In-situ growth hydrotalcite zinc negative electrode interface coating as well as preparation method and application thereof
By growing hydrotalcite-based coating on the surface of zinc negative electrode, the problems of zinc dendrites and side reactions are solved, the stability and utilization rate of zinc negative electrodes are improved, and the efficient cycle life of water-based zinc-based batteries is achieved and the feasibility of large-scale production is achieved. .
Patent Information
- Application Number
- CN202411315344.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-20
AI Technical Summary
During the repeated electroplating/stripping process, commercial zinc sheets have low Coulomb efficiency and poor circulation stability due to zinc dendrites and side reactions, which hinder the practical application of water-based zinc-based batteries.
The method of growing hydrotalcite-based coating on the surface of zinc negative electrode is adopted. The hydrotalcite-based coating is grown vertically in situ through the etch-nucleation-growth mechanism to prevent direct contact between the electrode and the electrolyte and avoid zinc dendrites and other side reactions. .
Improve the utilization rate of zinc negative electrode, suppress dendrite reaction, increase the contact area between the electrode and the electrolyte, provide Zn2+ migration channel, enhance the uniform distribution and stability of the electrode surface, and realize ultra-stable electroplating of zinc negative electrode/ The stripping behavior and simplify the preparation process and is suitable for large-scale production.
Smart Images

Figure CN119170901A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy batteries and relates to a method for preparing a zinc negative electrode surface modification material and its application in aqueous zinc-based batteries. Background Art
[0002] With the continuous depletion of fossil fuels and the intensification of environmental pollution, the development of clean energy has received widespread attention, and the development of secondary batteries for energy redistribution has received attention from academia and industry. Aqueous zinc-based batteries have broader application prospects and greater competitive potential due to their advantages such as high theoretical capacity, low redox potential, abundant reserves and high stability in water. However, commercial zinc flakes are accompanied by uncontrollable zinc dendrites and other side reactions during repeated electroplating / stripping, resulting in low Coulombic efficiency (CE) and poor cycle stability, which hinders the practical application of aqueous zinc-based batteries.
[0003] Since zinc negative electrode side reactions often occur at the electrode / electrolyte interface. Therefore, solving zinc negative electrode side reactions by constructing a zinc negative electrode interface modification layer to isolate the direct contact between the electrode and the electrolyte in the interface has become a research hotspot. Chinese patent CN117105207A discloses a method for preparing nitrogen co-doped mesoporous carbon coatings, the process of which is to use zinc salt as an inducer, nitrogen-containing high molecular polymers as carbon sources and nitrogen sources, and nano-silicon dioxide as a sacrificial template, and obtain zinc / nitrogen co-doped mesoporous carbon materials through two calcinations. Carbon material as a coating can effectively prevent direct contact between the zinc negative electrode and the electrolyte, and effectively reduce interface side reactions. However, since the carbon material itself is conductive, Zn 2+ Directly deposited on the surface of the modified layer, the deposited zinc is still exposed to the electrolyte, which again leads to side reactions. Chinese patent CN116169239A discloses a method for preparing a metal oxide coating, wherein the process is to electro-deposit Al2O3 on zinc foil under a three-electrode system with AlCl3 solution as the electrolyte at a certain voltage. The raw material cost is low, the preparation process is simple, and it is convenient for large-scale production. However, this type of metal oxide is not Zn itself. 2+ Conductor, as a coating will hinder Zn to a certain extent 2+Migration, thereby affecting the electrochemical performance of the zinc negative electrode at a high current density. Chinese patent CN117438528A discloses a method for preparing a phytic acid zinc-polyanion gel coating, the process of which is to use a chemical conversion method to generate a phytic acid zinc coating in situ using a zinc sheet; the polyanion gel layer obtained by mixing the phytic acid zinc coating with acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate, N,N'-methylenebisacrylamide, a photoinitiator and water is connected by ultraviolet light to initiate hydrogen bonds, so that the polyanion gel layer is tightly combined with the phytic acid zinc to modify the zinc negative electrode, reduce impedance and improve the cycle stability of the zinc negative electrode. However, this type of organic polymer coating is often costly, has a complex preparation process and poor mechanical properties, making it difficult to achieve large-scale application.
[0004] It can be seen from the above patents that constructing an artificial protective layer on the zinc negative electrode to meet the following requirements: (1) low electron transfer number; (2) high ionic conductivity; and (3) good mechanical strength and high stability in the electrolyte, thereby improving the stability of the electrode / electrolyte interface, is one of the most urgently needed technological breakthroughs for the large-scale application of aqueous zinc-based batteries. Summary of the invention
[0005] In view of the shortcomings of traditional materials, the present invention provides a method for growing a hydrotalcite-based coating on the surface of a zinc negative electrode, which utilizes the "etching-nucleation-growth" mechanism to vertically grow the hydrotalcite-based coating in situ, aiming to prevent direct contact between the electrode and the electrolyte, avoid zinc dendrites and other side reaction problems at the zinc negative electrode, and maintain the stability of the electrode / electrolyte interface.
[0006] To achieve the above objectives, the technical means adopted by the present invention are as follows:
[0007] The present invention provides a method for in-situ growth of a coating on a zinc negative electrode of an aqueous zinc-based battery, comprising the following steps:
[0008] S1. Ultrasonicate the zinc sheet in mineral acid, water and ethanol to remove surface zinc oxide.
[0009] S2. Immerse the zinc sheet with the surface oxide removed in an organic acid solution of a certain pH and etch for a period of time to obtain a zinc sheet with a zincate surface.
[0010] S3. Place the treated zinc sheet in a mixed solution of zinc metal salt and other metal salts in a certain proportion, add a certain amount of precipitant, carry out "nucleation-growth" under hydrothermal conditions, then vacuum dry, and finally calcine in a muffle furnace to obtain a modified zinc negative electrode.
[0011] In S1, the thickness of all zinc sheets is 0.01-1 mm, the inorganic acid can be one or more of nitric acid, boric acid, hydrochloric acid, sulfuric acid, phosphoric acid, the concentration of the acid solution is 0.1-1 mol / L, and the water used is one of deionized water and ultrapure water. The ultrasonic time is 10-50 min.
[0012] In S2, the acidic solution may be any one or a combination of lactic acid, aminosulfonic acid, phytic acid, oxalic acid, citric acid, organic phosphonic acid, acetic acid, malic acid, and tartaric acid, with a pH value between 2 and 5 and an etching time between 2 and 10 minutes.
[0013] In S3, the zinc salt used is any one of zinc sulfate, zinc nitrate, zinc chloride, and zinc carbonate; the other metal salts are any one of stannous sulfate, magnesium sulfate, magnesium nitrate, magnesium chloride, indium chloride, indium nitrate, aluminum sulfate, aluminum nitrate, aluminum chloride, bismuth nitrate, copper sulfate, copper nitrate, and copper chloride, or a combination thereof; and the precipitant is any one of urea and sodium hydroxide.
[0014] In the mixed solution, the concentration of zinc salt is 0-0.1 mol / L, the concentration of other metal salts is 0.001-0.02 mol / L, and the concentration of precipitant is 0.1-0.5 mol / L.
[0015] The modified zinc negative electrode coating has a thickness of 0.1-50 μm.
[0016] The modified zinc negative electrode prepared by the present invention is used in an aqueous zinc-based battery, wherein the aqueous zinc-based battery is a symmetrical button cell or a button full cell.
[0017] Furthermore, when the modified zinc negative electrode is used to prepare an aqueous zinc-based symmetrical button battery, the steps are as follows: the modified zinc sheet is used as the positive electrode and the negative electrode, and is assembled with a separator and an electrolyte into an aqueous zinc ion symmetrical button battery, and allowed to stand for 2-12 hours.
[0018] Furthermore, when the modified zinc negative electrode is used to prepare an aqueous zinc ion button full battery, the steps are as follows: select a slurry prepared by mixing the positive electrode active material with conductive carbon black, a binder, and a solvent, and apply it on a current collector, and obtain the positive electrode after drying; assemble the positive electrode, the separator, the modified zinc negative electrode, and the electrolyte into an aqueous zinc ion button full battery, and let it stand for 2-12 hours.
[0019] The concentration of the electrolyte is 1-3 mol / L, and the amount of the electrolyte is 20-200 μL.
[0020] The positive electrode active material is one of manganese-based, vanadium-based and Prussian blue; the current collector is 20-200 μm graphite paper.
[0021] The advantages of the present invention are:
[0022] 1. Use inorganic-organic acid to pretreat the surface of the zinc negative electrode. The inorganic acid can slightly etch and activate the zinc sheet to make it a suitable site for crystal growth, enhance the adhesion of the coating to the zinc substrate, and the organic acid can regulate the crystal orientation of the zinc surface.
[0023] 2. The prepared hydrotalcite-based coating contains specific metals with zinc-philic properties, which can enhance zinc nucleation, inhibit the two-dimensional diffusion of zinc ions on the electrode surface, effectively promote interface stability, thereby improving zinc utilization and inhibiting dendrite reactions.
[0024] 3. The porous and dense array structure formed by the in-situ vertical growth of the hydrotalcite-based coating can increase the contact area between the negative electrode and the electrolyte, which is conducive to the full redox reaction and provides Zn 2+ Migration channel, increasing Zn on the electrode surface 2+ of uniform distribution.
[0025] 4. The hydrotalcite-based coating has excellent stability in the electrolyte, which enables it to be used in batteries to achieve ultra-stable zinc plating / stripping behavior of the zinc negative electrode.
[0026] 5. During the preparation process, the preparation process is simple and convenient, the conditions are mild, the preparation process is highly controllable, the reagents used are economical, and it is suitable for large-scale production.
[0027] In summary, the present invention uses an economical and simple method to prepare a stable inorganic interface coating, which can stabilize the zinc negative electrode interface and greatly improve the battery cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0029] Figure 1 This is a scanning electron microscope image of the bimetallic layered oxide modified zinc negative electrode material prepared in Example 1 of the present invention;
[0030] Figure 2 This is a scanning electron microscope image of the bimetallic layered oxide modified zinc negative electrode material prepared in Example 2 of the present invention;
[0031] Figure 3 This is the constant current charge and discharge curve of the modified zinc negative electrode in Example 2 of the present invention in a symmetrical battery;
[0032] Figure 4 Cyclic voltammetry curves of a full battery assembled with a modified zinc negative electrode at different scan rates in Example 2 of the present invention;
[0033] Figure 5 The full battery AC impedance curve of the zinc negative electrode assembled before and after modification in Example 2 of the present invention;
[0034] Figure 6 This is a scanning electron microscope image of the modified zinc negative electrode after cycling in Example 2 of the present invention. DETAILED DESCRIPTION
[0035] The present invention is further illustrated by the following specific examples.
[0036] Example 1
[0037] Cut multiple zinc sheets of 4cm×1cm and immerse them in zinc hydrochloric acid for 30min. Then wash the zinc sheets after ultrasound repeatedly with anhydrous ethanol and deionized water, and dry them in a natural environment. Next, etch the pretreated zinc sheet in a 10wt% phosphoric acid solution for 5min to obtain a zinc sheet with a zincate surface, rinse the excess acid solution on the surface with deionized water, and dry it in a natural environment for later use. Weigh 0.126g ZnSO4·7H2O, 0.124g Al2(SO4)3·18H2O, 0.011g NH4F and 6.26g urea and dissolve them in 60mL deionized water, stir for 30min to obtain a mixed solution. Transfer the mixed aqueous solution to a 100mL hydrothermal reactor and hydrothermally heat it at 95℃ for 6h. Then take it out after naturally cooling to room temperature and dry it at 80℃. Finally, calcine it at 350℃ for 4h in a muffle furnace to obtain the product. The obtained product was used as positive and negative electrodes to assemble a symmetrical battery. The assembly order was positive electrode shell, modified zinc negative electrode, glass fiber separator, modified zinc negative electrode, gasket, shrapnel and negative electrode shell. The electrolyte used was 100μL 2mol / L ZnSO4 solution. Constant current charge and discharge tests were carried out at different current densities and area capacities. Under the conditions of 0.5A / g and 0.25mAh / g, the symmetrical battery can be stably cycled for 500h.
[0038] Example 2
[0039] Cut multiple zinc sheets of 4cm×1cm and immerse them in zinc hydrochloric acid for ultrasonic treatment for 30min. Then wash the ultrasonic zinc sheet repeatedly with anhydrous ethanol and deionized water and dry it in a natural environment. Next, etch the pretreated zinc sheet in a 10wt% phosphoric acid solution for 5min to obtain a zinc sheet with a zincate surface, rinse the excess acid solution on the surface with deionized water, and dry it in a natural environment for later use. Weigh 0.108g ZnSO4·7H2O, 0.25g Al2(SO4)3·18H2O, 0.011g NH4F and 6.26g urea and dissolve them in 60mL deionized water, stir for 30min to obtain a mixed solution. Transfer the mixed aqueous solution to a 100mL hydrothermal reactor and hydrothermal it at 95℃ for 6h. Then take it out after naturally cooling to room temperature and dry it at 80℃. Finally, calcine it at 350℃ for 4h in a muffle furnace to obtain the product. The obtained product was used as positive and negative electrodes to assemble a symmetrical battery. The assembly order was positive electrode shell, modified zinc negative electrode, glass fiber separator, modified zinc negative electrode, gasket, shrapnel and negative electrode shell. The electrolyte used was 100μL 2mol / L ZnSO4 solution. Constant current charge and discharge tests were carried out at different current densities and area capacities. Under the conditions of 0.5A / g and 0.25mAh / g, the symmetrical battery can be stably cycled for 1000h.
[0040] Example 3
[0041] Cut multiple zinc sheets of 4cm×1cm and immerse them in zinc hydrochloric acid for ultrasonic treatment for 30min. Then wash the ultrasonic zinc sheet repeatedly with anhydrous ethanol and deionized water and dry it in a natural environment. Next, etch the pretreated zinc sheet in a 10wt% phosphoric acid solution for 5min to obtain a zinc sheet with a zincate surface, rinse the excess acid solution on the surface with deionized water, and dry it in a natural environment for later use. Weigh 0.126g ZnSO4·7H2O, 0.124g Al2(SO4)3·18H2O, 0.011g NH4F and 6.26g urea and dissolve them in 120mL deionized water, stir for 30min to obtain a mixed solution. Transfer the mixed aqueous solution to a 100mL hydrothermal reactor and hydrothermal it at 95℃ for 6h. Then cool it down naturally to room temperature and take it out and dry it at 80℃. Finally, calcine it at 350℃ for 4h in a muffle furnace to obtain the product. The obtained product was used as positive and negative electrodes to assemble a symmetrical battery. The assembly order was positive electrode shell, modified zinc negative electrode, glass fiber separator, modified zinc negative electrode, gasket, shrapnel and negative electrode shell. The electrolyte used was 100μL 2mol / L ZnSO4 solution. Constant current charge and discharge tests were carried out at different current densities and area capacities. Under the conditions of 0.5A / g and 0.25mAh / g, the symmetrical battery can be stably cycled for 800h.
[0042] The zinc-aluminum hydrotalcite-based protective layer prepared in Example 2 of the present invention has a scanning electron microscope image as shown in FIG. Figure 2 The hydrotalcite structure is arranged vertically on the zinc sheet to form a dense multi-level array structure. On the one hand, it increases the contact area between the zinc negative electrode and the electrolyte, which is conducive to the full redox reaction; on the other hand, the pores formed by vertical growth provide Zn 2+ The migration channel facilitates the transport of zinc ions. The constant current charge and discharge curve of the symmetrical battery assembled in Example 2 is as follows: Figure 3 As shown, at 0.5 mA / cm 2 The current density is 0.25 mAh / cm 2 The area capacity can achieve a stable cycle of more than 1000h, proving that the zinc negative electrode modified by the coating is conducive to achieving stable battery charge and discharge behavior. In Example 2, according to the cyclic voltammetry curves of the full battery at different scan rates ( Figure 4 ), which has two pairs of redox peaks during the charge and discharge process, and the two pairs of redox peaks correspond to the two-step redox reactions of MnO2 and MnOOH respectively. At different scan rates, the cyclic voltammetry curves show similar change trends. Even at a high scan rate of 10mV / s, the curves still maintain similar redox peaks, proving its excellent rate characteristics. Figure 5 This is the AC impedance spectrum of the full battery assembled in Example 2, which shows that the modified zinc negative electrode has a smaller semicircle in the high-frequency region, indicating that the modified zinc negative electrode interface has a smaller charge transfer impedance. Figure 6 This is a picture of the surface morphology of the zinc negative electrode after cycling, which shows that the surface is not obviously covered by corrosion products and no dendrites are generated.
[0043] Experiments have shown that the modified electrode exhibits a uniform plating / stripping process and has good cycle stability and rate characteristics. The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the contents of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that technicians in the relevant technical field can understand and use the present invention well.
Claims
1. A metallic zinc negative electrode interface coating constructed by in-situ growth of zinc-based hydrotalcite, Features Based on the process of "etching-nucleation-growth" to obtain a thin and uniform protective layer material, the method for in-situ growth of hydrotalcite at the negative electrode of an aqueous zinc-based battery is characterized by comprising the following steps: S1. Ultrasonicate the zinc sheet in mineral acid, water and ethanol to remove surface zinc oxide; S2, immersing the zinc sheet with the surface oxide removed in an organic acid solution of a certain pH and etching for a period of time to obtain a zinc sheet with a zincate surface; S3. Place the treated zinc sheet in a mixed solution of zinc metal salt and other metal salts in a certain proportion, add a certain amount of precipitant, carry out "nucleation-growth" under hydrothermal conditions, then vacuum dry, and finally calcine in a muffle furnace to obtain a modified zinc negative electrode.
2. The method for in-situ growth of hydrotalcite on a zinc negative electrode according to claim 1, wherein in S1, the thickness of all zinc sheets is 0.01-1 mm.
3. The method for in-situ growth of hydrotalcite on a zinc negative electrode according to claim 1 is characterized in that in S1, the inorganic acid can be one or more combinations of nitric acid, boric acid, hydrochloric acid, sulfuric acid, and phosphoric acid; the concentration of the acid solution is 0.1-1 mol / L; the water used is one of deionized water and ultrapure water; and the ultrasonic time is 10-50 min.
4. The method for in-situ growth of hydrotalcite at a zinc negative electrode according to claim 1 is characterized in that the organic acid in S2 can be any one or a combination of lactic acid, aminosulfonic acid, phytic acid, oxalic acid, citric acid, organic phosphonic acid, acetic acid, malic acid, and tartaric acid; the pH value is between 2-5; and the etching time is between 2-10 min.
5. The method for in-situ growth of hydrotalcite at a zinc negative electrode according to claim 1, wherein the zinc salt used in S3 is any one of zinc sulfate, zinc nitrate, zinc chloride, and zinc carbonate; the other metal salts are any one of stannous sulfate, magnesium sulfate, magnesium nitrate, magnesium chloride, indium chloride, indium nitrate, aluminum sulfate, aluminum nitrate, aluminum chloride, bismuth nitrate, copper sulfate, copper nitrate, and copper chloride or a combination thereof; and the precipitant is any one of urea and sodium hydroxide.
6. The method for in-situ growth of hydrotalcite at a zinc negative electrode according to claim 1, wherein in the mixed solution obtained in S3, the concentration of zinc salt is 0-0.1 mol / L; the concentration of other metal salts is 0.001-0.02 mol / L; and the concentration of the precipitant is 0.1-0.5 mol / L.
7. The method for in-situ growth of hydrotalcite on zinc negative electrode according to claim 1 is characterized in that the temperature of hydrothermal treatment in S3 is 80-180°C, and the reaction time is 2-12h; the calcination temperature is 100-500°C; and the reaction time is 2-12h.
8. A modified zinc negative electrode material prepared by the method according to any one of claims 1 to 7, Features The thickness of the in-situ grown coating is 0.1-50 μm.
9. The modified zinc negative electrode prepared by the preparation method according to any one of claims 1 to 7 is used in aqueous zinc-based batteries. It is characterized in that The aqueous zinc-based battery is a symmetrical button cell or a full button cell.
10. The use according to claim 9, characterized in that when the modified zinc negative electrode in S3 is used to prepare an aqueous zinc ion symmetrical button battery, the steps are: the modified zinc sheet is used as the positive electrode and the negative electrode, and is assembled with a separator and an electrolyte into an aqueous zinc ion symmetrical button battery, and the battery is left to stand for 2-12 hours.
11. The use according to claim 9 is characterized in that when the modified zinc negative electrode is used to prepare an aqueous zinc ion button full battery, the steps are: selecting a slurry prepared by mixing a positive electrode active material with conductive carbon black, a binder, and a solvent, and applying it on a current collector, and obtaining a positive electrode after drying; assembling the positive electrode, a separator, a modified zinc negative electrode, and an electrolyte into an aqueous zinc ion button full battery, and standing it for 2-12 hours.
12. The use according to claims 10 and 11, characterized in that the concentration of the electrolyte is 1-3 mol / L, and the amount of the electrolyte dripped onto the diaphragm is 20-200 μL.
13. The use according to claims 10 and 11, characterized in that the positive electrode active material is one of manganese-based, vanadium-based and Prussian blue, and the current collector is graphite paper with a thickness of 20-200 μm.
Citation Information
Cited By
Preparation method and application of zinc anode of aqueous zinc ion battery
CN120048836A