Olefin polymerization reaction catalyst component and process combination method

By using online mixing of external electron donors such as thiophene and tetrahydrothiophene and catalyst components in Ziegler-Natta polyethylene catalysts, the problem of unoptimized catalyst performance is solved, the processing performance and product performance of rotomold plastics are improved, and the performance of the product is realized. Low temperature rotary molding and efficient production.

CN119060230AActive Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310644615.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03
Estimated Expiration
2043-06-01

AI Technical Summary

Technical Problem

When the Ziegler-Natta polyethylene catalyst introduces an external electron donor during the polymerization process, the performance parameters of the catalyst cannot be fully optimized, resulting in some performance degradation and is rarely reported in industrial applications.

Method used

Use external electron donors (such as one or more of thiophene, tetrahydrothiophene and trimethylene sulfur) to mix them online with the catalyst components and work together with another part of the catalyst components to improve the crystallization structure of the ethylene copolymer and improve the Processing properties of rotomolded plastics.

Benefits of technology

Through this method, the processing forming temperature is reduced by 10-20℃, the forming cycle is shortened by 10-20%, the finish, toughness and environmental stress resistance of the product are improved, the risk of low-temperature brittle cracking is reduced, and the production efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060230A_ABST
    Figure CN119060230A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalyst preparation, and discloses an olefin polymerization reaction catalyst component and a process combination method. The catalyst comprises (A) a component 1, wherein the component 1 comprises a solid titanium catalyst component containing Mg, Ti, Si, Cl elements and tetrahydrofuran; (B) a component 2, wherein the component 2 is selected from one or more of thiophene, thiophane and trimethylene sulfide; the component 3 is an organic aluminum compound with the general formula of AlR'dX '3-d, R'is hydrogen or Cl-C20 alkyl, X' 'is halogen atom and 0 lt, and d is smaller than or equal to 3. The catalyst can improve the crystal structure of the ethylene copolymer and is finally combined with an additive (assistant), and the processability and product performance of rotational plastics are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to an olefin polymerization catalyst component and a process combination method. Background Art

[0002] The biggest disadvantage of rotational molding is that it requires long-term high-temperature heating, high energy consumption and low efficiency. The main reason is the particularity of its processing technology. The rotational molding raw materials must be powdered, and the processing process is in a pressure-free state, so bubbles are inevitable. The existing methods for eliminating bubbles in products are mainly improved by increasing the temperature and extending the heating time. Prolonging the time can discharge bubbles in the melt to a certain extent, but it is easy to cause the thermal oxidation of the material to intensify, which may cause discoloration or even a decrease in mechanical properties. Increasing the temperature can theoretically reduce the viscosity of the melt and facilitate the overflow of bubbles, but it still faces the problems of degradation and high energy consumption. It can be seen that extending the time and increasing the temperature cannot completely solve the bubble problem, but can only control the bubbles to a certain extent, because there is no pressure on the melt during processing, and it is difficult to discharge bubbles from the melt by heating. Therefore, to achieve efficient forming of roto-molded products, breakthroughs are needed in the base resin. The performance breakthrough of the base resin must be achieved by the organic combination of the catalyst system and the polymerization process.

[0003] Over the past 60 years, due to the continuous development of technology, the activity, hydrogen sensitivity, copolymerization performance of Ziegler-Natta type polyolefin catalysts and the bulk density, melt index, molecular weight distribution, fine powder content, copolymerization unit distribution and other parameters of their polymer powders have been significantly optimized. However, in order to better meet the needs of industrial production and produce products with better performance, the above parameters of such catalysts and their polymer powders need to be further improved.

[0004] In the prior art, an internal electron donor is usually introduced into the catalyst to improve its hydrogen modulation sensitivity. CN1958620A introduces a siloxane electron donor; CN1743347A introduces an ortho-alkoxy-substituted benzoate / carboxylate (or diether) composite electron donor; CN102295717A and CN103772536A introduce benzoate compounds as electron donors, thereby improving the hydrogen modulation sensitivity of the catalyst. It is also possible to introduce an internal / external electron donor into the catalyst to improve the copolymerization performance of the catalyst, such as CN1726230A, CN1798774A and CN101050248A respectively introduce electron donors such as alcohols, ketones, amines, amides, nitriles, alkoxysilanes, aliphatic ethers and aliphatic carboxylates.

[0005] According to the published patents and documents, it is a well-known technology in the field to introduce an external electron donor to adjust the polymer properties during the polymerization process of Ziegler-Natta type polypropylene catalyst; however, there are few reports on the introduction of an external electron donor during the polymerization process of Ziegler-Natta type polyethylene catalyst. The inventors have conducted in-depth research on this, and the results show that if an external electron donor is introduced during the polymerization process of Ziegler-Natta type polyethylene catalyst, the parameters such as the activity / hydrogen adjustment sensitivity / copolymerization performance of the catalyst and the bulk density / copolymerization unit content of the polymer powder cannot be fully optimized, and some performances are reduced. This may be the reason why the external electron donor technology of Ziegler-Natta type polyethylene catalyst has not yet been industrialized and is rarely reported in documents and patents.

[0006] Therefore, if we can find a special type of external electron donor and cooperate with specific process operations to improve the performance of a certain type of product, it will be a technological development with very high practical value. Summary of the invention

[0007] The purpose of the present invention is to overcome the defect problem in the prior art that the performance parameters of the catalyst cannot be fully optimized due to the introduction of an external electron donor in the polymerization process of a Ziegler-Natta type polyethylene catalyst, and to provide an olefin polymerization catalyst component and a process combination method. The olefin polymer adopts an external electron donor (component 2) and is mixed online with a catalyst component (component 1) and a part of a catalyst component 3 through an external addition technology, and then acts together with another component 3, so that the prepared olefin polymer can improve the crystal structure of the ethylene copolymer, and finally combined with an additive (auxiliary agent) to improve the processing performance and product performance of the rolled plastic.

[0008] In order to achieve the above object, the first aspect of the present invention provides an olefin polymer, wherein the olefin polymer comprises:

[0009] (A) Component 1: Component 1 comprises a solid titanium catalyst component of Mg, Ti, Si, Cl elements and tetrahydrofuran;

[0010] (B) component 2: the component 2 is selected from one or more of thiophene, tetrahydrothiophene and trimethylene sulfide;

[0011] (C) Component 3: General formula: AlR" d X"' 3-d An organoaluminum compound wherein R" is hydrogen or C l -C 20 Hydrocarbon group, X"' is a halogen atom, 0 <d≤3。

[0012] The second aspect of the present invention provides a method for preparing the aforementioned olefin polymer, wherein the preparation method comprises:

[0013] (1) mixing a portion of component 3 with component 2 and then mixing with component 1 to obtain component 4;

[0014] (2) Another part of the component 3 is contacted with the component 4 to react and obtain an olefin polymer.

[0015] The third aspect of the present invention provides a use of the aforementioned olefin polymer in olefin homopolymerization and / or olefin copolymerization.

[0016] The fourth aspect of the present invention provides an ethylene copolymer, wherein ethylene and α-olefin are copolymerized in the presence of an olefin polymerization catalyst to obtain the ethylene copolymer, wherein the olefin polymerization catalyst is the olefin polymer described above.

[0017] The fifth aspect of the present invention provides a low-temperature rotationally molded polyethylene composition, wherein the low-temperature rotationally molded polyethylene composition comprises a polyethylene resin and an additive, wherein the polyethylene resin is the ethylene copolymer described above.

[0018] A sixth aspect of the present invention provides a polyethylene rotomolded product, wherein the aforementioned low-temperature rotationally molded polyethylene composition is granulated, ground, and rotomolded to prepare a polyethylene rotomolded product.

[0019] Through the above technical solution, the present invention has the following beneficial effects:

[0020] Firstly, since the catalyst uses an external electron donor (component 2), due to the weak electron donating property of the heteroatoms in the external electron donor, the electron cloud density of the titanium active center can be appropriately adjusted, which has the advantage of improving the copolymerization performance of the catalyst;

[0021] Secondly, through the external addition technology, the external electron donor (component 2) and a part of the catalyst (component 3) are combined with the catalyst component (component 1), mixed online, and then enter the reactor together with another part of the catalyst (component 3), which has the advantages of mild reaction conditions, timely and efficient, and few side reactions.

[0022] Thirdly, the produced roto-molded plastic base resin combined with the preferred additives can reduce the processing temperature by 10-20°C, shorten the molding cycle by 10-20%, effectively improve the problems of degradation and high energy consumption, and reduce the risk of low-temperature brittle cracking of roto-molded products;

[0023] Fourthly, the raw material can be easily used to prepare one or more of leisure sports boats, military boxes and water tanks through rotational molding process, and the obtained products have good inner and outer surface finish, no odor, good whiteness, good toughness, high stiffness, easy demoulding, and good resistance to environmental stress and UV aging;

[0024] Fifthly, the production efficiency is improved and the economic efficiency is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The product 1 prepared in Example 1 is a 6.3-meter-long sports boat processed with the rotational molding raw material;

[0026] Figure 2 It is product 2 prepared in Example 2: a water tank processed with the rotationally molded raw material. DETAILED DESCRIPTION

[0027] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0028] The first aspect of the present invention provides an olefin polymer, wherein the olefin polymer comprises:

[0029] (A) Component 1: Component 1 comprises a solid titanium catalyst component of Mg, Ti, Si, Cl elements and tetrahydrofuran;

[0030] (B) component 2: the component 2 is selected from one or more of thiophene, tetrahydrothiophene and trimethylene sulfide;

[0031] (C) Component 3: General formula: AlR" d X"' 3-d An organoaluminum compound wherein R" is hydrogen or C l -C 20 Hydrocarbon group, X"' is a halogen atom, 0 <d≤3。

[0032] The inventors of the present invention have discovered that by combining a specific component 2 (sulfur-containing heterocyclic compound, external electron donor) with a catalyst component (component 1) through an external addition technology, mixing a portion of the catalyst component 3 online, and then acting together with another component 3, the responsiveness of the catalyst comonomer such as ethylene copolymer can be synergistically improved, and the crystal structure of the base resin (ethylene copolymer) can be improved through process adjustment in polymerization production, and finally combined with additives to improve the processing performance and product performance of the rolled plastic.

[0033] Furthermore, the inventors of the present invention have found that the use of one or more sulfur-containing heterocyclic compounds selected from thiophene, tetrahydrothiophene and trimethylene sulfide as external electron donors has the advantages of small molecular volume and small steric hindrance after coordination; and the inventors of the present invention have found that the use of "organic siloxane compounds containing two thienyl substituents" or "compounds containing two thienyl substituents" because of their large molecular volume, multiple heteroatoms, and strong coordination ability, such electron donors suitable for improving the directional ability of propylene polymerization, cannot bring beneficial effects in ethylene polymerization (ethylene polymerization does not require stereoregularity because polyethylene does not have chiral carbon), and seriously reduce the copolymerization performance of the catalyst.

[0034] The inventors use a special type of external electron donor, sulfur-containing heterocyclic compounds. This type of external electron donor has special properties. When used together with BSG catalyst, it can significantly improve the crystallization characteristics of the catalyst in the production of rotomolding base resin in a gas phase fluidized bed device.

[0035] According to the present invention, further, preferably, the component 1 comprises one or more of magnesium chloride, titanium chloride, silica gel and tetrahydrofuran. In the present invention, tetrahydrofuran is used as an internal electron donor to protect the catalyst of magnesium chloride, titanium chloride and silica gel, and can be prepared according to the preparation method of the catalyst described in CN106543316A.

[0036] According to the present invention, the weight ratio of the S element in the component 2 to the titanium element in the component 1 is 1:(5-100), preferably 1:(10-30).

[0037] According to the present invention, the weight ratio of the aluminum element in the component 3 to the titanium element in the component 1 is (1-10):1, preferably (3-6):1.

[0038] In addition, it should be noted that in the present invention, an industrial BSG catalyst is used, and the contents of the three main elements Ti, Mg and Si in the component 1 are relatively certain, and are implemented according to the contents described in CN106543316A.

[0039] According to the present invention, the organic aluminum compound is selected from alkyl aluminum compounds such as Al(CH3)3, Al(CH2CH3)3, Al(i-Bu)3, AlH(CH2CH3)2, AlH(i-Bu)2, AlCl(CH2CH3)2, Al2Cl3(CH2CH3)3, AlCl(CH2CH3)2, AlCl2(CH2CH3), Al(CH2CH2CH2CH2CH2CH3)3, and is preferably Al(CH2CH3)3 and / or Al(i-Bu)3.

[0040] In the present invention, it should be noted that i-Bu is CH3CH(CH3)CH2 (isobutyl).

[0041] The second aspect of the present invention provides a method for preparing the aforementioned olefin polymer, wherein the preparation method comprises:

[0042] (1) mixing a portion of component 3 with component 2 and then mixing with component 1 to obtain component 4;

[0043] (2) Another part of the component 3 is contacted with the component 4 to react and obtain an olefin polymerization catalyst.

[0044] In the present invention, component 2 is not introduced during the catalyst preparation process, but after the catalyst component 1 is prepared and before entering the reactor, it is preliminarily mixed with the catalyst component 1 outside the reactor in a special pipeline system at a suitable temperature and controlling a suitable reaction time. After sufficient reaction, component 4 is generated and enters the main reactor to catalyze olefin polymerization.

[0045] In the present invention, the catalyst component 4 is obtained by external administration. The molar ratio of the above-mentioned component 2 (sulfur-containing heterocyclic compound) to magnesium chloride in the component 4 can be 0.01-0.1 mol, preferably 0.02-0.05 mol.

[0046] According to the present invention, component 1 is formulated into a white oil slurry with a concentration of 25-30wt%; component 2 is formulated into a white oil slurry with a concentration of 0.1-3wt%; preferably, component 2 is formulated into a white oil slurry with a concentration of 0.2-0.8wt%.

[0047] According to the present invention, the component 3 comprises tri-n-hexylaluminum and diethylaluminum monochloride, which are respectively prepared into a white oil slurry with a concentration of 13-15wt% and a white oil slurry with a concentration of 49-51wt%.

[0048] According to the present invention, the other component 3 is composed of triethylaluminum and does not need to be configured. It is directly injected into the reactor using a reciprocating pump. The feed amount of the other component 3 is 0.01wt% of the total ethylene feed amount.

[0049] According to the present invention, the feed flow rate of component 1 is 3-15 kg slurry / hour; the feed flow rate of component 2 is 0.1-2 kg slurry / hour; the feed flow rate of one part of component 3 is 1-20 kg slurry / hour; the feed flow rate of another part of component 3 is 4-6 kg slurry / hour.

[0050] The third aspect of the present invention provides a use of the aforementioned olefin polymer in olefin homopolymerization and / or olefin copolymerization.

[0051] The fourth aspect of the present invention provides an ethylene copolymer, wherein ethylene and α-olefin are copolymerized in the presence of an olefin polymerization catalyst to obtain the ethylene copolymer, wherein the olefin polymerization catalyst is the olefin polymer described above.

[0052] According to the present invention, the α-olefin includes one or more of propylene, butene, pentene, hexene and 4-methyl-1-pentene.

[0053] According to the present invention, hydrogen is used as a molecular weight regulator in order to adjust the molecular weight of the final polymer.

[0054] The fifth aspect of the present invention provides a low-temperature rotationally molded polyethylene composition, wherein the composition comprises a polyethylene resin and an additive, wherein the polyethylene resin is the ethylene copolymer described above.

[0055] According to the present invention, based on the total weight of the low-temperature rotationally molded polyethylene composition, the content of the polyethylene resin is 97-99.9% by weight, and the content of the auxiliary agent is 0.1-3% by weight.

[0056] According to the present invention, the auxiliary agent comprises one or more of a composite antioxidant, a lubricant, an antistatic agent, a composite light stabilizer and a high-temperature defoaming agent.

[0057] According to the present invention, based on the total weight of the auxiliary agent, the content of the composite antioxidant is 20-35% by weight, the content of the lubricant is 4-15% by weight, the content of the antistatic agent is 3-12% by weight, the content of the composite light stabilizer is 20-35% by weight, and the content of the high-temperature defoaming agent is 6-15% by weight; preferably, based on the total weight of the auxiliary agent, the content of the composite antioxidant is 25-30% by weight, the content of the lubricant is 7-12% by weight, the content of the antistatic agent is 5-12% by weight, the content of the composite light stabilizer is 25-32% by weight, and the content of the high-temperature defoaming agent is 8-15% by weight.

[0058] According to the present invention, the composite antioxidant comprises a primary antioxidant and a secondary antioxidant, wherein the primary antioxidant is selected from one or more of 1076, 1010, 1330 and BHT; the secondary antioxidant is preferably selected from one or more of 168, 626, 618 and DLTP.

[0059] According to the present invention, the weight ratio of the primary antioxidant to the secondary antioxidant is 1:(0.3-3).

[0060] According to the present invention, the lubricant is selected from one or more of zinc stearate, pentaerythritol stearate, magnesium stearate, calcium stearate and barium stearate.

[0061] According to the present invention, the antistatic agent is selected from one or more of ethoxylated aliphatic alkylamines, ethoxylated alkyl acid amines and fatty acid polyol esters, wherein the aliphatic alkyl, alkyl acid and fatty acid preferably have a carbon number of C 10 -C 25 ; Further preferred is one or more of N,N-dihydroxyethyl octadecylamine, N,N-dimethyllaurylamine and glycerol monostearate.

[0062] According to the present invention, the composite light stabilizer is selected from two or more of UV531, UV329, UV1577, UV770, UV622, UV2020, UV944 and UV3346.

[0063] According to the present invention, the composite light stabilizer has an ash content of ≤0.1 parts by weight and a volatile content of ≤0.5 parts by weight.

[0064] According to the present invention, the high-temperature defoaming agent is selected from one or more of amides, polysiloxanes and wax oils, preferably one or more of ethylene bisstearamide, erucamide, oleamide, PE wax and white oil.

[0065] According to the present invention, the weight ratio of the external lubricant to the antistatic agent and the high-temperature defoaming agent is 1:(0.8-1.5):(1.0-1.5).

[0066] According to the present invention, the density of the polyethylene resin is 0.925-0.945 g / cm 3 , melt flow index is 2-8g / 10min, number average molecular weight (Mn) is 21000-31000, molecular weight distribution is 4.5-4.6, weight average molecular weight (Mw) is 85000-113000, melting point is 125-129°C, crystallinity is 50-60%; preferably, number average molecular weight (Mn) is 23500-24500, weight average molecular weight (Mw) is 95000-110000.

[0067] A sixth aspect of the present invention provides a polyethylene rotomolded product, wherein the aforementioned low-temperature rotationally molded polyethylene composition is granulated, ground, and rotomolded to prepare a polyethylene rotomolded product.

[0068] According to the present invention, the granulation is carried out using a twin-screw granulator, and the granulated material is ground into 35 mesh fine powder in a grinding mill to obtain a polyethylene composition powder for low-temperature rotational molding. A polyethylene rotational molded product made of the polyethylene composition powder for low-temperature rotational molding.

[0069] According to the present invention, the polyethylene rotomolded product comprises one or more of a sports boat, a military tank and a water tank; preferably a sports boat.

[0070] The present invention will be described in detail below through examples.

[0071] In the following examples and comparative examples:

[0072] (1) Relative weight percentage of titanium in the catalyst system: by spectrophotometry;

[0073] (2) Composition of catalyst components: Liquid nuclear magnetic resonance 1 H-NMR;

[0074] (3) Determination of polymer melt index (MI): according to GB / T 3682, load 2.16 kg;

[0075] (4) Powder copolymer unit content: liquid nuclear magnetic resonance 13 C-NMR;

[0076] (5) The parameters in the reactor are measured by online detectors and transmitted online to the host computer in the central control room;

[0077] (6) Determination of polymer density (D method): according to GB / T 1033.2;

[0078] (7) Low temperature impact performance (-40°C): GB / T 39933-2021, "Rotational molding low temperature impact test";

[0079] (8) Powder flowability: GB / T 40934-2021, Test method for flowability of powders for rotational molding;

[0080] (9) Odor test: The products obtained during and after production are subjected to sensory testing by 10 persons. If more than 2 persons think there is an odor, it is recorded as having an odor; otherwise, it is recorded as having no odor.

[0081] (10) Surface finish: Observe the surface flatness and smoothness with the naked eye, including whether there are a few small bubbles, and compare with the same products made of control materials to comprehensively evaluate the finish of the inner and outer surfaces of the product by combining the feeling of touch. If it is obviously smooth, does not contain small bubbles, and feels relatively flat, it is recorded as excellent; if it is relatively smooth, feels relatively flat, and has occasional small bubbles on the edge, it is recorded as good; if it does not look smooth enough, feels not very flat, and has a few small bubbles on the edge, it is recorded as fair;

[0082] (11) Heating time (bubble removal time): The time starts from the time when the mold frame (the mold filled with rotomolding powder is installed on the mold frame) is moved into the furnace cavity, until the raw materials are completely melted and the bubbles are eliminated, and the mold frame is moved out of the heating furnace. The unit is minutes;

[0083] (12) Cooling time: The time from when the mold frame is removed from the heating furnace to when the product is removed from the mold, in minutes. Note: This product is fan cooled.

[0084] (13) Demolding performance: It is determined by the difficulty of the operator pulling the product out of the mold, and is directly given three levels: easy, medium, and difficult.

[0085] (14) Rigidity: When the boat is traveling on a river at a certain speed, the stability of the boat and the degree of deformation of the boat are examined. Small deformation and fast speed are recorded as excellent. Relatively obvious deformation has some effect on the speed, which is recorded as good. The deformation is relatively obvious and has a significant effect on the speed, which is recorded as medium.

[0086] (15) Heat resistance: If the engine parts do not heat up or deform for a long time, it is recorded as excellent; if the engine parts are slightly deformed, it is recorded as good; if the engine parts are obviously deformed, it is recorded as medium.

[0087] Example 1

[0088] (I) Preparation of olefin polymers

[0089] (1) Preparation of catalyst component 1

[0090] According to the catalyst described in CN106543316A (application number 201510589972.3), the catalyst composition is shown in Table 1. The composition of the catalyst slurry entering the reactor.

[0091] (2) Polymerization reaction

[0092] The main reactor is a gas-phase fluidized bed with a diameter of 5.5 meters and a straight section height of 17 meters.

[0093] During the trial period, the production load was stable at 52-60 tons of polyethylene / hour.

[0094] During the test, the ethylene feed flow rate was maintained at 53 tons / hour, the temperature in the reactor was 87°C, the total pressure was 2.2MPa, and the ethylene partial pressure was 0.72MPa. The above data were required to be kept stable. The product density was required to be between 0.925-0.945g / cm 3 The melt index at 190°C under a load of 2.16kg is in the range of 2-8g / 10min. The feed amount of hydrogen and butene is automatically adjusted according to the online test feedback of density and melt index to adjust the hydrogen-ethylene ratio (hydrogen-ethylene ratio, used to adjust the product melt index) and butene-ethylene ratio (butene-ethylene ratio, used to adjust the product density) in the reactor.

[0095] Catalyst component 1 was fed in the form of a 28% concentration white oil slurry, and the feed rate was maintained at 8 kg slurry / hour.

[0096] Thiophene is selected as catalyst component 2, and is injected into the feed pipeline of component 1 in the form of 3% white oil slurry of the same grade at a feed rate of 0.5 kg slurry / hour, and is mixed evenly in static mixer 1.

[0097] A portion of the catalyst component 3 is composed of tri-n-hexylaluminum and diethylaluminum chloride, which are configured as white oil slurries with a concentration of 14% and 50%, respectively. They are injected into the feed relationship of component 1 at a feed rate of 10kg slurry / hour and 3kg slurry / hour, respectively, and are mixed evenly by static mixers 2 and 3. Then the slurry is injected into the reactor.

[0098] Another part of the catalyst component 3 consists of triethylaluminum, which does not require any preparation and is directly injected into the reactor at a feed rate of 5 kg / hour.

[0099] The test lasted 72 hours. After the product indicators stabilized, the parameter data in the reactor were collected. See Table 2 for the activity and light adjustment sensitivity of the catalyst.

[0100] (II) Preparation of resin products:

[0101] Step 1: Copolymerize ethylene and α-olefins by Unipol gas phase process to produce a product having a melt index of 3.2 g / 10 min at 190°C under a load of 2.16 kg and a density of 0.938 g / cm 3 Linear medium density polyethylene (powder), that is, polyethylene resin.

[0102] Step 2: 99.1wt% of the linear medium density polyethylene obtained in step 1 and 0.9wt% of the auxiliary agent composition (22wt% of the composite antioxidants, specifically 1010 and 168, 9wt% of the lubricant zinc stearate, 8wt% of the antistatic agent N,N-dihydroxyethyl octadecylamine, 25wt% of the composite light stabilizers UV2020 and UV944, and 11wt% of the defoaming agent erucic acid amide) are blended, and the linear medium density polyethylene composition particles are obtained by a twin-screw extrusion granulator (produced by CWP, Germany, model ZSK350), the extruder temperature is 240°C, and the power is 6600kW.

[0103] (III) Preparation of rolled plastic products:

[0104] The prepared polyethylene composition particles are ground into powder of about 35 meshes, a certain proportion of color powder is added, and the powdered material is injected into a mold. The mold is directly heated by an open flame and rolled and rotated vertically and horizontally, so that the material is evenly distributed in the mold cavity and melted by its own gravity and centrifugal force. After cooling, the mold is demolded to obtain a hollow product such as Figure 1 shown.

[0105] Example 2

[0106] An olefin polymer was prepared in the same manner as in Example 1, except that: the composition of the catalyst component 1 is shown in Table 1;

[0107] In addition, the feed flow rate of catalyst component 2 was adjusted to 0.15 kg slurry / hour and injected into the feed pipeline of component 1, and mixed evenly through static mixer 1.

[0108] A portion of the catalyst component 3 is composed of tri-n-hexylaluminum and diethylaluminum chloride, which are configured as white oil slurries with a concentration of 14% and 50%, respectively. They are injected into the feed relationship of component 1 at a feed rate of 11kg slurry / hour and 3kg slurry / hour, respectively, and are mixed evenly by static mixers 2 and 3. Then the slurry is injected into the reactor.

[0109] Another part of the catalyst component 3 consisted of triethylaluminum, which did not require any preparation and was directly injected into the reactor at a feed rate of 5.5 kg / hour.

[0110] The test lasted 72 hours. After the product indicators stabilized, the parameter data in the reactor were collected, see Table 2.

[0111] The resin product was prepared according to the same components and method as in Example 1, and its characterization is shown in Table 3.

[0112] The roto-molded plastic product was prepared according to the same components and method as in Example 1. The characteristics are shown in Table 4. In addition, the water tank processed with the roto-molded raw material is as follows: Figure 2 shown.

[0113] Example 3

[0114] The system polymer was prepared in the same manner as in Example 1, except that: the composition of catalyst component 1 is shown in Table 1;

[0115] In addition, the catalyst component 2 was replaced with tetrahydrothiophene, and the feed flow rate was the same as that in Example 1.

[0116] The composition and amount of one part of catalyst component 3 and another part of catalyst component 3 are the same as those in Example 1.

[0117] The test lasted 72 hours. After the product indicators stabilized, the parameter data in the reactor were collected, see Table 2.

[0118] The resin product was prepared according to the same components and method as in Example 1, and its characterization is shown in Table 3.

[0119] The rolled plastic product was prepared according to the same components and method as in Example 1, and its characteristics are shown in Table 4.

[0120] Example 4

[0121] An olefin polymer was prepared in the same manner as in Example 1, except that: the composition of the catalyst component 1 is shown in Table 1;

[0122] In addition, the catalyst component 2 was replaced with trimethylene sulfide, and the feed flow rate was the same as that in Example 1.

[0123] The composition and amount of one part of catalyst component 3 and another part of catalyst component 3 are the same as those in Example 1.

[0124] The test lasted 72 hours. After the product indicators stabilized, the parameter data in the reactor were collected, see Table 2.

[0125] The resin product was prepared according to the same components and method as in Example 1, and its characterization is shown in Table 3.

[0126] The rolled plastic product was prepared according to the same components and method as in Example 1, and its characteristics are shown in Table 4.

[0127] Example 5

[0128] An olefin polymer was prepared in the same manner as in Example 1, except that: the composition of the catalyst component 1 is shown in Table 1;

[0129] In addition, the catalyst component 2 was replaced with tetrahydrothiophene, and the feed flow rate was the same as that in Example 2.

[0130] The composition and amount of one part of catalyst component 3 and another part of catalyst component 3 are the same as those in Example 2.

[0131] The test lasted 72 hours. After the product indicators stabilized, the parameter data in the reactor were collected, see Table 2.

[0132] The resin product was prepared according to the same components and method as in Example 1, and its characterization is shown in Table 3.

[0133] The rolled plastic product was prepared according to the same components and method as in Example 1, and its characteristics are shown in Table 4.

[0134] Comparative Example 1

[0135] An olefin polymer was prepared in the same manner as in Example 1, except that: the composition of the catalyst component 1 is shown in Table 1;

[0136] The test conditions were the same as in Example 1, but without adding catalyst component 2.

[0137] The composition and amount of one part of catalyst component 3 and another part of catalyst component 3 are the same as those in Example 1.

[0138] The test lasted 72 hours. After the product indicators stabilized, the parameter data in the reactor were collected, see Table 2.

[0139] The resin product was prepared according to the same components and method as in Example 1, and its characterization is shown in Table 3.

[0140] The rolled plastic product was prepared according to the same components and method as in Example 1, and its characteristics are shown in Table 4.

[0141] Comparative Example 2

[0142] An olefin polymer was prepared in the same manner as in Example 1, except that: the composition of the catalyst component 1 is shown in Table 1;

[0143] The test conditions were the same as those in Example 1, except that the main catalyst was replaced with other domestic industrial catalysts for comparison.

[0144] The composition and amount of one part of catalyst component 3 and another part of catalyst component 3 are the same as those in Example 2.

[0145] The test lasted 72 hours. After the product indicators stabilized, the parameter data in the reactor were collected, see Table 2.

[0146] The resin product was prepared according to the same components and method as in Example 1, and its characterization is shown in Table 3.

[0147] The rolled plastic product was prepared according to the same components and method as in Example 1, and its characteristics are shown in Table 4.

[0148] Table 1

[0149]

[0150]

[0151] Table 2

[0152]

[0153] Note: The above data are obtained by online testing of the reactor after the reaction is stable and the product melt index and density are stable within the required range.

[0154] From Table 2, we can see that:

[0155] 1. After introducing sulfur-containing heterocyclic compounds as external electron donors into the catalyst polymerization system, they can improve the catalyst's butene responsiveness in the fluidized bed reactor, obtain products of the same density, and have a lower butene concentration in the reactor, which will bring about the benefits of reduced butene unit consumption and improved powder fluidity.

[0156] 2. From the results of stable catalyst feed flow and stable reactor load, it can be clearly seen that the introduction of such external electron donors has no effect on the catalyst activity, and the catalyst activity remains stable, which is beneficial for the smooth control of the reactor.

[0157] 3. Increasing the amount of this type of external electron donor can improve the responsiveness of the copolymer monomer to a certain extent.

[0158] Table 3

[0159]

[0160] As shown in Table 3, the resin product obtained by the composite catalyst system has a slightly higher number average molecular weight, but a slightly wider molecular weight distribution, which lays the foundation for taking into account both mechanical properties and processing properties. From the fluidity test of the powder after grinding, it can be seen that the uniformity and distribution of the powder particle size are relatively good. According to domestic and foreign data, the general fluidity is best in the range of 22-28. The powder in this size range has good fluidity, indicating that the resin has good grinding formability, which lays the foundation for powder spreading and bubble removal in the subsequent rotational molding process.

[0161] Table 4

[0162]

[0163] It can be seen from Table 4 that by using the new composite catalyst system, the performance of the roto-molded products is improved from molding to product performance, the heating time and cooling time of roto-molding are shortened, and the -40°C low-temperature impact performance of the roto-molded products is improved.

[0164] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An olefin polymer, characterized in that The olefin polymer comprises: (A) Component 1: Component 1 comprises a solid titanium catalyst component of Mg, Ti, Si, Cl elements and tetrahydrofuran; (B) component 2: the component 2 is selected from one or more of thiophene, tetrahydrothiophene and trimethylene sulfide; (C) Component 3: General formula: AlR" d X"' 3-d An organoaluminum compound, R" is hydrogen or C l -C 20 Hydrocarbyl, X"' is a halogen atom, 0 <d≤3。 2. The olefin polymer according to claim 1, wherein in, The weight ratio of the S element in the component 2 to the titanium element in the component 1 is 1:(5-100), preferably 1:(10-30); And / or, the weight ratio of the aluminum element in the component 3 to the titanium element in the component 1 is (1-10):1, preferably (3-6):

1.

3. The olefin polymer according to claim 1, wherein The organic aluminum compound is selected from alkyl aluminum compounds such as Al(CH3)3, Al(CH2CH3)3, Al(i-Bu)3, AlH(CH2CH3)2, AlH(i-Bu)2, AlCl(CH2CH3)2, Al2Cl3(CH2CH3)3, AlCl(CH2CH3)2, AlCl2(CH2CH3), Al(CH2CH2CH2CH2CH2CH3)3, etc.

4. A method for preparing an olefin polymer according to any one of claims 1 to 3, characterized in that: The preparation method comprises: (1) mixing a portion of component 3 with component 2 and then mixing with component 1 to obtain component 4; (2) Another part of the component 3 is contacted with the component 4 to react and obtain an olefin polymer.

5. The preparation method according to claim 4, wherein The component 1 is formulated into a white oil slurry with a concentration of 25-30 wt%; the feed flow rate of the component 1 is 3-15 kg slurry / hour; and / or, the component 2 is formulated into a white oil slurry with a concentration of 0.1-3 wt%; the feed flow rate of the component 2 is 0.1-2 kg slurry / hour; And / or, in step (1), the part of component 3 includes tri-n-hexyl aluminum and diethyl aluminum chloride, which are respectively prepared into white oil slurries with concentrations of 13-15wt% and 49-51wt%; the feed flow rate of the part of component 3 is 1-20kg slurry / hour; And / or, in step (2), the other component 3 is triethylaluminum, and the feed flow rate of the other component 3 is 4-6 kg slurry / hour.

6. Use of the olefin polymer according to any one of claims 1 to 3 in olefin homopolymerization and / or olefin copolymerization.

7. An ethylene copolymer, characterized in that In the presence of an olefin polymerization catalyst, ethylene and α-olefin are copolymerized to obtain an ethylene copolymer, wherein the olefin polymerization catalyst is the olefin polymer according to any one of claims 1 to 3.

8. A low temperature rotationally molded polyethylene composition, characterized in that: The low-temperature rotational molding polyethylene composition comprises a polyethylene resin and an additive, wherein the polyethylene resin is the ethylene copolymer according to claim 7.

9. The composition according to claim 8, wherein The density of the polyethylene resin is 0.925-0.945 g / cm 3 , melt flow index is 2-8g / 10min, number average molecular weight is 21000-31000, molecular weight distribution is 4.5-4.6, and weight average molecular weight is 85000-113000.

10. The composition according to claim 8, wherein Based on the total weight of the low-temperature rotationally molded polyethylene composition, the content of the polyethylene resin is 97-99.9% by weight, and the content of the auxiliary agent is 0.1-3%; And / or, the auxiliary agent comprises one or more of a composite antioxidant, a lubricant, an antistatic agent, a composite light stabilizer and a high-temperature defoaming agent; And / or, based on the total weight of the auxiliary agent, the content of the composite antioxidant is 20-35% by weight, the content of the lubricant is 4-15% by weight, the content of the antistatic agent is 3-12% by weight, the content of the composite light stabilizer is 20-35% by weight, and the content of the high-temperature defoaming agent is 6-15% by weight.

11. A polyethylene rotomolded product, characterized in that: The low-temperature rotationally molded polyethylene composition according to any one of claims 8 to 10 is granulated, ground, and rotationally molded to prepare a polyethylene rotationally molded product.

12. The polyethylene rotomoulded article according to claim 11, wherein The polyethylene rotomolded product includes one or more of a sports boat, a military tank and a water tank.

Citation Information

Patent Citations

  • Polyethylene composition for rotational molding, and preparation method thereof

    CN105273294A

  • Catalyst component used for olefin polymerization, catalyst, and preparation method of catalyst component

    CN106543316A

  • Catalyst component for olefin polymerization reaction, catalyst thereof, and preparation method and application of catalyst

    CN112812205A

  • Solid catalyst component for olefin polymerization and catalyst

    JP2006206662A