Corrosion-resistant aluminum material for automobile and preparation method of corrosion-resistant aluminum material

By using a composite reinforcement system of cerium-loaded alumina nanorods and scandium/boron nitride nanotubes in aluminum alloys, the problem of aluminum alloys being easily corroded in high humidity, high salt spray and complex working conditions is solved, and the mechanical properties and corrosion resistance of aluminum are synchronized.

CN120082778AActive Publication Date: 2025-06-03ZHAOQING XINLIANCHANG METAL IND CO LTD

Patent Information

Application Number
CN202510250508.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-04
Publication Date
2025-06-03
Estimated Expiration
2045-03-04

AI Technical Summary

Technical Problem

Existing aluminum alloys are susceptible to corrosion in high humidity, high salt spray and complex working conditions, resulting in mechanical properties decay and shortened service life. They are prone to interface peeling or microcracking propagation in high stress environments, affecting the overall performance stability.

Method used

A composite reinforcement system of cerium oxide-loaded alumina nanorods and scandium/boron nitride nanotubes was used to synthesize alumina nanorods by hydrothermal method and load cerium oxide nanoparticles on the surface to form a duplex composite reinforcement system. At the same time, the nanoscale Al3Sc precipitated phase is generated by the synergistic action of the scandium nanolayer and the aluminum matrix to form a co-categorical interface to enhance material strength and corrosion resistance.

Benefits of technology

The mechanical properties and corrosion resistance of aluminum are synchronously improved, which is better than the existing single reinforcement system, enhances the stable combination of phase and matrix, and improves the stability and comprehensive performance of the material in high temperature and high stress environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120082778A_ABST
    Figure CN120082778A_ABST
Patent Text Reader

Abstract

The invention relates to the field of aluminum materials, and provides an automobile corrosion-resistant aluminum material and a preparation method thereof.The automobile corrosion-resistant aluminum material is prepared from cerium oxide loaded aluminum oxide nanorods, scandium / boron nitride nanotubes, zirconium powder, magnesium powder, copper powder, manganese powder, silicon carbide nanoparticles, TiB2 nanoparticles, aluminum powder and stearic acid. Wherein the cerium oxide loaded aluminum oxide nanorod is composed of an aluminum oxide nanorod and cerium oxide nanoparticles loaded on the surface of the aluminum oxide nanorod, and the scandium / boron nitride nanotube is composed of a boron nitride nanotube and a scandium nanolayer uniformly coated on the surface of the boron nitride nanotube. The material is prepared through mechanical ball milling, cold isostatic pressing forming, vacuum sintering and aging treatment, and finally the aluminum-based composite material containing the Al3Sc nano precipitated phase and the boron nitride nanotube reinforced phase is formed. And an Al3Sc precipitated phase and an aluminum matrix form a coherent interface, so that the strength, the corrosion resistance and the wear resistance of the material are improved. Through nanostructure optimization, high performance of the aluminum alloy is achieved, and the aluminum alloy is suitable for the fields of automobiles, aerospace and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of aluminum materials, and particularly to a corrosion-resistant aluminum material for automobiles and a preparation method thereof. Background Art

[0002] In the fields of automobiles, aerospace, and high-end manufacturing, aluminum alloys are widely used in structural components and load-bearing parts due to their excellent specific strength, good processability, and lightweight characteristics. However, in high-humidity, high-salt spray, and complex working condition environments, traditional aluminum alloys are easily eroded by corrosive media, resulting in the decline of material mechanical properties and the shortening of service life. At the same time, vehicles and aircrafts are subjected to complex alternating loads during operation, requiring the material to have excellent fatigue resistance and wear resistance to ensure the stability of long-term service. Therefore, developing an aluminum-based composite material with high corrosion resistance, high strength, and excellent wear resistance is of great significance for improving the safety of the whole vehicle, extending the service life, and reducing maintenance costs. In recent years, the introduction of nano-reinforcing phases has provided new possibilities for improving the performance of aluminum alloys. Especially through fine microstructure regulation, the interfacial bonding force of the material can be effectively optimized, the stability of the precipitated phases can be strengthened, and the overall mechanical properties can be improved. Therefore, for automotive aluminum alloys, researching high-performance aluminum-based composite materials with excellent corrosion resistance and mechanical properties has become a key technical direction for promoting the development of lightweight and highly reliable equipment.

[0003] Although there are many optimization schemes for aluminum alloys in terms of corrosion resistance and mechanical properties, the existing technologies still have certain limitations. For example, Chinese Patent No. CN107723526A discloses a corrosion-resistant rare-earth aluminum alloy and its preparation method. However, due to the unstable morphology of the strengthening phase, the precipitated phases coarsen during the long-term service of the material, thereby reducing the corrosion resistance and mechanical properties. In addition, another CN patent proposes a method of strengthening the aluminum matrix with nano-ceramic particles. Although the wear resistance and mechanical properties are improved to a certain extent, due to the weak interfacial bonding force between the particles and the matrix, the material is prone to interfacial peeling or microcrack propagation in a high-stress environment, thus affecting the overall performance stability. At the same time, the corrosion resistance of traditional aluminum alloys mainly depends on the optimization of alloying elements. However, in a high-temperature service environment, the corrosion products are prone to spread along the grain boundaries, accelerating the local failure of the material. Therefore, how to ensure the stable combination of the reinforcing phase and the matrix while improving the mechanical properties and further improving the corrosion resistance of the material remains the core challenge in the current research of aluminum-based composite materials. Summary of the Invention

[0004] (1) Technical Problems to be Solved

[0005] The purpose of the present invention is to provide a corrosion-resistant aluminum material for automobiles and a preparation method thereof, so as to solve the problems of insufficient corrosion resistance and mechanical properties of current aluminum materials.

[0006] (2) Technical Solution

[0007] To achieve the above object, the present invention provides the following technical solution:

[0008] A corrosion-resistant aluminum material for automobiles, comprising the following raw materials in parts by weight: 4.0 - 6.0 parts of cerium oxide-supported alumina nanorods, 1.5 - 3.5 parts of scandium / boron nitride nanotubes, 0.2 - 0.5 parts of zirconium powder, 1.0 - 1.5 parts of magnesium powder, 0.5 - 1.0 parts of copper powder, 0.2 - 0.5 parts of manganese powder, 2.0 - 4.0 parts of silicon carbide nanoparticles, 0.2 - 0.4 parts of TiB2 nanoparticles, 85.0 - 90.0 parts of aluminum powder, and 0.2 - 0.6 parts of stearic acid;

[0009] The cerium oxide-supported alumina nanorods are composed of alumina nanorods and cerium oxide nanoparticles supported on the surface of the alumina nanorods;

[0010] The scandium / boron nitride nanotubes are composed of boron nitride nanotubes and scandium nanolayers uniformly distributed on the surface of the boron nitride nanotubes;

[0011] Furthermore, the average diameter of the cerium oxide-supported alumina nanorods is 20 - 60 nm, and the average length is 2.0 - 10.0 μm.

[0012] Furthermore, the volume fraction of the cerium oxide nanoparticles and the alumina nanorods is (24.5 - 35.0):(65.0 - 75.5).

[0013] Furthermore, the preparation method of the cerium oxide-supported alumina nanorods is as follows: in parts by weight, dissolve 2.0 - 5.0 parts of Ce(NO3)3·6H3O in 100 parts of ethanol solution, add 5 - 10 parts of alumina nanorods, after ultrasonic dispersion for 30 - 60 min, dropwise add ammonia water to adjust the pH to 8 - 10, continue stirring for 2 - 4 h, then let it stand for 6 - 12 h. After standing, dry the alumina nanorods loaded with the CeO2 precursor at 80 - 120 °C for 6 - 12 h, and finally calcine at 400 - 600 °C for 120 - 240 min to finally obtain the cerium oxide-supported alumina nanorods.

[0014] Furthermore, the preparation method of the aluminum oxide nanorods is as follows: by weight, 10 to 20 parts of aluminum nitrate are dissolved in 100 to 200 parts of deionized water, stirred for 30 to 60 minutes, then 0.5 to 2.0 parts of hexamethylenetetramine and 0.1 to 0.5 parts of urea are added to the solution, stirring is continued for 10 to 30 minutes, and then the solution is transferred to a hydrothermal reactor, reacted at 160 to 200° C. for 6 to 12 hours, after the hydrothermal reaction is completed, the product is centrifuged at 6000 to 10000 rpm for 10 to 15 minutes, and then the precipitate is taken out and washed with deionized water for 3 to 5 times, then dried at 80 to 120° C. for 6 to 12 hours, and then the dried powder is calcined at 500 to 600° C. for 120 to 180 minutes, and then ground to obtain aluminum oxide nanorods after cooling to room temperature.

[0015] The present invention adopts the design of cerium oxide loaded alumina nanorods to enhance the synergistic enhancement performance of the mechanical properties and corrosion resistance of aluminum materials. The alumina nanorods synthesized by the hydrothermal method have a high aspect ratio structural feature, and the surface of the alumina nanorods is loaded with cerium oxide nanoparticles through a cerium nitrate precursor to form a two-phase composite reinforcement system. The alumina nanorods as a rigid skeleton can effectively improve the deformation resistance of the aluminum matrix, and the cerium oxide nanoparticles can form a dynamic repair type passivation film in a corrosive environment by virtue of their unique redox characteristics, inhibiting the development of pitting and intergranular corrosion. The two realize interface matching through volume fraction regulation, and the synergistic effect of cerium oxide and alumina not only optimizes the dispersibility of the nano-reinforcement phase in the aluminum matrix, but also improves the load bearing efficiency of the composite material through the stress transfer mechanism. In the preparation process, the synergistic hydrolysis of hexamethylenetetramine and urea regulates the crystal orientation growth of the alumina nanorods, and the controllable hydrolysis of cerium nitrate under alkaline conditions realizes the uniform anchoring of cerium oxide nanoparticles on the surface of alumina. During the calcination process, the two-phase interface is reconstructed by oxygen vacancies to form chemical bonding, further strengthening the bonding strength of the heterogeneous interface. This multi-scale composite structure design enables the aluminum matrix to achieve uniform stress distribution when subjected to mechanical loads. At the same time, a continuous protective layer is formed in the corrosive medium through the electron migration characteristics of cerium oxide, ultimately achieving simultaneous improvement in the mechanical properties and corrosion resistance of the material.

[0016] Furthermore, the average diameter of the scandium / boron nitride nanotubes is 35 to 80 nm; and the average thickness of the scandium nanolayer is 10 to 20 nm.

[0017] Furthermore, the preparation method of the scandium / boron nitride nanotube is as follows: First, the boron nitride nanotube is subjected to hydrothermal reaction in an aqueous hydrogen peroxide solution with a concentration of 30-50 vol% at 60-80 °C for 2-6 h to achieve surface hydroxylation. Subsequently, a precursor solution containing 0.1-0.5 mol / L scandium nitrate and 0.1-0.5 wt% polyvinylpyrrolidone is prepared, and the pH is adjusted to 8.0-10.0 with ammonia water to form a Sc(OH)₂ colloidal suspension; the functionalized nanotubes are dispersed in the suspension at a mass ratio of 1:(50-200), and treated for 12-36 h under the synergistic action of 200-500 W ultrasonic wave and 300-600 rpm mechanical stirring, and then the precipitate is collected by filtration; then a multi-stage reduction and calcination process is adopted: the completely dried precipitate is heated to 400-450 °C at a rate of 1-2 °C / min in a pure N₂ atmosphere, switched to a 5 vol% H₂ / Ar mixed gas and continued to be heated to 600-620 °C, and finally kept at 700-800 °C for 3-5 h in a 20 vol% H₂ / Ar atmosphere, and after the treatment, it is cooled to room temperature in the furnace to obtain the scandium / boron nitride nanotube.

[0018] Furthermore, the preparation method of the boron nitride nanotube is as follows: By weight, 1.0-3.0 parts of Fe₂O₃, 1.0-3.0 parts of MgO and 5.0-9.5 parts of amorphous boron powder are weighed and mixed evenly, and then ball-milled for 2-4 h to form a uniform powder. Then the uniform powder is put into a chemical vapor deposition furnace and reacted at 1100-1400 °C for 120-180 min to form a crude product of boron nitride nanotube. After cooling to room temperature, the crude product is immersed in a sufficient amount of 1.0-3.0 mol / L hydrochloric acid solution for 24-30 h. After the immersion is completed, the precipitate is filtered and retained, then washed 3-5 times with deionized water, and finally dried at 100-200 °C for 6-12 h to obtain the boron nitride nanotube.

[0019] Furthermore, the microstructure of the corrosion-resistant aluminum alloy contains an Al₃Sc precipitation phase; the volume fraction of the Al₃Sc precipitation phase is 2.5-5.0 vol.%; the average size of the Al₃Sc precipitation phase is 8-30 nm; the interface between the Al₃Sc precipitation phase interface and the Al matrix is a coherent interface.

[0020] Furthermore, the microstructure of the corrosion-resistant aluminum alloy contains boron nitride nanotubes and an Al₃Sc precipitation phase distributed on the surface of the boron nitride nanotubes; the Al₃Sc precipitation phase is formed by the reaction of the scandium nanolayer on the surface of the scandium / boron nitride nanotube and the Al matrix at high temperature; the interface between the Al₃Sc precipitation phase and the Al matrix is a coherent interface.

[0021] Through the synergistic effect of the scandium / nanoscale scandium layer on the surface of boron nitride nanotubes and the aluminum matrix, a corrosion-resistant and high-temperature stable composite reinforcement system is constructed. The nanoscale scandium layer reacts with aluminum during high-temperature sintering to form nanoscale Al3Sc precipitation phases. The coherent interface characteristics thereof significantly improve the material strength by pinning dislocations and refining grains, while suppressing the high-temperature interface reaction between the boron nitride nanotubes and the aluminum matrix. The Al3Sc phase forms a continuous coating layer on the surface of boron nitride, blocking the erosion of the aluminum melt and maintaining the high-temperature structural stability by virtue of its high melting point characteristics. The chemical inertness of the boron nitride nanotubes combined with the preferential oxidation characteristics of scandium form a passivation film, constructing a double barrier for the corrosive medium. During the preparation, the surface hydroxylation and multistage reduction calcination processes precisely control the uniformity of the scandium layer, and the Fe2O3 / MgO catalytic system and hydrochloric acid purification ensure the structural integrity of boron nitride, ultimately realizing the multifunctional synergy of mechanical strengthening, corrosion resistance improvement, and high-temperature protection.

[0022] The present invention also discloses a preparation method for corrosion-resistant aluminum materials for automobiles, comprising the following steps:

[0023] S1. Weigh the raw materials by weight parts and place them in a V-type mixer, and perform mechanical ball milling under argon protection, with a dry mixing at a rotation speed of 150-250 rpm for 1.5-2.5 hours; the ball-to-material ratio for ball milling is (8-12):1. After loading the mixed powder into a mold, perform cold isostatic pressing at a pressure of 180-220 MPa for 15-20 min to obtain a green body preform.

[0024] S2. Place the formed compact in a vacuum sintering furnace, and gradually heat it to 550-580 °C at a heating rate of 5-10 °C / min for solid-phase sintering in a vacuum environment of 0.01-0.1 Pa, and maintain this temperature for 2-5 h. Subsequently, continue to heat it to 600-620 °C for liquid-phase assisted sintering and maintain it for 60-90 min. After sintering is completed, cool it to room temperature with the furnace under argon protection to finally obtain a densified aluminum alloy blank.

[0025] S3. Then place the aluminum alloy blank in an environment of 115-125 °C for a first-stage aging treatment for 7-9 hours, and then heat it to 150-170 °C for a second-stage aging treatment for 3-5 hours, and cool it to room temperature with the furnace after the treatment.

[0026] The present invention adopts the design of multi-stage sintering and aging process mainly to enhance the structural density and comprehensive performance of corrosion-resistant aluminum materials for automobiles, and optimizes the material performance through the coordinated control of the whole process of ball milling mixing-cold pressing-gradient sintering-graded aging. Mechanical ball milling achieves uniform dispersion of nano-reinforced phase and metal powder through the synergistic effect of shear force and impact force under argon protection, and the preform formed by cold isostatic pressing has low porosity and high structural uniformity, laying the foundation for subsequent sintering. In the gradient sintering process, the solid phase sintering stage realizes the neck growth between particles through atomic diffusion, the liquid phase sintering stage uses the molten flow of low melting point components to fill the pores and promote densification, and the vacuum environment and argon cooling synergistically suppress oxidation defects. The graded aging treatment promotes the gradient regulation of the distribution of Al3Sc precipitation phase inside the matrix through low temperature-high temperature dual-stage temperature control, forms high-density crystal nuclei in the low temperature stage, and optimizes the size of the precipitation phase in the high temperature stage. The synergistic effect of the coherent interface and boron nitride nanotubes simultaneously improves the material strength and corrosion resistance. During the preparation process, the matching design of ball milling parameters and sintering curve ensures the structural integrity of the reinforcement phase. The coupling of the aging temperature sequence and the phase transformation dynamics of the aluminum matrix realizes the precise control of the precipitated phase morphology, and finally forms a multi-level reinforcement system of dense matrix-nano-reinforcement phase-coherent interface.

[0027] (3) Beneficial technical effects

[0028] 1. The present invention achieves the simultaneous improvement of the mechanical properties and corrosion resistance of aluminum materials through the synergistic reinforcement design of cerium oxide loaded alumina nanorods, which is superior to the existing single reinforcement system. Alumina nanorods serve as a rigid skeleton to improve the deformation resistance of the aluminum matrix, while cerium oxide nanoparticles dynamically generate a passivation film in a corrosive environment by virtue of their redox characteristics, inhibiting pitting and intergranular corrosion. The volume fractions of the two are optimized to ensure interface matching, and the load-bearing efficiency is improved through the stress transfer mechanism. During the preparation process, hexamethylenetetramine and urea synergistically regulate the crystallization orientation of alumina nanorods, cerium nitrate is hydrolyzed to achieve uniform anchoring of cerium oxide, and calcination induces oxygen vacancy reconstruction to enhance interface bonding. The multi-scale composite structure optimizes stress distribution and constructs an electron migration protection layer, so that the material has both high strength and corrosion resistance, and is suitable for aerospace, automotive and marine engineering fields.

[0029] 2. The present invention constructs a corrosion-resistant and high-temperature stable composite reinforcement system through the synergistic effect of scandium / boron nitride nanotubes, breaking through the limitations of the prior art in the high-temperature stability of the aluminum matrix and the control of interface reactions. The scandium nanolayer generates a nanoscale Al3Sc precipitation phase during high-temperature sintering, forming a coherent interface, pinning dislocations and refining grains, improving material strength, and inhibiting the interface reaction between boron nitride and aluminum. The Al3Sc phase coats the boron nitride to block the erosion of the aluminum melt, and combines the chemical inertness of boron nitride and the preferential oxidation characteristics of scandium to construct a double barrier to corrosive media. Hydroxylation and multi-stage reduction calcination accurately control the uniformity of the scandium layer, and Fe2O3 / MgO catalysis and hydrochloric acid purification maintain the structural integrity of the boron nitride nanotubes, achieving multifunctional synergy of mechanical strengthening, corrosion resistance improvement and high-temperature protection, and enhancing the application value of aluminum alloys in aerospace, high-temperature structural parts and other fields.

[0030] 3. The present invention optimizes the structural density and comprehensive performance of aluminum materials through multi-stage sintering and aging processes, which is superior to the existing technology. Ball milling mixing ensures uniform dispersion of the nano-reinforcement phase, cold pressing reduces porosity, and gradient sintering combines solid and liquid phase sintering to achieve high densification and inhibit oxidation defects. Graded aging accurately controls the Al3Sc precipitation phase, combined with boron nitride nanotubes to improve strength and corrosion resistance. Optimize the matching of ball milling parameters and sintering curves, construct a multi-stage strengthening system of matrix-reinforcement phase-coherent interface, improve service life, reduce maintenance costs, and promote the application of high-performance aluminum materials in automobile manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a morphology picture of the aluminum oxide nanorods prepared in Example 1 of the present invention.

[0032] Figure 2 This is the XRD phase analysis diagram of the aluminum oxide nanorods prepared in Example 1 of the present invention.

[0033] Figure 3 This is a morphology picture of the cerium oxide-loaded aluminum oxide nanorods prepared in Example 1 of the present invention.

[0034] Figure 4 This is the XRD phase analysis diagram of the cerium oxide-loaded aluminum oxide nanorods prepared in Example 1 of the present invention.

[0035] Figure 5 This is a morphology diagram of the boron nitride nanotubes prepared in Example 1 of the present invention.

[0036] Figure 6 This is the XRD phase analysis diagram of the boron nitride nanotubes prepared in Example 1 of the present invention.

[0037] Figure 7 This is a morphology picture of the scandium / boron nitride nanotubes prepared in Example 1 of the present invention.

[0038] Figure 8 XRD phase analysis diagram of scandium / boron nitride nanotubes prepared in Example 1 of the present invention.

[0039] Figure 9 Interface morphology diagram of the microstructure of the aluminum material prepared in Example 1 of the present invention. Detailed implementation manners

[0040] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings in the embodiments of the present invention.

[0041] Example 1

[0042] A corrosion-resistant aluminum material for automobiles, comprising the following raw materials in parts by weight: 4.0 parts of cerium oxide-supported alumina nanorods, 1.5 parts of scandium / boron nitride nanotubes, 0.2 part of zirconium powder, 1.0 part of magnesium powder, 0.5 part of copper powder, 0.2 part of manganese powder, 2.0 parts of silicon carbide nanoparticles, 0.2 part of TiB2 nanoparticles, 85.0 parts of aluminum powder, and 0.2 part of stearic acid;

[0043] The cerium oxide-supported alumina nanorods are composed of alumina nanorods and cerium oxide nanoparticles supported on the surface of the alumina nanorods; the scandium / boron nitride nanotubes are composed of boron nitride nanotubes and scandium nanolayers uniformly distributed on the surface of the boron nitride nanotubes; the average diameter of the cerium oxide-supported alumina nanorods is 20 nm, and the average length is 2.0 μm. The volume fraction of the cerium oxide nanoparticles and the alumina nanorods is 24.5:75.5.

[0044] The preparation method of the cerium oxide-supported alumina nanorods in this example is as follows: in parts by weight, 2.0 parts of Ce(NO3)3·6H2O are dissolved in 100 parts of an ethanol solution, 5 parts of alumina nanorods are added, after ultrasonic dispersion for 30 min, ammonia water is added dropwise to adjust the pH to 8, stirring is continued for 2 h, then left standing for 6 h, after standing, the alumina nanorods loaded with the CeO2 precursor are dried at 80 °C for 6 h, and finally calcined at 400 °C for 120 min to finally obtain the cerium oxide-supported alumina nanorods.

[0045] The preparation method of the alumina nanorods in this example is as follows: in parts by weight, 10 parts of aluminum nitrate are dissolved in 100 parts of deionized water, stirred for 30 min, then 0.5 part of hexamethylenetetramine and 0.1 part of urea are added to the solution, stirring is continued for 10 min, then the solution is transferred to a hydrothermal reaction kettle and reacted at 160 °C for 6 h. After the hydrothermal reaction, the product is centrifuged at 6000 rpm for 10 min, then the precipitate is taken out and washed 3 times with deionized water, then dried at 80 °C for 6 h, and then the dried powder is calcined at 500 °C for 120 min, and ground after cooling to room temperature to obtain the alumina nanorods.

[0046] The average diameter of the scandium / boron nitride nanotubes in this embodiment is 35 nm; the average thickness of the scandium nanolayer is 10 nm.

[0047] The preparation method of the scandium / boron nitride nanotubes in this embodiment is as follows: First, the boron nitride nanotubes are subjected to a hydrothermal reaction in a 30 vol% hydrogen peroxide aqueous solution at 60 °C for 2 h to achieve surface hydroxylation. Subsequently, a precursor solution containing 0.1 mol / L scandium nitrate and 0.1 wt% polyvinylpyrrolidone is prepared, and the pH is adjusted to 8.0 with ammonia water to form a Sc(OH)3 colloidal suspension; the functionalized nanotubes are dispersed in the suspension at a mass ratio of 1:50, and treated under the synergistic action of 200 W ultrasonic and 300 rpm mechanical stirring for 12 h, and then the precipitate is collected by filtration; then a multi-stage reduction and calcination process is adopted: the completely dried precipitate is heated to 400 °C at a rate of 1 °C / min in a pure N2 atmosphere, switched to a 5 vol% H2 / Ar mixed gas and continued to be heated to 600 °C, and finally held at 700 °C for 3 h in a 20 vol% H2 / Ar atmosphere, and after treatment, it is cooled to room temperature in the furnace to obtain scandium / boron nitride nanotubes.

[0048] The preparation method of the boron nitride nanotubes in this embodiment is as follows: By weight, 1.0 part of Fe2O3, 1.0 part of MgO and 5.0 parts of amorphous boron powder are weighed and mixed evenly, and then ball-milled for 2 h to form a uniform powder. Then the uniform powder is put into a chemical vapor deposition furnace and reacted at 1100 °C for 120 min to form a crude product of boron nitride nanotubes. After cooling to room temperature, the crude product is immersed in a sufficient amount of 1.0 mol / L hydrochloric acid solution for 24 h. After the immersion is completed, the precipitate is filtered and retained, then washed 3 times with deionized water, and finally dried at 100 °C for 6 h to obtain boron nitride nanotubes.

[0049] The microstructure of the corrosion-resistant aluminum alloy in this embodiment contains Al3Sc precipitate phases; the volume fraction of the Al3Sc precipitate phases is 2.5 vol.%; the average size of the Al3Sc precipitate phases is 8 nm; the interface between the Al3Sc precipitate phase interface and the Al matrix is a coherent interface; the microstructure of the corrosion-resistant aluminum alloy contains boron nitride nanotubes and Al3Sc precipitate phases distributed on the surface of the boron nitride nanotubes; the Al3Sc precipitate phases are formed by the reaction of the scandium nanolayer on the surface of the scandium / boron nitride nanotubes and the Al matrix at high temperature; the interface between the Al3Sc precipitate phase and the Al matrix is a coherent interface.

[0050] The preparation method of a corrosion-resistant aluminum alloy for automobiles in this embodiment includes the following steps:

[0051] S1. Weigh the raw materials according to the parts by weight and place them in a V-type mixer. Conduct mechanical ball milling under argon protection, and perform dry mixing at a speed of 150 rpm for 1.5 hours. The ball-to-material ratio for ball milling is 8:1. After loading the mixed powder into a mold, perform cold isostatic pressing at a pressure of 180 MPa for 15 minutes to obtain a green body preform.

[0052] S2. Place the formed compact in a vacuum sintering furnace. Under a vacuum environment of 0.01 Pa, gradually heat it at a heating rate of 5 °C / min to 550 °C for solid-phase sintering, and maintain this temperature for 2 h. Subsequently, continue to heat it to 600 °C for liquid-phase assisted sintering, and maintain it for 60 min. After sintering is completed, cool it to room temperature under argon protection to finally obtain a densified aluminum alloy billet.

[0053] S3. Then place the aluminum alloy billet in an environment of 115 °C for the first-stage aging treatment for 7 hours, and then heat it to 150 °C for the second-stage aging treatment for 3 hours. After treatment, cool it to room temperature with the furnace.

[0054] By analyzing the morphology and phase of the material prepared in Example 1, the structure and distribution of the nano-reinforcing phase adopted in the present invention can be demonstrated. Figure 1 and Figure 2 The analysis results show that the alumina nanorods have a clear rod-like morphology and exhibit the phase characteristics of pure alumina. Figure 3 and Figure 4 Further prove that cerium oxide is successfully loaded on the surface of the alumina nanorods, and the phases of both cerium oxide and alumina are verified. Figure 5 and Figure 6 The results show that boron nitride nanotubes (BNNTs) have a typical nanotube morphology and exhibit the phase characteristics of boron nitride. Figure 7 and Figure 8 Further confirm that scandium metal is uniformly distributed on the surface of the boron nitride nanotubes, and the phases of scandium and boron nitride are clearly detected in the XRD analysis. Finally, Figure 9 The microstructure analysis shows that the Al3Sc precipitate phase inside the aluminum material is uniformly distributed on the surface of the BNNTs, proving that the microstructure optimization strategy adopted in the present invention effectively promotes the precipitation of the Al3Sc precipitate phase and enhances the bonding force between the aluminum matrix and the reinforcing phase. These results together verify that the method of the present invention can successfully prepare nano-reinforced aluminum materials and provide a microstructural basis for their excellent comprehensive properties.

[0055] Example 2

[0056] A corrosion-resistant aluminum material for automobiles, comprising the following raw materials in parts by weight: 4.6 parts of cerium oxide-loaded alumina nanorods, 2.1 parts of scandium / boron nitride nanotubes, 0.3 parts of zirconium powder, 1.2 parts of magnesium powder, 0.7 parts of copper powder, 0.3 parts of manganese powder, 2.6 parts of silicon carbide nanoparticles, 0.3 parts of TiB2 nanoparticles, 86.5 parts of aluminum powder, and 0.3 parts of stearic acid;

[0057] The cerium oxide-loaded alumina nanorods are composed of alumina nanorods and cerium oxide nanoparticles loaded on the surface of the alumina nanorods; the scandium / boron nitride nanotubes are composed of boron nitride nanotubes and scandium nanolayers uniformly distributed on the surface of the boron nitride nanotubes; the average diameter of the cerium oxide-loaded alumina nanorods is 32 nm, and the average length is 4.4 μm. The volume fraction of the cerium oxide nanoparticles and the alumina nanorods is 27.7:72.3.

[0058] The preparation method of the cerium oxide-loaded alumina nanorods in this example is as follows: in parts by weight, dissolve 2.9 parts of Ce(NO3)3·6H2O in 100 parts of ethanol solution, add 7 parts of alumina nanorods, after ultrasonic dispersion for 39 min, dropwise add ammonia water to adjust the pH to 8.6, continue stirring for 2.6 h, then let it stand for 7.8 h. After standing, dry the alumina nanorods loaded with the CeO2 precursor at 92 °C for 7.8 h, and finally calcine at 460 °C for 156 min to finally obtain the cerium oxide-loaded alumina nanorods.

[0059] The preparation method of the alumina nanorods in this example is as follows: in parts by weight, dissolve 13 parts of aluminum nitrate in 130 parts of deionized water, stir for 39 min, then add 0.9 parts of hexamethylenetetramine and 0.2 parts of urea to the solution, continue stirring for 16 min, then transfer the solution to a hydrothermal reaction kettle, react at 172 °C for 7.8 h. After the hydrothermal reaction, centrifuge the product at 7200 rpm for 11.5 min, then take out the precipitate and wash it with deionized water 3.6 times, then dry it at 92 °C for 7.8 h, and then calcine the dried powder at 530 °C for 138 min, and grind it to obtain alumina nanorods after cooling to room temperature.

[0060] The average diameter of the scandium / boron nitride nanotubes in this example is 48.5 nm; the average thickness of the scandium nanolayers is 13 nm.

[0061] The preparation method of scandium / boron nitride nanotubes in this embodiment is as follows: First, boron nitride nanotubes are subjected to hydrothermal reaction in 36 vol% hydrogen peroxide aqueous solution at 66 °C for 3.2 h to achieve surface hydroxylation. Subsequently, a precursor solution containing 0.2 mol / L scandium nitrate and 0.2 wt% polyvinylpyrrolidone is prepared, and the pH is adjusted to 8.6 with ammonia water to form a Sc(OH)3 colloidal suspension; the functionalized nanotubes are dispersed in the suspension at a mass ratio of 1:95, and treated under the synergistic action of 290 W ultrasonic and 390 rpm mechanical stirring for 19.2 h, and then the precipitate is collected by filtration; then a multi-stage reduction and calcination process is adopted: the completely dried precipitate is heated to 415 °C at a rate of 1.3 °C / min in a pure N2 atmosphere, switched to a 5 vol% H2 / Ar mixed gas and continued to be heated to 606 °C, and finally kept at 730 °C for 3.6 h in a 20 vol% H2 / Ar atmosphere, and after the treatment, it is cooled to room temperature in the furnace to obtain scandium / boron nitride nanotubes.

[0062] The preparation method of boron nitride nanotubes in this embodiment is as follows: By weight, 1.6 parts of Fe2O3, 1.6 parts of MgO and 6.4 parts of amorphous boron powder are weighed and mixed evenly, and then ball-milled for 2.6 h to form a uniform powder. Then, the uniform powder is put into a chemical vapor deposition furnace and reacted at 1190 °C for 138 min to form a crude product of boron nitride nanotubes. After cooling to room temperature, the crude product is soaked in a sufficient amount of 1.6 mol / L hydrochloric acid solution for 25.8 h. After the soaking is completed, the precipitate is filtered and retained, then washed 3.6 times with deionized water, and finally dried at 130 °C for 7.8 h to obtain boron nitride nanotubes.

[0063] The microstructure of the corrosion-resistant aluminum alloy in this embodiment contains Al3Sc precipitate phase; the volume fraction of the Al3Sc precipitate phase is 3.3 vol.%; the average size of the Al3Sc precipitate phase is 14.6 nm; the interface between the Al3Sc precipitate phase interface and the Al matrix is a coherent interface; the microstructure of the corrosion-resistant aluminum alloy contains boron nitride nanotubes and Al3Sc precipitate phases distributed on the surface of the boron nitride nanotubes; the Al3Sc precipitate phase is formed by the reaction of the scandium nanolayer on the surface of the scandium / boron nitride nanotubes and the Al matrix at high temperature; the interface between the Al3Sc precipitate phase and the Al matrix is a coherent interface.

[0064] The preparation method of a corrosion-resistant aluminum alloy for automobiles in this embodiment includes the following steps:

[0065] S1. Weigh the raw materials by weight and place them in a V-type mixer, and carry out mechanical ball milling under argon protection, and perform dry mixing at a speed of 180 rpm for 1.8 hours; the ball-to-material ratio of the ball milling is 9.2:1. After loading the mixed powder into the mold, cold isostatic pressing is carried out at a pressure of 192 MPa for 16.5 min to obtain a green body preform;

[0066] S2. Place the formed green compact in a vacuum sintering furnace. Under a vacuum environment of 0.037 Pa, gradually heat it to 559 °C at a heating rate of 6.5 °C / min for solid-phase sintering, and maintain this temperature for 2.9 h. Subsequently, continue to heat it to 606 °C for liquid-phase assisted sintering, and maintain it for 69 min. After sintering is completed, cool it to room temperature in the furnace under argon protection to finally obtain a densified aluminum alloy blank.

[0067] S3. Then place the aluminum alloy blank in an environment of 118 °C for the first-stage aging treatment for 7.6 hours, and then heat it to 156 °C for the second-stage aging treatment for 3.6 hours. After treatment, cool it to room temperature in the furnace.

[0068] Example 3

[0069] A corrosion-resistant aluminum material for automobiles, comprising the following raw materials in parts by weight: 5.2 parts of cerium oxide-loaded alumina nanorods, 2.7 parts of scandium / boron nitride nanotubes, 0.4 parts of zirconium powder, 1.3 parts of magnesium powder, 0.8 parts of copper powder, 0.4 parts of manganese powder, 3.2 parts of silicon carbide nanoparticles, 0.3 parts of TiB2 nanoparticles, 88.0 parts of aluminum powder, and 0.4 parts of stearic acid.

[0070] The cerium oxide-loaded alumina nanorods are composed of alumina nanorods and cerium oxide nanoparticles loaded on the surface of the alumina nanorods; the scandium / boron nitride nanotubes are composed of boron nitride nanotubes and scandium nanolayers uniformly distributed on the surface of the boron nitride nanotubes; the average diameter of the cerium oxide-loaded alumina nanorods is 44 nm, and the average length is 6.8 μm. The volume fraction of the cerium oxide nanoparticles and the alumina nanorods is 30.8:69.2.

[0071] The preparation method of the cerium oxide-loaded alumina nanorods in this example is as follows: In parts by weight, dissolve 3.8 parts of Ce(NO3)3·6H2O in 100 parts of ethanol solution, add 8 parts of alumina nanorods, after ultrasonic dispersion for 48 min, dropwise add ammonia water to adjust the pH to 9.2, continue to stir for 3.2 h, and then let it stand for 9.6 h. After standing, dry the alumina nanorods loaded with the CeO2 precursor at 104 °C for 9.6 h, and finally calcine it at 520 °C for 192 min to finally obtain the cerium oxide-loaded alumina nanorods.

[0072] The preparation method of the alumina nanorods in this example is as follows: By weight, dissolve 16 parts of aluminum nitrate in 160 parts of deionized water, stir for 48 min, then add 1.4 parts of hexamethylenetetramine and 0.3 parts of urea to the solution, continue to stir for 22 min, then transfer the solution to a hydrothermal reaction kettle, react at 184 °C for 9.6 h. After the hydrothermal reaction is completed, centrifuge the product at 8400 rpm for 13 min, then take out the precipitate and wash it 4 times with deionized water, then dry it at 104 °C for 9.6 h, and then calcine the dried powder at 560 °C for 156 min. After cooling to room temperature, grind it to obtain alumina nanorods.

[0073] The average diameter of the scandium / boron nitride nanotubes in this example is 62 nm; the average thickness of the scandium nanolayer is 16 nm.

[0074] The preparation method of the scandium / boron nitride nanotubes in this example is as follows: First, subject the boron nitride nanotubes to a hydrothermal reaction in a 42 vol% aqueous hydrogen peroxide solution at 72 °C for 4.4 h to achieve surface hydroxylation. Subsequently, prepare a precursor solution containing 0.3 mol / L scandium nitrate and 0.3 wt% polyvinylpyrrolidone and adjust the pH to 9.2 with ammonia water to form a Sc(OH)3 colloidal suspension; disperse the functionalized nanotubes in the suspension at a mass ratio of 1:140, and treat them under the synergistic action of 380 W ultrasonic waves and 480 rpm mechanical stirring for 26.4 h, then filter and collect the precipitate; then adopt a multi-stage reduction calcination process: heat the completely dried precipitate in a pure N2 atmosphere to 430 °C at a rate of 1.6 °C / min, switch to a 5 vol% H2 / Ar mixed gas and continue to heat to 612 °C, and finally keep it at 760 °C for 4.2 h in a 20 vol% H2 / Ar atmosphere. After the treatment, cool it to room temperature with the furnace to obtain scandium / boron nitride nanotubes.

[0075] The preparation method of the boron nitride nanotubes in this example is as follows: By weight, weigh 2.2 parts of Fe2O3, 2.2 parts of MgO and 7.7 parts of amorphous boron powder, mix them evenly, and ball mill for 3.2 h to form a uniform powder. Then put the uniform powder into a chemical vapor deposition furnace and react at 1280 °C for 156 min to form a crude product of boron nitride nanotubes. After cooling to room temperature, soak the crude product in a sufficient amount of 2.2 mol / L hydrochloric acid solution for 27.6 h. After the soaking is completed, filter and retain the precipitate, then wash it 4 times with deionized water, and finally dry it at 160 °C for 9.6 h to obtain boron nitride nanotubes.

[0076] The microstructure of the corrosion-resistant aluminum alloy in this embodiment contains Al3Sc precipitation phases; the volume fraction of the Al3Sc precipitation phases is 4.0 vol.%; the average size of the Al3Sc precipitation phases is 21.2 nm; the interface between the Al3Sc precipitation phase interface and the Al matrix is a coherent interface; the microstructure of the corrosion-resistant aluminum alloy contains boron nitride nanotubes and Al3Sc precipitation phases distributed on the surface of the boron nitride nanotubes; the Al3Sc precipitation phases are formed by the reaction of scandium / nanoscale scandium layers on the surface of the boron nitride nanotubes with the Al matrix at high temperature; the interface between the Al3Sc precipitation phases and the Al matrix is a coherent interface.

[0077] A method for preparing a corrosion-resistant aluminum alloy for automobiles in this embodiment includes the following steps:

[0078] S1. Weigh raw materials by weight parts and place them in a V-type mixer. Under argon protection, mechanical ball milling is carried out, and dry mixing is carried out for 2.1 hours at a rotation speed of 210 rpm; the ball-to-powder ratio is 10.4:1. After loading the mixed powder into a mold, cold isostatic pressing is carried out at a pressure of 204 MPa for 18 minutes to obtain a green body preform.

[0079] S2. Place the formed compact in a vacuum sintering furnace. Under a vacuum environment of 0.064 Pa, it is gradually heated to 568 °C at a heating rate of 8 °C / min for solid-phase sintering, and this temperature is maintained for 3.8 h. Subsequently, it is continuously heated to 612 °C for liquid-phase assisted sintering, and this is maintained for 78 minutes. After sintering is completed, it is cooled to room temperature with the furnace under argon protection, and finally a densified aluminum alloy blank is obtained.

[0080] S3. Then, place the aluminum alloy blank in an environment of 121 °C for the first-stage aging treatment for 8.2 hours, and then heat it to 162 °C for the second-stage aging treatment for 4.2 hours. After treatment, it is cooled to room temperature with the furnace.

[0081] Example 4

[0082] A corrosion-resistant aluminum alloy for automobiles includes the following raw materials by weight parts: 6.0 parts of cerium oxide-supported alumina nanorods, 3.5 parts of scandium / boron nitride nanotubes, 0.5 part of zirconium powder, 1.5 parts of magnesium powder, 1.0 part of copper powder, 0.5 part of manganese powder, 4.0 parts of silicon carbide nanoparticles, 0.4 part of TiB2 nanoparticles, 90.0 parts of aluminum powder, and 0.6 part of stearic acid;

[0083] The cerium oxide-supported alumina nanorods are composed of alumina nanorods and cerium oxide nanoparticles loaded on the surface of the alumina nanorods; the scandium / boron nitride nanotubes are composed of boron nitride nanotubes and scandium nanolayers uniformly distributed on the surface of the boron nitride nanotubes; the average diameter of the cerium oxide-supported alumina nanorods is 60 nm, and the average length is 10.0 μm. The volume fraction of the cerium oxide nanoparticles and the alumina nanorods is 35.0:65.0.

[0084] The preparation method of the cerium oxide-supported alumina nanorods in this example is as follows: by weight, 5.0 parts of Ce(NO3)3·6H2O are dissolved in 100 parts of ethanol solution, 10 parts of alumina nanorods are added, after ultrasonic dispersion for 60 min, ammonia water is added dropwise to adjust the pH to 10, and stirring is continued for 4 h, then left standing for 12 h. After standing, the alumina nanorods loaded with the CeO2 precursor are dried at 120 °C for 12 h, and finally calcined at 600 °C for 240 min to finally obtain the cerium oxide-supported alumina nanorods.

[0085] The preparation method of the alumina nanorods in this example is as follows: by weight, 20 parts of aluminum nitrate are dissolved in 200 parts of deionized water, stirred for 60 min, then 2.0 parts of hexamethylenetetramine and 0.5 part of urea are added to the solution, and stirring is continued for 30 min. Then the solution is transferred to a hydrothermal reaction kettle and reacted at 200 °C for 12 h. After the hydrothermal reaction, the product is centrifuged at 10000 rpm for 15 min, then the precipitate is taken out and washed 5 times with deionized water, then dried at 120 °C for 12 h, and then the dried powder is calcined at 600 °C for 180 min, and ground after cooling to room temperature to obtain the alumina nanorods.

[0086] The average diameter of the scandium / boron nitride nanotubes in this example is 80 nm; the average thickness of the scandium nanolayers is 20 nm.

[0087] The preparation method of the scandium / boron nitride nanotubes in this example is as follows: First, the boron nitride nanotubes are subjected to a hydrothermal reaction in a 50 vol% hydrogen peroxide aqueous solution at 80 °C for 6 h to achieve surface hydroxylation. Subsequently, a precursor solution containing 0.5 mol / L scandium nitrate and 0.5 wt% polyvinylpyrrolidone is prepared and the pH is adjusted to 10.0 with ammonia water to form a Sc(OH)3 colloidal suspension; the functionalized nanotubes are dispersed in the suspension at a mass ratio of 1:200, and treated under the synergistic action of 500 W ultrasonic and 600 rpm mechanical stirring for 36 h, and then the precipitate is collected by filtration; then a multi-stage reduction calcination process is adopted: the completely dried precipitate is heated to 450 °C at a rate of 2 °C / min in a pure N2 atmosphere, switched to a 5 vol% H2 / Ar mixed gas and continued to be heated to 620 °C, and finally held at 800 °C for 5 h in a 20 vol% H2 / Ar atmosphere, and cooled to room temperature with the furnace after treatment to obtain the scandium / boron nitride nanotubes.

[0088] The preparation method of the boron nitride nanotubes in this embodiment is as follows: by weight, 3.0 parts of Fe2O3, 3.0 parts of MgO and 9.5 parts of amorphous boron powder are weighed and mixed evenly, then ball-milled for 4 h to form a uniform powder. Then, the uniform powder is put into a chemical vapor deposition furnace and reacted at 1400 °C for 180 min to form a crude product of boron nitride nanotubes. After cooling to room temperature, the crude product is immersed in a sufficient amount of 3.0 mol / L hydrochloric acid solution for 30 h. After the immersion is completed, the precipitate is retained by filtration, then washed 5 times with deionized water, and finally dried at 200 °C for 12 h to obtain boron nitride nanotubes.

[0089] The microstructure of the corrosion-resistant aluminum alloy in this embodiment contains Al3Sc precipitate phases; the volume fraction of the Al3Sc precipitate phases is 5.0 vol.%; the average size of the Al3Sc precipitate phases is 30 nm; the interface between the Al3Sc precipitate phases and the Al matrix is a coherent interface; the microstructure of the corrosion-resistant aluminum alloy contains boron nitride nanotubes and Al3Sc precipitate phases distributed on the surfaces of the boron nitride nanotubes; the Al3Sc precipitate phases are formed by the reaction of scandium / nanoscale scandium layers on the surfaces of the boron nitride nanotubes with the Al matrix at high temperature; the interface between the Al3Sc precipitate phases and the Al matrix is a coherent interface.

[0090] A preparation method of a corrosion-resistant aluminum alloy for automobiles in this embodiment includes the following steps:

[0091] S1. Weigh the raw materials by weight and place them in a V-type mixer, and perform mechanical ball milling under argon protection, and perform dry mixing at a rotation speed of 250 rpm for 2.5 h; the ball-to-material ratio of the ball milling is 12:1. After loading the mixed powder into a mold, perform cold isostatic pressing at a pressure of 220 MPa for 20 min to obtain a green body preform.

[0092] S2. Place the formed compact in a vacuum sintering furnace, and gradually heat it to 580 °C at a heating rate of 10 °C / min in a vacuum environment of 0.1 Pa for solid-phase sintering, and maintain this temperature for 5 h. Subsequently, continue to heat it to 620 °C for liquid-phase assisted sintering, and maintain it for 90 min. After the sintering is completed, cool it to room temperature with the furnace under argon protection to finally obtain a densified aluminum alloy blank.

[0093] S3. Then place the aluminum alloy blank in an environment of 125 °C for the first-stage aging treatment for 9 h, and then heat it to 170 °C for the second-stage aging treatment for 5 h, and cool it to room temperature with the furnace after the treatment.

[0094] Comparative Example 1

[0095] Basically the same as Example 1, except that cerium oxide-supported alumina nanorods are removed, and other components and preparation conditions remain unchanged.

[0096] Comparative Example 2

[0097] Basically the same as Example 1, except that the content of cerium oxide-supported alumina nanorods is increased to 7.0 parts, and other components and preparation conditions remain unchanged.

[0098] Comparative Example 3

[0099] Basically the same as Example 1, except that scandium / boron nitride nanotubes are removed, and other components and preparation conditions remain unchanged.

[0100] Comparative Example 4

[0101] Basically the same as Example 1, except that the content of scandium / boron nitride nanotubes is reduced to 1.0 part, and other components and preparation conditions remain unchanged.

[0102] Comparative Example 5

[0103] Basically the same as Example 1, except that cerium oxide is not supported on the surface of cerium oxide-supported alumina nanorods.

[0104] Comparative Example 6

[0105] Basically the same as Example 1, except that scandium is not prepared on the surface of scandium / boron nitride nanotubes.

[0106] Performance test:

[0107] Mechanical property test: The tensile test of aluminum materials was carried out using an electronic universal testing machine. Dumbbell-shaped specimens were prepared according to the standard of GB / T228.1-2021, and tensile tests were carried out at a loading rate of 2 mm / min. The yield strength, tensile strength and elongation at break were recorded to evaluate the mechanical properties of the materials.

[0108] Corrosion resistance test: Potentiodynamic polarization test was carried out using an electrochemical workstation. The samples were immersed in 3.5% NaCl solution, and the self-corrosion potential (Ecorr) and self-corrosion current density (Icorr) were measured at a scanning rate of 5 mV / s to evaluate the corrosion resistance of the materials. At the same time, a salt spray corrosion experiment was carried out. According to the ASTM B117 standard, the samples were exposed in a neutral salt spray environment for 500 h, and the surface corrosion morphology was observed.

[0109] Wear property test: The wear test of aluminum materials was carried out using a pin-on-disc friction and wear testing machine under dry sliding conditions. The normal load was set to 10 N and the rotational speed was set to 200 rpm. The friction coefficient and wear rate were measured to evaluate the wear resistance and tribological behavior of the materials.

[0110] The properties of the aluminum materials in Examples 1 to 4 and Comparative Examples 1 to 6 are summarized in Table 1.

[0111] Table 1 Summary of the properties of the aluminum materials in Examples 1 to 4 and Comparative Examples 1 to 6

[0112]

[0113] The microstructure of the aluminum materials in the examples contains uniformly distributed Al3Sc precipitation phases, which form coherent interfaces with the aluminum matrix and adhere to the surface of scandium / boron nitride nanotubes, promoting grain refinement and strengthening effects. Cerium oxide-loaded alumina nanorods play a strengthening role in the material. Cerium oxide nanoparticles are uniformly attached to the surface of the alumina nanorods, helping to improve the interfacial bonding force and the stability of the material. The scandium / boron nitride nanotubes have good dispersibility, and the scandium nanolayer on their surface can promote the precipitation of the Al3Sc precipitation phase and enhance the coherence of the interface. In the microstructure of the materials in some of the comparative examples, due to the lack of key strengthening phases, the precipitation of the Al3Sc precipitation phase is hindered, resulting in grain coarsening, weakened interfacial bonding force, and even inhomogeneous tissue. In addition, when the alumina nanorods are not loaded with cerium oxide, their strengthening effect weakens and their dispersibility decreases, while when the content is too high, it may lead to an agglomeration effect, affecting the uniformity and stability of the matrix. Generally speaking, by reasonably regulating the content and distribution of cerium oxide-loaded alumina nanorods and scandium / boron nitride nanotubes, the microstructure of the aluminum material can be optimized and its comprehensive performance can be improved.

[0114] Finally, it should be noted that the above examples are only used to illustrate the technical solutions of the present invention and are not intended to limit them. Although the present invention has been described in detail with reference to the above examples, those of ordinary skill in the art should understand that any equivalent structural transformation made under the concept of the present invention by using the content of the specification and drawings of the present invention should be covered within the protection scope of the claims of the present invention.

Claims

1. A corrosion-resistant aluminum material for automobiles, characterized in that: The invention comprises the following raw materials in parts by weight: 4.0-6.0 parts of cerium oxide loaded alumina nanorods, 1.5-3.5 parts of scandium / boron nitride nanotubes, 0.2-0.5 parts of zirconium powder, 1.0-1.5 parts of magnesium powder, 0.5-1.0 parts of copper powder, 0.2-0.5 parts of manganese powder, 2.0-4.0 parts of silicon carbide nanoparticles, 0.2-0.4 parts of TiB2 nanoparticles, 85.0-90.0 parts of aluminum powder, and 0.2-0.6 parts of stearic acid; The cerium oxide-loaded alumina nanorods are composed of alumina nanorods and cerium oxide nanoparticles loaded on the surface of the alumina nanorods; The scandium / boron nitride nanotubes are composed of boron nitride nanotubes and scandium nanolayers uniformly distributed on the surfaces of the boron nitride nanotubes.

2. The corrosion-resistant aluminum material for automobiles according to claim 1, characterized in that: The average diameter of the cerium oxide loaded aluminum oxide nanorods is 20-60 nm, and the average length is 2.0-10.0 μm.

3. The corrosion-resistant aluminum material for automobiles according to claim 1, characterized in that: The volume fractions of the cerium oxide nanoparticles and the aluminum oxide nanorods are (24.5-35.0): (65.0-75.5).

4. The corrosion-resistant aluminum material for automobiles according to claim 1, characterized in that: The preparation method of the cerium oxide loaded alumina nanorods is as follows: by weight, 2.0 to 5.0 parts of Ce(NO3)3·6H2O are dissolved in 100 parts of ethanol solution, 5 to 10 parts of alumina nanorods are added, and after ultrasonic dispersion for 30 to 60 minutes, ammonia water is added dropwise to adjust the pH to 8 to 10, stirring is continued for 2 to 4 hours, and then the solution is allowed to stand for 6 to 12 hours. After the standing is completed, the alumina nanorods loaded with the CeO2 precursor are dried at 80 to 120°C for 6 to 12 hours, and finally calcined at 400 to 600°C for 120 to 240 minutes to finally obtain the cerium oxide loaded alumina nanorods.

5. The corrosion-resistant aluminum material for automobiles according to claim 4, characterized in that: The preparation method of the aluminum oxide nanorods is as follows: by weight, 10 to 20 parts of aluminum nitrate are dissolved in 100 to 200 parts of deionized water, stirred for 30 to 60 minutes, then 0.5 to 2.0 parts of hexamethylenetetramine and 0.1 to 0.5 parts of urea are added to the solution, stirring is continued for 10 to 30 minutes, then the solution is transferred to a hydrothermal reactor, reacted at 160 to 200° C. for 6 to 12 hours, after the hydrothermal reaction is completed, the product is centrifuged at 6000 to 10000 rpm for 10 to 15 minutes, then the precipitate is taken out and washed with deionized water for 3 to 5 times, then dried at 80 to 120° C. for 6 to 12 hours, then the dried powder is calcined at 500 to 600° C. for 120 to 180 minutes, and ground to obtain the aluminum oxide nanorods after cooling to room temperature.

6. The corrosion-resistant aluminum material for automobiles according to claim 1, characterized in that: The average diameter of the scandium / boron nitride nanotubes is 35-80 nm; the average thickness of the scandium nanolayer is 10-20 nm.

7. The corrosion-resistant aluminum material for automobiles according to claim 1, characterized in that: The preparation method of the scandium / boron nitride nanotubes is as follows: firstly, the boron nitride nanotubes are subjected to a hydrothermal reaction at 60-80° C. for 2-6 hours in a 30-50 vol% hydrogen peroxide aqueous solution to achieve surface hydroxylation; then, a precursor solution containing 0.1-0.5 mol / L scandium nitrate and 0.1-0.5 wt% polyvinyl pyrrolidone is prepared and the pH is adjusted to 8.0-10.0 by using ammonia water to form a Sc(OH)3 colloidal suspension; functionalized nanotubes are dispersed in the suspension at a mass ratio of 1:(50-200); and the suspension is heated to 200° C. to obtain a Sc(OH)3 colloidal suspension; and the functionalized nanotubes are ... The mixture is treated under the synergistic effect of 500W ultrasound and 300-600rpm mechanical stirring for 12-36h, and then the precipitate is collected by filtration; followed by a multi-stage reduction calcination process: the completely dried precipitate is heated to 400-450°C at 1-2°C / min in a pure N2 atmosphere, switched to a 5vol% H2 / Ar mixed gas and continued to be heated to 600-620°C, and finally kept at 700-800°C in a 20vol% H2 / Ar atmosphere for 3-5h, and after treatment, cooled to room temperature in the furnace to obtain scandium / boron nitride nanotubes.

8. The corrosion-resistant aluminum material for automobiles according to claim 1, characterized in that: The preparation method of the boron nitride nanotubes is as follows: by weight, 1.0 to 3.0 parts of Fe2O3, 1.0 to 3.0 parts of MgO and 5.0 to 9.5 parts of amorphous boron powder are weighed and mixed evenly, and then ball milled for 2 to 4 hours to form a uniform powder, and then the uniform powder is placed in a chemical vapor deposition furnace, and reacted at 1100 to 1400° C. for 120 to 180 minutes to form a crude product of boron nitride nanotubes, and after cooling to room temperature, the crude product is placed in a sufficient amount of 1.0 to 3.0 mol / L hydrochloric acid solution and soaked for 24 to 30 hours, and after the soaking is completed, the precipitate is filtered and retained, and then washed with deionized water for 3 to 5 times, and finally dried at 100 to 200° C. for 6 to 12 hours to obtain boron nitride nanotubes.

9. The corrosion-resistant aluminum material for automobiles according to claim 1, characterized in that: The corrosion-resistant aluminum material microstructure contains an Al3Sc precipitate phase; the volume fraction of the Al3Sc precipitate phase is 2.5-5.0 vol.%; the average size of the Al3Sc precipitate phase is 8-30 nm; the interface between the Al3Sc precipitate phase interface and the Al matrix is ​​a coherent interface; The corrosion-resistant aluminum material microstructure contains boron nitride nanotubes and Al3Sc precipitate phases distributed on the surface of the boron nitride nanotubes; the Al3Sc precipitate phases are generated by the reaction of the scandium nanolayer on the surface of the scandium / boron nitride nanotubes and the Al matrix at high temperature; the interface between the Al3Sc precipitate phase and the Al matrix is ​​a coherent interface.

10. A method for preparing a corrosion-resistant aluminum material for automobiles as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: S1. The raw materials were weighed in parts by weight and placed in a V-type mixer, mechanically ball-milled under argon protection, and dry-mixed at a speed of 150 to 250 rpm for 1.5 to 2.5 hours; the ball-to-material ratio was (8 to 12): 1, and the mixed powder was loaded into a mold and cold isostatically pressed at a pressure of 180 to 220 MPa for 15 to 20 min to obtain a green preform; S2. The formed green compact is placed in a vacuum sintering furnace, and is gradually heated to 550-580°C at a heating rate of 5-10°C / min for solid phase sintering under a vacuum environment of 0.01-0.1 Pa, and the temperature is maintained for 2-5 hours. Subsequently, the temperature is continued to be raised to 600-620°C for liquid phase assisted sintering, and the temperature is maintained for 60-90 minutes. After sintering, the green compact is cooled to room temperature with the furnace under argon protection, and finally a densified aluminum alloy green compact is obtained; S3. Then, the aluminum alloy blank is placed in an environment of 115-125°C for 7-9 hours of first aging treatment, and then the temperature is raised to 150-170°C for 3-5 hours of second aging treatment, and then the blank is cooled to room temperature in the furnace.

Citation Information

Patent Citations

  • Preparing method of rare earth oxide@graphene nanoplate / aluminum base blank

    CN111363942A

  • Aluminum sliding member, and its production method

    JP2005015827A

  • Synthesis of bulk, fully dense nanostructured metals and metal matrix composites

    US20060153728A1

  • Surface Modified Metallic Particulate In Sintered Products

    US20200276643A1

  • Coating for metal alloy

    US20240002983A1

Cited By

  • Preparation method of high-temperature-resistant memory metal for temperature control device

    CN121137440A

  • A method for preparing a high-temperature-resistant memory metal for a temperature control device

    CN121137440B

  • Six-series aluminum alloy material and preparation method thereof

    CN121294918A

  • A six-system aluminum alloy material and a preparation method thereof

    CN121294918B