ASA resin and preparation method thereof
Through the combination of emulsion polymerization and suspension polymerization, ASA resin with core-mantle-shell structure is directly prepared, which solves the problems of many process steps and high production costs in the prior art, and achieves high efficiency and low cost ASA Resin produced, with excellent melt flow rate and impact strength.
Patent Information
- Application Number
- CN202411261603.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-29
AI Technical Summary
There are many steps in the production process of ASA resins, large equipment investment, high production costs, and additional steps such as coagulation and SAN resin blending are required.
ASA resin with a core-mantle-shell structure from the inside to the outside is prepared directly by combining emulsion polymerization and suspension polymerization. The polymerization and blending steps of aggregation and SAN resin are omitted, and alkyl acrylate monomers are used. The aromatic vinyl monomer and the vinyl cyano monomer are cross-linked and polymerized to form a resin with high melt flow rate and impact strength.
ASA resin with simplified process flow and reduced production costs has been achieved, and it has a high melt flow rate and high impact strength is suitable for automobiles, building materials, electronics and electrical appliances.
Smart Images

Figure BDA0005036451360000021 
Figure BDA0005036451360000101 
Figure FDA0005036451120000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials and relates to an ASA resin and a method for preparing the resin by adopting emulsion polymerization and suspension polymerization. Background Art
[0002] ABS (acrylonitrile-butadiene-styrene copolymer) resin with polybutadiene as rubber phase has poor thermal stability and weather resistance due to the unsaturated double bonds in polybutadiene. ASA (acrylate-styrene-acrylonitrile copolymer) resin with acrylic polymer as rubber phase has no unsaturated double bonds in its molecular structure. In addition to having the same physical and mechanical properties and molding processing properties as ABS resin, it also has the unique advantages of good thermal stability and weather resistance. It is increasingly used in the fields of automobiles, building materials, electronic appliances, etc.
[0003] In the prior art disclosed in European patent document EP3519451, the following method is usually used to produce ASA resin: first, a core-shell structure ASA copolymer emulsion with polyacrylate as a core layer and styrene-acrylonitrile copolymer as a shell layer is prepared by emulsion polymerization, and then the emulsion is condensed to obtain ASA high-glue powder slurry, and the slurry is dehydrated and dried to obtain ASA high-glue powder, and finally the ASA high-glue powder is mixed with SAN (styrene-acrylonitrile copolymer) resin through a twin-screw extruder to obtain ASA resin.
[0004] In the above prior art methods, after the polymerization reaction is completed, ASA resin needs to be obtained through steps such as coagulation and blending with SAN resin, and the SAN resin used for blending needs to be produced separately. The process steps are numerous, the equipment investment is large, and the production cost is high. Summary of the invention
[0005] In order to improve the above technical problems, the present invention provides an ASA resin having a core-mantle-shell structure from inside to outside, wherein the core is a cross-linked polymer of an alkyl acrylate monomer, the mantle layer is a cross-linked polymer of an aromatic vinyl monomer and a vinyl cyan monomer, and the shell layer is a linear polymer of an aromatic vinyl monomer and a vinyl cyan monomer.
[0006] According to an embodiment of the present invention, the alkyl group in the alkyl acrylate monomer may be selected from C 2-20 Alkyl, preferably C 2-10 Alkyl, such as C2 alkyl (ethyl), C3 alkyl (propyl, isopropyl), C4 alkyl (butyl), C5 alkyl (pentyl), C6 alkyl (hexyl), C7 alkyl (heptyl), C8 alkyl (octyl, 2-ethylhexyl), C9 alkyl (nonyl), C 10Alkyl (decyl); for example, the alkyl acrylate monomer may be selected from one or more of ethyl acrylate, propyl acrylate, isopropyl acrylate, butyl acrylate, hexyl acrylate, octyl acrylate and 2-ethylhexyl acrylate.
[0007] According to an embodiment of the present invention, the aromatic vinyl monomer has a structure as shown in Formula I,
[0008]
[0009] Among them, R a and R b The same or different, independently selected from H, C 1-10 Alkyl or halogen; for example, independently selected from H, C 1-4 Alkyl or halogen; exemplarily selected from H, methyl, ethyl, propyl, butyl, fluorine, chlorine, bromine or iodine;
[0010] R a The number of R can be one, two, three, four or five, and each substitution position R a Same or different.
[0011] In some embodiments, R a Selected from H, C 1-10 Alkyl or halogen, R b Select from H or C 1-10 alkyl.
[0012] In some embodiments, R a The number of is one or two; when it is two, it can be a C 1-10 Alkyl or one halogen, two identical or different halogens, two identical or different C 1-10 alkyl.
[0013] According to some embodiments of the present invention, the aromatic vinyl monomer may be selected from one or more of styrene, α-methylstyrene, vinyltoluene and 3,4-dichlorostyrene.
[0014] According to an embodiment of the present invention, the vinyl cyanide monomer is selected from one or more of acrylonitrile and alkyl acrylonitrile, wherein the alkyl group in the alkyl acrylonitrile is C 1-4 The alkyl group is, for example, a methyl group, an ethyl group, a propyl group or a butyl group. In some embodiments, the vinyl cyano monomer may be selected from one or both of acrylonitrile and methacrylonitrile.
[0015] According to an embodiment of the present invention, the mantle layer is obtained by emulsion polymerization of aromatic vinyl monomer, vinyl cyan monomer and crosslinking monomer in the core layer emulsion in the presence of an emulsifier and an initiator;
[0016] For example, the crosslinking monomer is selected from one or more of diol di(meth)acrylate, divinylbenzene, diallyl maleate, diallyl fumarate, diallyl phthalate, allyl (meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane triacrylate and triallyl (iso)cyanurate.
[0017] According to an embodiment of the present invention, the ratio of the sum of parts by weight of the aromatic vinyl monomer and the vinyl cyan monomer for preparing the mantle layer to the sum of parts by weight of the aromatic vinyl monomer and the vinyl cyan monomer for preparing the shell layer is (10-80):(20-90), for example, 10:90, 20:80, 30:70, 40:60, 50:50, 60:40, 70:30, 80:20 or 10:90.
[0018] According to an embodiment of the present invention, the aromatic vinyl monomer of the mantle layer is the same as or different from the aromatic vinyl monomer of the shell layer.
[0019] According to an embodiment of the present invention, the vinyl cyan monomer of the mantle layer is the same as or different from the vinyl cyan monomer of the shell layer.
[0020] According to an embodiment of the present invention, the melt flow rate of the ASA resin is not less than 5g / 10min, for example, not less than 8g / 10min, such as 8-20g / 10min, exemplified by 8g / 10min, 9g / 10min, 10g / 10min, 11g / 10min, 12g / 10min, 14g / 10min, 15g / 10min, 16g / 10min, 17g / 10min, 18g / 10min, 19g / 10min; in one embodiment, the melt flow rate is obtained by testing according to GB / T 3682.1-2018.
[0021] According to an embodiment of the present invention, the impact strength of the ASA resin is not less than 12 kJ / m 2 , for example, not less than 15kJ / m 2 , for example, 15 to 60 kJ / m 2 , exemplified by 20 kJ / m 2 、25kJ / m 2 、30kJ / m 2 、35kJ / m 2 、40kJ / m 2 、45kJ / m 2 、50kJ / m 2 、55kJ / m 2 In one embodiment, the impact strength is tested according to GB / T 1843-2008.
[0022] According to an embodiment of the present invention, the particle size of the core is 100-500 nm, for example, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm or 450 nm.
[0023] According to an embodiment of the present invention, the thickness of the mantle layer is 2 to 80 nm, for example, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm or 70 nm.
[0024] According to an embodiment of the present invention, the thickness of the shell layer is 2 to 60 nm, for example, 5 nm, 10 nm, 20 nm, 30 nm, 40 nm or 50 nm.
[0025] In one embodiment, the ASA resin has a core-mantle-shell structure from inside to outside, the core is a cross-linked polymer of butyl acrylate monomer, the mantle is a cross-linked polymer of styrene monomer and acrylonitrile monomer, and the shell is a linear polymer of styrene monomer and acrylonitrile monomer.
[0026] The present invention also provides a method for preparing the above-mentioned ASA resin, comprising the following steps:
[0027] (a) Preparation of ASA emulsion
[0028] (a-1) an aromatic vinyl monomer, a vinyl cyan monomer and a crosslinking monomer are subjected to an emulsion polymerization reaction in a core layer emulsion to obtain a mantle layer emulsion;
[0029] The core layer emulsion is used to form the core, i.e., a cross-linked polymer of alkyl acrylate monomers;
[0030] (a-2) an aromatic vinyl monomer and a vinyl cyanide monomer are polymerized in the mantle layer emulsion in the presence of a molecular weight regulator to obtain a shell layer emulsion, i.e., an ASA emulsion;
[0031] (b) carrying out suspension polymerization of aromatic vinyl monomer and vinyl cyan monomer in water and the ASA emulsion in the presence of a stabilizer and a molecular weight regulator to obtain the ASA resin;
[0032] Preferably, the alkyl acrylate monomer, aromatic vinyl monomer, vinyl cyan monomer and crosslinking monomer have the definitions shown above.
[0033] According to an embodiment of the present invention, based on 100 parts by weight of the aromatic vinyl monomer and the vinyl cyanide monomer in step (a), the aromatic vinyl monomer and the vinyl cyanide monomer in step (a-1) total 10 to 80 parts by weight, and the aromatic vinyl monomer and the vinyl cyanide monomer in step (a-2) total 20 to 90 parts by weight; for example, the aromatic vinyl monomer and the vinyl cyanide monomer in step (a-1) total 10, 20, 30, 40, 50, 60, 70 or 80 parts by weight; the aromatic vinyl monomer and the vinyl cyanide monomer in step (a-2) total 90, 80, 70, 60, 50, 40, 30 or 20 parts by weight.
[0034] According to an embodiment of the present invention, the aromatic vinyl monomers in steps (a-1), (a-2) and (b) are the same or different; in some embodiments, the aromatic vinyl monomers used in any two or three steps are the same.
[0035] According to an embodiment of the present invention, the vinyl cyan monomers in steps (a-1), (a-2) and (b) are the same or different; in some embodiments, the vinyl cyan monomers used in any two or three steps are the same.
[0036] According to an embodiment of the present invention, the step (a) further comprises (a-3) preparing the core layer emulsion: an alkyl acrylate monomer and a cross-linking monomer are subjected to emulsion polymerization in a seed emulsion to obtain the core layer emulsion.
[0037] According to an embodiment of the present invention, the step (a) further comprises (a-4) preparing the seed emulsion: an alkyl acrylate monomer and a cross-linking monomer are subjected to an emulsion polymerization reaction in water to obtain the seed emulsion.
[0038] According to an embodiment of the present invention, based on 100 parts by weight of the alkyl acrylate monomers in steps (a-3) and (a-4), the alkyl acrylate monomer in step (a-3) is 5 to 50 parts by weight, and the alkyl acrylate monomer in step (a-4) is 50 to 95 parts by weight; for example, the alkyl acrylate monomer in step (a-3) is 5, 10, 15, 20, 25, 30, 35, 40, 45 or 50 parts by weight, and the alkyl acrylate monomer in step (a-4) is 95, 90, 85, 80, 75, 70, 65, 60, 55 or 50 parts by weight.
[0039] According to an embodiment of the present invention, the alkyl acrylate monomers of steps (a-3) and (a-4) are the same or different; in some embodiments, the alkyl acrylate monomers of the two steps are the same.
[0040] According to an embodiment of the present invention, the cross-linking monomers of steps (a-1), (a-3) and (a-4) are the same or different; in some embodiments, the cross-linking monomers of the three steps are the same.
[0041] According to an embodiment of the present invention, based on 100 parts by weight of all monomers in step (a), the alkyl acrylate monomer is 40 to 90 parts by weight, and the aromatic vinyl monomer and the vinyl cyan monomer are 10 to 60 parts by weight in total; for example, the alkyl acrylate monomer is 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight or 90 parts by weight, and the aromatic vinyl monomer and the vinyl cyan monomer are 60 parts by weight, 55 parts by weight, 50 parts by weight, 45 parts by weight, 40 parts by weight, 35 parts by weight, 30 parts by weight, 25 parts by weight, 20 parts by weight, 15 parts by weight or 10 parts by weight in total.
[0042] According to an embodiment of the present invention, the reaction system of steps (a-1), (a-2), (a-3) and / or (a-4) further contains an emulsifier. For example, the emulsifier is selected from one or more of alkyl sulfates, alkyl sulfonates, alkyl benzene sulfonates, alkyl ether sulfates, alkyl ether disulfates, alkyl aryl ether sulfates, alkyl aryl ether disulfates, alkyl ether sulfonates, alkyl ether disulfonates, alkyl aryl ether sulfonates, alkyl aryl ether disulfonates, alkyl polyether sulfates, alkyl aryl polyether sulfates, fatty acid alkyl ester sulfonates, alkyl sulfosuccinic acid diester salts, alkyl sulfosuccinic acid monoester salts, alkyl polyether sulfosuccinic acid diester salts, alkyl polyether sulfosuccinic acid monoester salts; for example, one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, etc. The emulsifiers used in the above steps are the same or different.
[0043] According to an embodiment of the present invention, the reaction system of steps (a-1), (a-2), (a-3) and / or (a-4) further comprises an initiator. For example, the initiator is a peroxide; for example, one or more of sodium persulfate, potassium persulfate, ammonium persulfate, cumene hydroperoxide, tert-butyl perbenzoate, etc. The initiators used in the above steps are the same or different.
[0044] According to an embodiment of the present invention, the molecular weight regulators in step (a-2) and step (b) are the same or different and are independently selected from one or more of n-dodecyl mercaptan, t-dodecyl mercaptan, n-decyl mercaptan, and a-methylstyrene dimer.
[0045] According to an embodiment of the present invention, the stabilizer may be selected from one or more of methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone, talc, clay, gelatin and the like.
[0046] According to an embodiment of the present invention, the reaction system of step (b) further contains an initiator selected from oil-soluble organic peroxides or azo compounds, such as one or more of benzoyl peroxide, azobisisobutyronitrile, azobisisoheptanenitrile and the like.
[0047] According to an embodiment of the present invention, the reaction temperatures of steps (a-1), (a-2), (a-3), (a-4) and step (b) are the same or different and are independently selected from 60-80°C, for example 65-70°C or 70-75°C.
[0048] According to an embodiment of the present invention, the reaction times of steps (a-1), (a-2), (a-3), (a-4) and step (b) are the same or different and are independently selected from 1-6 hours, for example 2 hours, 3 hours, 4 hours or 5 hours.
[0049] According to an embodiment of the present invention, step (b) further comprises filtering, washing and drying the obtained slurry after the suspension polymerization reaction is completed to obtain the ASA resin.
[0050] According to an embodiment of the present invention, based on 100 parts by weight of the prepared ASA resin, the polymerization product of step (a) is 20 to 50 parts by weight, and the polymerization product of step (b) is 50 to 80 parts by weight; for example, the polymerization product of step (a) is 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight or 50 parts by weight, and the polymerization product of step (b) is 80 parts by weight, 75 parts by weight, 70 parts by weight, 65 parts by weight, 60 parts by weight, 55 parts by weight or 50 parts by weight.
[0051] The present invention also provides the application of the ASA resin in the fields of automobiles, building materials, electronic appliances, etc.
[0052] Beneficial Effects
[0053] The present invention provides an ASA resin with a core-mantle-shell structure, wherein the mantle layer is a cross-linked polymer and the shell layer is a linear polymer, and the ASA resin has both high melt flow rate and high impact strength. At the same time, the present invention also provides a preparation method of the ASA resin, which directly prepares the ASA resin by a method combining emulsion polymerization and suspension polymerization, and compared with the prior art, omits the steps of coagulation, SAN resin polymerization, blending, etc. DETAILED DESCRIPTION
[0054] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0055] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0056] Example 1
[0057] (1) Seed emulsion preparation
[0058] In a reactor in a nitrogen atmosphere, 200 parts by weight of deionized water, 1 part by weight of sodium lauryl sulfate, 0.2 parts by weight of potassium persulfate, and then 60 parts by weight of butyl acrylate and 0.3 parts by weight of ethylene glycol dimethacrylate were added under stirring. The reactor temperature was raised to 65-70°C and kept warm for 3 hours to obtain a seed emulsion.
[0059] (2) Preparation of nuclear layer emulsion
[0060] Take 44 parts by weight of seed emulsion, add 50 parts by weight of deionized water and 0.2 parts by weight of potassium persulfate, then add a mixture of 50 parts by weight of deionized water, 0.1 parts by weight of sodium lauryl sulfate, 60 parts by weight of butyl acrylate, 0.3 parts by weight of ethylene glycol dimethacrylate and 0.3 parts by weight of hydroxyethyl methacrylate within 2 hours, and keep warm at 70-75°C for 2 hours after the addition to obtain a core layer emulsion with a particle size of 285nm.
[0061] (3) Mantle layer emulsion preparation
[0062] After the core layer emulsion is kept warm, 0.15 parts by weight of sodium formaldehyde sulfoxylate and 0.015 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70°C. A mixture of 12 parts by weight of deionized water, 0.15 parts by weight of sodium dodecyl sulfate, 9 parts by weight of styrene, 3 parts by weight of acrylonitrile, 0.09 parts by weight of diallyl phthalate and 0.1 parts by weight of isopropylbenzene hydroperoxide are added within 1 hour. After the addition, the mixture is kept warm at 70-75°C for 2 hours to obtain a mantle layer emulsion with a particle size of 299 nm.
[0063] (4) Shell emulsion preparation
[0064] After the insulation of the mantle layer emulsion is completed, 0.25 parts by weight of sodium formaldehyde sulfoxylate and 0.025 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70°C. A mixture of 20 parts by weight of deionized water, 0.25 parts by weight of sodium dodecyl sulfate, 13.5 parts by weight of styrene, 4.5 parts by weight of acrylonitrile, 0.09 parts by weight of n-dodecyl mercaptan and 0.15 parts by weight of cumene hydroperoxide is added within 1 hour. After the addition is completed, the mixture is kept at 70-75°C for 2 hours to obtain a shell layer emulsion, i.e., an ASA emulsion, with a particle size of 318 nm.
[0065] (5) Preparation of ASA resin
[0066] In a reactor in a nitrogen atmosphere, 150 parts by weight of deionized water and 100 parts by weight of ASA emulsion are mixed, and then a mixture of 45 parts by weight of styrene, 15 parts by weight of acrylonitrile, 0.4 parts by weight of dodecyl mercaptan and 0.08 parts by weight of azobisisobutyronitrile is added, and after stirring evenly, 0.2 parts by weight of polyvinyl alcohol is added, and the reactor temperature is raised to 70-75° C. and reacted for 5 hours to obtain ASA resin slurry. The obtained slurry is then filtered, washed and dried to obtain ASA resin.
[0067] Example 2
[0068] The same method as in Example 1 was used except that the mantle layer emulsion was prepared by the following method.
[0069] Preparation of mantle layer emulsion: After the core layer emulsion is kept warm, 0.1 parts by weight of sodium formaldehyde sulfoxylate and 0.01 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70°C. Within 1 hour, a mixture of 8 parts by weight of deionized water, 0.1 parts by weight of sodium dodecyl sulfate, 6 parts by weight of styrene, 2 parts by weight of acrylonitrile, 0.06 parts by weight of diallyl phthalate and 0.67 parts by weight of isopropylbenzene hydroperoxide are added. After the addition, the mixture is kept warm at 70-75°C for 2 hours to obtain a mantle layer emulsion with a particle size of 293 nm and a corresponding shell particle size of 317 nm.
[0070] Example 3
[0071] The same method as in Example 1 was used except that the mantle layer emulsion was prepared by the following method.
[0072] Preparation of mantle layer emulsion: After the core layer emulsion is kept warm, 0.2 parts by weight of sodium formaldehyde sulfoxylate and 0.02 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70°C. Within 1 hour, a mixture of 16 parts by weight of deionized water, 0.2 parts by weight of sodium dodecyl sulfate, 12 parts by weight of styrene, 4 parts by weight of acrylonitrile, 0.12 parts by weight of diallyl phthalate and 0.13 parts by weight of isopropylbenzene hydroperoxide are added. After the addition, the mixture is kept warm at 70-75°C for 2 hours to obtain a mantle layer emulsion with a particle size of 304 nm and a corresponding shell particle size of 319 nm.
[0073] Example 4
[0074] The same method as in Example 1 was used except that the shell emulsion was prepared by the following method.
[0075] Preparation of shell emulsion: After the insulation of the mantle layer emulsion is completed, 0.1 parts by weight of sodium formaldehyde sulfoxylate and 0.01 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70°C. Within 1 hour, a mixture of 8 parts by weight of deionized water, 0.1 parts by weight of sodium dodecyl sulfate, 5.4 parts by weight of styrene, 1.8 parts by weight of acrylonitrile, 0.04 parts by weight of n-dodecyl mercaptan and 0.06 parts by weight of cumene hydroperoxide are added. After the addition is completed, the mixture is kept at 70-75°C for 2 hours to obtain a shell emulsion, i.e., ASA emulsion, with a particle size of 307 nm.
[0076] Example 5
[0077] The same method as in Example 1 was used except that the shell emulsion was prepared by the following method.
[0078] Preparation of shell emulsion: After the insulation of the mantle layer emulsion is completed, 0.5 parts by weight of sodium formaldehyde sulfoxylate and 0.05 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70°C. A mixture of 40 parts by weight of deionized water, 0.5 parts by weight of sodium dodecyl sulfate, 27 parts by weight of styrene, 9 parts by weight of acrylonitrile, 0.18 parts by weight of n-dodecyl mercaptan and 0.3 parts by weight of cumene hydroperoxide are added within 1 hour. After the addition is completed, the mixture is kept at 70-75°C for 2 hours to obtain a shell emulsion, i.e., ASA emulsion, with a particle size of 335 nm.
[0079] Example 6
[0080] The same method as in Example 1 was used except that the ASA resin was prepared by the following method.
[0081] Preparation of ASA resin: In a reactor in a nitrogen atmosphere, 160 parts by weight of deionized water and 150 parts by weight of ASA emulsion are mixed, and then a mixture of 45 parts by weight of styrene, 15 parts by weight of acrylonitrile, 0.4 parts by weight of dodecyl mercaptan, and 0.08 parts by weight of azobisisobutyronitrile is added, and after stirring evenly, 0.2 parts by weight of polyvinyl alcohol is added, and the reactor temperature is raised to 70-75°C for reaction for 5 hours to obtain ASA resin slurry. The obtained slurry is then filtered, washed, and dried to obtain ASA resin.
[0082] Comparative Example 1
[0083] (1) Seed emulsion preparation
[0084] In a reactor in a nitrogen atmosphere, 200 parts by weight of deionized water, 1 part by weight of sodium lauryl sulfate, 0.2 parts by weight of potassium persulfate, and then 60 parts by weight of butyl acrylate and 0.3 parts by weight of ethylene glycol dimethacrylate were added under stirring. The reactor temperature was raised to 65-70°C and kept warm for 3 hours to obtain a seed emulsion.
[0085] (2) Preparation of nuclear layer emulsion
[0086] Take 44 parts by weight of seed emulsion, add 50 parts by weight of deionized water and 0.2 parts by weight of potassium persulfate, then add a mixture of 50 parts by weight of deionized water, 0.1 parts by weight of sodium lauryl sulfate, 60 parts by weight of butyl acrylate, 0.3 parts by weight of ethylene glycol dimethacrylate and 0.3 parts by weight of hydroxyethyl methacrylate within 2 hours, and keep warm at 70-75°C for 2 hours after the addition to obtain a core layer emulsion with a particle size of 285nm.
[0087] (3) Shell emulsion preparation
[0088] After the core layer emulsion is kept warm, 0.42 parts by weight of sodium formaldehyde sulfoxylate and 0.042 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70° C. Within 1 hour, a mixture of 33 parts by weight of deionized water, 0.42 parts by weight of sodium dodecyl sulfate, 22.5 parts by weight of styrene, 7.5 parts by weight of acrylonitrile, 0.15 parts by weight of n-dodecyl mercaptan and 0.25 parts by weight of cumene hydroperoxide is added, and after the addition is completed, the mixture is kept warm at 70-75° C. for 2 hours to obtain a shell layer emulsion, i.e., an ASA emulsion, with a particle size of 320 nm.
[0089] (4) Preparation of ASA resin
[0090] In a reactor in a nitrogen atmosphere, 150 parts by weight of deionized water and 100 parts by weight of ASA emulsion are mixed, and then a mixture of 45 parts by weight of styrene, 15 parts by weight of acrylonitrile, 0.4 parts by weight of dodecyl mercaptan and 0.08 parts by weight of azobisisobutyronitrile is added, and after stirring evenly, 0.2 parts by weight of polyvinyl alcohol is added, and the reactor temperature is raised to 70-75° C. and reacted for 5 hours to obtain ASA resin slurry. The obtained slurry is then filtered, washed and dried to obtain ASA resin.
[0091] Comparative Example 2
[0092] (1) Seed emulsion preparation
[0093] In a reactor in a nitrogen atmosphere, 200 parts by weight of deionized water, 1 part by weight of sodium lauryl sulfate, 0.2 parts by weight of potassium persulfate, and then 60 parts by weight of butyl acrylate and 0.3 parts by weight of ethylene glycol dimethacrylate were added under stirring. The reactor temperature was raised to 65-70°C and kept warm for 3 hours to obtain a seed emulsion.
[0094] (2) Preparation of nuclear layer emulsion
[0095] Take 44 parts by weight of seed emulsion, add 50 parts by weight of deionized water and 0.2 parts by weight of potassium persulfate, then add a mixture of 50 parts by weight of deionized water, 0.1 parts by weight of sodium lauryl sulfate, 60 parts by weight of butyl acrylate, 0.3 parts by weight of ethylene glycol dimethacrylate and 0.3 parts by weight of hydroxyethyl methacrylate within 2 hours, and keep warm at 70-75°C for 2 hours after the addition to obtain a core layer emulsion with a particle size of 285nm.
[0096] (3) Shell emulsion preparation
[0097] After the core layer emulsion is kept warm, 0.42 parts by weight of sodium formaldehyde sulfoxylate and 0.042 parts by weight of ferrous sulfate heptahydrate are added to the core layer emulsion, and the temperature is raised to 70°C. A mixture of 33 parts by weight of deionized water, 0.42 parts by weight of sodium lauryl sulfate, 22.5 parts by weight of styrene, 7.5 parts by weight of acrylonitrile, 0.23 parts by weight of diallyl phthalate and 0.25 parts by weight of cumene hydroperoxide is added within 1 hour. After the addition is completed, the mixture is kept warm at 70-75°C for 2 hours to obtain a shell layer emulsion, i.e., an ASA emulsion, with a particle size of 320 nm.
[0098] (4) Preparation of ASA resin
[0099] In a reactor in a nitrogen atmosphere, 150 parts by weight of deionized water and 100 parts by weight of ASA emulsion are mixed, and then a mixture of 45 parts by weight of styrene, 15 parts by weight of acrylonitrile, 0.4 parts by weight of dodecyl mercaptan and 0.08 parts by weight of azobisisobutyronitrile is added, and after stirring evenly, 0.2 parts by weight of polyvinyl alcohol is added, and the reactor temperature is raised to 70-75° C. and reacted for 5 hours to obtain ASA resin slurry. The obtained slurry is then filtered, washed and dried to obtain ASA resin.
[0100] Comparative Example 3
[0101] An ASA emulsion was prepared according to steps (1) to (3) of Comparative Example 2, and then:
[0102] (4) Preparation of ASA high-rubber powder
[0103] 2 parts by weight of calcium chloride and 200 parts by weight of deionized water are prepared into a solution and heated to 80°C. The ASA emulsion prepared above is added to the solution. After the addition, the temperature is raised to 95°C and kept for half an hour. The obtained solid is then washed and dried to obtain ASA high-rubber powder.
[0104] (5) Preparation of ASA resin
[0105] 35 parts by weight of the ASA high-rubber powder prepared above, 50 parts by weight of SAN resin (LG Chemical 82TR), 0.1 parts by weight of antioxidant 168, and 0.1 parts by weight of EBS lubricant were premixed. The premix was then fed into a twin-screw extruder, melt-extruded at an extrusion temperature of 220° C. and a screw speed of 300 rpm, and cooled and granulated to obtain ASA resin.
[0106] Test Example: Test of ASA resin performance
[0107] (1) Determination of melt flow rate: According to the requirements of GB / T 3682.1-2018, the melt flow rate of the ASA resin in the above embodiment and comparative example was tested using a melt flow rate meter.
[0108] (2) Determination of impact strength: According to the requirements of GB / T 1843-2008, ASA resin was injection molded into sheets using an injection molding machine, and the cantilever beam notched impact strength was tested.
[0109] The test results are shown in Table 1.
[0110] Table 1
[0111]
[0112] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An ASA resin, It is characterized in that The ASA resin has a core-mantle-shell structure from inside to outside, wherein the core is a cross-linked polymer of alkyl acrylate monomers, the mantle is a cross-linked polymer of aromatic vinyl monomers and vinyl cyan monomers, and the shell is a linear polymer of aromatic vinyl monomers and vinyl cyan monomers.
2. The ASA resin according to claim 1, It is characterized in that The alkyl group in the alkyl acrylate monomer is selected from C 2-20 Alkyl, preferably C 2-10 Alkyl; for example, the alkyl acrylate monomer is selected from one or more of ethyl acrylate, propyl acrylate, isopropyl acrylate, butyl acrylate, hexyl acrylate, octyl acrylate and 2-ethylhexyl acrylate; And / or, the aromatic vinyl monomer has a structure as shown in Formula I, Among them, R a and R b The same or different, independently selected from H, C 1-10 Alkyl or halogen; R a The number of substitutions is one, two, three, four or five, and the number of substitutions at each position is R a Same or different; Preferably, the aromatic vinyl monomer is selected from one or more of styrene, α-methylstyrene, vinyltoluene and 3,4-dichlorostyrene; And / or, the vinyl cyanide monomer is selected from one or more of acrylonitrile and alkyl acrylonitrile, wherein the alkyl group in the alkyl acrylonitrile is C 1-4 alkyl.
3. The ASA resin according to claim 1 or 2, It is characterized in that The mantle layer is obtained by emulsion polymerization of aromatic vinyl monomer, vinyl cyan monomer and crosslinking monomer in the core layer emulsion in the presence of an emulsifier and an initiator; And / or, the shell layer is obtained by polymerizing aromatic vinyl monomers and vinyl cyan monomers in a mantle layer emulsion in the presence of a molecular weight regulator; And / or, the core is obtained by emulsion polymerization of alkyl acrylate monomers and crosslinking monomers in a seed emulsion.
4. The ASA resin according to claim 3, It is characterized in that The crosslinking monomer is selected from one or more of diol di(meth)acrylate, divinylbenzene, diallyl maleate, diallyl fumarate, diallyl phthalate, allyl (meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane triacrylate and triallyl (iso)cyanurate; and / or, the ratio of the sum of the weight parts of the aromatic vinyl monomer and the vinyl cyan monomer used to prepare the mantle layer to the sum of the weight parts of the aromatic vinyl monomer and the vinyl cyan monomer used to prepare the shell layer is (10-80):(20-90); and / or, the aromatic vinyl monomer of the mantle layer is the same as or different from the aromatic vinyl monomer of the shell layer; And / or, the vinyl cyan monomer of the mantle layer is the same as or different from the vinyl cyan monomer of the shell layer.
5. The ASA resin according to any one of claims 1 to 4, It is characterized in that The melt flow rate of the ASA resin is not less than 5 g / 10 min, preferably not less than 8 g / 10 min; The impact strength of the ASA resin is not less than 12 kJ / m 2 , preferably not less than 15 kJ / m 2 .
6. The ASA resin according to any one of claims 1 to 5, It is characterized in that The particle size of the core is 100 to 500 nm; The thickness of the mantle layer is 2 to 80 nm; The thickness of the shell layer is 2-60 nm.
7. The method for preparing the ASA resin according to any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: (a) Preparation of ASA emulsion (a-1) an aromatic vinyl monomer, a vinyl cyan monomer and a crosslinking monomer are subjected to an emulsion polymerization reaction in a core layer emulsion to obtain a mantle layer emulsion; The core layer emulsion is used to form the core, i.e., a cross-linked polymer of alkyl acrylate monomers; (a-2) an aromatic vinyl monomer and a vinyl cyanide monomer are polymerized in the mantle layer emulsion in the presence of a molecular weight regulator to obtain a shell layer emulsion, i.e., an ASA emulsion; (b) Aromatic vinyl monomer and vinyl cyan monomer are subjected to suspension polymerization reaction in water and the ASA emulsion in the presence of a stabilizer and a molecular weight regulator to obtain the ASA resin.
8. The preparation method according to claim 7, It is characterized in that Based on 100 parts by weight of the aromatic vinyl monomer and the vinyl cyanide monomer in step (a), the aromatic vinyl monomer and the vinyl cyanide monomer in step (a-1) total 10 to 80 parts by weight, and the aromatic vinyl monomer and the vinyl cyanide monomer in step (a-2) total 20 to 90 parts by weight; And / or, the step (a) further comprises (a-3) preparing the core layer emulsion: carrying out emulsion polymerization of alkyl acrylate monomer and cross-linking monomer in the seed emulsion to obtain the core layer emulsion; And / or, the step (a) further comprises (a-4) preparing the seed emulsion: performing emulsion polymerization of alkyl acrylate monomer and cross-linking monomer in water to obtain the seed emulsion; and / or, based on 100 parts by weight of the alkyl acrylate monomers in steps (a-3) and (a-4), the alkyl acrylate monomer in step (a-3) is 5 to 50 parts by weight, and the alkyl acrylate monomer in step (a-4) is 50 to 95 parts by weight; And / or, based on 100 parts by weight of all the monomers in step (a), the alkyl acrylate monomer is 40 to 90 parts by weight, and the aromatic vinyl monomer and the vinyl cyan monomer are 10 to 60 parts by weight in total; And / or, the reaction system of steps (a-1), (a-2), (a-3) and / or (a-4) further contains an emulsifier and / or an initiator.
9. The preparation method according to claim 7 or 8, It is characterized in that The reaction system of step (b) further contains an initiator selected from oil-soluble organic peroxides or azo compounds; And / or, based on 100 parts by weight of the prepared ASA resin, the polymerization product of step (a) is 20 to 50 parts by weight, and the polymerization product of step (b) is 50 to 80 parts by weight.
10. Use of the ASA resin according to any one of claims 1 to 6 in the fields of automobiles, building materials or electronic appliances.
Citation Information
Cited By
Method for preparing low-temperature-resistant ASA (acrylonitrile-styrene-acrylate) resin by continuous bulk process
CN122188060A