Castable used on wall position of aluminum smelting furnace

By using a new type of castable material at the wall of the aluminum furnace, the raw material composition includes coarse aggregate corundum, silicon carbide, alumina micro powder, etc., the problem of insufficient thermal shock resistance of the existing castable material is solved, and the thermal shock resistance and service life of the castable material is significantly improved.

CN120004603APending Publication Date: 2025-05-16CHONGQING SHUNBO TAIDONG MECHANICAL & ELECTRICAL EQUIP CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510097238.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-01-22
Publication Date
2025-05-16

AI Technical Summary

Technical Problem

The refractory castables used in existing aluminum furnaces are inadequate in thermal shock resistance under high temperature and frequent temperature changes, and are prone to small cracks, resulting in quality problems in the inner wall of the castable.

Method used

A new castable raw material is composed of coarse aggregate corundum, coarse aggregate silicon carbide, fine aggregate silicon carbide, alumina micro powder, phosphate binder, stainless steel explosion-proof fiber and thermally conductive fiber. Through the combination of these components, the thermal shock resistance of the castable is improved.

Benefits of technology

The thermal shock resistance of the castable material at the wall on the aluminum furnace was significantly improved, with medium temperature strength ≥110MPa, high temperature strength ≥105MPa, and water quenching times ≥62 times, extending the service life of the castable material and reducing the phenomenon of slag hanging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120004603A_ABST
    Figure CN120004603A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of refractory castable materials, and particularly relates to a castable material used at a wall position of an aluminum smelting furnace. The castable comprises the following raw material components: coarse aggregate corundum, coarse aggregate silicon carbide, fine aggregate silicon carbide, alumina micro powder, a phosphate binder, stainless steel explosion-proof fibers and heat-conducting fibers. The casting material at least has the beneficial effects that slag is not prone to adhering to the wall position casting material, then the cleanliness and quality of molten aluminum are improved, and the effective service life of the casting material is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of refractory castables, and in particular relates to a castable used on the upper wall of an aluminum melting furnace. Background Art

[0002] Aluminum melting furnace, also known as aluminum melting furnace, is mainly used to heat and melt aluminum ingots to produce various aluminum products. Among them, the inner wall material of the furnace body of aluminum melting furnace is generally various refractory castables, so as to obtain sufficient high temperature resistance and fire resistance.

[0003] Generally, the raw materials of the common refractory castables for aluminum melting furnaces mainly include: bauxite, mullite, silica sand, alumina powder, calcium aluminate cement, and steel fiber. The refractory castables have basic fire resistance, corrosion resistance and thermal shock resistance.

[0004] However, the above-mentioned thermal shock resistance is relatively general. When the temperature inside the aluminum melting furnace changes rapidly, or after the furnace body is used for a long time, small cracks are likely to appear on the castable, which will lead to a series of subsequent castable inner wall quality problems.

[0005] Correspondingly, various new castable products with improved thermal shock resistance are now available. For example, the Chinese invention patent application with application publication number CN109336627A and application publication date 2019.02.15 discloses a castable for aluminum melting furnace lining, the raw materials of which include: fused brown corundum, alumina powder, alumina powder, calcium aluminate cement, supersilica powder, stainless steel fiber, high-efficiency water reducer, and explosion-proof fiber.

[0006] The castable in the invention patent application has the following advantages: high density, high strength, good toughness, impact resistance, stable thermal shock resistance, and long service life.

[0007] However, when the castable is actually used in an aluminum melting furnace, it still has at least the following problems of insufficient thermal shock resistance, which are specifically manifested as follows: Its medium temperature strength is only at the general level of 62-66MPa, and its high temperature strength is less than 83MPa. These two parameters indicate that the thermal shock resistance of the castable is relatively general, so it is easy to have small cracks during use. Summary of the invention

[0008] The present application provides a castable used at the upper wall of an aluminum melting furnace, and the technical problem to be solved is: how to make the castable specially used at the upper wall of an aluminum melting furnace have outstanding thermal shock resistance.

[0009] The technical solution adopted by the present application to solve the above-mentioned problem is: a castable used on the upper wall of an aluminum melting furnace, the raw material composition of which includes the following components: coarse aggregate corundum, coarse aggregate silicon carbide, fine aggregate silicon carbide, alumina powder, phosphate binder, stainless steel explosion-proof fiber, and thermal conductive fiber.

[0010] A further preferred technical solution is that the particle size of the coarse aggregate corundum is 2.0-5.5 mm, the particle size of the coarse aggregate silicon carbide is 3.5-7.0 mm, the particle size of the fine aggregate silicon carbide is 0.5-1.2 mm, and the particle size of the alumina powder is 3.0-6.0 μm.

[0011] A further preferred technical solution is that the phosphate binder is any one of aluminum phosphate, aluminum dihydrogen phosphate, magnesium phosphate, and zinc phosphate, or a mixture of several of them.

[0012] A further preferred technical solution is that the thermal conductive fiber is any one of or a mixture of aluminum oxide fiber, silicon carbide fiber, copper fiber, ceramic fiber, and boron nitride fiber, and the length of the thermal conductive fiber is 5.0-12.0 mm and the diameter is 0.10-0.14 mm.

[0013] A further preferred technical solution is that the raw material composition is the following components by weight: coarse aggregate corundum 44-47%, coarse aggregate silicon carbide 30-35%, fine aggregate silicon carbide 11-15%, alumina powder 3-5%, phosphate binder 2.0-3.0%, stainless steel explosion-proof fiber 0.5-0.6%, thermal conductive fiber 0.20-0.22%, and the balance is additives.

[0014] A further preferred technical solution is that the additive is any one of a water reducer, an antioxidant, an anti-stripping agent, and a coagulant, or a mixture of several of them.

[0015] A further preferred technical solution is that the casting range of the castable is the upper 15-20% height area of ​​the inner wall of the aluminum melting furnace, or above the slag line area of ​​the aluminum melting furnace, wherein the height difference between the upper and lower edges of the slag line area is 5.0-8.0 cm.

[0016] A method for using a castable material used at the upper wall of an aluminum melting furnace comprises the following steps in sequence: S1, add water and stir; S2, compaction into mold; S3, curing and demoulding; S4. Dry naturally.

[0017] A further preferred technical solution is that in S1, the weight of water added is 5-7% of the weight of the castable.

[0018] A further preferred technical solution is that in S2, the castable is only cast at the upper wall position, and the refractory castable used in the slag line area and the main area of ​​the aluminum melting furnace is vibrated and compacted together with the castable to obtain a complete aluminum melting furnace casting body.

[0019] In the method of use of the present application, the inner wall of the vertical aluminum melting furnace is divided into the following three areas from top to bottom: the upper wall position, the slag line area, and the main body area. The upper wall position refers to the upper 15-20% height area of ​​the inner wall of the aluminum melting furnace, the slag line area is set to have a height difference of 5.0-8.0 cm between the upper and lower edges, and the main body area is the entire area below the slag line area and above the bottom surface of the furnace body.

[0020] On the other hand, the applicant found that: First, the inner wall of the aluminum melting furnace can be divided into the upper wall position, the slag line area and the main body area from top to bottom. The slag line area and the main body area together constitute the aluminum molten pool. The temperature of these two places is generally 700-750℃, while the temperature of the upper wall position is relatively higher, generally around 1100℃. In addition, the upper wall position is mainly exposed to air, and the amplitude and speed of its temperature difference change are relatively larger. Therefore, for the castable at the upper wall position, one of its main performance requirements is thermal shock resistance, while for the castable in the main area, one of its main performance requirements is high temperature resistance; Second, the liquid surface of aluminum liquid will frequently hit the slag line area, so one of the main performance requirements for the castable in the slag line area is impact erosion resistance; Third, if tiny cracks appear on the castable at the upper wall, aluminum vapor will penetrate into the tiny cracks and react chemically with the components in the castable, eventually forming nodules and bulges on the surface of the castable, leading to harmful slag. This harmful phenomenon will not only reduce the cleanliness and quality of the aluminum liquid, but also greatly shorten the effective service life of the castable.

[0021] The applicant also found that the reasons for generating and / or exacerbating the above-mentioned harmful drossing phenomenon are mainly the following three points: 1. The thermal shock resistance of the castable is relatively insufficient, and harmful cracks are generated during large and / or frequent temperature changes, which intensifies the chemical reaction between aluminum vapor and the castable; 2. In the raw material composition of castable, SiO 2 It is the main component that reacts with aluminum vapor, and the two easily react to form additional, later-produced corundum (Al 2 O 3 ), the corundum product is the main component of the above-mentioned nodule and bulge structure; 3. In the early stage of heating and melting aluminum ingots in the aluminum melting furnace, the temperature of the castable at the upper wall is much lower than the temperature of the castable in the main area. However, aluminum vapor has been generated at this time. When the aluminum vapor encounters the colder castable at the upper wall, drossing is very likely to occur. In other words, this harmful drossing phenomenon mainly occurs in the early stage of the heating and melting operation.

[0022] Therefore, the upper wall castable in the present application has the advantage of not being easily slag-coated by aluminum vapor. The reasons are mainly the following three points: First, SiO is almost completely eliminated from the raw material composition of the castable. 2 By combining corundum, silicon carbide, and alumina powder, the problems of reduced castable strength, reduced corrosion resistance, and lack of expansion regulation function caused by not using Si element can be fully supplemented and solved; Second, the raw material composition of the castable, which consists of silicon carbide, alumina powder, and phosphate binder, already has relatively high density and thermal shock resistance. The additional stainless steel explosion-proof fiber and thermal conductive fiber can further balance the stress difference and temperature difference at various locations on the wall, which is also beneficial to thermal shock resistance and is not easy to produce fine cracks under frequent temperature difference conditions. Thirdly, the content of the additionally added heat-conducting fiber in the raw material composition of the castable is sufficient and appropriate, which can quickly and evenly increase the temperature of various locations on the upper wall in the early stage of the melting operation, thereby increasing the difficulty of aluminum vapor drossing.

[0023] It should be noted that the additional addition of thermal conductive fibers will indeed increase the heat loss of the inner wall of the aluminum melting furnace in the thickness direction. However, since high-temperature resistant thermal insulation cotton is generally installed between the castable and the steel wall of the furnace body, the harmful conditions of the above-mentioned improved thermal conductivity have little effect on the actual working conditions of the aluminum melting furnace. Compared with the advantage of improving the slag phenomenon, this part of the increased heat conduction consumption is completely worthwhile.

[0024] The beneficial effects of this application include at least the following two points.

[0025] First, it is not easy for slag to hang on the castable at the upper wall position, thereby improving the cleanliness and quality of the aluminum liquid and extending the effective service life of the castable.

[0026] Second, the castable at the upper wall position has outstanding thermal shock resistance. The specific parameters are: medium temperature strength (800℃×3h) ≥110MPa, high temperature strength (1400℃×3h) ≥105MPa, and water quenching times ≥62 times.

[0027] Among them, the test method for the above-mentioned water quenching times refers to Method 2 of GB / T 30873-2014 Test method for thermal shock resistance of refractory materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is the average test data of the castables in 3 embodiments and 4 comparative examples of the present application.

[0029] Figure 2 This is a schematic diagram of the upper wall position in this application.

[0030] Figure 3 This is a photo of the dross phenomenon in Comparative Example 4 of the present application, in which the dross phenomenon is obvious.

[0031] Figure 4 for Figure 3 The photo shows the dross phenomenon during the heating operation of the aluminum melting furnace. The dross is heated to red and then easily falls into the aluminum liquid, reducing the quality of the aluminum liquid.

[0032] Figure 5 This is a photo of Example 1 of the present application, in which the drossing phenomenon is relatively mild.

[0033] In the figure, the meanings of the symbols are as follows.

[0034] Upper wall position a, slag line area b, main area c, refractory insulation cotton d. DETAILED DESCRIPTION

[0035] The following description is merely a preferred embodiment of the present application and does not limit the scope of the present application.

[0036] Example 1 As attached Figure 1 , 2 As shown, a castable used in the upper wall of an aluminum melting furnace, the raw material composition of which is the following components by weight: Coarse aggregate corundum 45%, coarse aggregate silicon carbide 32%, fine aggregate silicon carbide 12%, alumina powder 4%, phosphate binder 2.5%, stainless steel explosion-proof fiber 0.5%, thermal conductive fiber 0.20%, and the balance is 3.8% of additives.

[0037] The particle size of the coarse aggregate corundum is 2.2-4.7 mm, the particle size of the coarse aggregate silicon carbide is 4.0-6.4 mm, the particle size of the fine aggregate silicon carbide is 0.6-1.1 mm, and the particle size of the alumina powder is 4.2-4.8 μm.

[0038] Wherein, the phosphate binder is aluminum phosphate, the thermal conductive fiber is silicon carbide fiber, the length of the silicon carbide fiber is 8.9-10.5 mm, and the diameter is 0.10-0.12 mm.

[0039] The additives are polycarboxylic acid-based high-efficiency water reducing agent, zircon antioxidant, acrylic emulsion anti-stripping agent, and calcium chloride coagulant.

[0040] The preparation method of the castable comprises the following steps in sequence: T1. Mixing: Add all the coarse aggregate corundum, coarse aggregate silicon carbide, fine aggregate silicon carbide, alumina powder, phosphate binder, stainless steel explosion-proof fiber, thermal conductive fiber, and additives into a mixer and mix for 10 minutes to obtain a mixture; T2. Bag filling: bag the mixture to obtain the final castable product.

[0041] The method for using the castable comprises the following steps in sequence: S1. Add water and stir: the weight of water added is 6% of the weight of the castable; S2. Vibration compaction into mold: the castable is only cast at the upper wall position, the slag line area uses impact erosion resistant castable, such as mullite high-strength wear-resistant castable JD-M20-65 produced by Changxing Xingying New Refractory Material Co., Ltd., and the main body area uses high-temperature resistant castable, such as high-aluminum high-strength refractory castable JD-16F produced by Changxing Xingying New Refractory Material Co., Ltd. The above three castables are vibrated and compacted together to obtain a complete aluminum furnace casting body; S3, curing and demoulding: the curing operation is carried out in the curing kiln, the maximum temperature in the kiln is 450℃, and the overall curing time is 22h; S4. Natural drying: time is 3 days.

[0042] Example 2 As attached Figure 1 , 2 As shown, a castable used in the upper wall of an aluminum melting furnace, the raw material composition of which is the following components by weight: Coarse aggregate corundum 46%, coarse aggregate silicon carbide 31%, fine aggregate silicon carbide 13%, alumina powder 5%, phosphate binder 3.0%, stainless steel explosion-proof fiber 0.6%, thermal conductive fiber 0.20%, and the balance is 1.2% of additives.

[0043] The particle size of the coarse aggregate corundum is 3.5-4.7 mm, the particle size of the coarse aggregate silicon carbide is 3.6-6.8 mm, the particle size of the fine aggregate silicon carbide is 0.7-1.0 mm, and the particle size of the alumina powder is 4.2-5.4 μm.

[0044] Wherein, the phosphate binder is aluminum phosphate, the thermal conductive fiber is silicon carbide fiber, the length of the silicon carbide fiber is 7.4-11.2 mm, and the diameter is 0.10-0.11 mm.

[0045] The additives are polycarboxylic acid-based high-efficiency water reducing agent, acrylic emulsion anti-stripping agent, and calcium chloride coagulant.

[0046] The preparation method of the castable comprises the following steps in sequence: T1. Mixing: Add all the coarse aggregate corundum, coarse aggregate silicon carbide, fine aggregate silicon carbide, alumina powder, phosphate binder, stainless steel explosion-proof fiber, thermal conductive fiber, and additives into a mixer and mix for 12 minutes to obtain a mixture; T2. Bag filling: bag the mixture to obtain the final castable product.

[0047] The method for using the castable comprises the following steps in sequence: S1. Add water and stir: the weight of water added is 5.5% of the weight of the castable; S2. Vibration compaction into mold: the castable is only cast at the upper wall position, the slag line area uses impact erosion resistant castable, such as mullite high-strength wear-resistant castable JD-M20-65 produced by Changxing Xingying New Refractory Material Co., Ltd., and the main body area uses high-temperature resistant castable, such as high-aluminum high-strength refractory castable JD-16F produced by Changxing Xingying New Refractory Material Co., Ltd. The above three castables are vibrated and compacted together to obtain a complete aluminum furnace casting body; S3, curing and demoulding: the curing operation is carried out in the curing kiln, the maximum temperature in the kiln is 500℃, and the overall curing time is 24h; S4. Natural drying: time is 2 days.

[0048] Example 3 As attached Figure 1 , 2 As shown, a castable used in the upper wall of an aluminum melting furnace, the raw material composition of which is the following components by weight: Coarse aggregate corundum 45.5%, coarse aggregate silicon carbide 31%, fine aggregate silicon carbide 14%, alumina powder 5%, phosphate binder 2.5%, stainless steel explosion-proof fiber 0.6%, thermal conductive fiber 0.22%, and the balance is 1.18% of additives.

[0049] The particle size of the coarse aggregate corundum is 3.5-4.1 mm, the particle size of the coarse aggregate silicon carbide is 5.2-5.7 mm, the particle size of the fine aggregate silicon carbide is 0.7-1.1 mm, and the particle size of the alumina powder is 4.7-5.3 μm.

[0050] Wherein, the phosphate binder is magnesium phosphate, the thermal conductive fiber is ceramic fiber, the length of the ceramic fiber is 6.1-9.9 mm, and the diameter is 0.11-0.12 mm.

[0051] The additives are aminosulfonate water reducer, zircon antioxidant, acrylic emulsion anti-stripping agent, and sodium sulfate coagulant.

[0052] The preparation method of the castable comprises the following steps in sequence: T1. Mixing: Add all the coarse aggregate corundum, coarse aggregate silicon carbide, fine aggregate silicon carbide, alumina powder, phosphate binder, stainless steel explosion-proof fiber, thermal conductive fiber, and additives into a mixer and mix for 15 minutes to obtain a mixture; T2. Bag filling: bag the mixture to obtain the final castable product.

[0053] The method for using the castable comprises the following steps in sequence: S1. Add water and stir: the weight of water added is 7% of the weight of the castable; S2. Vibration compaction into mold: the castable is only cast at the upper wall position, the slag line area uses impact erosion resistant castable, such as mullite high-strength wear-resistant castable JD-M20-65 produced by Changxing Xingying New Refractory Material Co., Ltd., and the main body area uses high-temperature resistant castable, such as high-aluminum high-strength refractory castable JD-16F produced by Changxing Xingying New Refractory Material Co., Ltd. The above three castables are vibrated and compacted together to obtain a complete aluminum furnace casting body; S3, curing and demoulding: the curing operation is carried out in the curing kiln, the maximum temperature in the kiln is 550℃, and the overall curing time is 22h; S4. Natural drying: time is 2 days.

[0054] Comparative Example 1 The castable in this comparative example has only one difference from Example 1 in terms of raw material composition and preparation method: The coarse aggregate silicon carbide and the fine aggregate silicon carbide are replaced by the coarse aggregate mullite and the fine aggregate mullite respectively, wherein the particle size of the coarse aggregate mullite is 3.7-8.8 mm, and the particle size of the fine aggregate mullite is 0.5-1.0 mm.

[0055] Comparative Example 2 The castable in this comparative example has only one difference from Example 1 in terms of raw material composition and preparation method: The stainless steel explosion-proof fiber is replaced with an equal weight of alumina micro powder.

[0056] Comparative Example 3 The castable in this comparative example has only one difference from Example 1 in terms of raw material composition and preparation method: The thermal conductive fiber was replaced with an equal weight of alumina powder.

[0057] Comparative Example 4 The castable in this comparative example has only the following three differences in raw material composition and preparation method compared with Example 1: 1. Replace the coarse aggregate silicon carbide and the fine aggregate silicon carbide with coarse aggregate mullite and fine aggregate mullite respectively, wherein the particle size of the coarse aggregate mullite is 3.7-8.8 mm, and the particle size of the fine aggregate mullite is 0.5-1.0 mm; 2. Replace the stainless steel explosion-proof fiber with an equal weight of alumina powder; 3. Replace the thermal conductive fiber with an equal weight of alumina powder.

[0058] Comparative Example 5 The castable in this comparative example has only one difference from Example 1 in terms of raw material composition and preparation method: The amount of additives was adjusted from 0.20% for thermal conductive fiber and 3.8% for balance to 1.20% for thermal conductive fiber and 2.8% for balance.

[0059] Performance Testing A total of 8 castable products in the above 3 embodiments and 5 comparative examples were subjected to 5 medium temperature strength tests and 5 high temperature strength tests respectively, and the average value was finally taken and recorded in the attached Figure 1 The test method is: After adding water to the castable and stirring, it was injected into a 40mm×40mm×160mm mold and vibrated to be dense. The sample was demoulded after 24 hours and then placed in an oven to dry at 110℃×24h. The dried sample was then calcined at 800℃×3h and 1400℃×3h, respectively. The calcined sample was then subjected to medium-temperature strength and high-temperature strength tests.

[0060] A total of 8 castable products in the above 3 embodiments and 5 comparative examples were subjected to 3 water quenching tests respectively, and the average value was finally taken and recorded in the attached Figure 1 The test method refers to method 2 of GB / T 30873-2014 Test method for thermal shock resistance of refractory materials.

[0061] Casting use On two opposite inner sides of a large natural gas thermal storage aluminum melting furnace, the upper wall castables in Example 1 and Comparative Example 4 were used respectively, and the slag hanging phenomenon was observed. Figure 5 , and attached Figure 3 , 4 shown.

[0062] analyze The upper wall castables in the first and third embodiments all have relatively more outstanding thermal shock resistance, which can be seen from the attached Figure 1 is obtained from the table.

[0063] Second, it is precisely because the upper wall castables in the three embodiments have the prerequisite of relatively outstanding thermal shock resistance, combined with appropriate vertical thermal conductivity and SiO 2 The complete replacement feature ensures that the castable material at the upper wall position in the embodiment has the advantage of not being easy to hang slag, which can be seen from the attached Figure 5 and 3 It can be concluded.

[0064] Third, the three embodiments are first compared with comparative examples 1, 2, and 3, and then compared with comparative example 4. It can be clearly seen that the above-mentioned "relatively outstanding thermal shock resistance, appropriate vertical thermal conductivity, SiO 2 Under the premise of fully combining these three points, an unexpectedly large gain can be obtained, which far exceeds the castable performance of comparative examples 1, 2, and 3 with only two of them.

[0065] Fourth, the thermal conductive fiber content of the castable at the upper wall in Comparative Example 5 obviously exceeds the standard, which ultimately leads to a significant decrease in thermal shock resistance, which is not conducive to the purpose of reducing slag. This also shows that the condition of "0.20-0.22% thermal conductive fiber" is necessary for the effect of preventing slag.

[0066] The above detailed description of the implementation methods of the present application is made in conjunction with the accompanying drawings, but the present application is not limited to the above implementation methods. Various modifications can be made within the knowledge of ordinary technicians in the technical field without departing from the purpose of the present application. These are all non-creative modifications and are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A castable used on the upper wall of an aluminum melting furnace, characterized in that The raw material composition includes the following components: Coarse aggregate corundum, coarse aggregate silicon carbide, fine aggregate silicon carbide, alumina powder, phosphate binder, stainless steel explosion-proof fiber, and thermal conductive fiber.

2. The castable material used in the upper wall of an aluminum melting furnace according to claim 1, characterized in that: The particle size of the coarse aggregate corundum is 2.0-5.5 mm, the particle size of the coarse aggregate silicon carbide is 3.5-7.0 mm, the particle size of the fine aggregate silicon carbide is 0.5-1.2 mm, and the particle size of the alumina powder is 3.0-6.0 μm.

3. The castable material used in the upper wall of an aluminum melting furnace according to claim 1, characterized in that: The phosphate binder is any one of aluminum phosphate, aluminum dihydrogen phosphate, magnesium phosphate, and zinc phosphate, or a mixture of several of them.

4. The castable material used in the upper wall of an aluminum melting furnace according to claim 1, characterized in that: The thermal conductive fiber is any one of aluminum oxide fiber, silicon carbide fiber, copper fiber, ceramic fiber, and boron nitride fiber, or a mixture of several thereof. The length of the thermal conductive fiber is 5.0-12.0 mm, and the diameter is 0.10-0.14 mm.

5. The castable material for use on the upper wall of an aluminum melting furnace according to claim 1, characterized in that The raw material composition is the following components by weight: 44-47% of coarse aggregate corundum, 30-35% of coarse aggregate silicon carbide, 11-15% of fine aggregate silicon carbide, 3-5% of alumina powder, 2.0-3.0% of phosphate binder, 0.5-0.6% of stainless steel explosion-proof fiber, 0.20-0.22% of thermal conductive fiber, and the balance is additives.

6. The castable material used in the upper wall of an aluminum melting furnace according to claim 5, characterized in that: The additive is any one of a water reducing agent, an antioxidant, an anti-stripping agent, and a coagulant or a mixture of several of them.

7. The castable material used in the upper wall of an aluminum melting furnace according to claim 1, characterized in that: The pouring range of the castable is the upper 15-20% height area of ​​the inner wall of the aluminum melting furnace, or above the slag line area of ​​the aluminum melting furnace, wherein the height difference between the upper and lower edges of the slag line area is 5.0-8.0 cm.

8. A method for using the castable material for the upper wall of an aluminum melting furnace as claimed in claim 7, characterized in that The following steps are included in sequence: S1, add water and stir; S2, compaction into mold; S3, curing and demoulding; S4. Dry naturally.

9. The method for using the castable material used at the upper wall of an aluminum melting furnace according to claim 8, characterized in that: In S1, the added weight of water is 5-7% of the castable weight.

10. The method for using the castable material used at the upper wall of an aluminum melting furnace according to claim 8, characterized in that: In S2, the castable is only cast at the upper wall position, and the refractory castable used in the slag line area and the main body area of ​​the aluminum melting furnace is vibrated and compacted together with the castable to obtain a complete aluminum melting furnace casting body.

Citation Information

Patent Citations

  • Castable for aluminum melting furnace lining and preparation method and using method of castable

    CN109336627A