Organic vapor jet printing system

The single-molecular thick layer of electroluminescent material is formed on the substrate by organic vapor jet printing technology, which solves the problem of uneven deposition of electroluminescent materials in the prior art, achieves efficient and uniform deposition effect, and improves the performance and life of the display.

CN120091744APending Publication Date: 2025-06-03UNIVERSAL DISPLAY CORP
View PDF 36 Cites 0 Cited by

Patent Information

Application Number
CN202411736233.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-11-14
Filing Date
2024-11-29
Publication Date
2025-06-03

AI Technical Summary

Technical Problem

In the prior art, when manufacturing organic emission devices, it is difficult to achieve efficient and uniform electroluminescent material deposition, resulting in uneven thickness of the emission layer, affecting the performance and life of the display.

Method used

Using organic vapor jet printing (OVJP) technology, a single-molecular thick layer of electroluminescent material is formed on the substrate through a vapor deposition system, and a continuous monolayer is formed by chemical reaction with the substrate surface using the vapor precursor.

Benefits of technology

Efficient and uniform electroluminescent material deposition is achieved, the thickness uniformity of the emission layer is improved, and the performance and life of the display is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120091744A_ABST
    Figure CN120091744A_ABST
Patent Text Reader

Abstract

The invention relates to an organic vapor jet printing system. A vapor deposition system is provided that includes an array of deposits in fluid communication with an ambient inert gas, the deposits held in proximity to a substrate carried on a heated vehicle such that the substrate and deposits move relative to each other during deposition. Here, each depositor has one or more delivery holes that eject a gas jet that includes a vapor precursor that chemically reacts with the surface of the substrate to form a single molecule thick layer of an electroluminescent compound on the substrate. Further, each depositor has one or more discharge holes that accumulate a molar flow of gas withdrawn greater than cumulative ejection by the delivery holes in the same depositor.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross - Reference to Related Applications

[0002] This application claims priority to U.S. Provisional Application No. 63 / 605,005, filed on Dec. 1, 2023, which is incorporated herein by reference in its entirety. Technical Field

[0003] The present invention relates to organic vapor jet printing (OVJP) type devices and techniques for manufacturing organic emissive devices, such as organic light emitting diodes, and to devices and techniques including organic emissive devices. Background Art

[0004] For many reasons, optoelectronic devices using organic materials have become increasingly popular. Many of the materials used to make such devices are relatively inexpensive, so organic optoelectronic devices have the potential for cost advantages over inorganic devices. Additionally, the inherent properties of organic materials, such as their flexibility, can make them more suitable for certain applications, such as fabrication on flexible substrates. Examples of organic optoelectronic devices include organic light emitting diodes / devices (OLEDs), organic phototransistors, organic photovoltaic cells, and organic photodetectors. For OLEDs, organic materials can have performance advantages over conventional materials. For example, the wavelength at which the organic emissive layer emits light can generally be easily adjusted with appropriate dopants.

[0005] OLEDs utilize organic thin films that emit light when a voltage is applied across the device. OLEDs are becoming an increasingly attractive technology for applications such as flat panel displays, lighting, and backlighting. Several OLED materials and configurations are described in U.S. Patent Nos. 5,844,363, 6,303,238, and 5,707,745, each of which is incorporated herein by reference in its entirety.

[0006] One application of phosphorescent emissive molecules is full-color displays. Industry standards for such displays require pixels that are suitable for emitting specific colors (referred to as "saturated" colors). Specifically, these standards require saturated red, green, and blue pixels. Alternatively, an OLED can be designed to emit white light. In conventional liquid crystal displays, absorption filters are used to filter the emission from a white backlight to produce red, green, and blue emissions. The same technique can be used for OLEDs. White OLEDs can be single EML devices or stacked structures. CIE coordinates, well known in the art, can be used to measure color.

[0007] As used herein, the term "organic" includes polymeric materials and small molecule organic materials that can be used to fabricate organic optoelectronic devices. "Small molecule" refers to any organic material that is not a polymer, and a "small molecule" may actually be quite large. In some cases, a small molecule may include repeating units. For example, the use of a long-chain alkyl group as a substituent does not remove the molecule from the "small molecule" category. Small molecules can also be incorporated into polymers, such as as a side group on the polymer backbone or as part of the backbone. Small molecules can also be the core part of a dendrimer, which contains a series of chemical shells built on the core part. The core part of the dendrimer can be a fluorescent or phosphorescent small molecule emitter. Dendrimers can be "small molecules", and all dendrimers currently used in the OLED field are considered small molecules.

[0008] As used herein, "top" means furthest from the substrate, and "bottom" means closest to the substrate. Where a first layer is described as "disposed over" a second layer, the first layer is disposed further from the substrate. There may be other layers between the first and second layers unless it is specified that the first layer "contacts" the second layer. For example, even though there are various organic layers between the cathode and the anode, the cathode can still be described as "disposed over" the anode.

[0009] As used herein, "solution processable" means capable of being dissolved, dispersed, or transported in a liquid medium in the form of a solution or suspension and / or deposited from a liquid medium.

[0010] When a ligand is considered to directly contribute to the photosensitive properties of an emissive material, the ligand can be called "photosensitive". When a ligand is not considered to contribute to the photosensitive properties of an emissive material, the ligand can be called "auxiliary", but an auxiliary ligand can modify the properties of a photosensitive ligand.

[0011] As used herein, and as would be generally understood by one of ordinary skill in the art, a first "highest occupied molecular orbital" (HOMO) or "lowest unoccupied molecular orbital" (LUMO) energy level "is greater than" or "is higher than" a second HOMO or LUMO energy level of a first energy level closer to the vacuum energy level. Since the ionization potential (IP) is measured as a negative energy relative to the vacuum energy level, a higher HOMO energy level corresponds to an IP with a smaller absolute value (a less negative IP). Similarly, a higher LUMO energy level corresponds to an electron affinity (EA) with a smaller absolute value (a less negative EA). On a conventional energy level diagram with the vacuum energy level at the top, the LUMO energy level of a material is higher than the HOMO energy level of the same material. A "higher" HOMO or LUMO energy level appears closer to the top of this diagram than a "lower" HOMO or LUMO energy level.

[0012] As used herein, and as would be generally understood by one of ordinary skill in the art, if a first work function has a higher absolute value, then the first work function "is greater than" or "is higher than" a second work function. Since the work function is generally measured as a negative number relative to the vacuum energy level, this means that a "higher" work function is more negative. On a conventional energy level diagram with the vacuum energy level at the top, a "higher" work function is illustrated as being farther from the vacuum energy level in the downward direction. Thus, the definitions of HOMO and LUMO energy levels follow different rules than the work function.

[0013] The present disclosure may describe layers, materials, regions, and devices in reference to the color of the light emitted therefrom. In general, as used herein, an emission region described as producing light of a particular color may include one or more emission layers disposed on top of one another in a stacked arrangement.

[0014] As used herein, a "red" layer, material, region, or device refers to a layer, material, region, or device that emits light in the range of about 580 - 700 nm or has an emission spectrum with a peak in that region. Similarly, a "green" layer, material, region, or device refers to a layer, material, region, or device that emits or has an emission spectrum with a peak wavelength in the range of about 500 - 600 nm; a "blue" layer, material, or device refers to a layer, material, or device that emits or has an emission spectrum with a peak wavelength in the range of about 400 - 500 nm; and a "yellow" layer, material, region, or device refers to a layer, material, region, or device that has an emission spectrum with a peak wavelength in the range of about 540 - 600 nm. In some arrangements, individual regions, layers, materials, regions, or devices can provide separate "dark blue" and "light blue" light. As used herein, in an arrangement that provides separate "light blue" and "dark blue" components, the "dark blue" component refers to a component whose peak emission wavelength is at least about 4 nm less than the peak emission wavelength of the "light blue" component. Generally, the peak emission wavelength of the "light blue" component is in the range of about 465 nm to 500 nm, and the peak emission wavelength of the "dark blue" component is in the range of about 400 nm to 470 nm, but these ranges can vary for some configurations. Similarly, a color - changing layer refers to a layer that converts or modifies light of one color into light having a wavelength specified for that color. For example, a "red" color filter refers to a color filter that forms light having a wavelength in the range of about 580 - 700 nm. Generally, there are two types of color - changing layers: color filters that modify the spectrum by removing non - desired wavelengths of light, and color - changing layers that convert higher - energy photons into lower - energy ones. A "colored" component refers to a component that, when activated or used, generates or otherwise emits light having a specific color as previously described. For example, a "first emission region of a first color" and a "second emission region of a second color different from the first color" describe two emission regions that emit two different colors as previously described when activated within a device.

[0015] As used herein, emissive materials, layers, and regions can be distinguished from each other and from other structures based on the light initially generated by the material, layer, or region, rather than the light ultimately emitted by the same or different structures. Initial light generation is typically the result of a change in energy levels that causes photon emission. For example, an organic emissive material can initially generate blue light, which can be converted into red or green light by a color filter, quantum dots, or other structures, such that the complete emission stack or sub - pixel emits red or green light. In this case, the initial emissive material or layer can be referred to as the "blue" component, even though the sub - pixel is a "red" or "green" component.

[0016] In some cases, it may be preferable to describe the color of a component, such as the color of an emission region, a sub-pixel, a color-changing layer, etc., according to 1931 CIE coordinates. For example, a yellow emissive material may have multiple peak emission wavelengths, one at or near the edge of the "green" region and one at or near the edge within the "red" region, as previously described. Thus, as used herein, each color term also corresponds to a shape in the 1931 CIE coordinate color space. The shape in the 1931 CIE color space is constructed by following the locus between two color points and any other internal points. For example, the internal shape parameters for red, green, blue, and yellow can be defined as follows:

[0017]

[0018] More details regarding OLEDs and the definitions described above can be found in U.S. Patent No. 7,279,704, which is incorporated herein by reference in its entirety. SUMMARY OF THE INVENTION

[0019] According to one embodiment, an organic light emitting diode / device (OLED) is also provided. The OLED may include an anode, a cathode, and an organic layer disposed between the anode and the cathode. According to one embodiment, the organic light emitting device is incorporated into one or more devices selected from consumer products, electronic component modules, and / or lighting panels.

[0020] In one aspect, a vapor deposition system includes an array of depositors in fluid communication with an ambient inert gas, the depositors being maintained near a substrate carried on a heated transport such that the substrate and the depositors move relative to each other during deposition, wherein each depositor has one or more delivery holes that eject a gas jet including a vapor precursor that chemically reacts with the substrate surface to form a monolayer of an electroluminescent compound on the substrate, and wherein each depositor has one or more exhaust holes that cumulatively extract a molar flow rate of gas greater than the cumulative jetting from the delivery holes in the same depositor.

[0021] In one embodiment, the temperature of the substrate surface exceeds the temperature of the depositor.

[0022] In one embodiment, the temperature of the substrate is between 100 °C and 200 °C.

[0023] In one embodiment, the temperature of the substrate is between 60 °C and 180 °C.

[0024] In one embodiment, the pressure of the ambient inert gas is between 20 Torr and 300 Torr.

[0025] In one embodiment, the depositor array is maintained at a distance between 20 μm and 60 μm from the substrate.

[0026] In one embodiment, the delivery orifice or the discharge orifice has a secondary width between 5 μm and 50 μm.

[0027] In one embodiment, each depositor has a width between 40 μm and 400 μm.

[0028] In one embodiment, the vapor precursor comprises a metal-organic compound capable of pyrolysis and chemical bonding to the substrate.

[0029] In one embodiment, the vapor precursor is a transition metal triacetylacetonate.

[0030] In one embodiment, the deposited material adheres to the substrate via one or more of an ether group, a thioether group, and an acetylthio group.

[0031] In one embodiment, the deposited material forms a continuous monolayer on the substrate area acted upon by the depositor.

[0032] In another aspect, an organic vapor jet printing (OVJP) deposition apparatus includes one or more depositors, wherein at least one of the one or more depositors includes one or more delivery orifices; one or more discharge orifices, wherein at least one of the one or more discharge orifices is fluidly coupled to at least one of the one or more delivery orifices; and a substrate, wherein the one or more delivery orifices are configured to eject a gas jet including a vapor precursor onto the substrate, thereby causing a chemical reaction between the vapor precursor and the substrate.

[0033] In one embodiment, the apparatus further includes a heated substrate chuck configured to hold the substrate and provide heat to the substrate.

[0034] In one embodiment, the apparatus is configured to form a monolayer of sorbate on the substrate via a chemical reaction between the vapor precursor and the substrate.

[0035] In one embodiment, the one or more discharge orifices are configured to extract a molar flow rate of gas greater than the molar flow rate of gas ejected by the one or more delivery orifices.

[0036] In one embodiment, the temperature of the substrate is higher than the temperature of the vapor precursor material.

[0037] In another aspect, the temperature of the substrate is between 100 °C and 200 °C.

[0038] In one embodiment, the temperature of the substrate is between 60 °C and 180 °C.

[0039] In one embodiment, the pressure of the ambient inert gas is between 20 Torr and 300 Torr.

[0040] In one embodiment, at least one of the one or more delivery holes has a minor axis dimension between 5 μm and 50 μm.

[0041] In one embodiment, at least one of the one or more depositors has a width between 40 μm and 400 μm, where the width is perpendicular to the printing direction.

[0042] In one embodiment, one or more depositors are located 20 μm to 60 μm from the substrate.

[0043] In one embodiment, the vapor precursor comprises an organometallic compound.

[0044] In one embodiment, the vapor precursor is configured to chemically bond to the substrate via a covalent bond.

[0045] In one embodiment, the covalent bond is formed via one or more of an ether group, a thioether group, and an acetylthio group.

[0046] In another aspect, a chemical vapor deposition system includes a substrate that includes a conductive oxide layer thermally connected to a heater; and a nozzle block facing the conductive oxide layer, the nozzle block including at least one delivery hole configured to eject an organic vapor, and at least one discharge hole proximate to the at least one delivery hole, the discharge hole being configured to create a deposition zone by aspirating an ambient confinement gas and at least a portion of the ejected organic vapor, wherein a total volumetric flow rate of the ejected organic vapor is less than a total volumetric flow rate aspirated by the at least one discharge hole, wherein the heater is configured to heat the substrate to between 60 °C and 200 °C, wherein the ambient confinement gas has a pressure between 20 Torr and 300 Torr, and wherein the nozzle block is located between 20 μm and 60 μm from the substrate.

[0047] In one embodiment, the organic vapor is configured to condense on the substrate or the conductive oxide to form an electroluminescent film.

[0048] In one embodiment, the electroluminescent film comprises a single layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 An organic light emitting device is shown.

[0050] Figure 2 An inverted organic light emitting device without an independent electron transport layer is shown.

[0051] Figure 3A And 3B An exemplary OVJP depositor is shown.

[0052] Figure 4 An emissive layer of an OLED deposited by a current embodiment of OVJP is shown.

[0053] Figure 5 Shows a depiction of an organic vapor reacting with a substrate surface to form a monolayer.

[0054] Figure 6 Shows a comparison of the thickness cross-section of a thin film printed by the current OVJP process with the thickness cross-section of an organic monolayer deposited by the disclosed process.

[0055] Figure 7 Shows the thin film layer structure of an OLED fabricated using the disclosed process.

[0056] Figure 8 Shows the architecture of a full-color OLED pixel comprising side-by-side red, green, and blue sub-pixels fabricated using the disclosed process.

[0057] Figure 9 Shows a flow chart of the steps required to fabricate an OLED using the disclosed process. Detailed Description

[0058] Generally, an OLED comprises at least one organic layer disposed between and electrically connected to an anode and a cathode. When a current is applied, the anode injects holes and the cathode injects electrons into the organic layer. The injected holes and electrons each migrate towards the electrode of opposite charge. When an electron and a hole are located on the same molecule, an "exciton" is formed, which is a localized electron-hole pair with an excited energy state. When the exciton relaxes through a light emission mechanism, light is emitted. In some cases, the exciton can be localized on an excimer or an exciplex. Non-radiative mechanisms such as thermal relaxation may also occur, but are generally considered undesirable.

[0059] Initial OLEDs used emissive molecules that emit light from a singlet state ("fluorescence"), as disclosed, for example, in U.S. Patent No. 4,769,292, which is incorporated herein by reference in its entirety. Fluorescent emission typically occurs within a time frame of less than 10 nanoseconds.

[0060] Recently, OLEDs having emissive materials that emit light from triplets (“phosphorescence”) have been demonstrated. Baldo et al., “Highly Efficient Phosphorescent Emission from Organic Electroluminescent Devices”, Nature, Vol. 395, 151 - 154, 1998 (“Baldo - I”); and Baldo et al., “Very high - efficiency green organic light - emitting devices based on electrophosphorescence”, Appl. Phys. Lett., Vol. 75, No. 3, 4 - 6 (1999) (“Baldo - II”), which are incorporated herein by reference in their entirety. Phosphorescence is described in more detail in U.S. Patent No. 7,279,704, columns 5 - 6, which is incorporated by reference.

[0061] Figure 1 An organic light - emitting device 100 is shown. The figures are not necessarily drawn to scale. Device 100 may include a substrate 110, an anode 115, a hole - injection layer 120, a hole - transport layer 125, an electron - blocking layer 130, an emissive layer 135, a hole - blocking layer 140, an electron - transport layer 145, an electron - injection layer 150, a protective layer 155, a cathode 160, and a barrier layer 170. Cathode 160 is a composite cathode having a first conductive layer 162 and a second conductive layer 164. Device 100 may be fabricated by depositing the layers in sequence. The nature and function of these different layers and example materials are described in more detail in U.S. 7,279,704, columns 6 - 10, which is incorporated by reference.

[0062] More examples of each of these layers are available. For example, a flexible and transparent substrate - anode combination is disclosed in U.S. Patent No. 5,844,363, which is incorporated herein by reference in its entirety. An example of a p - doped hole - transport layer is doped with F in a molar ratio of 50:1 4m-MTDATA of -TCNQ, as disclosed in U.S. Patent Application Publication No. 2003 / 0230980, which is incorporated herein by reference in its entirety. Examples of the emissive and host materials are disclosed in U.S. Patent No. 6,303,238 to Thompson et al., which is incorporated herein by reference in its entirety. An example of an n-doped electron transport layer is BPhen doped with Li in a 1:1 molar ratio, as disclosed in U.S. Patent Application Publication No. 2003 / 0230980, which disclosure is incorporated herein by reference in its entirety. U.S. Patents Nos. 5,703,436 and 5,707,745, which are incorporated herein by reference in their entireties, disclose examples of cathodes that include a composite cathode having a thin layer of metal (such as Mg:Ag) with an overlying transparent, conductive, sputter-deposited ITO layer. The theory and use of the barrier layer are described in more detail in U.S. Patent No. 6,097,147 and U.S. Patent Application Publication No. 2003 / 0230980, which patents are incorporated herein by reference in their entireties. An example of an injection layer is provided in U.S. Patent Application Publication No. 2004 / 0174116, which is incorporated herein by reference in its entirety. A description of the protective layer can be found in U.S. Patent Application Publication No. 2004 / 0174116, which is incorporated herein by reference in its entirety. The barrier layer 170 can be a single or multi-layer barrier layer and can cover or surround other layers of the device. The barrier layer 170 can also surround the substrate 110, and / or it can be disposed between the substrate and other layers of the device. The barrier layer can also be referred to as an encapsulant, encapsulation layer, protective layer, or permeation barrier and generally provides protection against moisture, ambient air, and other similar substances passing through other layers of the device. Examples of barrier layer materials and structures are provided in U.S. Patents Nos. 6,537,688, 6,597,111, 6,664,137, 6,835,950, 6,888,305, 6,888,307, 6,897,474, 7,187,119, and 7,683,534, each of which is incorporated herein by reference in its entirety.

[0063] Figure 2 An inverted OLED 200 is shown. The device includes a substrate 210, a cathode 215, an emissive layer 220, a hole transport layer 225, and an anode 230. The device 200 can be fabricated by depositing the layers in sequence. Since the most common OLED configuration has a cathode disposed above the anode, and the device 200 has a cathode 215 disposed under the anode 230, the device 200 can be referred to as an "inverted" OLED. Materials similar to those described with respect to the device 100 can be used in the corresponding layers of the device 200. Figure 2 An example is provided of how some layers can be omitted from the structure of the device 100.

[0064] Figure 1 and 2 The simple layered structure described in, by way of non-limiting example, and it should be understood that embodiments of the present invention may be used in conjunction with a variety of other structures. The specific materials and structures described are exemplary in nature, and other materials and structures may be used. Functional OLEDs may be obtained by combining the various layers described in different ways, or the layers may be omitted altogether based on design, performance, and cost factors. Other layers not specifically described may also be included. Materials other than those specifically described may be used. Although many of the examples provided herein describe the various layers as including a single material, it should be understood that combinations of materials may be used, such as a mixture of host and dopant, or more generally, mixtures. In addition, the layers may have various sub-layers. The names given to the various layers herein are not intended to be strictly limiting. For example, in device 200, hole transport layer 225 transports holes and injects holes into emissive layer 220, and may be described as a hole transport layer or a hole injection layer. In one embodiment, an OLED may be described as having an "organic layer" disposed between a cathode and an anode. This organic layer may comprise a single layer, or may further comprise multiple layers of different organic materials such as, for example, with respect to Figure 1 and 2 described.

[0065] Structures and materials not specifically described may also be used, such as OLEDs (PLEDs) comprising polymeric materials, as disclosed, for example, in U.S. Patent No. 5,247,190 to Friend et al., which is incorporated herein by reference in its entirety. By way of another example, an OLED having a single organic layer may be used. OLEDs may be stacked, for example, as described in U.S. Patent No. 5,707,745 to Forrest et al., which is incorporated herein by reference in its entirety. The OLED structure may deviate from Figure 1 and 2 the simple layered structure described in. For example, the substrate may include angled reflective surfaces to improve out-coupling, such as the mesa structure described in U.S. Patent No. 6,091,195 to Forrest et al., and / or the dimpled structure described in U.S. Patent No. 5,834,893 to Bulovic et al., which are incorporated herein by reference in their entirety.

[0066] In some embodiments disclosed herein, the emissive layer or material, such as Figure 1 - 2The emission layer 135 and the emission layer 220 shown respectively therein may include quantum dots. Unless explicitly indicated to the contrary or indicated as appropriate according to the understanding of those skilled in the art, as used herein, an "emission layer" or "emission material" may include an organic emission material and / or an emission material that includes quantum dots or equivalent structures. Generally, an emission layer includes an emission material within a host matrix. Such an emission layer may include only a quantum dot material that converts the light emitted by a separate emission material or other emitter, or it may further include a separate emission material or other emitter, or it may directly emit light itself by applying an electric current. Similarly, a color-changing layer, a color filter, an upconversion or downconversion layer or structure may include a material that includes quantum dots, but such a layer may not be considered an "emission layer" as disclosed herein. Generally, an "emission layer" or material is a material that emits initial light based on the injected charge, where the initial light may be altered by another layer, such as a color filter or other color-changing layer, which does not itself emit the initial light within the device but may re-emit altered light with a different spectral content based on the absorption and downconversion of the initial light emitted by the emission layer to lower energy light emission. In some embodiments disclosed herein, a color-changing layer, a color filter, an upconversion and / or downconversion layer may be disposed outside the OLED device, for example, above or below the electrodes of the OLED device.

[0067] Unless otherwise specified, any one of the layers of the various embodiments can be deposited by any suitable method. For organic layers, preferred methods include thermal evaporation, inkjet (as described in U.S. Pat. Nos. 6,013,982 and 6,087,196, which are incorporated herein by reference in their entireties), organic vapor phase deposition (OVPD) (as described in U.S. Pat. No. 6,337,102 to Forrest et al., which is incorporated herein by reference in its entirety), and deposition by organic vapor jet printing (OVJP) (as described in U.S. Pat. No. 7,431,968, which is incorporated herein by reference in its entirety). Other suitable deposition methods include spin coating and other solution-based processes. Solution-based processes are preferably carried out in nitrogen or an inert atmosphere. For other layers, preferred methods include thermal evaporation. Preferred patterning methods include deposition through a mask, cold welding (as described in U.S. Pat. Nos. 6,294,398 and 6,468,819, which are incorporated herein by reference in their entireties), and patterning associated with some of the deposition methods such as inkjet and OVJD. Other methods can also be used. The materials to be deposited can be modified to make them suitable for a particular deposition method. For example, substituents such as alkyl and aryl groups that are branched or unbranched and preferably contain at least 3 carbons can be used in small molecules to enhance their ability to withstand solution processing. Substituents having 20 or more carbons can be used, and a range of 3 to 20 carbons is preferred. Materials having an asymmetric structure can have better solution processability than materials having a symmetric structure because asymmetric materials may have a lower tendency to recrystallize. Dendrimer substituents can be used to enhance the ability of small molecules to withstand solution processing.

[0068] Devices fabricated according to embodiments of the present invention may further optionally include a barrier layer. One use of the barrier layer is to protect the electrodes and organic layers from damage by harmful substances in an environment exposed to, including moisture, vapor, and / or gases. The barrier layer may be deposited on the substrate, on the electrodes, under the substrate, under the electrodes, beside the substrate, beside the electrodes, or on any other part of the device (including the edges). The barrier layer may include a single layer or multiple layers. The barrier layer may be formed by various known chemical vapor deposition techniques and may include compositions having a single phase and compositions having multiple phases. Any suitable material or combination of materials may be used for the barrier layer. The barrier layer may include inorganic compounds or organic compounds or both. Preferred barrier layers include a mixture of a polymeric material and a non-polymeric material, as described in U.S. Patent No. 7,968,146, PCT Patent Application Nos. PCT / US2007 / 023098 and PCT / US2009 / 042829, which are incorporated herein by reference in their entirety. For a material to be considered a "mixture", the aforementioned polymeric and non-polymeric materials constituting the barrier layer should be deposited under the same reaction conditions and / or simultaneously. The weight ratio of the polymeric material to the non-polymeric material may range from 95:5 to 5:95. The polymeric material and the non-polymeric material may be produced from the same precursor material. In one example, the mixture of the polymeric material and the non-polymeric material substantially comprises polymeric silicon and inorganic silicon.

[0069] In some embodiments, at least one of the anode, cathode, or a new layer disposed above the organic emission layer serves as an enhancement layer. The enhancement layer comprises a plasmonic material that exhibits surface plasmon resonance, which non-radiatively couples to the emitter material and transfers the excited state energy from the emitter material to a non-radiative mode of surface plasmon polaritons. The enhancement layer is provided at a threshold distance not exceeding that from the organic emission layer, wherein due to the presence of the enhancement layer, the emitter material has a total non-radiative decay rate constant and a total radiative decay rate constant, and the threshold distance is the distance at which the total non-radiative decay rate constant equals the total radiative decay rate constant. In some embodiments, the OLED further comprises an outcoupling layer. In some embodiments, the outcoupling layer is disposed above the enhancement layer on the opposite side of the organic emission layer. In some embodiments, the outcoupling layer is disposed on the side of the emission layer opposite to the enhancement layer but still outcouples the energy from the surface plasmon mode of the enhancement layer. The outcoupling layer scatters the energy from the surface plasmon polaritons. In some embodiments, this energy is scattered as photons into free space. In other embodiments, the energy is scattered from the surface plasmon mode of the device into other modes, such as but not limited to organic waveguide modes, substrate modes, or another waveguide mode. If the energy is scattered into a non-free space mode of the OLED, other outcoupling schemes can be incorporated to extract the energy into free space. In some embodiments, one or more intervening layers can be disposed between the enhancement layer and the outcoupling layer. Examples of the intervening layer can be dielectric materials, including organic, inorganic, perovskite, oxide, and can include stacks and / or mixtures of these materials.

[0070] The enhancement layer modifies the effective properties of the medium in which the emitter material resides, thereby causing any one or all of the following: reduced emissivity, modification of the emission spectral line shape, variation of the emission intensity with angle, change in the stability of the emitter material, change in the efficiency of the OLED, and reduction of the efficiency decay of the OLED device. Placing the enhancement layer on the cathode side, anode side, or both sides results in an OLED device that exploits any of the above effects. In addition to the specific functional layers illustrated in the various OLED examples mentioned herein and shown in the figures, the OLEDs according to the present invention can also include any one of the other functional layers commonly seen in OLEDs.

[0071] The enhancement layer can be composed of plasmonic materials, optically active metamaterials, or hyperbolic metamaterials. As used herein, a plasmonic material is a material in which the real part of the dielectric constant crosses zero in the visible or ultraviolet region of the electromagnetic spectrum. In some embodiments, the plasmonic material includes at least one metal. In such embodiments, the metal can include at least one of the following: Ag, Al, Au, Ir, Pt, Ni, Cu, W, Ta, Fe, Cr, Mg, Ga, Rh, Ti, Ru, Pd, In, Bi, Ca, alloys or mixtures of these materials, and stacks of these materials. Generally speaking, a metamaterial is a medium composed of different materials, and the overall effect of the medium is different from the sum of the effects of its material parts. Specifically, we define an optically active metamaterial as a material having both a negative dielectric constant and a negative magnetic permeability. On the other hand, a hyperbolic metamaterial is an anisotropic medium in which the permittivity or magnetic permeability has different signs for different spatial directions. Optically active metamaterials and hyperbolic metamaterials are strictly distinguished from many other photonic structures, such as Distributed Bragg Reflectors ("DBRs"), because the medium should appear uniform in the direction of propagation for the length scale of the light wavelength. Using terms understandable to those skilled in the art: the dielectric constant of the metamaterial in the direction of propagation can be described by the effective medium approximation. Plasmonic materials and metamaterials provide methods for controlling light propagation that can enhance OLED performance in various ways.

[0072] In some embodiments, the enhancement layer is provided as a planar layer. In other embodiments, the enhancement layer has features of wavelength size arranged periodically, quasi-periodically, or randomly, or features of sub-wavelength size arranged periodically, quasi-periodically, or randomly. In some embodiments, the features of wavelength size and sub-wavelength size have sharp edges.

[0073] In some embodiments, the outcoupling layer has features of wavelength size arranged periodically, quasi-periodically, or randomly, or has features of sub-wavelength size arranged periodically, quasi-periodically, or randomly. In some embodiments, the outcoupling layer may be composed of a plurality of nanoparticles, and in other embodiments, the outcoupling layer is composed of a plurality of nanoparticles disposed above a material. In these embodiments, outcoupling can be tuned by at least one of the following: changing the size of the plurality of nanoparticles, changing the shape of the plurality of nanoparticles, changing the material of the plurality of nanoparticles, adjusting the thickness of the material, changing the refractive index of the material or an additional layer disposed on the plurality of nanoparticles, changing the thickness of the enhancement layer, and / or changing the material of the enhancement layer. The plurality of nanoparticles of the device may be formed by at least one of the following: metal, dielectric material, semiconductor material, metal alloy, mixture of dielectric materials, stack or layer of one or more materials, and / or core of one type of material coated with a shell layer of a different type of material. In some embodiments, the outcoupling layer is composed of at least metal nanoparticles, where the metal is selected from the group consisting of: Ag, Al, Au, Ir, Pt, Ni, Cu, W, Ta, Fe, Cr, Mg, Ga, Rh, Ti, Ru, Pd, In, Bi, Ca, alloys or mixtures of these materials, and stacks of these materials. The plurality of nanoparticles may have additional layers disposed above them. In some embodiments, the polarization of the emission can be tuned using the outcoupling layer. Changing the dimensions and periodicity of the outcoupling layer can select a preferred type of polarization outcoupled to air. In some embodiments, the outcoupling layer also serves as an electrode of the device.

[0074] It is believed that the internal quantum efficiency (IQE) of fluorescent OLEDs can exceed the 25% spin statistics limit by delayed fluorescence. As used herein, there are two types of delayed fluorescence, namely P-type delayed fluorescence and E-type delayed fluorescence. P-type delayed fluorescence is generated by triplet-triplet annihilation (TTA).

[0075] On the other hand, E-type delayed fluorescence does not rely on the collision of two triplets, but rather on the thermal population between the triplet and the singlet excited state. Compounds capable of generating E-type delayed fluorescence are required to have a very small singlet-triplet gap. Thermal energy can activate the transition from the triplet state back to the singlet state. This type of delayed fluorescence is also called thermally activated delayed fluorescence (TADF). A remarkable feature of TADF is that, due to the increase in thermal energy, the delayed component increases with increasing temperature. If the reverse intersystem crossing rate is fast enough to minimize the non-radiative decay of the triplet state, the fraction of the singlet excited state refilled may reach 75%. The total singlet fraction can be 100%, far exceeding the spin statistics limit of electrically generated excitons.

[0076] E-type delayed fluorescence characteristics can be seen in exciplex systems or single compounds. Without being bound by theory, it is believed that E-type delayed fluorescence requires the luminescent material to have a small singlet-triplet energy gap (ΔES-T). Organic, metal-free donor-acceptor luminescent materials may be able to achieve this. The emission of these materials is typically characterized by donor-acceptor charge transfer (CT) type emission. The spatial separation of the HOMO and LUMO in these donor-acceptor type compounds usually results in a small ΔES-T. These states may involve CT states. Generally, donor-acceptor luminescent materials are constructed by connecting an electron donor moiety (such as an amino or carbazole derivative) to an electron acceptor moiety (such as an N-containing six-membered aromatic ring).

[0077] Devices manufactured according to embodiments of the present invention can be incorporated into a wide variety of electronic component modules (or units), and the electronic component modules can be incorporated into a variety of electronic products or intermediate components. Examples of the electronic products or intermediate components include display screens, lighting devices (such as discrete light source devices or lighting panels), etc. that can be utilized by end-user product manufacturers. The electronic component modules can optionally include driving electronic devices and / or power sources. Devices manufactured according to embodiments of the present invention can be incorporated into a wide variety of consumer products that have one or more electronic component modules (or units) incorporated therein. Disclosed is a consumer product including an OLED, and the OLED includes the compounds of the present disclosure in the organic layers of the OLED. The consumer product should include any kind of product that includes one or more of one or more light sources and / or a certain type of visual display. Some examples of the consumer product include flat panel displays, curved displays, computer monitors, medical monitors, televisions, billboards, lights for internal or external lighting and / or signaling, head-up displays, fully transparent or partially transparent displays, flexible displays, rollable displays, foldable displays, stretchable displays, laser printers, telephones, cellular phones, tablet computers, phablets, personal digital assistants (PDAs), wearable devices, laptop computers, digital cameras, video cameras, viewfinders, microdisplays with a diagonal of less than 2 inches, 3D displays, virtual reality or augmented reality displays, vehicles, video walls including multiple tiled-together displays, theater or stadium screens, and signs. Various control mechanisms can be used to control the devices manufactured according to the present invention, including passive matrix and active matrix. It is intended that many of the devices be used in a temperature range comfortable for humans, such as 18 °C to 30 °C, and more preferably at room temperature (20 - 25 °C), but they can be used outside of this temperature range (e.g., -40 °C to 80 °C).

[0078] The materials and structures described herein can be applied to devices other than OLEDs. For example, other optoelectronic devices such as organic solar cells and organic photodetectors can employ the materials and structures. More generally, organic devices such as organic transistors can employ the materials and structures.

[0079] In some embodiments, the OLED has one or more characteristics selected from the group consisting of flexible, rollable, foldable, stretchable, and bendable. In some embodiments, the OLED is transparent or translucent. In some embodiments, the OLED further includes a layer comprising carbon nanotubes.

[0080] In some embodiments, the OLED further includes a layer comprising a delayed fluorescence emitter. In some embodiments, the OLED comprises an RGB pixel arrangement or a white plus color filter pixel arrangement. In some embodiments, the OLED is a mobile device, a handheld device, or a wearable device. In some embodiments, the OLED is a display panel with a diagonal less than 10 inches or an area less than 50 square inches. In some embodiments, the OLED is a display panel with a diagonal of at least 10 inches or an area of at least 50 square inches. In some embodiments, the OLED is a lighting panel.

[0081] In some embodiments of the emission region, the emission region further includes a host.

[0082] In some embodiments, the compound can be an emissive dopant. In some embodiments, the compound can generate emission via phosphorescence, fluorescence, thermally activated delayed fluorescence (i.e., TADF, also known as E-type delayed fluorescence), triplet-triplet annihilation, or a combination of these processes.

[0083] The OLEDs disclosed herein can be incorporated into one or more of consumer products, electronic component modules, and lighting panels. The organic layer can be an emission layer, and the compound can be an emissive dopant in some embodiments and a non-emissive dopant in other embodiments.

[0084] The organic layer can also include a host. In some embodiments, two or more hosts are preferred. In some embodiments, the host used can be a) bipolar, b) electron transporting, c) hole transporting, or d) wide bandgap materials that play a minor role in charge transport. In some embodiments, the host can include metal complexes. The host can be an inorganic compound.

[0085] Combinations with other materials

[0086] The materials described herein as suitable for use in a particular layer in an organic light-emitting device can be used in combination with a wide variety of other materials present in the device. For example, the emissive dopants disclosed herein can be used in combination with a wide variety of hosts, transport layers, blocking layers, injection layers, electrodes, and other layers that may be present. The materials described or mentioned below are non-limiting examples of materials that can be used in combination with the compounds disclosed herein, and one of ordinary skill in the art can readily consult the literature to identify other materials that can be used in combination.

[0087] The various emissive and non-emissive layers and arrangements disclosed herein can use different materials. Examples of suitable materials are disclosed in U.S. Patent Application Publication No. 2017 / 0229663, which is incorporated herein by reference in its entirety.

[0088] Conductive dopants:

[0089] The charge transport layer can be doped with a conductive dopant to substantially change its charge carrier density, which in turn will change its conductivity. Conductivity is increased by generating charge carriers in the matrix material, and depending on the type of dopant, a change in the Fermi level of the semiconductor can also be achieved. The hole transport layer can be doped with a p-type conductive dopant, and an n-type conductive dopant is used in the electron transport layer.

[0090] HIL / HTL:

[0091] The hole injection / transport materials used in the present invention are not particularly limited, and any compound can be used as long as the compound is commonly used as a hole injection / transport material.

[0092] EBL:

[0093] An electron blocking layer (EBL) can be used to reduce the number of electrons and / or excitons leaving the emissive layer. The presence of such a blocking layer in the device can result in generally higher efficiency and / or longer lifetime compared to a similar device lacking a blocking layer. Additionally, a blocking layer can be used to confine emission to the desired region of the OLED. In some embodiments, the EBL material has a higher LUMO (closer to the vacuum level) and / or a higher triplet energy compared to the emitter closest to the EBL interface. In some embodiments, the EBL material has a higher LUMO (closer to the vacuum level) and / or a higher triplet energy compared to one or more of the hosts closest to the EBL interface. In one aspect, the compound used in the EBL contains the same molecule or the same functional group as used in one of the hosts described below.

[0094] Host:

[0095] The light-emitting layer of the organic EL device of the present invention preferably contains at least a metal complex as a light-emitting material, and may contain a host material using a metal complex as a dopant material. Examples of the host material are not particularly limited, and any metal complex or organic compound can be used as long as the triplet energy of the host is greater than that of the dopant. Any host material can be used with any dopant as long as the triplet criterion is satisfied.

[0096] HBL:

[0097] A hole blocking layer (HBL) can be used to reduce the number of holes and / or excitons leaving the emissive layer. The presence of such a blocking layer in the device can result in generally higher efficiency and / or longer lifetime compared to a similar device lacking the blocking layer. Additionally, a blocking layer can be used to confine emission to the desired region of the OLED. In some embodiments, the HBL material has a lower HOMO (farther from the vacuum level) and / or a higher triplet energy compared to the emitter closest to the HBL interface. In some embodiments, the HBL material has a lower HOMO (farther from the vacuum level) and / or a higher triplet energy compared to one or more of the hosts closest to the HBL interface.

[0098] ETL:

[0099] The electron transport layer (ETL) can include materials capable of transporting electrons. The electron transport layer can be intrinsic (undoped) or doped. Doping can be used to enhance conductivity. Examples of ETL materials are not particularly limited, and any metal complex or organic compound can be used as long as it is commonly used to transport electrons.

[0100] Charge generation layer (CGL)

[0101] In a tandem or stacked OLED, the CGL plays a fundamental role in performance and consists of an n-doped layer and a p-doped layer for injecting electrons and holes, respectively. Electrons and holes are supplied by the CGL and the electrodes. The electrons and holes consumed in the CGL are refilled by electrons and holes injected from the cathode and anode, respectively; subsequently, the bipolar current gradually reaches a steady state. Typical CGL materials include n- and p-conductive dopants used in the transport layers.

[0102] As previously disclosed, the deposition within the features to be printed by OVJP is non-uniform. As a result, the thickness cross-section of the printed lines is not flat, and is typically thicker at the center of the printed feature relative to the edges of the effective width of the feature. Here, the effective width is the width of the line that overlaps the electrode and can be irradiated. The effective width itself is limited by the thickness uniformity within the line. Additionally, variations in the film thickness across the entire effective width can create efficiency and lifetime issues for the OVJP printing apparatus. Furthermore, variations in the average thickness between printed lines or along the length of a printed line can create non-uniformities in the display.

[0103] Compared to other deposition techniques designed to deposit a material overlay on a substrate, such as organic vapor deposition (OVPD), chemical vapor deposition (CVD), atomic layer deposition (ALD), etc., the OVJP technique deposits narrow lines of material, sometimes but not limited to organic materials, on a substrate without using a shadow mask, a fine metal mask, or an equivalent device.

[0104] Conventional devices and techniques for manufacturing displays such as mobile phone and laptop computer displays typically use evaporation sources and fine metal masks to pattern the deposition, as is common in non-OVJP deposition techniques. Fine metal masks are generally not suitable for manufacturing large area displays because the mask cannot be stretched with sufficient force to prevent sagging. Inkjet printing is a potential patterning technique for organic light emitting diode (OLED) displays, but using solvents to make the ink severely degrades the performance of the light emitting device. OVJP eliminates both of these problems by printing lines with pixel widths without using a fine metal mask. It is noted that OVJP uses state-of-the-art OLED materials or other materials without dissolving them in a solvent.

[0105] In some embodiments, OVJP is used to deposit lines of precursor materials that react with the substrate or materials previously deposited on the substrate to form a single layer material, and more specifically an electroluminescent material. In one embodiment, the single layer is formed to be self-limiting, such that the entire printed width of the line will be one single layer thickness. In other words, the print head of the OVJP apparatus can remain over an area long enough to form a single layer over the entire area without depositing excess material on portions of the area. In one embodiment, the convective curtain produced by the OVJP depositor prevents the precursor material from leaving the defined deposition area, and this enables precise patterning. In one embodiment, material can be deposited on a row of sub-pixels or pixels without contaminating adjacent sub-pixels or pixels. Alternatively, material can be deposited in a specific area without depositing / contaminating any adjacent areas. For example, a side-by-side RGB display can be fabricated by depositing red, green, and blue electroluminescent single layers over the electrodes of the respective pixels.

[0106] In one embodiment, a method is disclosed herein for maskless additive patterning of a single layer material (such as an electroluminescent material) on an electrode substrate to enable the fabrication of a display (such as an RGB display). The method includes sequentially depositing precursors using OVJP, which react to form red, green, and blue emissive materials on different electrodes, respectively.

[0107] Embodiments of the present invention are provided to identify suitable material systems (precursor materials and electrode materials), and then print device arrays on a properly prepared substrate using OVJP. In one embodiment, conventional vacuum thermal evaporation (VTE) can then be used to deposit an electron transport layer, electrode materials, or other layers known in the art. In one embodiment, maskless additive patterning of a single layer electroluminescent material on an electrode substrate enables the fabrication of an RGB display by sequentially depositing precursors using OVJP, which react to form red, green, and blue emissive materials on different electrodes, respectively.

[0108] In one embodiment, the material used can include M(B)k(C)l(D)m(E)n, where the material is emissive; M is a transition metal; B, C, D, E are ligands coordinated to the metal; k + l + m + n represents the maximum number of ligands that can be bonded to the metal; and any one of the ligands B, C, D, E is capable of forming a covalent bond with the metal or metal oxide surface. In an alternative embodiment, one or more of the ligands B, C, D, E are removed from the material, and the metal M is capable of forming a covalent bond with the surface.

[0109] In one embodiment, the vapor precursor is a cyclopentadienyl metal complex, such as (methylcyclopentadienyl)trimethylplatinum. In alternative embodiments, the vapor precursor may include, but is not limited to, (trimethyl)methylcyclopentadienylplatinum(IV), bis(ethylcyclopentadienyl)magnesium, cyclopentadienylindium(I), bis(cyclopentadienyl)ruthenium (ruthenocene), bis(ethylcyclopentadienyl)ruthenium(II), bis(ethylcyclopentadienyl)manganese, cyclopentadienylcobalt dicarbonyl, tris(methylcyclopentadienyl)yttrium, (methylcyclopentadienyl)yttrium, (methylcyclopentadienyl)(1,5-cyclooctadiene)iridium(I), and / or transition metal triacetylacetonates. In the transition metal triacetylacetonates, the metal includes, but is not limited to, Al, Sc, Cr, Mn, Fe, Co, Ru, Rh, In, Ir, Pt, Pd. Alternatively, the metal includes, but is not limited to, barium, bismuth, cerium, chromium, cobalt, copper, dysprosium, erbium, gadolinium, hafnium, indium, iron, lanthanum, magnesium, manganese, molybdenum, neodymium, nickel, niobium, osmium, platinum, praseodymium, rhenium, rhodium, ruthenium, samarium, thallium, thulium, titanium, tungsten, vanadium, ytterbium, yttrium, and zirconium. In an alternative embodiment, the metal may include iridium-based, platinum-based, rhodium-based, or palladium-based metal halides, metal β-diketones, carbonyl complexes, allyl complexes, cyclopentadienyl complexes, cyclooctadienyl complexes, alkyl complexes, metal carboxylates, metal phosphines, and / or ethylene complexes. In another alternative embodiment, the vapor precursor may be any metal chelated with a ligand, where the ligand can be removed by heating, oxidizing (e.g., by O 2 , H 2 O) or reducing (e.g., by H 2 , NH 3 ) in the gas phase.

[0110] In one embodiment, the chemical vapor deposition system may deposit a material adhering to the substrate through a thioether group or an acetylthio group linked to ligand B, C, D, or E. In one embodiment, the chemical vapor deposition system may deposit any doping material, such as a volatile compound, such as (1-((4-acetylthienyl)ethynyl)-4-((4-pyridyl)ethynyl)benzene) or such a compound linked with an active organometallic group.

[0111] As previously disclosed, one type of technology for manufacturing OLEDs and similar devices is OVJP, which is a maskless, solventless method for printing large area OLED displays. In OVJP, a series of holes formed in a silicon wafer are used to print narrow lines of OLED material on a display backplane, and the silicon wafer can be fabricated using microelectromechanical systems (MEMS) technology. Specific examples of OVJP systems are disclosed in U.S. Patent Nos. 10,170,701 and 11,267,012, the disclosures of each of which are incorporated herein by reference in their entireties, as well as U.S. Applications Nos. 16 / 245,554 and 16 / 324,703, the disclosures of each of which are incorporated herein by reference in their entireties.

[0112] When OVJP systems and techniques are used to manufacture OLEDs and similar devices, the OLED material is printed over anode columns separated by thin lines of insulating material. To maximize display performance, the ratio of the anode area to the pixel isolation area is maximized. This requires the OVJP printing profile to approximate a square wave profile; the profile must have steep sidewalls and a flat top between the sidewalls. Computational fluid dynamics (CFD) modeling of the deposition profile is typically used to assist in the design of the holes. The CFD modeled hole design can produce a deposition profile with steep sidewalls or a flat top. However, as described in further detail herein, it has been found that when such designs are combined in a single mirror symmetric wafer, the actual deposition profile can deviate significantly from the predicted profile. CFD loses its predictive ability when evaluating depositors with extremely small features. The printed wafer geometries disclosed herein allow for the printing of profiles with steep sidewalls and a flat top using appropriately sized printing holes. Additionally, the depositor arrangements disclosed herein provide fully decoupled depositors, and the combination of such decoupled depositors in a fully functional printing array.

[0113] Compared to other deposition techniques designed to deposit a material overlay on a substrate, such as organic vapor deposition (OVPD), chemical vapor deposition (CVD), atomic layer deposition (ALD), etc., the OVJP technique deposits narrow lines of organic material on a substrate without using a shadow mask, a fine metal mask, or an equivalent device.

[0114] Conventional devices and techniques for manufacturing displays such as mobile phone and laptop computer displays typically use evaporation sources and fine metal masks to pattern depositions, such as is common in non-OVJP deposition techniques. Fine metal masks are generally not suitable for manufacturing large area displays because the masks cannot be stretched with sufficient force to prevent sagging. Inkjet printing is a potential patterning technique for organic light emitting diode (OLED) displays, but using solvents to make the inks severely degrades the performance of the light emitting devices. OVJP eliminates both of these problems by printing lines with pixel widths without using a fine metal mask. Notably, OVJP uses state-of-the-art OLED materials without dissolving them in solvents.

[0115] In OVJP, the OLED material is heated to an elevated sublimation temperature in a closed container and conveyed to a printhead using an inert carrier gas through a heated gas line. The printhead contains ejection holes whose pitch corresponds to the pixel pitch of the display. The holes are formed on a silicon wafer using standard microelectromechanical systems (MEMS) fabrication techniques. A functional OVJP die is cut from the wafer and has holes located along one face of the die. Excess organic material is removed from the printing area through a vacuum channel inserted into the printed die. The hole face of the die is held above a moving display backplane and lines corresponding to the pixels are printed on the backplane.

[0116] An example of an OVJP depositor with a single delivery hole is shown in Figure 3A - 3B FIG. Figure 3A FIG. shows a face-up depositor presented from the substrate surface, which may be located above or below the depositor, with the surface of the substrate onto which the deposition material is to be deposited facing the depositor. The sides of the delivery hole 453 are two discharge holes 454. The die is made of two Si wafers 451 and 452, where the shaded / dotted areas represent regions of solid wafer material and the non-shaded areas represent holes on the die edge. The midline of the depositor 457 corresponds to a seam previously disclosed as formed between two halves of the die by wafer bonding. The holes are formed by etching channels in the faces of the two wafers 451, 452 and bonding the two wafers together. The direction of relative movement of the depositor with respect to the substrate onto which the deposition material is to be deposited is shown by arrow 99, which is used throughout the figures to indicate the same direction. The holes (453, 454) can have any suitable geometry, including but not limited to square, rectangular, triangular, annular, circular, oval, and n-sided, where n is greater than 2.

[0117] Figure 3B FIG. shows a cross-sectional view of channels disposed within the die above the substrate 450 and perpendicular to the printing scan direction. Figure 3AThe delivery holes 453 and the discharge holes 454 therein are formed through a delivery channel 455 and a discharge channel 456 etched to the lower edge of the die in each wafer, respectively, to form a hole array.

[0118] The various depositors disclosed herein can be fabricated by etching the described channels and holes in one or more wafers and then bonding the wafers to each other to achieve the described hole arrangement. As part of the bonding process, the matching delivery holes and / or discharge holes and channels in each wafer can be aligned or offset to achieve the desired hole arrangement.

[0119] Additional exemplary OVJP systems, methods, and details are described in U.S. Patent Applications Nos. 18 / 104,353, 18 / 311,550, and 18 / 228,892, the disclosures of each of which are incorporated herein by reference in their entireties.

[0120] Figure 4 A cross-section of a sub-pixel in an OLED display printed by an embodiment of an OVJP depositor is shown. A nozzle block 301 including a delivery hole 302 jets a stream 303 of organic vapor entrained in an inert carrier gas onto a substrate 304. In this example, a thin film of transparent conductive oxide 305 on the substrate surface serves as the anode of a complete OLED. The organic vapor in the stream condenses on the substrate in the area below the delivery hole to form a thin film 306 of an electroluminescent material. The width of the deposition zone is bounded by two stagnation planes 307 defined by the positions where the outward movement of the stream is blocked by the inward flow of a confinement gas 308 drawn from the environment surrounding the depositor. The flow of the confinement gas prevents the organic vapor from diffusing beyond the stagnation planes. This allows for high-resolution printing by preventing the organic material intended for one sub-pixel from diffusing into and / or contaminating adjacent sub-pixels. The confinement gas, the inert gas from the stream, and the remaining organic vapor are all drawn into a discharge hole 309 disposed next to the delivery hole on the nozzle block. The discharge hole cumulatively draws a greater molar flow of gas from the printing zone than the delivery hole jets, thus ensuring the inward flow of the confinement gas. The illumination width of the pixel is defined by a non-conductive pixel defining layer (PDL) 310 defined on the substrate prior to OVJP deposition. The PDL ensures that the illumination area of the thin film stack is uniform and of high quality. The edges of both the printed thin film and the electrode can additionally be detrimental to the device performance.

[0121] Figure 5Shows a stylized depiction of a metalorganic chemical vapor deposition (MOCVD) reaction. The precursor molecule 401 for this reaction can vary, but typical precursors can include an organometallic group 402 that serves as a radiative exciton recombination site and a tether group 403 that connects the organometallic group to a reactive group 404. A tether group of limited length is shown here, but the disclosed techniques can also be used with precursor materials having a reactive group directly attached to the organometallic group, such that the tether group has zero length. The reactive group can include relatively weak chemical bonds, such as an ether or thioether that breaks upon contact with the substrate surface and chemisorbs the organometallic group to the substrate. The precursor molecule is delivered to the substrate 405 in the gas phase. The precursor molecule can react with an activated metal or metal oxide film 406 on the substrate to form a molecular monolayer 407 of an electroluminescent material that is chemically bonded to the substrate. The electroluminescent molecules in this layer can include the organometallic group and the tether group from the precursor. An effluent group 408 can dissociate from the precursor molecule during chemisorption and remain in the gas phase. These are vented as reaction by-products. Given sufficient precursor, the reaction will proceed until a monolayer of electroluminescent material is deposited on the substrate. Once the monolayer is formed, no more material is deposited because there are no sites available on the substrate for chemisorption of the precursor.

[0122] In some embodiments, the vapor deposition system 300 includes an array of depositors 301 in fluid communication with an ambient inert gas 308, the depositors being held near a substrate 304 carried on a heated transporter 399 such that the substrate 304 and the depositors 301 move relative to each other during deposition. In some embodiments, each depositor 301 has one or more delivery holes 302 that eject a gas jet 303 including a vapor precursor that chemically reacts with the substrate surface to form a single-molecule-thick layer 306 of an electroluminescent compound on the substrate 304. In some embodiments, each depositor 301 has one or more exhaust holes 309 that cumulatively extract a greater molar flow rate of gas than is cumulatively ejected by the delivery holes 302 in the same depositor 301.

[0123] In one embodiment, the temperature of the substrate 304 surface exceeds the temperature of the depositor 301. In one embodiment, the temperature of the substrate is between 100 °C and 200 °C, between 60 °C and 180 °C, or between 40 °C and 350 °C. In one embodiment, the pressure of the ambient inert gas is between 20 Torr and 300 Torr, between 10 Torr and 350 Torr, or between 100 Torr and 200 Torr.

[0124] In one embodiment, the depositor array 301 is maintained at a distance between 20 μm and 60 μm, between 10 μm and 100 μm, or between 30 μm and 50 μm from the substrate 304. In one embodiment, the delivery holes and / or the discharge holes have a minor width 460 between 5 μm and 50 μm and a major width 461 between 5 μm and 1000 μm. In one embodiment, each depositor 301 has a width 462 between 100 μm and 1000 μm.

[0125] In one embodiment, the vapor precursor comprises a metal-organic compound capable of pyrolysis and chemical bonding to the substrate. In one embodiment, the vapor precursor is a transition metal triacetylacetonate. In one embodiment, the deposited material adheres to the substrate 304 via one or more of an ether group, a thioether group, and an acetylthio group. In one embodiment, the deposited material forms a continuous monolayer on the area of the substrate 304 acted upon by the depositor 301.

[0126] In some embodiments, the organic vapor jet printing (OVJP) deposition apparatus 300 includes one or more depositors 301, where at least one of the one or more depositors 301 includes one or more delivery holes 302; one or more discharge holes 309, where at least one of the one or more discharge holes 309 is fluidly coupled to at least one of the one or more delivery holes 302; and a substrate 304. In some embodiments, the one or more delivery holes 302 are configured to eject a gas jet 303 including a vapor precursor onto the substrate 304, thereby causing a chemical reaction between the vapor precursor and the substrate 304.

[0127] In one embodiment, the apparatus further includes a heated substrate chuck 399 configured to hold the substrate 304 and provide heat to the substrate. In one embodiment, the apparatus 300 is configured to form a monolayer of adsorbates on the substrate 304 via a chemical reaction between the vapor precursor and the substrate 304.

[0128] In one embodiment, the one or more discharge holes are configured to extract a molar flow rate of gas that is greater than the molar flow rate of gas ejected by the one or more delivery holes.

[0129] In one embodiment, the temperature of the substrate 304 is higher than the temperature of the vapor precursor material. In one embodiment, the temperature of the substrate 304 is lower than or equal to the temperature of the vapor precursor material. On the other hand, the temperature of the substrate 304 is between 100 °C and 200 °C. In one embodiment, the temperature of the substrate 304 is between 60 °C and 180 °C.

[0130] In one embodiment, the pressure of the ambient inert gas 308 is between 20 Torr and 300 Torr. In one embodiment, at least one of the one or more delivery holes 302 has a minor axis dimension between 5 μm and 50 μm. In one embodiment, at least one of the one or more depositors 301 has a width between 40 μm and 400 μm, where the width is perpendicular to the printing direction. In one embodiment, the one or more depositors 301 are located 20 μm to 60 μm from the substrate 304.

[0131] In one embodiment, the vapor precursor comprises an organometallic compound. In one embodiment, the vapor precursor is configured to chemically bond to the substrate via a covalent bond. In one embodiment, the covalent bond is formed via one or more of an ether group, a thioether group, and an acetylthio group.

[0132] In some embodiments, the chemical vapor deposition system 300 includes a substrate 304 that includes a conductive oxide layer 305 thermally connected to a heater 399; and a nozzle block 301 facing the conductive oxide layer 305. In some embodiments, the nozzle block 301 includes at least one delivery hole 302 configured to eject an organic vapor 303, and at least one exhaust hole 309 proximate to the at least one delivery hole 302, the exhaust hole being configured to create a deposition zone bounded by a stagnation plane 307 by aspirating an ambient confinement gas 308 and at least a portion of the ejected organic vapor 303. In some embodiments, the total volumetric flow rate of the ejected organic vapor 303 is less than the total volumetric flow rate of the ambient confinement gas 308 and the portion of the ejected organic vapor 303 aspirated by the at least one exhaust hole 309. In some embodiments, the heater 399 is configured to heat the substrate to between 60 °C and 200 °C. In some embodiments, the ambient confinement gas 308 has a pressure between 20 Torr and 300 Torr. In some embodiments, the nozzle block 301 is located between 20 μm and 60 μm from the substrate 304.

[0133] In one embodiment, the organic vapor 303 is configured to condense on the substrate 304 and / or the conductive oxide 305 to form an electroluminescent film. In one embodiment, the electroluminescent film comprises a single layer.

[0134] Figure 6Shows a comparison of the printed profile generated by OVJP when depositing materials by physical vapor deposition (PVD) with the profile expected when depositing MOCVD precursors. The upper figure shows the results of the PVD process by OVJP. For illustrative purposes, the printed profile 501 is superimposed over the PDL. (Note that the thickness is not to scale.) The deposition of the organic vapor is faster near the center of the printed area than at the edges. This results in a non-uniform thickness profile of the printed film that can adversely affect device performance. In contrast, as shown in the lower figure, a chemically adsorbed film 502 of MOCVD precursor is expected to form a uniform monolayer over the entire printed area. In some embodiments, the deposition reaction is self-limiting, so the material cannot accumulate in areas of higher flux. Additionally, in some embodiments, the precursor cannot be deposited on the PDL because it will not react. Here, the non-reactive precursor is removed by evacuation.

[0135] Figure 7 Shows an embodiment of an OLED produced by the disclosed process. The substrate 304 includes a transparent conductive oxide first electrode 305 and a pixel definition layer 310. The first electrode 305 can be a suitable anode or cathode. The first electrode 305 can be coated with an activated metal or metal oxide film 406 adsorbed with a precursor. When the precursor vapor reacts with the first electrode, a monolayer of electroluminescent material 502 is formed. An electron transport material layer 601 can be deposited over the monolayer of electroluminescent material. Finally, a second electrode 602 can be deposited over the electron transport material. The second electrode 602 can be a suitable cathode or anode.

[0136] Figure 8 Shows a cross-section of an RGB pixel printed with this technique. Each sub-pixel has Figure 7 the structure shown in. The sub-pixels are distinguished only by receiving a monolayer of red 701, green 702, or blue 703 electroluminescent material. Each monolayer can be deposited on the substrate in successive steps using OVJP.

[0137] Figure 9 Shows a flowchart of a process that can be used to fabricate an OLED by the disclosed technique. Front-end substrate processing 801 refers to the substrate preparation that is typically required before depositing organic materials. This generally includes fabricating a backplane that can include active circuit elements, electrodes, and PDL layers. Substrate preparation can include depositing a thin layer of metal oxide on the electrodes using an MOCVD precursor (such as Ni(tta)2(tmeda)) along with O2 and Ar. This deposition process is typically carried out at a pressure of 1 - 10 Torr and a substrate temperature of 400 °C.

[0138] In one embodiment, the adsorption surface on the electrode must be activated 802 before a monolayer of organic electroluminescent material can be deposited. This must be carried out in an inert environment just before the monolayer deposition. H at a pressure of 300 Torr and 300 °C2 O vapor and O 2 can be used to activate the metal oxide layer on the electrode. A variety of other chemical treatments can be used to activate the electrode surface. Physical methods such as plasma etching, ion milling, or laser ablation can also be used to produce an active surface.

[0139] Next, as disclosed herein, a single layer of electroluminescent material 803 is deposited using OVJP. The gas phase precursor reacts with the metal or metal oxide surface to form a single layer of emissive molecules. At a gas pressure between 10 Torr and 200 Torr, the vapor is entrained in an inert carrier gas such as N 2 or Ar. The source is heated to a temperature sufficient to evaporate the precursor, up to 400 °C. The substrate is heated to between 100 °C and 300 °C. Chemical bonds between the precursor molecules and the activated substrate are formed as shown in the following illustration. Single layer materials emitting different colors can be deposited on different sub-pixels of the RGB array in successive deposition steps, where different colored sub-pixels are coated in each step.

[0140] It should be understood that the various embodiments described herein are by way of example only and are not intended to limit the scope of the invention. For example, many of the materials and structures described herein can be replaced with other materials and structures without departing from the spirit of the invention. The invention as claimed can thus include variations of the specific examples and preferred embodiments described herein, as will be apparent to those skilled in the art. It should be understood that the various theories as to why the invention works are not intended to be limiting.

Claims

1. A vapor deposition system, comprising: an array of depositors in fluid communication with an ambient inert gas, the depositors being held proximate to a substrate carried on a heated transport such that the substrate and depositors move relative to each other during deposition; wherein each depositor has one or more delivery holes configured to eject a gas jet comprising a vapor precursor that chemically reacts with a substrate surface to form a monomolecular thick layer of an electroluminescent compound on the substrate; as well as Each depositor has one or more exhaust holes configured to cumulatively extract a greater molar flow rate of gas than is cumulatively ejected by the delivery holes in the same depositor.

2. The vapor deposition system of claim 1, wherein the temperature of the substrate surface exceeds the temperature of the depositor.

3. The vapor deposition system of claim 2, wherein the temperature of the substrate surface is between 100°C and 200°C.

4. The vapor deposition system of claim 2, wherein the temperature of the substrate surface is between 60°C and 180°C. 5 . The vapor deposition system of claim 1 , wherein the pressure of the ambient inert gas is between 20 Torr and 300 Torr. 6 . The vapor deposition system according to claim 1 , wherein the depositor array is maintained at a distance of 20 μm to 60 μm from the substrate. 7 . The vapor deposition system of claim 1 , wherein the delivery or exhaust holes have a minor width between 5 μm and 50 μm.

8. The vapor deposition system of claim 1, wherein each depositor has a width between 100 μm and 1000 μm.

9. The vapor deposition system of claim 1, wherein the vapor precursor comprises an organometallic compound capable of pyrolyzing and chemically bonding to the substrate.

10. The vapor deposition system of claim 1, wherein the deposition material adheres to the substrate via one or more of an ether group, a thioether group, and an acetylthio group.

11. The vapor deposition system of claim 1, wherein the deposited material forms a continuous monolayer over the area of ​​the substrate acted upon by the depositor.

12. An organic vapor jet printing (OVJP) deposition apparatus, comprising: one or more depositors, wherein at least one of the one or more depositors comprises: one or more delivery holes; one or more exhaust holes, wherein at least one of the one or more exhaust holes is fluidly coupled to at least one transfer hole of the one or more transfer holes; and A substrate, wherein the one or more delivery holes are configured to eject a gas jet including a vapor precursor onto the substrate, thereby causing a chemical reaction between the vapor precursor and the substrate.

13. A vapor deposition system comprising: a substrate comprising a conductive oxide layer thermally connected to a heater; and A nozzle block facing the conductive oxide layer, comprising: at least one delivery hole configured to eject organic vapor; and at least one exhaust orifice proximate to the at least one delivery orifice configured to create a deposition zone by drawing in an ambient confining gas and at least a portion of the injected organic vapor; wherein the total volume flow rate of the injected organic vapor is less than the total volume flow rate of the at least one exhaust hole sucked in; wherein the heater is configured to heat the substrate to between 60° C. and 200° C.; wherein the ambient limiting gas has a pressure between 20 Torr and 300 Torr; and Wherein the nozzle block is located between 20 μm and 60 μm from the substrate.

14. The system of claim 13, wherein the organic vapor is configured to condense on the substrate or conductive oxide to form an electroluminescent film.

15. The system of claim 14, wherein the electroluminescent film comprises a single layer.

Citation Information

Patent Citations

  • Controlled deposition of materials using a differential pressure regime

    US10170701B2

  • Spatial control of vapor condensation using convection

    US11267012B2

  • Very low voltage, high efficiency phosphorescent OLED in a p-i-n structure

    US20030230980A1

  • Transparent electrodes

    US20040174116A1

  • Organic electroluminescent materials and devices

    US20170229663A1