Hot spinning forming manufacturing method for titanium alloy large-length cylindrical part

Through the hot spin forming manufacturing method, the problem of difficult forming of titanium alloys at room temperature is solved, and the efficient forming of large-length cylindrical parts is achieved, and the dimensional accuracy and performance consistency of the finished product are improved.

CN120133363APending Publication Date: 2025-06-13BEIJING SATELLITE MFG FACTORY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202510354544.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-03-25
Publication Date
2025-06-13

AI Technical Summary

Technical Problem

Titanium alloys are difficult to form at room temperature, are prone to cracking, have serious rebound, are obvious anisotropy and are difficult to guarantee dimensional accuracy. It is difficult to process large-length cylindrical parts in the prior art.

Method used

By adopting the hot spin forming manufacturing method, the round titanium alloy blank head is welded at one end of the thick-wall cylindrical blank, sprayed the mold release agent and heated with an array arranged flame spray gun, combined with an infrared temperature measurement device to adjust the temperature in real time, and perform multiple spinning passages, and finally release the mold at a higher temperature and cut the end blank to obtain a large-length cylindrical piece.

Benefits of technology

It effectively improves the forming performance of titanium alloy, has a large total deformation of the material, a large length of the formed cylindrical part, has a high aspect ratio, and improves the dimensional accuracy and performance consistency of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120133363A_ABST
    Figure CN120133363A_ABST
Patent Text Reader

Abstract

A hot spinning forming manufacturing method for a titanium alloy large-length cylindrical part belongs to the technical field of spaceflight manufacturing and comprises the following steps: welding a titanium alloy circular blank end socket at one end of a titanium alloy thick-wall cylindrical blank to form a thick-wall cylindrical part; the thick-wall cylindrical part with one end sealed is installed on a core mold of the spinning machine and fixed, then flame spray guns arranged in an array mode are used for heating the outer surface of the thick-wall cylindrical part, the heating process is intermittently stopped, and the temperature of the thick-wall cylindrical part is measured in real time; when the temperature of the thick-wall cylindrical part reaches the spinning temperature, multi-pass spinning is carried out, and the flame heating intensity is adjusted according to the measured temperature of the thick-wall cylindrical part in the spinning process; and when the wall thickness of the thick-wall cylindrical part meets the requirement, spinning and demolding are stopped, the thick-wall cylindrical part is taken down at the preset temperature, after the room temperature is reached, the round blank with the welded end is cut off, and the large-length cylindrical part is obtained. The method can improve the product temperature uniformity in the hot spinning process, improve the spinning process stability and improve the product forming quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a hot spinning forming manufacturing method for large-length titanium alloy cylindrical parts, belonging to the field of aerospace manufacturing technology. Background Art

[0002] Spinning technology is an advanced plastic processing technology for realizing near-net forming of hollow rotary components. By driving the blank to rotate with the main shaft and the spinning wheel feeding axially successively, continuous and point-by-point plastic deformation of the blank is generated. During the spinning process, the area of the deformation zone is small, the deformation force is small, the unit pressure is high, the dimensional accuracy of the spun product is high, and the surface quality is good.

[0003] Titanium alloy has high specific strength, corrosion resistance, fatigue resistance, and good weldability, so its application in the aerospace field is increasing day by day. However, it is difficult to form titanium alloy at room temperature, and there are problems such as easy cracking, serious springback, obvious anisotropy, and difficulty in ensuring dimensional accuracy. Therefore, it has become a trend to process titanium alloy components by hot forming methods.

[0004] Cylindrical parts are a common structural form. At present, there are many methods for processing titanium alloy cylindrical parts. In the prior art, rolling or extrusion methods are usually used for processing titanium alloy cylindrical parts, but special molds are required and the processing technology is difficult. During ordinary spinning, the temperature uniformity of the blank is poor, the formability of the blank is limited, and the final performance consistency of the parts is poor, making it difficult to process large-length cylindrical parts. Summary of the Invention

[0005] The technical problem solved by the present invention is: overcoming the deficiencies of the prior art, providing a hot spinning forming manufacturing method for large-length titanium alloy cylindrical parts, and solving the problems such as difficult forming at room temperature of titanium alloy, easy cracking, serious springback, obvious anisotropy, and difficulty in ensuring dimensional accuracy.

[0006] The technical solution of the present invention is: a hot spinning forming manufacturing method for large-length titanium alloy cylindrical parts, including:

[0007] Welding a titanium alloy circular blank head at one end of the thick-walled titanium alloy cylindrical blank to form a thick-walled cylindrical part;

[0008] Spraying a release agent on the outer surface of the core mold of the spinning machine, installing the thick-walled cylindrical part with one end head on the core mold of the spinning machine and fixing it, then heating the outer surface of the thick-walled cylindrical part with an array of flame spray guns, and intermittently stopping the heating process, and using an infrared temperature measuring device to measure the temperature of the thick-walled cylindrical part in real time; when the temperature of the thick-walled cylindrical part reaches the spinning temperature, multi-pass spinning is carried out, and during the spinning process, the flame heating intensity is adjusted according to the temperature of the thick-walled cylindrical part measured by the infrared temperature measuring device;

[0009] When the wall thickness of the thick-walled cylindrical part meets the requirements, stop spinning, demold, remove the thick-walled cylindrical part at the preset temperature, and after reaching room temperature, cut off the circular blank welded at the end to obtain a large-length cylindrical part.

[0010] Further, the titanium alloy thick-walled cylindrical blank is TC4 or TA15 titanium alloy, the original wall thickness is 60 mm to 110 mm, the inner diameter of the titanium alloy large-length cylindrical part is 500 mm to 600 mm, and the length is 1.5 m to 3 m.

[0011] Further, the mold release agent is graphite, BN mold release agent or MoS 2 mold release agent.

[0012] Further, spray a mold release agent on the surface of the spinning machine mandrel for demolding the component after spinning, and install a harmful gas collection device above the spinning machine to collect the gas generated by the mold release agent under high-temperature conditions.

[0013] Further, the spinning machine mandrel is a cylindrical mandrel. There are 12 M20 threaded holes on the surface of the mandrel end. The threaded holes are distributed along the circumference of Φ260 mm. Process through holes at the corresponding positions of the blank head, and fix the blank to the mandrel with bolts; at the same time, use a Φ160 mm ejector rod to tighten the blank head.

[0014] Further, the flame spray gun uses propane and oxygen for gas supply. Along the circumferential direction of the thick-walled cylindrical part, multiple groups of flame spray gun matrices are arranged. The flame spray gun matrices are placed below or on both sides of the thick-walled cylindrical part to avoid the spinning wheels, and there are flame spray guns for heating throughout the entire length range of the thick-walled cylindrical part.

[0015] Further, the spinning temperature is set to 780 ± 30 °C.

[0016] Further, during the spinning process, the temperature of the thick-walled cylindrical part shows a two-stage stepped distribution. Within the range of 0 to 500 mm in front of the spinning wheel, the temperature of the thick-walled cylindrical part is 780 ± 30 °C, and within the remaining range, the temperature of the thick-walled cylindrical part is 700 °C to 760 °C; during the spinning process, the thick-walled cylindrical part is always heated, and according to the temperature of the thick-walled cylindrical part measured by the infrared temperature measuring device, adjust the number of working flame spray guns. Set air valves at the air inlets of each flame spray gun, and determine the number of open air valves according to the relationship between the real-time temperature of the thick-walled cylindrical part and the spinning temperature. When the temperature is lower than the preset low value, increase the number of open air valves; when the temperature is higher than the preset high value, reduce the number of open air valves.

[0017] Further, after the temperature of the thick-walled cylindrical part reaches the spinning temperature, before the formal spinning operation, heat and keep the thick-walled cylindrical part warm to make the internal temperature of the thick-walled cylindrical part consistent with the surface temperature. The heat preservation time is 2 to 3 h;

[0018] The core die of the spinning machine and the thick-walled cylindrical part are subjected to the same heating and heat preservation operation, and during the spinning process, the temperature of the core die of the spinning machine is ensured to be between 300°C and 400°C.

[0019] Furthermore, the placement position of the flame spray gun is related to the wall thickness of the thick-walled cylindrical part. During the spinning process, as the wall thickness of the thick-walled cylindrical part decreases, the position of the flame spray gun is adjusted so that the distance between the flame spray gun and the outer surface of the thick-walled cylindrical part remains unchanged; the outer flame of the flame spray gun is used to heat the outer surface of the thick-walled cylindrical part;

[0020] The spinning process is divided into multiple spinning passes. Three spinning wheels are set, the installation angle of the spinning wheels is 15°, the forming angle of the spinning wheels is 30°, the spindle speed is 20 r / min, and the axial feed speed of the spinning wheels is 15 mm / min to 20 mm / min;

[0021] For each spinning pass, the downward pressure of each of the three spinning wheels satisfies where d is the downward pressure of the spinning wheel, and h is the theoretical wall thickness of the thick-walled cylindrical part before spinning in this pass, with the unit of mm;

[0022] During the demolding process, first wait for the core die of the spinning machine and the thick-walled cylindrical part to cool naturally, and then heat the thick-walled cylindrical part at the maximum power, with a heating rate ≥ 500°C / h. When the thick-walled cylindrical part reaches the preset temperature of 400°C to 550°C, demolding is carried out.

[0023] The advantages of the present invention compared with the prior art are as follows:

[0024] (1) During the spinning process of the present invention, a matrix-distributed flame spray gun is used to heat the cylindrical part, with uniform temperature distribution and a large adjustable temperature range.

[0025] (2) The present invention processes titanium alloy by the hot spinning method, effectively improving the forming performance of titanium alloy. The total deformation of the material is large. With a suitable downward pressure in a single pass, the formed cylindrical part has a large length and a high length-diameter ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] By reading the following detailed description of the preferred embodiments, various other advantages and benefits will become clear to those of ordinary skill in the art. The drawings are only for the purpose of showing the preferred embodiments and are not considered to be a limitation of the present invention. Moreover, throughout the drawings, the same reference numerals are used to represent the same components. In the drawings:

[0027] Figure 1 is the process flow chart of the present invention.

[0028] Figure 2 is the schematic diagram of the spinning process of the large-length cylindrical part. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0029] To better understand the above technical solution, the technical solution of the present invention will be described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood that the embodiments of the present invention and the specific features in the embodiments are detailed descriptions of the technical solution of the present invention, rather than limitations on the technical solution of the present invention. Without conflict, the technical features in the embodiments of the present invention and the embodiments can be combined with each other.

[0030] The following further describes in detail a hot spinning forming manufacturing method for a large-length cylindrical titanium alloy part provided by an embodiment of the present invention with reference to the accompanying drawings of the specification. The specific implementation manner may include:

[0031] Step 1: Weld a titanium alloy circular blank head at one end of a thick-walled titanium alloy cylindrical blank.

[0032] Step 2: Spray a release agent on the outer surface of the spinning machine mandrel, install the thick-walled cylindrical part with a head at one end on the spinning machine mandrel and fix it. Then, use an array of flame spray guns to heat the outer surface of the cylindrical part, and intermittently stop the heating process. Use an infrared temperature measuring device to measure the temperature of the cylindrical part in real time.

[0033] Step 3: When the temperature of the cylindrical part reaches the spinning temperature, perform multi-pass spinning, and adjust the flame heating intensity according to the temperature of the cylindrical part measured by the infrared temperature measuring device during the spinning process.

[0034] Step 4: When the wall thickness of the cylindrical part meets the requirements, stop spinning, perform demolding, remove the cylindrical part at a higher temperature, and after reaching room temperature, cut off the circular blank welded at the end to obtain a large-length cylindrical part.

[0035] Preferably, the original wall thickness of the thick-walled titanium alloy cylindrical blank is 60 mm to 110 mm, the inner diameter of the large-length titanium alloy cylindrical part is 500 mm to 600 mm, and the length is 1.5 m to 3 m.

[0036] Preferably, the release agent is graphite, BN release agent or MoS 2 release agent, etc., and the spinning machine mandrel is a cylindrical mandrel.

[0037] Preferably, the flame spray gun uses propane and oxygen for gas supply.

[0038] Preferably, the spinning temperature is 780 ± 30 °C. During the spinning process, the temperature of the cylindrical part is distributed in a two-stage step shape. In the range of 0 to 500 mm in front of the spinning wheel, the temperature of the cylindrical part is 780 ± 30 °C, and in the remaining range, the temperature of the cylindrical part is 700 °C to 760 °C. During the spinning process, the cylindrical part is always heated, and the number of working flame spray guns is adjusted according to the temperature of the cylindrical part measured by the infrared temperature measuring device.

[0039] Preferably, after the tubular part reaches the spinning temperature, before the spinning operation is officially carried out, the tubular part needs to be heated and kept warm for 2 to 3 hours. The spinning machine core mold needs to be subjected to the same heating and heat preservation operation as the tubular part. During the spinning process, ensure that the temperature of the spinning machine core mold is between 300°C and 400°C.

[0040] Preferably, the placement position of the flame spray gun is related to the wall thickness of the tubular part. During the spinning process, the wall thickness of the tubular part decreases. Adjust the position of the flame spray gun so that the distance between the flame spray gun and the outer surface of the tubular part remains unchanged. The flame spray gun uses the outer flame to heat the outer surface of the tubular part.

[0041] Preferably, the spinning process is divided into multiple spinning passes. Set 3 spinning wheels, the installation angle of the spinning wheel is 15°, the forming angle of the spinning wheel is 30°, the spindle speed is 20 r / min, and the axial feed speed of the spinning wheel is 15 mm / min to 20 mm / min. In each spinning pass, the downward pressure of each of the 3 spinning wheels satisfies:

[0042]

[0043] where d is the downward pressure of the spinning wheel, in mm, and h is the theoretical wall thickness of the tubular part before spinning in this pass, in mm.

[0044] Preferably, during the demolding process, first wait for the spinning machine core mold and the tubular part to cool naturally, then heat the tubular part at the maximum power, and the heating rate is ≥500°C / h. When the tubular part reaches the preset temperature of 400°C to 550°C, carry out demolding.

[0045] In the solution provided by the embodiment of the present invention, as Figure 1 shown, a hot spinning forming manufacturing method for a large-length titanium alloy tubular part is provided. The method includes:

[0046] Step 1: Weld a titanium alloy circular blank head at one end of the thick-walled titanium alloy tubular blank.

[0047] Step 2: Spray a demolding agent on the outer surface of the spinning machine core mold, install the thick-walled tubular part with a head at one end on the spinning machine core mold and fix it. Then use an array of flame spray guns to heat the outer surface of the tubular part, and intermittently stop the heating process. Use an infrared temperature measuring device to measure the temperature of the tubular part in real time.

[0048] Step 3: As Figure 2 , when the temperature of the tubular part reaches the spinning temperature, carry out multi-pass spinning, and during the spinning process, adjust the flame heating intensity according to the temperature of the tubular part measured by the infrared temperature measuring device.

[0049] Step 4: When the wall thickness of the cylindrical part meets the requirements, stop spinning, demold, remove the cylindrical part at a relatively high temperature, and after reaching room temperature, cut off the circular blank welded at the end to obtain a long cylindrical part.

[0050] In some embodiments, the thick-walled titanium alloy cylindrical blank is a TC4 titanium alloy with an original wall thickness of 60 mm to 110 mm. The inner diameter of the large-length titanium alloy cylindrical part is 500 mm to 600 mm, and the length is 1.5 m to 3 m.

[0051] In some embodiments, the release agent is graphite, BN release agent or MoS 2 Release agent, etc. Spray the release agent on the surface of the core mold of the spinning machine to facilitate the demolding of the component after spinning. Install a harmful gas collection device above the spinning machine to collect the gas generated by the release agent under high-temperature conditions; the core mold of the spinning machine is a cylindrical core mold, and 12 M20 threaded holes are provided on the surface of the end of the core mold. The threaded holes are distributed along the circumference of Φ260 mm. Process through holes at the corresponding positions of the blank head, and fix the blank to the core mold with bolts; at the same time, use a Φ160 mm ejector rod to tighten the blank head.

[0052] In some embodiments, the flame spray gun uses propane and oxygen for gas supply. Along the circumferential direction of the cylindrical part, multiple groups of flame spray gun matrices are arranged. The flame spray gun matrices are placed below or on both sides of the cylindrical part to avoid the spinning wheels, and there are flame spray guns for heating throughout the entire length of the cylindrical part.

[0053] In some embodiments, the spinning temperature is set to 780 ± 30 °C; during the spinning process, the temperature of the cylindrical part is distributed in a two-stage stepped manner. Within the range of 0 to 500 mm in front of the spinning wheel, the temperature of the cylindrical part is 780 ± 30 °C, and within the remaining range, the temperature of the cylindrical part is 700 °C to 760 °C. During the spinning process, the cylindrical part is always heated, and according to the temperature of the cylindrical part measured by the infrared temperature measurement device, the number of working flame spray guns is adjusted. An air valve is set at the air inlet of each flame spray gun. According to the relationship between the real-time temperature of the blank and the spinning temperature, the number of open air valves is determined. When the temperature is too low, the number of open air valves is increased, and when the temperature is too high, the number of open air valves is decreased.

[0054] In some embodiments, after the temperature of the cylindrical part reaches the spinning temperature, before the spinning operation is formally carried out, the cylindrical part needs to be heated and insulated to adjust the internal temperature of the cylindrical part to be the same as the surface temperature. The heating and insulation time is 2 to 3 h; the core mold of the spinning machine needs to be subjected to the same heating and insulation operation as the cylindrical part, and the temperature of the core mold of the spinning machine is ensured to be 300 °C to 400 °C during the spinning process.

[0055] In some embodiments, the placement position of the flame spray gun is related to the wall thickness of the cylindrical part. During the spinning process, the wall thickness of the cylindrical part decreases. The position of the flame spray gun is adjusted so that the distance between the flame spray gun and the outer surface of the cylindrical part remains unchanged. The outer flame of the flame spray gun is used to heat the outer surface of the cylindrical part.

[0056] In some embodiments, the spinning process is divided into multiple spinning passes. Three spinning wheels are provided. The installation angle of the spinning wheels is 15°, the forming angle of the spinning wheels is 30°, the spindle speed is 20 r / min, and the axial feed speed of the spinning wheels is 15 mm / min to 20 mm / min. In each spinning pass, the downward pressure of each of the three spinning wheels satisfies:

[0057]

[0058] where d is the downward pressure of the spinning wheel, in mm, and h is the theoretical wall thickness of the cylindrical part before spinning in this pass, in mm.

[0059] In some embodiments, during the demolding process, first, the core mold of the spinning machine and the cylindrical part are allowed to cool naturally, and then the cylindrical part is heated at the maximum power, with a heating rate ≥ 500 °C / h until the cylindrical part reaches a preset temperature of 400 °C to 550 °C, and then demolding is carried out.

[0060] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalent technologies, the present invention is also intended to include these modifications and variations.

[0061] The content not described in detail in the specification of the present invention belongs to the well-known technology of those skilled in the art.

Claims

1. A hot spinning forming method for manufacturing a long-length cylindrical part of a titanium alloy, characterized in that: include: Welding a titanium alloy round billet head at one end of the titanium alloy thick-walled cylindrical billet to form a thick-walled cylindrical part; A mold release agent is sprayed on the outer surface of the spinning machine core mold, a thick-walled cylindrical part with a capped end is mounted on the spinning machine core mold and fixed, and then the outer surface of the thick-walled cylindrical part is heated with an array of flame spray guns, and the heating process is stopped intermittently, and the temperature of the thick-walled cylindrical part is measured in real time; when the temperature of the thick-walled cylindrical part reaches the spinning temperature, multiple passes of spinning are performed, and during the spinning process, the flame heating intensity is adjusted according to the measured temperature of the thick-walled cylindrical part; When the wall thickness of the thick-walled cylindrical part meets the requirements, the spinning is stopped and demoulding is carried out. The thick-walled cylindrical part is removed at a preset temperature. After reaching room temperature, the circular blank welded at the end is cut off to obtain a long-length cylindrical part.

2. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 1 is characterized in that: The titanium alloy thick-walled cylindrical blank is TC4 or TA15 titanium alloy, the original wall thickness is 60mm-110mm, the inner diameter of the titanium alloy long-length cylindrical piece is 500mm-600mm, and the length is 1.5m-3m.

3. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 1 is characterized in that: The release agent is graphite, BN release agent or MoS2 release agent.

4. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 3 is characterized in that: A release agent is sprayed on the surface of the core mold of the spinning machine for demoulding the component after spinning. A harmful gas collection device is installed above the spinning machine to collect the gas generated by the release agent under high temperature conditions.

5. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 4 is characterized in that: The core mold of the spinning machine is a cylindrical core mold, and 12 M20 threaded holes are arranged on the surface of the end of the core mold, and the threaded holes are distributed along a Φ260mm circumference. Through holes are processed at corresponding positions of the blank head, and the blank is fixed to the core mold with bolts; a Φ160mm push rod is also used to tighten the blank head.

6. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 1 is characterized in that: The flame spray gun uses propane and oxygen as gas supply. Multiple groups of flame spray gun matrices are arranged along the circumferential direction of the thick-walled cylindrical part. The flame spray gun matrix is ​​placed below or on both sides of the thick-walled cylindrical part to avoid the rotating wheel, and the flame spray gun is used to heat the entire length range of the thick-walled cylindrical part.

7. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 1 is characterized in that: The spinning temperature is set to 780±30°C.

8. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 1 is characterized in that: During the spinning process, the temperature of the thick-walled cylindrical parts is distributed in a two-level stepped manner. In the range of 0 to 500 mm in front of the spinning wheel, the temperature of the thick-walled cylindrical parts is 780±30°C, and in the remaining range, the temperature of the thick-walled cylindrical parts is 700°C to 760°C. During the spinning process, the thick-walled cylindrical parts are always heated, and the number of working flame spray guns is adjusted according to the measured temperature of the thick-walled cylindrical parts, and an air valve is set at the air inlet of each flame spray gun. The number of air valves to be opened is determined according to the relationship between the real-time temperature of the thick-walled cylindrical parts and the spinning temperature. When the temperature is lower than a preset low value, the number of air valves to be opened is increased, and when the temperature is higher than a preset high value, the number of air valves to be opened is reduced.

9. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 1 is characterized in that: After the temperature of the thick-walled cylindrical part reaches the spinning temperature, before the spinning operation is officially carried out, the thick-walled cylindrical part is heated and kept warm, and the internal temperature of the thick-walled cylindrical part is adjusted to be consistent with the surface temperature, and the heating and keeping warm time is 2 to 3 hours; The core mold of the spinning machine is subjected to the same heating and heat preservation operation as the thick-walled cylindrical parts, and the temperature of the core mold of the spinning machine is ensured to be between 300°C and 400°C during the spinning process.

10. The hot spinning forming manufacturing method of a titanium alloy long-length cylindrical part according to claim 1, characterized in that: The placement position of the flame spray gun is related to the wall thickness of the thick-walled cylindrical part. The wall thickness of the thick-walled cylindrical part decreases during the spinning process. The position of the flame spray gun is adjusted so that the distance between the flame spray gun and the outer surface of the thick-walled cylindrical part remains unchanged. The flame spray gun uses external flame to heat the outer surface of the thick-walled cylindrical part; The spinning process is divided into multiple spinning passes, and three spinning wheels are set, the spinning wheel installation angle is 15°, the spinning wheel forming angle is 30°, the spindle speed is 20r / min, and the spinning wheel axial feed speed is 15mm / min-20mm / min; In each spinning pass, the pressing amount of each of the three spinning wheels meets Wherein, d is the amount of downward pressure of the spinning wheel, h is the theoretical wall thickness of the thick-walled cylindrical part before spinning in this pass, in mm; In the demoulding process, the spinning machine core mold and the thick-walled cylindrical part are first cooled naturally, and then the thick-walled cylindrical part is heated at maximum power with a heating rate of ≥500°C / h. The thick-walled cylindrical part is demoulded when the temperature reaches a preset temperature of 400°C to 550°C.

Citation Information

Patent Citations

  • Independent digital flame following and heating device of hot spinning machine

    CN101972808A

  • Method for hot-spinning accurate temperature control of titanium alloy thin wall component

    CN103706716A

  • Precision spinning machining method for small-diameter multi-step variable-wall-thickness cylinder

    CN109604407A

  • Integral spinning machining method for variable cross-section cylinder workpiece with spherical end socket

    CN114769405A

  • Die-free flexible spinning temperature control method for high-temperature alloy and titanium alloy

    CN117583454A