Urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection
The urease-induced calcium carbonate selective cementing method injected with heterogeneous foam segment plugs solves the problems of low viscosity and uncontrollable regional areas in the prior art, and achieves low cost and controllable range urease-induced calcium carbonate precipitation, which significantly increases the cost and controllable range. Improves the strength and seepage of rock and soil bodies.
Patent Information
- Application Number
- CN202411529039.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-30
- Publication Date
- 2024-12-24
AI Technical Summary
The existing urease-induced calcium carbonate precipitation technology has problems such as low viscosity of cementitious fluid, easy flow, accumulation and blockage of calcium carbonate at the injection point, uncontrollable cementing area and large amount of consumables, which limits its application scope and cost-effectiveness.
The urease-induced calcium carbonate selective cementing method injected with heterogeneous foam segment plugs is used to prepare foams of different viscosity through high-speed shearing, and circulate the formation to achieve selective precipitation and cementation of calcium carbonate, reducing engineering costs and expanding the construction scope.
The fluidity and range controllability of cementitious liquid are achieved, the project cost is reduced, the construction scope is expanded, and the template is provided through heterogeneous foam is provided to build a stable calcium carbonate structure, which significantly improves the strength and seepage of rock and soil bodies. sex.
Smart Images

Figure CN119177647A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of underground rock and soil reinforcement and anti-seepage, and in particular to a urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection. Background Art
[0002] Loose, weakly cemented soil and porous rock mass have the characteristics of low strength and high water permeability, which are prone to ground subsidence or water gushing in underground target work areas, seriously threatening the long-term safety of ground buildings or the safety of underground tunnels, tunnels, and mining operations. The urease-induced calcium carbonate precipitation (EICP) technology can generate calcium carbonate crystals between loose soil particles or in the pores of rock mass, cementing particles and inter-fracture structures, which has the effect of significantly improving the strength of rock and soil and reducing its water permeability. It has potential application prospects in the fields of foundation strengthening and reinforcement, concrete crack repair, and underground rock crack sealing. In particular, the plant-extracted urease-induced calcium carbonate precipitation method has the technical advantages of easy access to raw materials and simple process methods.
[0003] However, the existing technology still has the following defects: the viscosity of the cementing fluid injected into the formation is low, cross-flow is prone to occur, and the cementing area is uncontrollable; calcium carbonate accumulation and blockage at the injection point are very likely to occur, reducing the feasibility of the process; the cementing area from the injection point to the target area has a large amount of cementing consumables in the entire range, increasing the construction cost; there is still a lack of selective cementing strategies for specific areas, which weakens the application potential and scope of this technology. Therefore, it is necessary to develop a new type of urease-induced calcium carbonate precipitation technology with low cost and controllable cementing range. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and propose a urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection. The slug injection method of alternately cyclically injecting heterogeneous foam into the formation is adopted to cause the foam containing only the cementing liquid to undergo the calcium carbonate generation, precipitation and cementation process, thereby achieving the purpose of selective cementation in the formation.
[0005] To achieve the above object, the present invention adopts the following specific technical solutions:
[0006] The present invention provides a urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection, comprising the following steps:
[0007] S1. preparing a plant urease solution: crushing, soaking, dissolving, filtering, centrifuging and acidifying the soybean, pea or melon seed plant raw materials to obtain a plant urease solution;
[0008] S2. preparing heterogeneous foam: preparing displacement foam by subjecting the plant urease solution to high-speed shearing, mixing the plant urease solution with a calcium ion solution and a urea solution to prepare a binder, and subjecting the binder to high-speed shearing to prepare a binder foam;
[0009] S3. Pretreatment of construction strata: inject water into the construction strata to remove alkaline and toxic substances contained in the strata to ensure the activity of the subsequently injected protein;
[0010] S4, heterogeneous foam slug injection: inject cementing liquid foam and displacement foam into the construction stratum in sequence, and let it stand after injection to allow the cementing liquid foam to fully undergo urea decomposition, calcium carbonate generation and precipitation cementation processes, accompanied by foam defoaming process;
[0011] S5. Foam plug cyclic injection: repeat step S4 to make the urea decomposition, calcium carbonate generation and precipitation cementation process of the cementing liquid foam occur repeatedly in the designed selective cementation area, and repeat the cycle until the cementation degree of the area reaches the preset standard.
[0012] Furthermore, in step S2, the preparation of heterogeneous foam also includes preparing pre-foam, and the plant urease solution is subjected to high-speed shearing to prepare the pre-foam. The viscosity of the pre-foam and the displacement foam is different. The viscosity of the pre-foam, the displacement foam, and the cementing liquid foam is in the order of displacement foam viscosity>cementing liquid foam viscosity>pre-foam viscosity. The viscosity of the prepared pre-foam, displacement foam, and cementing liquid foam is lower than 100 MPa / s to ensure fluidity. In step S4, the pre-foam, the cementing liquid foam, and the displacement foam are injected into the construction formation in sequence.
[0013] Furthermore, in step S1, the solvent for soaking and dissolving is water, and the dissolution ratio is 40g / L to 200g / L; the acidifying reagent is hydrochloric acid or acetic acid with a concentration of 0.2mol / L to 4mol / L.
[0014] Furthermore, in step S2, the concentrations of calcium ions and urea in the binder are between 0.5 mol / L and 1.5 mol / L; and the foam quality of the prepared binder foam is not higher than 80%.
[0015] Furthermore, in step S4, the gas used for injecting heterogeneous foam into the construction stratum is air, carbon dioxide or nitrogen to improve the cementation efficiency of calcium carbonate precipitation; the injection method can be to transport the prefabricated heterogeneous foam on the ground to the bottom of the hole and then inject it into the stratum, or to directly inject it through the bottom of the hole foaming device, or to inject the gas and foaming liquid into the stratum at the same time for in-situ shear foaming; after the injection is completed, the standing time is 6 to 24 hours.
[0016] The present invention can achieve the following technical effects:
[0017] 1. The present invention uses the foaming property of plant urease solution to prepare self-source foam, which does not require the addition of other surfactants, thereby reducing costs;
[0018] 2. The heterogeneous foam plug injection method can be used to design the precipitation area of calcium carbonate in the formation, achieve selective formation cementation, greatly reduce the engineering cost of enzyme-induced calcium carbonate precipitation technology, and expand the construction scope;
[0019] 3. Using heterogeneous foam as a carrier, the viscosity of the cementing fluid injected into the formation can be adjusted, so as to achieve the purpose of stable and controllable fluidity, flow range and front profile of the cementing fluid, and enhance the technical effect;
[0020] 4. Using heterogeneous foam as a carrier, the foam has a long half-life and controllable bubble size. The foam structure can provide a template for the precipitation of calcium carbonate crystals and the connection between particles. It can construct a three-dimensional calcium carbonate structure in the pores of the formation and enhance the technical effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a flow chart of a urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection provided in an embodiment of the present invention;
[0022] Figure 2 is a schematic diagram of urease-induced selective cementation of calcium carbonate based on three-stage heterogeneous foam slug injection according to an embodiment of the present invention;
[0023] Figure 3 is a schematic diagram of urease-induced selective cementation of calcium carbonate based on two-stage heterogeneous foam slug injection according to an embodiment of the present invention;
[0024] Figure 4 It is a schematic diagram and a photo image of a visualization model of a simulated rock mass fracture provided according to an embodiment of the present invention;
[0025] Figure 5 is a photo image of a heterogeneous foam injection experiment provided in an embodiment of the present invention;
[0026] Figure 6 It is a comparison chart of experimental results of urease-induced calcium carbonate selective cementation based on the heterogeneous foam slug injection method provided in an embodiment of the present invention.
[0027] Reference numerals include:
[0028] Injection hole 1, displacement foam boundary 2, cementing fluid foam boundary 3, pre-foam boundary 4, formation boundary 5, simulation area 6, outflow end 7, displacement foam 8, cementing fluid foam 9, pre-foam 10, calcium carbonate 11, selective cementing area 12. DETAILED DESCRIPTION
[0029] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In the following description, the same modules are represented by the same reference numerals. In the case of the same reference numerals, their names and functions are also the same. Therefore, the detailed description thereof will not be repeated.
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.
[0031] The present invention provides a urease-induced calcium carbonate selective cementation method based on heterogeneous foam plug injection, the process is as follows: Figure 1 As shown, the following steps are included:
[0032] S1. Preparation of plant urease solution: using soybeans, peas, melon seeds and other plants as raw materials, the urease plant raw materials are crushed, soaked and dissolved, filtered, centrifuged and acidified in sequence to obtain the plant urease solution.
[0033] In the process of extracting plant urease, the solvent is water, the dissolution ratio is 40g / L to 200g / L, and the reagent required for acidification can be hydrochloric acid, acetic acid, etc. with a concentration between 0.2mol / L and 4mol / L. The prepared plant urease solution contains not only urease that can decompose urea, but also other plant protein components, which have the effect of reducing surface tension.
[0034] S2. Preparation of heterogeneous foam: preparing pre-foam and displacement foam of different viscosities by high-speed shearing of plant urease solution, mixing plant urease solution with calcium ion solution and urea solution to prepare a binder, and preparing a binder foam by high-speed shearing of the binder.
[0035] The concentrations of calcium ions and urea in the cementing fluid are both 0.5mol / L-1.5mol / L, and the viscosity of the pre-foam, displacement foam and cementing fluid foam is in the order of displacement foam viscosity > cementing fluid foam viscosity > pre-foam viscosity; the viscosities of the prepared pre-foam, displacement foam and cementing fluid foam are all lower than 100mpa / s to ensure fluidity; during the preparation of heterogeneous foam, the foam quality of the cementing fluid foam is not higher than 80%; the reagent for acidifying the plant urease solution is selected as hydrochloric acid or acetic acid with a concentration of 0.2mol / L-4mol / L.
[0036] S3. Pretreatment of construction strata: Inject water into the construction strata and remove alkaline and toxic substances contained in the strata to ensure the activity of the subsequently injected protein.
[0037] S4, Heterogeneous foam plug injection: Inject pre-foam, cementing liquid foam and displacement foam into the construction stratum in sequence, such as Figure 2As shown in a~2c, the injection amount of the three foams is based on the designed selective bonding area; after the injection is completed, it is left to stand for 6 to 24 hours to allow the cementing liquid foam to fully undergo urea decomposition, calcium carbonate generation and precipitation bonding process, accompanied by the foam defoaming process.
[0038] S5, foam slug cyclic injection: repeat step S4, so that the urea decomposition, calcium carbonate generation and precipitation cementation process of the cementing liquid foam will occur repeatedly in the designed selective cementation area, such as Figure 2 As shown in Figure d, the cycle is repeated until the bonding degree of the area reaches the preset standard.
[0039] In some embodiments, the preparation of the pre-foam can be omitted in the preparation of the heterogeneous foam in step S2, and in step S4, only the cementing liquid foam and the displacement foam are injected alternately and cyclically, such as Figure 3 As shown, the front foam can be eliminated.
[0040] During the injection of the heterogeneous foam plug in step S4, the injection method may be to transport the prefabricated foam on the ground to the bottom of the hole and then inject it into the formation, or to directly inject it through the bottom of the hole foaming device, or to simultaneously inject the gas and the foaming liquid into the formation for in-situ shear foaming.
[0041] The above method is described below in conjunction with specific embodiments.
[0042] 1. Prepare a visualization model for simulating rock mass fractures: construct an experimental model according to the actual working conditions of the invention, such as Figure 4 As shown in the figure, the model consists of two pieces of quartz glass with a size of 60mm×60mm. The gap width between the glass pieces is controlled by a 0.2mm gasket. The effective flow simulation area is fan-shaped, which is used to simulate a part of a single injection hole under actual working conditions. The narrow end of the model is the fluid injection hole, which simulates the injection hole under actual working conditions; the wide end of the model is the fluid outflow end, which simulates the surrounding boundary under actual working conditions.
[0043] 2. Preparation of plant urease solution: In this embodiment, soybeans are selected as the raw material for urease extraction. The soybeans are crushed into 100-200 meshes and soaked and dissolved in distilled water with a dissolution ratio of 100 g / L. The soaking and dissolution are carried out at 4°C for 12 hours, and then the suspension is centrifuged at 8000 rpm for 15 minutes, and the supernatant is taken as the finished urease solution.
[0044] 3. Prepare calcium ion solution and urea solution: select anhydrous calcium chloride as a calcium source, and dissolve it in distilled water to obtain a 4 mol / L calcium ion solution; use 99% purity urea, and dissolve it in distilled water to obtain a 4 mol / L urea solution.
[0045] 4. Experimental model pretreatment: Inject 10 times the pore volume of distilled water into the above experimental model to fully clean the inner wall of the model and remove highly alkaline and toxic substances on the wall.
[0046] 5. Preparation of heterogeneous foam: In this embodiment, urease solution is used to prepare self-source foam. 5 ml of urease solution is taken, and high-speed shear method is used to prepare pre-foam and replacement foam, and the foam quality is 90%; 5 ml of urease solution is taken, and it is acidified to a pH value of 5.5 with 2 mol / L hydrochloric acid, and it is mixed with calcium ion solution and urea solution in a ratio of 2:1:1 to prepare a binder. The concentrations of calcium ions and urea in the binder are both 1 mol / L. The binder is also foamed by high-speed shear method to prepare a binder foam, and the foam quality is 40%.
[0047] 6. Heterogeneous foam injection: After the self-source foam is prepared, the pre-foam is immediately injected into the experimental model through the injection hole, and the injection amount is 2 times the pore volume, so that the model is filled with the pre-foam; then 0.25mL of cementing liquid foam is injected into the experimental model; finally, 0.5mL of displacement foam is injected into the experimental model. The final three types of foam distribution are as follows Figure 5 As shown in a~5b.
[0048] 7. Calcium carbonate precipitation: After the above three types of foams are completely injected, let it stand for 12 hours to allow the cementing liquid foam to undergo urea decomposition, calcium carbonate generation and precipitation cementation processes, which are accompanied by a foam defoaming process.
[0049] 8. Foam segment cycle injection: Repeat the above steps 6 and 7 for a total of 10 times, so that the urea decomposition, calcium carbonate generation and precipitation cementation process of the cementing liquid foam will occur repeatedly in the designed selective cementing area, and circulate until the cementing degree in this area reaches the design standard.
[0050] 9. Evaluation of cementation effect: After completing the above steps, the constant head permeability test method was used to evaluate the effect of calcium carbonate precipitation on the water permeability of the model. The test results showed that the permeability of the experimental model was reduced by more than 92%. A high-definition camera was used to record the distribution area of calcium carbonate on the inner wall of the model to evaluate the selective cementation effect of urease-induced calcium carbonate using self-sourced protein foam as a carrier. Figure 6 As shown, calcium carbonate is precipitated in the designed area, achieving a selective cementation effect.
[0051] The embodiment may also adopt the method of alternately cyclically injecting the cementing liquid foam and the displacement foam, such as Figure 5 As shown in c~5d, the pre-foam is eliminated; the test results show that the permeability of the experimental model is also reduced by more than 90%, and the calcium carbonate is precipitated in the designed area, which also achieves the selective cementation effect.
[0052] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0053] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
[0054] The above specific implementations of the present invention do not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection, characterized in that: The steps include: S1. preparing a plant urease solution: crushing, soaking, dissolving, filtering, centrifuging and acidifying the soybean, pea or melon seed plant raw materials to obtain a plant urease solution; S2. preparing heterogeneous foam: preparing displacement foam by subjecting the plant urease solution to high-speed shearing, mixing the plant urease solution with a calcium ion solution and a urea solution to prepare a binder, and subjecting the binder to high-speed shearing to prepare a binder foam; S3. Pretreatment of construction strata: inject water into the construction strata to remove alkaline and toxic substances contained in the strata to ensure the activity of the subsequently injected protein; S4, heterogeneous foam slug injection: inject cementing liquid foam and displacement foam into the construction stratum in sequence, and let it stand after injection to allow the cementing liquid foam to fully undergo urea decomposition, calcium carbonate generation and precipitation cementation processes, accompanied by foam defoaming process; S5. Foam plug cyclic injection: repeat step S4 to make the urea decomposition, calcium carbonate generation and precipitation cementation process of the cementing liquid foam occur repeatedly in the designed selective cementation area, and repeat the cycle until the cementation degree of the area reaches the preset standard.
2. The urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection according to claim 1, characterized in that: In step S2, the preparation of heterogeneous foam also includes the preparation of pre-foam, and the plant urease solution is subjected to high-speed shearing to prepare the pre-foam. The viscosity of the pre-foam and the displacement foam is different. The viscosity of the pre-foam, the displacement foam, and the cementing liquid foam is in the order of displacement foam viscosity>cementing liquid foam viscosity>pre-foam viscosity. The viscosity of the prepared pre-foam, displacement foam, and cementing liquid foam is lower than 100 MPa / s to ensure fluidity. In step S4, the pre-foam, the cementing liquid foam, and the displacement foam are injected into the construction stratum in sequence.
3. The urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection according to claim 1, characterized in that: In step S1, the solvent for soaking and dissolving is water, and the dissolution ratio is 40g / L to 200g / L; the acidifying reagent is hydrochloric acid or acetic acid with a concentration of 0.2mol / L to 4mol / L.
4. The urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection according to claim 1, characterized in that: In step S2, the concentration of calcium ions and urea in the binder is 0.5 mol / L to 1.5 mol / L; and the foam quality of the prepared binder foam is not higher than 80%.
5. The urease-induced calcium carbonate selective cementation method based on heterogeneous foam slug injection according to claim 1, characterized in that: In step S4, the gas used for injecting heterogeneous foam into the construction stratum is air, carbon dioxide or nitrogen to improve the cementation efficiency of calcium carbonate precipitation; the injection method can be to transport the prefabricated heterogeneous foam on the ground to the bottom of the hole and then inject it into the stratum, or to directly inject it through the bottom of the hole foaming device, or to inject the gas and foaming liquid into the stratum at the same time for in-situ shear foaming; after the injection is completed, the standing time is 6 to 24 hours.
Citation Information
Cited By
Grouting material suitable for Luhe group sandstone and preparation method thereof
CN120988664A