500 g / 10 min, about 4600 g / 10 min, about 4700 g / 10 min, about 4800 g / 10 min, about 4900 g / 10 min, about 5000 g / 10 min, about 5100 g / 10 min, about About 2500g / 10min, about 2600g / 10min, about 2700g / 10min, about 2800g / 10min, about 2900g / 10min, about 3000g / 10min, about 3100g / 10min, about 3200g / 10min, about 3300g / 10min, about 3400g / 10min, about 3500g / 10min, about 3600g / 10min, about 3700g / 10min, about 3800g / 10min, about 3900g / 10min, and about 4000g / 10min.
[0100] The polypropylene polymer may be a polypropylene homopolymer. Polypropylene copolymers may also be formed by the method, including polypropylene random copolymers and polypropylene block copolymers. The comonomer may include ethylene or butene.
[0101] By using a Ziegler-Natta catalyst system, it is possible to form a polymer having a molecular weight distribution (M) of generally greater than about 4.5 or greater than about 6. w / M n ). In some embodiments, the polypropylene polymer has a molecular weight distribution greater than about 4.5. In some embodiments, the polypropylene polymer has a molecular weight distribution greater than about 6. In some embodiments, the polypropylene polymer has a molecular weight distribution greater than about 7. In some embodiments, the polypropylene polymer has a molecular weight distribution greater than about 6.0 to about 10.0, including a molecular weight distribution of about 6.0, about 6.5, about 7.0, about 7.5, about 8.0, about 8.5, about 9.0, about 9.5 and about 10.0. When manufacturing a nonwoven web, maintaining the molecular weight distribution between about 6 and about 10 can provide various advantages. For example, maintaining the molecular weight distribution within the above range can manufacture a web with dimensional stability and not necking during production and operation.
[0102] Polypropylene polymers made according to the present disclosure may have an M of less than about 8, including less than about 7 and less than about 6. z+1 / Mw In some embodiments, the polypropylene polymer has an M of less than about 7. z+1 / M w In some embodiments, the polypropylene polymer has an M of about 6.0 to about 8.0, including about 6.0, about 7.0, and about 8.0. z+1 / M w Compare.
[0103] Polypropylene polymers prepared according to the present disclosure generally have a controlled xylene soluble content. In some embodiments, the xylene soluble content is less than about 4.0 weight %. In some embodiments, the xylene soluble content is about 1.5 weight % to about 4 weight %, including about 1.5 weight %, about 2.0 weight %, about 2.5 weight %, about 3.0 weight %, about 3.5 weight % and about 4.0 weight %. The xylene soluble content can be less than about 2 weight %. Lower xylene soluble content can provide processing advantages, and higher amount can produce nonwovens with softer feel.
[0104] The polypropylene polymers described herein may have a melting temperature greater than about 155° C., including greater than about 160° C., greater than about 165° C., greater than about 170° C., greater than about 175° C., and greater than about 180° C. In some embodiments, the polypropylene polymer exhibits a melting temperature of about 155° C. to about 180° C., including about 155° C., about 160° C., about 165° C., about 170° C., about 175° C., and about 180° C. In some embodiments, the polypropylene polymer exhibits a melting temperature of about 155° C. to about 165° C.
[0105] In some embodiments, the polypropylene polymer has a weight average molecular weight (Mw) of less than about 80,000 g / mol, including less than about 75,000 g / mol, less than about 70,000 g / mol, less than about 65,000 g / mol, less than about 60,000 g / mol, less than about 55,000 g / mol, less than about 50,000 g / mol. In some embodiments, the polypropylene polymer has a weight average molecular weight of about 55,000 g / mol to about 70,000 g / mol, including about 55,000 g / mol, about 60,000 g / mol, about 65,000 g / mol, and about 70,000 g / mol.
[0106] The polypropylene polymer of the present disclosure may have a number average molecular weight (Mn) of less than about 8,500 g / mol, including less than about 8,000 g / mol, less than about 7,700 g / mol, and less than about 7,000 g / mol. In some embodiments, the polypropylene polymer has a number average molecular weight of less than about 8,500 g / mol. In some embodiments, the polypropylene polymer has a number average molecular weight of about 7,000 g / mol to about 8,000 g / mol, including about 7,000 g / mol, about 7,500 g / mol, and about 8,000 g / mol.
[0107] As described above, the polypropylene polymer is Ziegler-Natta catalyzed. As described herein, the Ziegler-Natta catalyst may comprise an internal electron donor comprising a substituted phenylene diester or phthalate compound. The catalyst may comprise a solid catalyst component that may vary depending on the specific application.
[0108] The solid catalyst component may comprise (i) magnesium, (ii) a transition metal compound of an element of Groups IV to VIII of the periodic table, (iii) a halide, oxyhalide and / or alkoxide of (i) and / or (ii), and (iv) a combination of (i), (ii) and (iii). Non-limiting examples of suitable catalyst components include halides, oxyhalides and alkoxides of magnesium, manganese, titanium, vanadium, chromium, molybdenum, zirconium, hafnium and combinations thereof.
[0109] In one embodiment, the preparation of the catalyst component comprises the halogenation of mixed magnesium and titanium alkoxides.
[0110] In various embodiments, the catalyst component is a magnesium moiety compound (MagMo), a mixed magnesium titanium compound (MagTi), or a magnesium chloride compound containing a benzoate (BenMag). In one embodiment, the catalyst precursor is a magnesium moiety ("MagMo") precursor. The MagMo precursor comprises a magnesium moiety. Non-limiting examples of suitable magnesium moieties include anhydrous magnesium chloride and / or its alcohol adducts, magnesium alkoxides or aromatic oxides, mixed alkoxy magnesium halides and / or carboxylated magnesium dialkoxides or aromatic oxides. In one embodiment, the MagMo precursor is magnesium di(C 1-4 In another embodiment, the MagMo precursor is diethoxymagnesium.
[0111] In another embodiment, the catalyst component is a mixed magnesium / titanium compound ("MagTi"). The "MagTi precursor" has the formula Mg d Ti(OR e )fX g , where R eis an aliphatic or aromatic hydrocarbon group having 1 to 14 carbon atoms or COR', wherein R' is an aliphatic or aromatic hydrocarbon group having 1 to 14 carbon atoms; each OR e The groups are the same or different; X is independently chlorine, bromine or iodine, preferably chlorine; d is 0.5 to 56, or 2 to 4; f is 2 to 116 or 5 to 15; and g is 0.5 to 116 or 1 to 3. The precursor is prepared by controlled precipitation by removing alcohol from the reaction mixture used in its preparation. In one embodiment, the reaction medium comprises a mixture of an aromatic liquid (especially a chlorinated aromatic compound, most especially chlorobenzene) and an alkanol (especially ethanol). Suitable halogenating agents include titanium tetrabromide, titanium tetrachloride or titanium trichloride, especially titanium tetrachloride. Removing the alkanol from the solution used in the halogenation results in the precipitation of a solid precursor having a particularly desirable morphology and surface area. In addition, the particle size of the resulting precursor is particularly uniform.
[0112] In another embodiment, the catalyst precursor is a magnesium chloride material containing benzoate ("BenMag"). "Magnesium chloride containing benzoate" ("BenMag") used herein can be a catalyst containing an internal electron donor of benzoate (i.e., a halogenated catalyst component). The BenMag material can also contain a titanium portion, such as a titanium halide. Benzoate internal donors are unstable and can be replaced by other electron donors during the catalyst and / or catalyst synthesis process. Non-limiting examples of suitable benzoate groups include ethyl benzoate, methyl benzoate, ethyl p-methoxybenzoate, methyl p-ethoxybenzoate, ethyl p-ethoxybenzoate, and ethyl p-chlorobenzoate. In one embodiment, the benzoate group is ethyl benzoate. In one embodiment, the BenMag catalyst component can be the product of the halogenation of any catalyst component (i.e., a MagMo precursor or a MagTi precursor) in the presence of a benzoate compound.
[0113] In another embodiment, the solid catalyst component can be formed by a magnesium portion, a titanium portion, an epoxy compound, an organosilicon compound, and an internal electron donor. In one embodiment, an organophosphorus compound can also be incorporated into the solid catalyst component. For example, in one embodiment, a magnesium compound containing a halide ion can be dissolved in a mixture comprising an epoxy compound, an organophosphorus compound, and a hydrocarbon solvent. The resulting solution can be treated with a titanium compound in the presence of an organosilicon compound, and optionally treated with an internal electron donor to form a solid precipitate. The solid precipitate can then be treated with an additional amount of a titanium compound. The titanium compound used to form the catalyst can have the following chemical formula:
[0114] Ti(OR) g X 4-g
[0115] Where each R is independently C1 -C 4 alkyl; X is Br, Cl or I; and g is 0, 1, 2, 3 or 4.
[0116] In some embodiments, the organosilicon is a monomeric or polymeric compound. The organosilicon compound may contain -Si-O-Si- groups within a molecule or between other molecules. Other illustrative examples of organosilicon compounds include polydialkylsiloxanes and / or tetraalkoxysilanes. Such compounds may be used alone or as a combination thereof. The organosilicon compound may be used in combination with aluminum alkoxides and internal electron donors.
[0117] The aluminum alkoxide may have the formula Al(OR') 3 , wherein each R' is independently a hydrocarbon having up to 20 carbon atoms. This can include wherein each R' is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, and the like.
[0118] Examples of the magnesium compound containing halide ions include magnesium chloride, magnesium bromide, magnesium iodide and magnesium fluoride. In one embodiment, the magnesium compound containing halide ions is magnesium chloride.
[0119] Illustrative epoxy compounds include, but are not limited to, glycidyl-containing compounds of the formula:
[0120]
[0121] wherein "a" is 1, 2, 3, 4 or 5; X is F, Cl, Br, I or methyl; and Ra is H, alkyl, aryl or cyclyl. In one embodiment, the alkyl epoxide is epichlorohydrin. In some embodiments, the epoxy compound is a halogenated alkyl epoxide or a non-halogenated alkyl epoxide.
[0122] According to some embodiments, the epoxy compound is selected from ethylene oxide; propylene oxide; 1,2-butylene oxide; 2,3-butylene oxide; 1,2-hexylene oxide; 1,2-octylene oxide; 1,2-decylene oxide; 1,2-dodecylene oxide; 1,2-tetradecylene oxide; 1,2-hexadecylene oxide; 1,2-octadecylene oxide; 7,8-epoxy-2-methyloctadecane; 2-vinyl oxirane; 2-methyl-2-vinyl oxirane; 1,2-epoxy-5-hexene; 1,2-epoxy-7-octene; 1-phenyl-2,3 -propylene oxide; 1-(1-naphthyl)-2,3-propylene oxide; 1-cyclohexyl-3,4-butylene oxide; 1,3-butadiene dioxide; 1,2,7,8-diepoxyoctane; cyclopentene oxide; cyclooctene oxide; α-epoxypinane; 2,3-epoxynorbornane; limonene oxide; cyclodecane epoxide; 2,3,5,6-diepoxynorbornane; styrene oxide; 3-methylstyrene oxide; 1,2-epoxybutylbenzene; 1,2-epoxyoctylbenzene; stilbene oxide; 3-vinylstyrene oxide; 1-( 1-methyl-1,2-epoxyethyl)-3-(1-methylvinylbenzene); 1,4-bis(1,2-epoxypropyl)benzene; 1,3-bis(1,2-epoxy-1-methylethyl)benzene; 1,4-bis(1,2-epoxy-1-methylethyl)benzene; epifluoropropane; epichlorohydrin; epibromopropane; hexafluoroepoxypropane; 1,2-epoxy-4-fluorobutane; 1-(2,3-epoxypropyl)-4-fluorobenzene; 1-(3,4-epoxybutyl)-2-fluorobenzene; 1-(2,3-epoxypropyl)-4-chlorobenzene; 1-( 3,4-Epoxybutyl)-3-chlorobenzene; 4-fluoro-1,2-cyclohexene oxide; 6-chloro-2,3-epoxybicyclo[2.2.1]heptane; 4-fluorostyrene oxide; 1-(1,2-epoxypropyl)-3-trifluorobenzene; 3-acetyl-1,2-epoxypropane; 4-benzoyl-1,2-epoxybutane; 4-(4-benzoyl)phenyl-1,2-epoxybutane; 4,4′-bis(3,4-epoxybutyl)benzophenone; 3,4-epoxy-1-cyclohexanone; 2,3-epoxy-5-oxobicyclo[2.2.1] Heptane; 3-acetylstyrene oxide; 4-(1,2-epoxypropyl)benzophenone; methyl glycidyl ether; butyl glycidyl ether; 2-ethylhexyl glycidyl ether; allyl glycidyl ether; ethyl 3,4-epoxybutyl ether; phenyl glycidyl ether; 4-tert-butylphenyl glycidyl ether; 4-chlorophenyl glycidyl ether; 4-methoxyphenyl glycidyl ether; 2-phenylphenyl glycidyl ether; 1-naphthyl glycidyl ether; 2-phenylphenyl glycidyl ether; 1-naphthyl glycidyl ether; 4-indolyl glycidyl ether; N-methyl-α-quinolone-4-yl glycidyl ether; ethylene glycol diglycidyl ether; 1,4-butanediol diglycidyl ether Glyceryl ethers; 1,2-diglycidyloxybenzene; 2,2-bis(4-glycidyloxyphenyl)propane; tris(4-glycidyloxyphenyl)methane; poly(propylene oxide) triol triglycidyl ether; glycidyl ethers of phenolic resins; 1,2-epoxy-4-methoxycyclohexane; 2,3-epoxy-5,6-dimethoxybicyclo[2.2.1]heptane; 4-methoxystyrene oxide; 1-(1,2-epoxybutyl)-2-phenoxybenzene; glycidyl formate; glycidyl acetate; 2,3-epoxybutyl acetate; glycidyl butyrate; glycidyl benzoate; diglycidyl terephthalate; poly(glycidyl acrylate); Poly(glycidyl methacrylate); copolymer of glycidyl acrylate and another monomer; copolymer of glycidyl methacrylate and another monomer; 1,2-epoxy-4-methoxycarbonylcyclohexane; 2,3-epoxy-5-butoxycarbonylbicyclo[2.2.1]heptane; ethyl 4-(1,2-epoxyethyl)benzoate; methyl 3-(1,2-epoxybutyl)benzoate; methyl 3-(1,2-epoxybutyl)-5-phenylbenzoate; N,N-glycidyl-methylacetamide; N,N-ethylglycidylpropionamide; N,N-glycidylmethylbenzamide; N-(4,5-epoxypentyl)-N-methyl-benzamide amide; N,N-diglycidylaniline; bis(4-diglycidylaminophenyl)methane; poly(N,N-glycidylmethacrylamide); 1,2-epoxy-3-(diphenylcarbamoyl)cyclohexane; 2,3-epoxy-6-(dimethylcarbamoyl)bicyclo[2.2.1]heptane; 2-(dimethylcarbamoyl)styrene oxide; 4-(1,2-epoxybutyl)-4′-(dimethylcarbamoyl)biphenyl; 4-cyano-1,2-epoxybutane; 1-(3-cyanophenyl)-2,3-epoxybutane; 2-cyanostyrene oxide; and 6-cyano-1-(1,2-epoxy-2-phenylethyl)naphthalene.
[0123] As an example of an organic phosphorus compound, a phosphoric acid ester such as a trialkyl phosphate can be used. Such a compound can be represented by the following formula:
[0124]
[0125] Where R 1 , R 2 and R 3 Each independently selected from methyl, ethyl and linear or branched (C 3 -C 10 In one embodiment, the trialkyl phosphate is tributyl phosphate.
[0126] In yet another embodiment, the substantially spherical MgCl 2 The -nEtOH adduct can be formed by a spray crystallization method. In this method, MgCl is sprayed inside the container while an inert gas is introduced to the upper part of the container at a temperature of 20-80°C. 2 -nROH melt (where n is 1-6). The melt droplets are transferred to a crystallization zone, and an inert gas is introduced into the crystallization zone at a temperature of -50 to 20°C to crystallize the melt droplets into non-agglomerated solid particles in a spherical shape. The spherical MgCl 2 The particles are sorted into the desired size. Particles of undesirable size can be recycled. In a preferred embodiment of the catalyst synthesis, spherical MgCl 2 The precursor has an average particle size of about 15-150 microns, preferably 20-100 microns, and most preferably 35-85 microns (Malvern d 50 ).
[0127] The catalyst component can be converted into a solid catalyst by halogenation. Halogenation includes contacting the catalyst component with a halogenating agent in the presence of an internal electron donor. Halogenation converts the magnesium portion present in the catalyst component into a magnesium halide support, on which the titanium portion (such as a titanium halide) is deposited. Without wishing to be bound by any particular theory, it is believed that during the halogenation process, the internal electron donor (1) adjusts the position of the titanium on the magnesium-based support, (2) promotes the conversion of the magnesium and titanium portions into corresponding halides, and (3) adjusts the crystallite size of the magnesium halide support during the conversion process. Thus, providing an internal electron donor produces a catalyst composition with enhanced stereoselectivity.
[0128] In one embodiment, the halogenating agent is a compound having the formula Ti(OR e ) f X h Titanium halide, where R e and X are as defined above, f is an integer from 0 to 3; h is an integer from 1 to 4; and f+h is 4. In one embodiment, the halogenating agent is TiCl 4In another embodiment, the halogenation is carried out in the presence of a chlorinated or non-chlorinated aromatic liquid such as dichlorobenzene, o-chlorotoluene, chlorobenzene, benzene, toluene or xylene. In yet another embodiment, the halogenation is carried out by using a halogenating agent (such as TiCl 4 ) and a mixture of a chlorinated aromatic liquid for halogenation.
[0129] The reaction mixture can be heated during the halogenation process. The catalyst component and the halogenating agent are initially contacted at a temperature of less than about 10°C, such as less than about 0°C, such as less than about -10°C, such as less than about -20°C, such as less than about -30°C. The initial temperature is generally greater than about -50°C, such as greater than about -40°C. The mixture is then heated at a rate of 0.1 to 10.0°C / minute, or at a rate of 1.0 to 5.0°C / minute. The internal electron donor can be added later, after the initial contact period between the halogenating agent and the catalyst component. The temperature of the halogenation is 20°C to 150°C (or any value or sub-range therebetween), or 0°C to 120°C. In the absence of an internal electron donor, the halogenation can continue for 5 to 60 minutes, or 10 to 50 minutes.
[0130] The mode of contacting the catalyst component, the halogenating agent and the internal electron donor can vary. In one embodiment, the catalyst component is first contacted with a mixture containing a halogenating agent and a chlorinated aromatic compound. The resulting mixture is stirred and heated if necessary. Next, the internal electron donor is added to the same reaction mixture without separating or recovering the precursor. The aforementioned method can be carried out in a single reactor, wherein the addition of various components is controlled by automated process control.
[0131] In one embodiment, the catalyst component is contacted with an internal electron donor prior to reaction with the halogenating agent.
[0132] The contact time of the catalyst component with the internal electron donor is at least 10 minutes, or at least 15 minutes, or at least 20 minutes, or at least 1 hour at a temperature of at least -30°C, or at least -20°C, or at least 10°C to a maximum of 150°C, or a maximum of 120°C, or a maximum of 115°C, or a maximum of 110°C.
[0133] In one embodiment, the catalyst components, internal electron donor, and halogenating agent are added simultaneously or substantially simultaneously.
[0134] The halogenation procedure can be repeated one, two, three or more times as desired. In one embodiment, the resulting solid material is recovered from the reaction mixture and contacted with a mixture of a halogenating agent in a chlorinated aromatic compound at a temperature of at least about -20°C, or at least about 0°C, or at least about 10°C to a maximum of about 150°C, or a maximum of about 120°C, or a maximum of about 115°C for at least about 10 minutes, or at least about 15 minutes, or at least about 20 minutes, and up to about 10 hours, or up to about 45 minutes, or up to about 30 minutes, in the absence (or presence) of the same (or different) internal electron donor component.
[0135] After the aforementioned halogenation procedure, the resulting solid catalyst composition is separated from the reaction medium used in the final process by, for example, filtration to produce a wet cake. The wet cake can then be rinsed or washed with a liquid diluent to remove unreacted TiCl 4 , and if necessary can be dried to remove residual liquid. Typically, the resulting solid catalyst composition is washed one or more times with a "washing liquid", which is a liquid hydrocarbon, such as an aliphatic hydrocarbon, such as isopentane, isooctane, isohexane, hexane, pentane or octane. The solid catalyst composition can then be separated and dried or slurried in a hydrocarbon, especially a relatively heavy hydrocarbon such as mineral oil for further storage or use.
[0136] In one embodiment, the resulting solid catalyst composition has a titanium content of about 1.0 wt % to about 6.0 wt %, or about 1.5 wt % to about 4.5 wt %, or about 2.0 wt % to about 3.5 wt %, based on the total solid weight. The weight ratio of titanium to magnesium in the solid catalyst composition is suitably about 1:3 to about 1:160, or about 1:4 to about 1:50, or about 1:6 to 1:30. In one embodiment, the internal electron donor may be present in the catalyst composition in a molar ratio of internal electron donor to magnesium of about 0.005:1 to about 1:1, or about 0.01:1 to about 0.4:1. The weight percentages are based on the total weight of the catalyst composition.
[0137] Before or after isolating the solid catalyst composition, the catalyst composition can be further treated by one or more of the following procedures. If desired, the solid catalyst composition can be contacted with an additional amount of a titanium halide compound (halogenated); it can be exchanged with an acyl chloride such as phthaloyl dichloride or benzoyl chloride under metathesis conditions; and it can be rinsed or washed, heat treated; or aged. The foregoing additional procedures can be combined in any order or used alone, or not used at all.
[0138] As described above, the catalyst composition may comprise a combination of a magnesium moiety, a titanium moiety and an internal electron donor. The catalyst composition is manufactured by the aforementioned halogenation procedure, which converts the catalyst component and the internal electron donor into a combination of a magnesium and titanium moiety into which the internal electron donor is incorporated. The catalyst component forming the catalyst composition may be any of the above-mentioned catalyst precursors, including a magnesium moiety precursor, a mixed magnesium / titanium precursor, a benzoate-containing magnesium chloride precursor, a magnesium, titanium, epoxy and phosphorus precursor, or a spherical precursor.
[0139] Various different types of internal electron donors can be incorporated into the solid catalyst component. In one embodiment, the internal electron donor is an aromatic diester, such as a phenylene-substituted diester. In one embodiment, the internal electron donor may have the following chemical structure:
[0140]
[0141] Where R 1 , R 2 , R 3 and R 4 Each is a hydrocarbon group having 1 to 20 carbon atoms, the hydrocarbon group having a branched or linear structure or containing a cycloalkyl group having 7 to 15 carbon atoms, and wherein E 1 and E 2 are the same or different and are selected from an alkyl group having 1 to 20 carbon atoms, a substituted alkyl group having 1 to 20 carbon atoms, an aryl group having 1 to 20 carbon atoms, a substituted aryl group having 1 to 20 carbon atoms, or an inert functional group having 1 to 20 carbon atoms and optionally containing heteroatoms, and wherein X 1 and X 2 Each is O, S, alkyl or NR 5 , and R 5 is a hydrocarbyl group having 1 to 20 carbon atoms or hydrogen.
[0142] As used herein, the terms "hydrocarbyl" and "hydrocarbon" refer to substituents containing only hydrogen and carbon atoms, including branched or unbranched, saturated or unsaturated, cyclic, polycyclic, fused or acyclic species, and combinations thereof. Non-limiting examples of hydrocarbyl groups include alkyl-, cycloalkyl-, alkenyl-, dienyl-, cycloalkenyl-, cycloalkadienyl-, aryl-, aralkyl, alkylaryl, and alkynyl.
[0143] The terms "substituted hydrocarbyl" and "substituted hydrocarbon" as used herein refer to hydrocarbyl substituted with one or more non-hydrocarbyl substituents. A non-limiting example of a non-hydrocarbyl substituent is a heteroatom. "Heteroatom" as used herein refers to an atom other than carbon or hydrogen. A heteroatom can be a non-carbon atom selected from Groups IV, V, VI and VII of the periodic table. Non-limiting examples of heteroatoms include: halogens (F, Cl, Br, I), N, O, P, B, S and Si. Substituted hydrocarbyl also includes halogenated hydrocarbyl and silicon-containing hydrocarbyl. The term "halogenated hydrocarbyl" as used herein refers to a hydrocarbyl substituted with one or more halogen atoms. The term "silicon-containing hydrocarbyl" as used herein is a hydrocarbyl substituted with one or more silicon atoms. One or more silicon atoms may or may not be in the carbon chain.
[0144] In one aspect, the substituted phenylene diester has the following structure (I):
[0145]
[0146] In one embodiment, structure (I) comprises R as isopropyl 1 and R 3 . R 2 , R 4 and R 5 -R 14 Each of is hydrogen.
[0147] In one embodiment, structure (I) comprises R as a methyl group 1 , R 5 and R 10 Every one of R 3 R is tert-butyl. 2 , R 4 , R 6 -R 9 and R 11 -R 14 Each of is hydrogen.
[0148] In one embodiment, structure (I) comprises R as a methyl group 1 , R 7 and R 12 Every one of R 3 R is tert-butyl. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0149] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is a 1,1 group. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0150] In one embodiment, structure (I) comprises R as a methyl group 1 , R 5 , R 7 , R 9 , R 10 , R 12 and R 14 Every one of R 3 R is tert-butyl. 2 , R 4 , R 6 , R 8 , R 11 and R 13 Each of is hydrogen.
[0151] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 5 , R 7 , R 9 , R 10 , R 12 and R 14 Each of R is isopropyl. 2 , R 4 , R 6 , R 8 , R 11 and R 13 Each of is hydrogen.
[0152] In one embodiment, the substituted phenylene aromatic diester has a structure selected from structures (II)-(V), including R 1 To R 14 Alternatives to each of which are described in detail in U.S. Patent No. 8,536,372, which is incorporated herein by reference.
[0153] In one embodiment, structure (I) comprises R as a methyl group 1 And R3 R is tert-butyl. 7 and R 12 Each of R is an ethoxy group. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0154] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is a fluorine atom. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0155] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is a chlorine atom. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0156] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is a bromine atom. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R13 and R 14 Each of is hydrogen.
[0157] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is an iodine atom. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0158] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 6 , R 7 , R 11 and R 12 Each of R is a chlorine atom. 2 , R 4 , R 5 , R 8 , R 9 , R 10 , R 13 and R 14 Each of is hydrogen.
[0159] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 6 , R 8 , R 11 and R 13 Each of R is a chlorine atom. 2 , R 4 , R 5 , R 7 , R 9 , R 10 , R 12 and R 14 Each of is hydrogen.
[0160] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 2 , R 4 and R 5 -R 14Each of is a fluorine atom.
[0161] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is trifluoromethyl. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0162] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is ethoxycarbonyl. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0163] In one embodiment, R 1 is methyl and R 3 R is tert-butyl. 7 and R 12 Each of R is an ethoxy group. 2 , R 4 , R 5 , R 6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0164] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 R is tert-butyl. 7 and R 12 Each of R is a diethylamino group. 2 , R 4 , R 5 , R6 , R 8 , R 9 , R 10 , R 11 , R 13 and R 14 Each of is hydrogen.
[0165] In one embodiment, structure (I) comprises R as a methyl group 1 And R 3 It is 2,4,4-trimethylpentan-2-yl. 2 , R 4 and R 5 -R 14 Each of is hydrogen.
[0166] In one embodiment, structure (I) comprises R 1 and R 3 , each of which is sec-butyl. 2 , R 4 and R 5 -R 14 Each of is hydrogen.
[0167] In one embodiment, structure (I) comprises R 1 and R 4 , each of which is methyl. 2 , R 3 , R 5 -R 9 and R 10 -R 14 Each of is hydrogen.
[0168] In one embodiment, structure (I) comprises R as a methyl group 1 . R 4 is isopropyl. 2 , R 3 , R 5 -R 9 and R 10 -R 14 Each of is hydrogen.
[0169] In one embodiment, structure (I) comprises R 1 , R 3 and R 4 , each of which is isopropyl. 2 , R 5 -R 9 and R 10 -R 14 Each of is hydrogen.
[0170] On the other hand, the internal electron donor can be a phthalate compound. For example, the phthalate compound can be dimethyl phthalate, diethyl phthalate, dipropyl phthalate, diisopropyl phthalate, dibutyl phthalate, diisobutyl phthalate, dipentyl phthalate, diisopentyl phthalate, methyl butyl phthalate, ethyl butyl phthalate or ethyl propyl phthalate.
[0171] In addition to the solid catalyst component as described above, the catalyst system of the present disclosure may also include a co-catalyst. The co-catalyst may include a hydride, alkylate or arylate of aluminum, lithium, zinc, tin, cadmium, beryllium, magnesium and combinations thereof. In one embodiment, the co-catalyst is a 3 A hydrocarbyl aluminum cocatalyst represented by Al, wherein each R is an alkyl, cycloalkyl, aryl or hydride group; at least one R is a hydrocarbyl; two or three R groups can be joined in a cyclic group to form a heterocyclic structure; each R can be the same or different; and each R as a hydrocarbyl has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms. In another embodiment, each alkyl group can be linear or branched, and such hydrocarbyl groups can be mixed groups, i.e., the group can contain alkyl, aryl and / or cycloalkyl groups. Non-limiting examples of suitable groups are: methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, 2-methylpentyl, n-heptyl, n-octyl, isooctyl, 2-ethylhexyl, 5,5-dimethylhexyl, n-nonyl, n-decyl, isodecyl, n-undecyl, n-dodecyl.
[0172] Non-limiting examples of suitable hydrocarbyl aluminum compounds are as follows: triisobutylaluminum, tri-n-hexylaluminum, diisobutylaluminum hydride, di-n-hexylaluminum hydride, isobutylaluminum dihydride, n-hexylaluminum dihydride, diisobutylhexylaluminum, isobutyldihexylaluminum, trimethylaluminum, triethylaluminum, tri-n-propylaluminum, triisopropylaluminum, tri-n-butylaluminum, tri-n-octylaluminum, tri-n-decylaluminum, tri-n-dodecylaluminum. In one embodiment, the cocatalyst is selected from triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, diisobutylaluminum hydride and di-n-hexylaluminum hydride.
[0173] In one embodiment, the cocatalyst is triethylaluminum. The molar ratio of aluminum to titanium is from about 5:1 to about 500:1, or from about 10:1 to about 200:1, or from about 15:1 to about 150:1, or from about 20:1 to about 100:1. In another embodiment, the molar ratio of aluminum to titanium is about 45:1.
[0174] Suitable catalyst compositions may comprise a solid catalyst component, a cocatalyst and an external electron donor, which may be a mixed external electron donor (M-EED) of two or more different components. Suitable external electron donors or "external donors" include one or more activity limiting agents (ALA) and / or one or more selectivity control agents (SCA). "External donors" as used herein are components added independently of the formation of the main catalyst to change the performance of the catalyst or compositions comprising a mixture of components. "Activity limiting agents" as used herein are compositions that reduce catalyst activity when the polymerization temperature is raised to a threshold temperature (e.g., a temperature greater than about 95°C) in the presence of a catalyst. "Selectivity control agents" are compositions that improve polymer stereoregularity, wherein improved stereoregularity is generally understood to refer to increased stereoregularity and / or reduced xylene solubles. It should be understood that the above definitions are not mutually exclusive, and a single compound may be classified as, for example, both activity limiting agents and selectivity control agents.
[0175] The selectivity control agent according to the present disclosure is typically an organosilicon compound. For example, in one aspect, the selectivity control agent can be an alkoxysilane.
[0176] In one embodiment, the alkoxysilane may have the following general formula: SiR m (OR′) 4-m (I), wherein R at each occurrence is independently hydrogen or a hydrocarbon group or amino group optionally substituted with one or more substituents containing one or more heteroatoms of Groups 14, 15, 16 or 17, excluding hydrogen and halogen, said R containing up to 20 atoms; R′ is C 1-4 and m is 0, 1, 2 or 3. In one embodiment, R is C 6-12 Aryl, alkyl or aralkyl, C 3-12 Cycloalkyl, C 3-12 Branched alkyl, or C 3-12 Cyclic or acyclic amino group, R' is C 1-4 wherein the second selectivity control agent comprises n-propyl triethoxy silane, ...
[0177] In one embodiment, the catalyst system may include an activity limiting agent (ALA). ALA inhibits or otherwise prevents polymerization reactor abnormalities and ensures the continuity of the polymerization process. Typically, the activity of Ziegler-Natta catalysts increases as the reactor temperature increases. Ziegler-Natta catalysts also typically maintain high activity near the melting point temperature of the produced polymer. The heat generated by the exothermic polymerization reaction can cause the polymer particles to form agglomerates, and can ultimately lead to the destruction of the continuity of the polymer production process. ALA reduces catalyst activity at elevated temperatures, thereby preventing reactor abnormalities, reducing (or preventing) particle agglomeration, and ensuring the continuity of the polymerization process.
[0178] The activity limiting agent may be a carboxylic acid ester. The aliphatic carboxylic acid ester may be C 4 -C 30 The aliphatic acid ester may be a mono- or poly- (di- or more) ester, may be linear or branched, may be saturated or unsaturated, and any combination thereof. 4 -C 30 The aliphatic acid esters may also be substituted with one or more substituents containing heteroatoms from Groups 14, 15 or 16. Suitable C 4- C 30 Non-limiting examples of aliphatic acid esters include aliphatic C 4-30 Monocarboxylic acid C 1-20 Alkyl esters, aliphatic C 8-20 Monocarboxylic acid C 1-20 Alkyl esters, aliphatic C 4-20 C of monocarboxylic and dicarboxylic acids 1-4 Allyl monoesters and diesters, aliphatic C 8-20 C of monocarboxylic and dicarboxylic acids 1-4 Alkyl esters, and C 2-100 (Poly) glycol or C 2-100 C of (poly)glycol ether 4-20 In another embodiment, the C 4 -C 30 The aliphatic acid ester may be laurate, myristate, palmitate, stearate, oleate, sebacate, (poly)(alkylene glycol) mono- or diacetate, (poly)(alkylene glycol) mono- or dimyristate, (poly)(alkylene glycol) mono- or dilaurate, (poly)(alkylene glycol) mono- or dioleate, triacetin, C 2-40 In another embodiment, the C 4 -C 30 The aliphatic ester is isopropyl myristate, di-n-butyl sebacate and / or amyl valerate. 4 -C 30 The aliphatic ester is isopropyl myristate and / or amyl valerate.
[0179] In one embodiment, the selectivity control agent and / or the activity limiting agent can be added to the reactor separately. In another embodiment, the selectivity control agent and the activity limiting agent can be pre-mixed together and then added to the reactor as a mixture. In addition, the selectivity control agent and / or the activity limiting agent can be added to the reactor in different ways. For example, in one embodiment, the selectivity control agent and / or the activity limiting agent can be directly added to the reactor, such as added to a fluidized bed reactor. Alternatively, the selectivity control agent and / or the activity limiting agent can be indirectly added to the reactor space by feeding via, for example, a circulating loop. The selectivity control agent and / or the activity limiting agent can be combined with catalyst particles in a circulating loop before being fed into the reactor.
[0180] The catalyst system of the present disclosure as described above can be used to produce olefin-based polymers. The method includes contacting an olefin with the catalyst system under polymerization conditions.
[0181] One or more olefin monomers can be introduced into the polymerization reactor to react with the catalyst system and form a polymer, such as a fluidized bed of polymer particles. The olefin monomer can be propylene, for example. Any suitable reactor can be used, including a fluidized bed reactor, a stirred gas reactor, a moving packed bed reactor, a multi-zone reactor, a bulk phase reactor, a slurry reactor or a combination thereof. Suitable commercial reactors include UNIPOL reactors, SPHERIPOL, SPHERIZONE reactors, etc.
[0182] As used herein, "polymerization conditions" are temperature and pressure parameters within a polymerization reactor suitable for promoting polymerization between the catalyst composition and olefins to form the desired polymer. The polymerization process may be a gas phase, slurry or bulk polymerization process operating in one or more than one reactor.
[0183] In one embodiment, polymerization occurs by gas phase polymerization. "Gas phase polymerization" as used herein is to pass an ascending fluidizing medium through a fluidized bed of polymer particles maintained in a fluidized state by the fluidizing medium in the presence of a catalyst, the fluidizing medium containing one or more monomers. "Fluidization", "fluidized" or "fluidization" is a gas-solid contact process in which a bed of finely divided polymer particles is lifted and stirred by an ascending gas stream. Fluidization occurs in a particle bed when the upward flow of a fluid through the interstices of a particle bed obtains a pressure difference and a friction resistance increment that exceeds the weight of the particles. Thus, a "fluidized bed" is a plurality of polymer particles suspended in a fluidized state by a stream of a fluidizing medium. A "fluidizing medium" is one or more olefin gases, an optional carrier gas (such as H 2 or N 2 ) and optionally a liquid (such as a hydrocarbon), which rises through the gas phase reactor.
[0184] Typical gas phase polymerization reactor (or gas phase reactor) comprises container (i.e. reactor), fluidized bed, distributor plate, inlet and outlet pipelines, compressor, circulating gas cooler or heat exchanger and product discharge system.The container comprises reaction zone and deceleration zone, each of which is located above the distributor plate.The bed is located in the reaction zone.In one embodiment, the fluidizing medium comprises propylene gas and at least one other gas such as olefin and / or carrier gas such as hydrogen or nitrogen.
[0185] In one embodiment, by feeding the catalyst composition into a polymerization reactor and introducing olefins into the polymerization reactor and contacting occurs. In one embodiment, a cocatalyst can be mixed with the catalyst composition (premix) before the catalyst composition is introduced into the polymerization reactor. In another embodiment, the cocatalyst is added to the polymerization reactor independently of the catalyst composition. The cocatalyst is introduced independently into the polymerization reactor and can occur simultaneously or substantially simultaneously with the catalyst composition feed. In some embodiments, the cocatalyst and the external electron donor are fed into the polymerization reactor in a molar ratio of about 1.5 to about 15, including about 1.5, about 2.0, about 2.5, about 3.0, about 3.5, about 4.0, about 4.5, about 5.0, about 5.5, about 6.0, about 6.5, about 7.0, about 7.5, about 8.0, about 8.5, about 9.0, about 9.5, about 10, about 10.5, about 11, about 11.5, about 12, about 12.5 and about 13.
[0186] In one embodiment, the polymerization process may include a preactivation step. Preactivation includes contacting the catalyst composition with a cocatalyst and a selectivity control agent and / or an activity limiting agent. The resulting preactivated catalyst stream is then introduced into the polymerization reaction zone and contacted with the olefin monomer to be polymerized. Optionally, an additional amount of selectivity control agent and / or activity limiting agent may be added.
[0187] The method can include mixing a selectivity control agent (and optional activity limiting agent) with a catalyst composition. The selectivity control agent can be compounded with a cocatalyst and mixed with the catalyst composition (premix) before the contact between the catalyst composition and the olefin. In another embodiment, the selectivity control agent and / or the activity limiting agent can be added independently in a polymerization reactor. In one embodiment, the selectivity control agent and / or the activity limiting agent can be fed into a reactor by a recycle loop.
[0188] The above method can be used to make polypropylene polymers with very high melt flow rates. In addition, polymers with relatively low fines and relatively high bulk density can be produced. However, polymers made according to the present disclosure can contain fines in an amount less than about 8 wt%, such as less than about 7 wt%, such as less than about 6 wt%. For example, the bulk density can be greater than about 0.30 g / cc, such as greater than about 0.4 g / cc, such as greater than about 0.42 g / cc, such as greater than about 0.45 g / cc. The bulk density is generally less than about 0.6 g / cc, such as less than about 0.5 g / cc, such as less than about 0.4 g / cc.
[0189] The polypropylene polymer prepared according to the present disclosure can then be incorporated into various polymer compositions to manufacture molded articles. The polymer composition can contain the high melt flow rate polypropylene polymer in an amount generally greater than about 70% by weight, such as in an amount greater than about 80% by weight, such as in an amount greater than about 90% by weight, such as in an amount greater than about 95% by weight. The polymer composition can contain various additives and ingredients. For example, the polymer composition can contain one or more antioxidants. For example, on the one hand, the polymer composition can contain a sterically hindered phenol antioxidant and / or a phosphite antioxidant. The polymer composition can also contain an acid scavenger, such as calcium stearate. In addition, the polymer composition can contain a colorant, a UV stabilizer, etc. Each of the above-mentioned additives can generally be present in the polymer composition in an amount of about 0.015 to about 2% by weight.
[0190] Alternatively, high melt flow rate polypropylene polymer can be used as a processing aid. Processing aids can be flow agents, lubricants, mold release agents, waxes, etc. for improving the melt flow properties of other polymers. In some embodiments, high melt flow rate polypropylene polymers include waxes, lubricants, mold release agents or flow aids. In this embodiment, the high melt flow rate polypropylene polymer of the present disclosure can be present in the polymer composition in an amount of about 2% by weight to about 50% by weight, including all increments of 1% therebetween. For example, high melt flow rate polypropylene polymers can be present in the polymer composition in an amount of less than about 50% by weight, such as less than 40% by weight, such as less than about 30% by weight, such as less than about 25% by weight, such as less than about 20% by weight, such as less than about 10% by weight and generally greater than about 5% by weight. In some embodiments, the polypropylene polymer includes a processing aid combined with at least one other polymer showing a lower melt flow rate, and the polypropylene polymer is included in the composition in an amount less than about 50% by weight. Polymers that can be combined with the high melt flow rate polypropylene polymer include other lower melt flow rate polypropylene polymers, polyethylene polymers, polyester polymers, and the like.
[0191] Polyolefin polymers (such as polypropylene polymers) with very high melt flow rates are very suitable for various applications to produce various articles and products. In some embodiments, the polyolefin polymers (such as polypropylene polymers) do not contain any peroxide. High melt flow rate polymers generally have excellent flow properties, which makes the polymer easy to process, even in extrusion or molding processes with very small sizes. For example, high melt flow rate polyolefin polymers are very suitable for forming fine fibers and films. The polymer produced by the method can produce fibers with ultra-low denier and / or with higher processing speeds. For example, the polyolefin polymers prepared according to the present disclosure are particularly suitable for forming melt-blown fibers and melt-blown nonwoven webs. Such fibers can be continuous or discontinuous, and can have a fiber diameter of less than about 5 microns, such as less than about 3 microns, such as less than about 2 microns, such as less than about 1 micron and such as less than about 0.5 micron. The nonwoven web made of the polymer is dimensionally stable and does not show necking during production and processing. The melt-blown nonwoven web made of the fiber has excellent filtering properties, making it very suitable for use as a barrier layer. For example, the meltblown webs prepared according to the present disclosure can form an excellent barrier to fluids, airborne contaminants, and microorganisms such as viruses.Therefore, the meltblown webs prepared according to the present disclosure are particularly suitable for incorporation into protective clothing and apparel.
[0192] For example, refer to Figure 1 , shows an embodiment of a mask 10 that can be made using a meltblown web of the present disclosure. The mask 10 includes a main body portion 12 attached to straps 14 and 16. The straps 14 and 16 are designed to extend around the user's ears so as to hold the main body portion 12 over the wearer's nose and mouth. The main body portion 12 can be made of a meltblown web of the present disclosure. For example, the main body portion 12 can be made of a single layer of meltblown material. Alternatively, the meltblown web of the present disclosure can be one of several layers used to form the main body portion 12. For example, in one aspect, the main body portion 12 can include a meltblown layer of the present disclosure positioned between two outer layers.
[0193] Polyolefin polymers such as polypropylene polymers having very high melt flow rates as described herein are well suited for meltblown nonwoven applications. In one aspect, a meltblown web comprising nonwoven meltblown fibers made from any of the polymer compositions described herein is provided.
[0194] In one aspect, meltblown fibers made from any of the polymer compositions described herein are provided, the meltblown fibers having a diameter of less than about 5 microns, including less than about 4.5 microns, less than about 4.0 microns, less than about 3.5 microns, less than about 3.0 microns, less than about 2.5 microns, less than about 2.0 microns. In some embodiments, the meltblown fibers have a diameter of less than about 3 microns. In some embodiments, the meltblown fibers have a diameter of about 5 microns, about 4.5 microns, about 4.0 microns, about 3.5 microns, about 3.0 microns, about 2.5 microns, about 2.0 microns, or about 1.5 microns. In some embodiments, the meltblown fibers have a diameter of about 1.5 to about 3.0 microns. The meltblown fiber size and its distribution can be determined by the resin MFR and / or MFR. z+1 / M w ratio (high MW polymer chains).
[0195] In one aspect, a nonwoven web is provided that includes a multi-layer structure, the multi-layer structure including: one or more meltblown layers, the meltblown layers including any of the meltblown fibers described herein.
[0196] In some embodiments, the nonwoven web comprises a meltblown layer. In some embodiments, the nonwoven web comprises two or more meltblown layers. In some embodiments, two or more meltblown layers comprise the same meltblown layer. In some embodiments, two or more meltblown layers comprise different meltblown layers.
[0197] In some embodiments, the nonwoven web further comprises two or more spunbond layers comprising spunbond fibers. In some embodiments, the spunbond fibers are prepared from a polymer composition comprising a polypropylene polymer having one or more of the following properties: exhibiting a melt flow rate of about 20 g / 10 min to about 70 g / 10 min; having a molecular weight distribution (M) of less than about 4. w / M n ); and having a xylene solubles content of about 1.5 wt % to about 4 wt %.
[0198] In some embodiments, the polypropylene polymer has an M of about 3.0 to about 4.0, including about 3.0, about 3.5, and about 4.0. w / M nIn some embodiments, the polypropylene polymer has a weight average molecular weight of less than about 300,000 g / mol, including less than about 250,000, less than about 200,000, and less than about 150,000. In some embodiments, the polypropylene polymer has a weight average molecular weight of about 150,000 to about 250,000, including about 150,000, about 200,000, and about 250,000. In some embodiments, the polypropylene polymer has a number average molecular weight of less than about 60,000 g / mol, including less than about 55,000 g / mol, less than about 50,0000 g / mol, less than about 45,000 g / mol, and less than about 40,000 g / mol. In some embodiments, the polypropylene polymer has a number average molecular weight of about 40,000 to about 55,000 g / mol, including about 40,000 g / mol, about 45,000 g / mol, about 50,000 g / mol, and about 55,000 g / mol. In some embodiments, the polypropylene polymer exhibits a melting temperature greater than 155°C.
[0199] In some embodiments, the nonwoven web comprises two or more spunblown layers. In some embodiments, the two or more spunblown layers comprise the same spunblown layer. In some embodiments, the two or more spunblown layers comprise different spunblown layers.
[0200] In some embodiments, the nonwoven web has a multilayer structure including a first spunbond layer, a meltblown layer, and a second spunbond layer. In some embodiments, the first spunbond layer and the second spunbond layer are the same. In some embodiments, the first spunbond layer and the second spunbond layer are different.
[0201] In some embodiments, the nonwoven web has a density of less than about 100 1 / m 2 / s, including less than about 95l / m 2 / s, less than about 90l / m 2 / s, less than about 85l / m 2 / s, less than about 80l / m 2 / s, less than about 75l / m 2 / s, less than about 70l / m 2 / s, less than about 65l / m 2 / s, less than about 60l / m 2 / s, less than about 65l / m 2 / s, less than about 50l / m 2 / s, less than about 55l / m 2 / s, and less than about 50 l / m 2 / s air permeability. In some embodiments, the nonwoven web has an air permeability of about 40 to about 80 l / m 2 / s, including about 40l / m 2 / s, about 45l / m 2 / s, about 50l / m 2 / s, about 55l / m 2 / s, about 60l / m 2 / s, about 65l / m 2 / s, about 70l / m 2 / s, about 75l / m 2 / s, and 80l / m 2 / s air permeability. The air permeability can be determined by the meltblown fiber size (average fiber diameter) and / or the meltblown fiber size distribution (fiber size standard deviation).
[0202] In some embodiments, the nonwoven web has a machine direction (MD) tensile strength of about 2500 g / inch to about 3500 g / inch, including about 2500 g / inch, about 3000 g / inch, and about 3500 g / inch.
[0203] In another aspect, a method for producing any of the nonwoven webs disclosed herein is provided, comprising contacting one or more meltblown layers with two or more spunbond layers at a bonding temperature of about 130°C to about 140°C.
[0204] The bonding temperature may be about 130° C., about 135° C., or about 140° C. In some embodiments, the bonding temperature is about 135° C.
[0205] The invention thus generally described will be more readily understood by reference to the following examples, which are provided by way of illustration and are not intended to be limiting of the invention. Example
[0206] Example 1. Various high melt flow rate polypropylene homopolymers were made using two different catalysts (catalyst A and catalyst B) according to the present disclosure. The preparation of these polypropylenes is also described in PCT application number PCT / US2021 / 049547 filed on September 9, 2021, and the disclosure of such polymers is incorporated herein by reference. The following sample numbers 13 to 18 were made using catalyst B, which is a LYNX 1010 catalyst available from WR Grace and Company. The LYNX 1010 catalyst comprises a solid catalyst component comprising a magnesium portion, a titanium portion, an epoxy compound, and an organosilicon compound. The LYNX 1010 catalyst comprises a phthalate compound as an internal electron donor.
[0207] Catalyst A (similar solid catalyst component but using a non-phthalate substituted phenylene diester internal electron donor) was used to prepare the following Sample Nos. 1 to 12 and 19 to 21.
[0208] Both catalyst systems were used in combination with a selectivity control agent. The selectivity control agent used was propyltriethoxysilane. The selectivity control agent was used together with amyl valerate as an activity limiting agent. The molar ratio of the selectivity control agent to the activity limiting agent was 40:60.
[0209] The reactor carries out polymerization in a gas phase fluidized bed with a compressor and a cooler connected to a recycle gas line.
[0210] The above catalyst was used in combination with triethylaluminum (TEA1) as a co-catalyst to produce a polypropylene resin powder in a fluidized bed reactor.
[0211] The fluidized bed reactor is operated under the following conditions:
[0212] Reactor Temperature: 72°C for Examples 1 to 17, or 80°C for Example 18 Bed Weight: 68 to 72 lbs
[0213] Superficial Gas Velocity: 1.0 to 1.6 ft / s.
[0214] All polymers were made with a hydrogen to monomer ratio of about 0.11 to about 0.23. All polymers produced had a xylene soluble content of 1.5 to 6 wt % and a molecular weight distribution greater than 2.5. Catalyst productivity was 10 to 40 tons / kg catalyst, averaging about 20 tons / kg. Ultra-high melt flow rate polymers were made without the need to use peroxides. Polymer particle size was determined using the GRADEX sieving test.
[0215] The following samples were manufactured and the following results were obtained:
[0216]
[0217]
[0218]
[0219] As shown above, all samples have a melt flow rate greater than 900 g / 10 min, with the highest melt flow rate being 8,152 g / 10 min. The results are also shown in Figures 2 to 4 In. Figure 4 As shown in , the amount of fines generated during this process is relatively low.
[0220] As shown above, higher reactor temperatures are beneficial. Sample 18 was made at 80°C, while samples 1-17 were made at 72°C. Comparing Examples 14 and 18, when the reactor temperature is higher, the molecular weight distribution (MWD) and Mw are both lower, while the melt flow rate is higher and the hydrogen ratio remains about the same.
[0221] As shown in the table below, additional samples were made with Catalyst A at higher reactor temperatures.
[0222] Table 5:
[0223]
[0224] The materials made with Catalysts A and B were evaluated on a meltblown line to produce fibers having average fiber diameters as shown in Table 6:
[0225] Table 6:
[0226]
[0227] Example 2. Resin properties:
[0228] All reactor grade powders were pelletized using a Brabender single screw extruder at a processing temperature of 200°C and 60 RPM. The additive package for all powders according to the present disclosure during pelletization was the same: 400 ppm 1010,800ppm 168 & 180ppm ZnO.
[0229] Comparative #4 is a commercial polypropylene grade intended for meltblown applications, made using a Ziegler-Natta catalyst and subjected to peroxide cleavage to achieve high MFR. Comparative #3 is a polypropylene resin made using a metallocene catalyst and not subjected to peroxide cleavage.
[0230] Inventions #1 and #2 were made using Catalyst B, which is LYNX 1010 catalyst commercially available from WR Grace and Company. The LYNX 1010 catalyst comprises a solid catalyst component comprising a magnesium moiety, a titanium moiety, an epoxy compound, and an organosilicon compound. The LYNX 1010 catalyst comprises a phthalate compound as an internal electron donor.
[0231] Comparatives #1 and #2 were made using Catalyst A, which was a similar solid catalyst component but used a non-phthalate substituted phenylene diester internal electron donor.
[0232]
[0233] Note: The properties of Comparative #3 were tested on powder, while all other samples were tested as pellets. The XS content of Comparative #3 was tested by wet method, while all other samples were tested by XS Viscotek method.
[0234] MB fabric properties: MB fabrics were manufactured on a lab scale LBRD extrusion line (5 / 8" extruder with L / D of 24:1) with an MB head (die with 23 holes). All samples were produced under the same manufacturing conditions. The processing temperature was maintained at 230°C and the throughput was maintained at 0.6 ghm (belt speed = 3.5 m / min). Air pressure of 5 psi and 259°C were provided for quenching. The fabric basis weight was maintained at 20 grams. No calendering or bonding was applied on the MB fabrics, and the fabrics were collected after low pressure rolling at room temperature.
[0235] The average fiber size (or fiber diameter) and size distribution in MB fabrics are the most important factors for MB fabrics. Generally, smaller fiber sizes result in softer fabrics, better liquid barrier and lower air permeability. As described in the test procedure section, the average fiber diameter is obtained by the average of 50 measurements of five SEM images at different locations on the fabric.
[0236]
[0237] As shown in the table above, under the same MB manufacturing conditions, the two MB fabrics made with Catalyst A (Comparative #1 and #2) have larger average fiber size and wider distribution than the two inventive samples. This is due to the larger Mz and Mz+1 of Comparative #1 and #2, which produce more long-chain molecular entanglements and more fiber breakage during attenuation. Fiber breakage prevents further attenuation of MB fibers and results in fibers with larger diameters.
[0238] SMS fabric properties: SMS multilayer fabrics (SBNW-MB-SBNW) were made from non-calendered MB fabric and SBNW fabric produced on NRX-12SBNW equipment calendered off-line. Six different MB fabrics were made with 4 inventive samples and 2 comparative samples were used in SMS fabrics. For the SBNW layer, two commercial grade SBNW pellets (X and Y) were used in different SMS fabrics. Pellets X were PP technology is available from WRGrace The pellets were prepared from a 35 MFR cracker grade hPP resin for SBNW applications using an unknown catalyst and process technology.
[0239]
[0240] All SBNW fabrics were first produced on a lab-scale BRD extrusion line (1.25" extruder with a L / D of 30:1) with a NRX-12SBNW device, which included an SBNW spinning pack with 72 holes and a diameter of 0.35 mm per hole. All samples were prepared under the same manufacturing conditions matching the MB manufacturing process. The processing temperature was maintained at 230°C, and the throughput was maintained at 0.6 ghm (belt speed = 3.5 m / min). The fabric basis weight was maintained at 20 gsm. The aspirator air pressure for attenuation was maintained at 28 psi. Immediately after the two layers of uncalendered SBNW fabrics were produced, they were calendered offline with uncalendered MB fabric in a sandwich structure (MB as the core layer) at a bonding temperature of 135°C. The tensile strength and air permeability of the SMS nonwoven fabrics were determined according to the methods described in the test procedures section.
[0241] Machine direction (MD) tensile strength is one of the most important properties of SMS fabrics as it affects the mechanical properties of SMS fabric final products such as diapers and masks. The MD tensile strength of SMS fabrics mainly depends on the bonding conditions between the two SBNW layers and the SBNW layer and the MB layer. Therefore, at the same bonding temperature of 135°C and the same SBNW layer (HT2511 or PP3155E5), the SMS fabric made with the MB layer of the present invention shows a tensile strength similar to that of the comparative counterpart (the difference in the average value is within 10%). The reason for the small difference in tensile strength between the inventive grade and the comparative grade is because the mechanical properties are determined by the SBNW layer in the SMS fabric instead of the MB core layer.
[0242]
[0243] Air permeability is another important property of SMS fabrics because it affects the filtration efficiency of SMS fabric end products such as industrial filters. Generally, finer fibers in the MB layer produce smaller pore sizes, which contribute to lower air permeability and high filtration efficiency. Low air permeability is usually associated with high hydrohead or high liquid barrier, which is important for SMS fabric end products used in medical and hygiene applications (such as diapers). The two inventive grades show similar air permeability to Comparative #3 and #4, while Comparative #1 and #2 have much higher air permeability. This is because of the larger average fiber diameter and larger standard deviation of Comparative #1 and #2, which is due to the high MB. z+1 / M w Than (or higher M z and M z+1 ).
[0244] Furthermore, these results highlight the balance of air permeability vs mechanical properties of the SMS fabric of Invention #1 (vs. Comparative Examples 3 and 4, commercial products with metallocene catalyst or cracking grade), and outperform Comparatives 1 & 2.
[0245] While certain embodiments have been shown and described, it should be understood that changes and modifications may be made thereto in accordance with ordinary skill in the art without departing from the technology in its broader aspects as defined in the following claims.
[0246] The embodiments exemplarily described herein may be suitably implemented in the absence of any elements, limitations, not specifically disclosed herein. Thus, for example, the terms "comprise", "include", "contain", etc. should be interpreted broadly and not restrictively. In addition, these terms and expressions used herein are used as descriptive and not restrictive terms, and in the use of these terms and expressions, there is no intention to exclude any equivalents of the features shown and described or parts thereof, but it is recognized that various modifications may be possible within the scope of the claimed technology. In addition, the phrase "essentially consisting of..." is understood to include those elements specifically listed and those additional elements that do not substantially affect the basic and novel features of the claimed technology. The phrase "consisting of..." excludes any element that is not specified.
[0247] The present disclosure is not limited to the specific embodiments described in this application. As will be apparent to those skilled in the art, many modifications and variations may be made without departing from its spirit and scope. Functionally equivalent methods and compositions within the scope of the present disclosure, except those listed herein, will be apparent to those skilled in the art from the above description. Such modifications and variations are intended to fall within the scope of the appended claims. The present disclosure is limited only by the terms of the appended claims and the full range of equivalents to which these claims are entitled. It is to be understood that the present disclosure is not limited to specific methods, reagents, compounds, compositions, or biological systems, which are of course variable. It is also to be understood that the terms used herein are only used to describe specific embodiments and are not intended to constitute limitations.
[0248] In addition, where features or aspects of the disclosure are described in terms of Markush groups, those skilled in the art will recognize that the disclosure is also thereby described in terms of any member or subgroup of members of the Markush group.
[0249] Those skilled in the art will appreciate that, for any and all purposes, particularly in providing a written description, all ranges disclosed herein also include any and all possible subranges and combinations of subranges thereof. Any enumerated range is readily identified as fully describing and allowing the same range to be split into at least two equal parts, three equal parts, four equal parts, five equal parts, ten equal parts, and the like. As a non-limiting example, each range discussed herein is easily split into the lower 1 / 3, the middle 1 / 3, and the upper 1 / 3, and the like. Those skilled in the art will also appreciate that all words such as "at most", "at least", "greater than", "less than" and the like include the enumerated values and refer to the ranges that can be subsequently split into subranges as discussed above. Finally, as those skilled in the art understand, a range includes each member.
[0250] All publications, patent applications, issued patents, and other documents mentioned in this specification are incorporated herein by reference, just as if each publication, patent application, issued patent, or other document was specifically and individually indicated to be incorporated herein by reference in its entirety. Definitions contained in the text incorporated by reference are excluded in the event of a conflict with a definition in this disclosure.
[0251] Other embodiments are set forth in the following claims.
Claims
1. A polymer composition comprising a polypropylene polymer having the following characteristics: exhibiting a melt flow rate greater than about 900 g / 10 min; Molecular weight distribution (M) greater than 4.5 w / M n ); Less than about 8 M z+1 / M w than; and A xylene soluble content of less than about 4.0 wt%.
2. The polymer composition of claim 1 wherein the polypropylene polymer exhibits a melt flow rate greater than about 1300 g / 10 min.
3. The polymer composition of claim 1 wherein the polypropylene polymer exhibits a melt flow rate of about 1300 g / 10 min to about 4000 g / 10 min.
4. The polymer composition of any one of claims 1 to 3, wherein the polypropylene polymer has an M greater than about 6. w / M n .
5. The polymer composition of any one of claims 1 to 3, wherein the polypropylene polymer has an M greater than about 7. w / M n .
6. The polymer composition of any one of claims 1-3, wherein the polypropylene polymer has an M of about 6.0 to about 10.
0. w / M n .
7. The polymer composition of any one of claims 1 to 6, wherein the polypropylene polymer has an M of less than about 7. z+1 / M w Compare.
8. The polymer composition of any one of claims 1-6, wherein the polypropylene polymer has an M of about 6.0 to about 8.
0. z+1 / M w Compare.
9. The polymer composition of any one of claims 1-8, wherein the polypropylene polymer has a xylene solubles content of about 1.5 wt% to about 4 wt%.
10. The polymer composition of any one of claims 1-9, wherein the polypropylene polymer exhibits a melting temperature greater than about 155°C.
11. The polymer composition of any one of claims 1-9, wherein the polypropylene polymer exhibits a melting temperature of about 155°C to about 165°C.
12. The polymer composition of any one of claims 1-11, wherein the polypropylene polymer has a weight average molecular weight of less than about 80,000 g / mol.
13. The polymer composition of any one of claims 1-11, wherein the polypropylene polymer has a weight average molecular weight of about 55,000 g / mol to about 70,000 g / mol.
14. The polymer composition of any one of claims 1-13, wherein the polypropylene polymer has a number average molecular weight of less than about 8,500 g / mol.
15. The polymer composition of any one of claims 1-13, wherein the polypropylene polymer has a number average molecular weight of about 7,000 g / mol to about 8,000 g / mol.
16. The polymer composition of any one of claims 1 to 15, wherein the polypropylene polymer is a polypropylene homopolymer.
17. The polymer composition according to any one of claims 1 to 16, wherein the polypropylene polymer has been Ziegler-Natta catalyzed.
18. The polymer composition of claim 17, wherein the polypropylene polymer has been catalyzed in the presence of a Ziegler-Natta catalyst comprising an internal electron donor comprising a substituted phenylene diester or phthalate compound.
19. The polymer composition of any one of claims 1-18, wherein the polypropylene polymer comprises a processing aid in combination with at least one other polymer exhibiting a relatively low melt flow rate, the polypropylene polymer being included in the composition in an amount less than about 50 wt%.
20. The polymer composition of claim 19, wherein the polypropylene polymer comprises a wax, a lubricant, a mold release agent, or a flow aid.
21. The polymer composition according to any one of claims 1 to 20, wherein the polypropylene polymer has been catalyzed in the presence of a Ziegler-Natta catalyst comprising a solid catalyst component comprising a magnesium moiety, a titanium moiety and an internal electron donor, a selectivity control agent and optionally an activity limiting agent.
22. The polymer composition of claim 21, wherein the solid catalyst component further comprises an organosilicon compound and an epoxy compound.
23. A polymer composition according to claim 21 or claim 22, wherein the selectivity control agent comprises an organosilicon compound.
24. The polymer composition of claim 23, wherein the selectivity control agent comprises propyltriethoxysilane, diisobutyldimethoxysilane, n-propyltrimethoxysilane, or a mixture thereof, and is used in combination with an activity limiting agent.
25. The polymer composition of any one of claims 1-24, wherein the polypropylene polymer does not contain any peroxide.
26. The polymer composition of any one of claims 1-25, wherein the composition is suitable for meltblown nonwoven applications.
27. A meltblown web comprising nonwoven meltblown fibers made from the polymer composition of any one of claims 1-26.
28. Meltblown fibers made from the polymer composition of any one of claims 1-26, the meltblown fibers having a diameter less than about 5 microns.
29. The meltblown fiber of claim 28, wherein the meltblown fiber has a diameter of less than about 3 microns.
30. The meltblown fibers of claim 28, wherein the meltblown fibers have a diameter of about 1.5 microns to about 3.0 microns.
31. A nonwoven web comprising a multi-layer structure comprising one or more meltblown layers, the meltblown layers comprising the meltblown fibers according to any one of claims 28-30.
32. The nonwoven web of claim 31 , wherein the nonwoven web comprises a meltblown layer.
33. The nonwoven web of claim 31 , wherein the nonwoven web comprises two or more meltblown layers.
34. The nonwoven web of claim 33, wherein the two or more meltblown layers comprise the same meltblown layer.
35. The nonwoven web of claim 33, wherein the two or more meltblown layers comprise different meltblown layers.
36. The nonwoven web of any one of claims 31-35, further comprising two or more spunbond layers comprising spunbond fibers.
37. The nonwoven web of claim 36, wherein the spunbond fibers are prepared from a polymer composition comprising a polypropylene polymer having one or more of the following properties: exhibiting a melt flow rate of about 20 g / 10 min to about 70 g / 10 min; Having a molecular weight distribution (M) of less than about 4 w / M n );and Having a xylene soluble content of about 1.5 wt % to about 4 wt %.
38. The nonwoven web of claim 37, wherein the polypropylene polymer has an M of about 3.0 to about 4.
0. w / M n .
39. The nonwoven web of claim 37 or claim 38, wherein the polypropylene polymer has a weight average molecular weight of less than about 300,000 g / mol.
40. The nonwoven web of claim 37 or claim 38, wherein the polypropylene polymer has a weight average molecular weight of about 150,000 to about 250,000 g / mol.
41. The nonwoven web of any one of claims 37-40, wherein the polypropylene polymer has a number average molecular weight of less than about 60,000 g / mol.
42. The nonwoven web of any of claims 37-40, wherein the polypropylene polymer has a number average molecular weight of about 40,000 to about 55,000 g / mol.
43. The nonwoven web of any one of claims 37-42, wherein the polypropylene polymer exhibits a melting temperature greater than 155°C.
44. The nonwoven web of any one of claims 36-43, wherein the nonwoven web comprises two or more spunblown layers.
45. The nonwoven web of claim 44, wherein the two or more spunblown layers comprise the same spunblown layer.
46. The nonwoven web of claim 44, wherein the two or more spunblown layers comprise different spunblown layers.
47. The nonwoven web according to any one of claims 37-46, wherein the nonwoven web has a multilayer structure including a first spunbond layer, a meltblown layer, and a second spunbond layer.
48. The nonwoven web of claim 47, wherein the first and second spunbond layers are identical.
49. The nonwoven web of claim 47, wherein the first and second spunbond layers are different.