Modified precision casting wax as well as preparation method and application thereof
By adjusting the component ratio of precision casting wax and heating and stirring process, a modified precision casting wax with high flexural strength and surface hardness was prepared, which solved the problem of insufficient strength and dimensional stability of wax materials in the prior art. It is suitable for the preparation of wax model for high-precision aviation casting structural parts.
Patent Information
- Application Number
- CN202510406395.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-02
- Publication Date
- 2025-06-13
AI Technical Summary
The existing precision casting waxes have shortcomings in strength performance, dimensional stability and ease of handling, and it is difficult to meet the needs of high-precision aero casting structural parts.
The formula of modified precision casting waxes is adopted, including microcrystalline wax, paraffin wax, stearic acid, ethylene-vinyl acetate, lignite wax, Piccotex75 resin, terpene resin, D-mannitol, adipic acid, rosin glyceride, carnauba wax, candlestick wax, hydroxyethyl cellulose and starch, and other components. By adjusting the component ratio and heating and stirring process, a modified precision casting wax with high bending hardness and surface hardness is prepared.
The high bending strength and surface hardness of modified precision casting wax is achieved, the shrinkage rate of wax material is reduced, the precision and stability of castings are improved, and it is suitable for the preparation of wax model for high-precision aviation casting structural parts.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of investment casting wax materials, and specifically relates to a modified precision casting wax, a preparation method thereof, and an application thereof.
Background Art
[0002] Investment casting, also known as lost-wax casting, is one of the oldest manufacturing processes. Investment casting is a high-precision and high-quality casting method, commonly used for producing parts with complex shapes and rich details. The investment casting process can manufacture components that are difficult to achieve through machining, and has the advantages of high reliability, low tooling cost, environmental friendliness, flexible design, and casting diversity.
[0004] There are many types of investment casting waxes, and the properties of different types of investment casting waxes vary greatly, but the raw materials used are not very different. These raw materials mainly include paraffin wax, microcrystalline wax, stearic acid, resin, and vegetable wax, etc. The raw materials of some investment casting waxes also include fillers. By changing the ratio between various raw materials and adding a small amount of modifiers, the investment casting wax exhibits different properties.
[0005] For investment castings, the most important performance index is dimensional accuracy, which requires the shrinkage rate of the investment casting wax to be as low as possible. See the Chinese patent document with the patent literature number CN110205092A, which proposes a preparation method of a repair wax for investment casting; the Chinese patent document with the patent literature number CN108329701A gives a preparation method of an investment casting wax; the Chinese patent document with the patent literature number CN109265847A proposes a preparation method of a quick-drying composite wax for investment casting. These patent documents mainly solve process problems such as demoulding property, product surface finish, and molding speed, and involve less in the strength performance, dimensional stability, and operability of investment casting wax.
Summary of the Invention
[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a modified precision casting wax, a preparation method thereof, and an application thereof.
[0007] To solve the above technical problems, the following technical solutions are adopted for the modified precision casting wax in the present invention: A modified precision casting wax, and the mass composition of the raw materials of the modified precision casting wax includes the following components: 17-25 parts of microcrystalline wax, 10-15 parts of paraffin wax, 5-10 parts of stearic acid, 2-4 parts of ethylene-vinyl acetate, 2-6 parts of montan wax, 2-5 parts of Piccotex75 resin, 10-15 parts of terpene resin, 5-15 parts of D-mannitol, 5-15 parts of adipic acid, 8-15 parts of glycerol ester of rosin, 1-3 parts of carnauba wax, 2-5 parts of candelilla wax, 1-3 parts of hydroxyethyl cellulose, 0-3 parts of starch, and the total of the above components is 100 parts.
[0008] The melting point of the paraffin wax is 60-62°C, and it is 60# fully refined paraffin wax; the melting point of the microcrystalline wax is 75°C; the melting point of the montan wax is 75-86°C, and the melting point of the stearic acid is 67-72°C; the softening point of the terpene resin is 80°C; the softening point of the candelilla wax is 67-71°C; the melting point of the carnauba wax is 83.5°C; the softening point of the glycerol ester of rosin is 78-90°C, and the acid value ≤ 9 ((KOH) / (mg / g)).
[0009] The content of vinyl acetate in the ethylene-vinyl acetate copolymer is 28 wt%, and the melt index is 400 g / 10 min; the melting point of the stearic acid is 67-72°C.
[0010] The Piccotex75 resin is a copolymer of α-methylstyrene and vinyltoluene, and the molar ratios are 75 / 25 respectively, and the softening point is 75°C.
[0011] The viscosity of the hydroxyethyl cellulose is 5000-6400 MPa·s (25°C).
[0012] For the starch and hydroxyethyl cellulose, 80% of them can pass through a 100-mesh sieve, and 50% can pass through a 200-mesh sieve.
[0013] The preparation method of the modified precision casting wax in the present invention adopts the following technical solutions. The preparation method includes the following steps: (1) First, heat and stir microcrystalline wax, paraffin wax, and stearic acid at 80-100°C until melted, add Piccotex75 resin, raise the temperature to 100-110°C, continue stirring, and keep warm for 20-40 minutes; (2) Continue to raise the temperature to 120-130°C, add ethylene-vinyl acetate copolymer, keep warm for 20-50 minutes, and continuously stir until completely melted; (3) Continue to heat at 120-130°C, add terpene resin, keep warm for 1-1.5 hours, and wait until completely melted into a transparent state; (4) Cool the material to 90-100°C, continue to add montan wax, carnauba wax, candelilla wax, and glycerol ester of rosin, and continuously stir until evenly mixed, then cool to 90-100°C, and keep warm for 30-60 minutes; (5) At 90-100°C, add one or several of D-mannitol, adipic acid, hydroxyethyl cellulose, and starch in sequence, and make granules after cooling to obtain the precision casting wax.
[0014] The modified precision casting wax prepared by the above technical solution can be applied to the preparation of wax models for high-precision aviation casting structural parts and wax models for other precision casting.
[0015] The present invention examines the effects of wax materials, ethylene-vinyl acetate, glycerol ester of rosin, and functional aids such as mannitol on the shrinkage rate, surface hardness, viscosity, shrinkage rate, bending strength, melting point and other properties of the modified precision casting wax, adjusts the composition and proportion of the wax mold material, and finally achieves the purpose of high bending hardness and surface hardness of the modified precision casting wax and reducing the shrinkage rate of the modified precision casting wax.
Specific Embodiments
[0016] The present invention relates to a preparation method of a modified precision casting wax and a specific application of the modified precision casting wax prepared by this preparation method.
[0017] When preparing the modified precision casting wax of the present invention, prepare raw materials according to the following mass component ratios
[0018] (1) 10-15 parts of paraffin wax;
[0019] (2) 17-25 parts of microcrystalline wax;
[0020] (3) 2-6 parts of montan wax;
[0021] (4) 2-4 parts of ethylene-vinyl acetate copolymer;
[0022] (5) 5-10 parts of stearic acid;
[0023] (6) 2-5 parts of Piccotex75 resin;
[0024] (7) 10 - 15 parts of terpene resin;
[0025] (8) 5 - 15 parts of D - mannitol;
[0026] (9) 5 - 15 parts of adipic acid;
[0027] (10) 2 - 5 parts of candelilla wax;
[0028] (11) 1 - 3 parts of carnauba wax;
[0029] (12) 8 - 15 parts of rosin glyceride;
[0030] (13) 1 - 3 parts of hydroxyethyl cellulose;
[0031] (14) 0 - 3 parts of starch (when the value is 0, it means not added).
[0032] The total of the above components is 100 parts.
[0033] The melting point of the paraffin wax is 60 - 62 °C, which is 60# fully refined paraffin wax; the melting point of the microcrystalline wax is 75 °C; the melting point of the lignite wax is 75 - 86 °C; the ethylene - vinyl acetate copolymer is 28 wt%, and the melt index is 400 g / 10 min; the melting point of the stearic acid is 67 - 72 °C; the softening point of the Piccotex resin is 75 °C; the softening point of the terpene resin is 80 °C; the D - mannitol is of ultra - pure grade, ≥99.0% (HPLC); 100% of the D - mannitol and adipic acid can pass through a 100 - mesh sieve, and 80% can pass through a 200 - mesh sieve; the softening point of the candelilla wax is 67 - 71 °C; the melting point of the carnauba wax is 83.5 °C; the softening point of the rosin glyceride is 78 - 90 °C, and the acid value ≤9 ((KOH) / (mg / g)); the viscosity of the hydroxyethyl cellulose is 5000 - 6400 MPa·s (25 °C); 80% of the starch and hydroxyethyl cellulose fillers can pass through a 100 - mesh sieve, and 50% can pass through a 200 - mesh sieve.
[0034] The rosin glyceride is preferably hydrogenated rosin glyceride, which has high stability, low shrinkage rate and color consistency, and is more suitable for aviation precision casting.
[0035] The preparation method of a modified precision casting wax pattern of the present invention is carried out according to the following steps:
[0036] (1) First, heat and stir the microcrystalline wax, paraffin wax and stearic acid at 80 - 100 °C until melted, add Piccotex 75 resin, raise the temperature to 100 - 110 °C and continue stirring, and keep warm for 20 - 40 min.
[0037] (2) Continue to raise the temperature to 120 - 130 °C, add ethylene-vinyl acetate copolymer, keep the temperature for 20 - 50 min and continuously stir until completely melted.
[0038] (3) Continue to heat at 120 - 130 °C, add terpene resin, keep the temperature for 1 - 1.5 h, and wait until it is completely melted into a transparent state.
[0039] (4) Cool the material to 90 - 100 °C, continue to add montan wax, carnauba wax, candelilla wax, and glycerol ester of rosin, and continuously stir until evenly mixed, then cool to 90 - 100 °C and keep the temperature for 30 - 60 min.
[0040] (5) At 90 - 100 °C, add D-mannitol, adipic acid, and hydroxyethyl cellulose in sequence, and add or not add starch. After cooling, make it into granules to obtain precision investment casting wax.
[0041] The obtained precision investment casting wax can be melted and injected by any injection machine to make various types of small mold parts, and various properties of the small mold parts can be tested.
[0042] The test methods for precision investment casting mold materials are as follows:
[0043] Melting point: Use DSC to test the melting point of precision investment casting wax;
[0044] Hardness: Use a Shore hardness tester to test the hardness of precision investment casting wax;
[0045] Viscosity: Execute according to the method specified in GB / T14235.1;
[0046] Flexural strength: Execute according to the method specified in GB / T14235.1;
[0047] Linear shrinkage rate: Execute according to the method specified in GB / T14235.1;
[0048] Ash content: Use TG to test the residual ash content of precision investment casting wax.
[0049] The viscosity of the investment casting wax modified by the present invention is between 140 and 300 MPa·s, and the shrinkage rate is between 0.10% and 0.4%. The lower shrinkage rate can improve the precision of the casting; the bending strength of the modified investment casting wax is between 5 and 8 MPa, and the hardness is between 45 and 55, which ensures the high strength and high hardness of the modified investment casting wax during the casting process and improves the stability; the ash content of the modified investment casting wax is below 0.02%, ensuring no pollution during the casting process; the melting point of the modified investment casting wax is between 54 and 58 °C, making it easier to demold during the casting process. The stability, high strength, high hardness, low ash content, suitable melting point, and easy demolding of the modified investment casting wax are beneficial to improving the efficiency of investment casting. The internal components of the modified investment casting wax provided by the present invention are uniform, the shrinkage rate of each part is uniform, and the wax has a relatively high strength, and it can be widely used in the preparation of wax models for high-precision aviation casting structural parts and other wax models for precision casting.
[0050] The following will further elaborate on the modified investment casting wax of the present invention in conjunction with the embodiments of the present invention:
[0051] Example 1
[0052] The raw materials and mass component ratios of the modified investment casting wax are as follows: 35.1 grams of microcrystalline wax, 19.5 grams of paraffin wax, 11.4 grams of stearic acid, 6.7 grams of Piccotex 75 resin, 4.3 grams of ethylene-vinyl acetate, 24.7 grams of terpene resin, 3 grams of carnauba wax, 8.3 grams of montan wax, 24 grams of rosin glyceride, 5 grams of adipic acid, 3.6 grams of candelilla wax, 3.6 grams of hydroxyethyl cellulose, 22.6 grams of D-mannitol, and 3.5 grams of starch.
[0053] Its preparation method includes the following steps:
[0054] (1) First, heat the microcrystalline wax, paraffin wax, and stearic acid at 90 °C, continuously stir until melted, add Piccotex 75 resin, and continue heating to 100 °C, continuously stir until melted.
[0055] (2) Continue to raise the temperature to 120 °C, add ethylene-vinyl acetate copolymer, and continuously stir until melted.
[0056] (3) Continue to add terpene resin and keep it at 120 °C for 90 min until it is evenly mixed.
[0057] (4) Cool the material to 90 °C, and successively add rosin glyceride, montan wax, carnauba wax, and candelilla wax, and continuously stir until evenly mixed.
[0058] (5) Finally, hydroxyethyl cellulose, starch, adipic acid, and D-mannitol are added sequentially and continuously stirred until evenly mixed. After maintaining the temperature for 60 min and cooling, granules are made to obtain the precision casting wax.
[0059] Example 2:
[0060] The raw materials and their mass component ratios in Example 2 are as follows: 33.0 g of microcrystalline wax, 20 g of paraffin wax, 13.5 g of stearic acid, 5.5 g of Piccotex 75 resin, 4.3 g of ethylene-vinyl acetate, 26.5 g of terpene resin, 4.6 g of carnauba wax, 10 g of montan wax, 20.4 g of rosin glyceride, 18.6 g of adipic acid, 8.6 g of candelilla wax, 3.0 g of hydroxyethyl cellulose, 20.4 g of D-mannitol, and 1 g of starch.
[0061] Its preparation method includes the following steps:
[0062] (1) First, heat the microcrystalline wax, paraffin wax, and stearic acid at 80°C, continuously stir until melted, add Piccotex 75 resin, and continue heating to 110°C, continuously stirring until melted.
[0063] (2) Continue to raise the temperature to 100°C, add ethylene-vinyl acetate copolymer, and continuously stir until melted.
[0064] (3) Continue to add terpene resin and maintain at 120°C for 90 min until evenly mixed.
[0065] (4) Cool the material to 90°C, sequentially add rosin glyceride, montan wax, carnauba wax, and candelilla wax, and continuously stir until evenly mixed.
[0066] (5) Finally, hydroxyethyl cellulose, starch, adipic acid, and D-mannitol are added sequentially and continuously stirred until evenly mixed. After maintaining the temperature for 60 min and cooling, granules are made to obtain the modified precision casting wax.
[0067] Example 3:
[0068] The raw materials and their mass component ratios in Example 3 are as follows: 38.4 g of microcrystalline wax, 20.5 g of paraffin wax, 15.6 g of stearic acid, 4.6 g of carnauba wax, 6.5 g of Piccotex 75 resin, 4.3 g of ethylene-vinyl acetate, 21.2 g of terpene resin, 10.3 g of montan wax, 8.5 g of candelilla wax, 18.6 g of adipic acid, 2.1 g of hydroxyethyl cellulose, 25 g of rosin glyceride, and 18.6 g of D-mannitol.
[0069] Its preparation method includes the following steps:
[0070] (1) First, heat microcrystalline wax, paraffin wax, and stearic acid at 100 °C, continuously stir until melted, add Piccotex 75 resin, continue heating to 110 °C, and continuously stir until melted.
[0071] (2) Continue to raise the temperature to 125 °C, add ethylene-vinyl acetate copolymer, and continuously stir until melted.
[0072] (3) Continue to add terpene resin and maintain at 125 °C for 90 min until evenly mixed.
[0073] (4) Cool the material to 100 °C, sequentially add glycerol ester of rosin, montan wax, carnauba wax, and candelilla wax, and continuously stir until evenly mixed.
[0074] (5) Finally, sequentially add hydroxyethyl cellulose and D-mannitol, continuously stir until evenly mixed, keep warm for 60 min, and make into granules after cooling to obtain the precision casting wax.
[0075] Example 4:
[0076] The raw materials and mass component ratios of Example 4 are as follows: 43.8 g of microcrystalline wax, 25.2 g of paraffin wax, 10.3 g of stearic acid, 28.2 g of glycerol ester of rosin, 5.5 g of carnauba wax, 8.5 g of Piccotex 75 resin, 4.1 g of ethylene-vinyl acetate, 20.2 g of terpene resin, 5.2 g of montan wax, 4.6 g of candelilla wax, 5.0 g of hydroxyethyl cellulose, 15.6 g of adipic acid, and 2.6 g of starch.
[0077] Its preparation method includes the following steps:
[0078] (1) First, heat microcrystalline wax, paraffin wax, and stearic acid at 90 °C, continuously stir until melted, add Piccotex 75 resin, continue heating to 100 °C, and continuously stir until melted.
[0079] (2) Continue to raise the temperature to 120 °C, add ethylene-vinyl acetate copolymer, and continuously stir until melted.
[0080] (3) Continue to add terpene resin and maintain at 120 °C for 90 - 120 min until evenly mixed.
[0081] (4) Cool the material to 90 °C, sequentially add glycerol ester of rosin, montan wax, carnauba wax, and candelilla wax, and continuously stir until evenly mixed.
[0082] (5) Finally, sequentially add hydroxyethyl cellulose, starch, and adipic acid, continuously stir until evenly mixed, keep warm for 60 - 90 min, and make into granules after cooling to obtain the precision casting wax.
[0083] Example 5:
[0084] The raw materials and mass component ratios of Example 5 are as follows: 33.5 g of microcrystalline wax, 28.6 g of paraffin wax, 16.8 g of stearic acid, 18.5 g of glycerol ester of rosin, 3.6 g of carnauba wax, 6.2 g of Piccotex75 resin, 5.2 g of ethylene-vinyl acetate, 26.5 g of terpene resin, 8.6 g of montan wax, 7.5 g of candelilla wax, 3.0 g of hydroxyethyl cellulose, 17.6 g of adipic acid, and 2.1 g of starch.
[0085] Its preparation method includes the following steps:
[0086] (1) First, heat the microcrystalline wax, paraffin wax, and stearic acid at 90 °C, continuously stir until melted, add Piccotex75 resin, and continue heating to 100 °C, continuously stir until melted.
[0087] (2) Continue to raise the temperature to 120 °C, add ethylene-vinyl acetate copolymer, and continuously stir until melted.
[0088] (3) Continue to add terpene resin and maintain at 120 °C for 90 - 120 min until evenly mixed.
[0089] (4) Cool the material to 90 °C, add glycerol ester of rosin, montan wax, carnauba wax, and candelilla wax in sequence, and continuously stir until evenly mixed.
[0090] (5) Finally, add hydroxyethyl cellulose, starch, and adipic acid in sequence, continuously stir until evenly mixed, keep warm for 60 - 90 min, and make granules after cooling to obtain the precision casting wax.
[0091] Comparative Examples 1 and 2
[0092] The raw materials and mass component ratios of Comparative Example 1 are as follows: 17.5 g of microcrystalline wax, 25.2 g of paraffin wax, 15.6 g of stearic acid, 17.6 g of glycerol ester of rosin, 4.6 g of carnauba wax, 7.9 g of Piccotex75 resin, 5.4 g of ethylene-vinyl acetate, 22.2 g of terpene resin, 8.3 g of montan wax, 5.5 g of candelilla wax, 3.6 g of hydroxyethyl cellulose, 18.6 g of D-mannitol, and 19.8 g of adipic acid.
[0093] Among them, the amounts of microcrystalline wax and Piccotex75 resin exceed the usage range of this application, and the surface hardness of the wax material is relatively low.
[0094] The preparation method is the same as that of Example 1.
[0095] Comparative Example 2:
[0096] The raw materials and mass component ratios of Comparative Example 2 are as follows: 33.0 g of microcrystalline wax, 22.1 g of paraffin wax, 13.5 g of stearic acid, 5.6 g of Piccotex 75 resin, 4.8 g of ethylene-vinyl acetate, 22.0 g of terpene resin, 10.3 g of carnauba wax, 5.0 g of montan wax, 22.0 g of glycerol ester of rosin, 5 g of adipic acid, 4.3 g of candelilla wax, 4.0 g of hydroxyethyl cellulose, 20.2 g of D-mannitol, and 3.0 g of starch.
[0097] Among them, the amounts of adipic acid and carnauba wax exceed the dosage ranges of this application, and the linear shrinkage rate of the wax material is relatively high.
[0098] The preparation method is the same as that of Example 1.
[0099] Comparative Example 3:
[0100] The raw materials and mass component ratios of Comparative Example 3 are as follows: 35.1 g of microcrystalline wax, 19.5 g of paraffin wax, 4.6 g of stearic acid, 6.7 g of Piccotex 75 resin, 4.3 g of ethylene-vinyl acetate, 24.7 g of terpene resin, 3 g of carnauba wax, 8.3 g of montan wax, 36 g of glycerol ester of rosin, 5 g of adipic acid, 3.6 g of candelilla wax, 3.6 g of hydroxyethyl cellulose, and 22.6 g of D-mannitol.
[0101] Among them, the amounts of stearic acid and glycerol ester of rosin exceed the dosage ranges of this application, the surface hardness of the wax material is relatively low, and the linear shrinkage rate is relatively high.
[0102] The preparation method is the same as that of Example 1.
[0103] Comparative Example 4:
[0104] The raw materials and mass component ratios of Comparative Example 4 are as follows: 35.1 g of microcrystalline wax, 22.5 g of paraffin wax, 9.6 g of stearic acid, 6.7 g of Piccotex 75 resin, 11.5 g of ethylene-vinyl acetate, 21.2 g of terpene resin, 4 g of carnauba wax, 4.5 g of montan wax, 24.5 g of glycerol ester of rosin, 13.8 g of adipic acid, 4.0 g of candelilla wax, 3.0 g of hydroxyethyl cellulose, 18.8 g of D-mannitol, and 2.0 g of starch.
[0105] Among them, the amount of ethylene-vinyl acetate exceeds the dosage range of this application, and the linear shrinkage rate of the wax material is relatively high.
[0106] The preparation method is the same as that of Example 1.
[0107] The casting waxes prepared in the above Examples 1-5 and Comparative Examples 1-4 were used to make small mold parts through an injection machine for testing. The test performances are shown in Table 1 below.
[0108] Table 1: Performance test data of modified precision investment casting wax
[0109]
[0110]
[0111] As can be seen from Table 1, the wax of the investment casting wax of the present invention has a moderate melting point, a small linear shrinkage rate, high hardness, high flexural strength, small ash content, and good viscosity control. At the same time, it can also be seen from Table 1 that when certain components in the modified precision casting wax pattern material formula exceed the range, it has a great impact on the comprehensive performance.
[0112] The above is a better technical solution of the embodiments of the present invention. The above embodiments are only used to illustrate the technical solutions of the embodiments of the present invention, and do not limit them. Those of ordinary skill in the art can still modify or equivalently replace the technical solutions of the embodiments of the present invention, and these modifications or equivalent replacements cannot make the modified technical solutions deviate from the scope of the technical plan of the embodiments of the present invention.
Claims
1. A modified precision casting wax, characterized in that: The mass composition of the modified precision casting wax raw material includes the following components: 17-25 parts of microcrystalline wax, 10-15 parts of paraffin, 5-10 parts of stearic acid, 2-4 parts of ethylene vinyl acetate, 2-6 parts of lignite wax, 2-5 parts of Piccotex75 resin, 10-15 parts of terpene resin, 5-15 parts of D-mannitol, 5-15 parts of adipic acid, 8-15 parts of rosin glycerol ester, 1-3 parts of carnauba wax, 2-5 parts of candelilla wax, 1-3 parts of hydroxyethyl cellulose, and 0-3 parts of starch, and the above components total 100 parts.
2. A modified precision casting wax according to claim 1, characterized in that: The melting point of the paraffin wax is 60-62°C, which is 60# fully refined paraffin wax; the melting point of the microcrystalline wax is 75°C; the melting point of the montan wax is 75-86°C, and the melting point of the stearic acid is 67-72°C; the softening point of the terpene resin is 80°C; the softening point of the candelilla wax is 67-71°C; the melting point of the carnauba wax is 83.5°C; the softening point of the rosin glycerol ester is 78-90°C, and the acid value is ≤9 ((KOH) / (mg / g)).
3. The modified precision casting wax according to claim 1, characterized in that: The vinyl acetate content in the ethylene-vinyl acetate copolymer is 28wt% and the melt index is 400g / 10min; the melting point of the stearic acid is 67-72°C.
4. The modified precision casting wax according to claim 1, characterized in that: The Piccotex 75 resin is a copolymer of α-methylstyrene and vinyltoluene, with a molar ratio of 75 / 25 and a softening point of 75°C.
5. The modified precision casting wax according to claim 1, characterized in that: The viscosity of the hydroxyethyl cellulose is 5000-6400 MPa·s (25° C.).
6. The modified precision casting wax according to claim 1, characterized in that: 80% of the starch and hydroxyethyl cellulose can pass through a 100-mesh sieve, and 50% can pass through a 200-mesh sieve.
7. A method for preparing a modified precision casting wax, characterized in that: A modified precision casting wax as claimed in any one of claims 1 to 6 is used, and the preparation method comprises the following steps: (1) First, heat microcrystalline wax, paraffin wax and stearic acid at 80-100°C and stir until they are melted, add Piccotex75 resin, raise the temperature to 100-110°C and continue stirring, and keep the temperature for 20-40 minutes; (2) Continue to raise the temperature to 120-130° C., add ethylene-vinyl acetate copolymer, keep the temperature for 20-50 minutes and continue stirring until it is completely melted; (3) Continue heating at 120-130° C., add terpene resin, and keep warm for 1-1.5 hours until it is completely melted and becomes transparent; (4) Cooling the material to 90-100°C, continuing to add montan wax, carnauba wax, candelilla wax, and rosin glycerol ester, and continuing to stir until the mixture is uniform, then cooling to 90-100°C and keeping warm for 30-60 minutes; (5) At 90-100° C., D-mannitol, adipic acid, and hydroxyethyl cellulose are added in sequence, with or without starch, and the mixture is cooled to form granules to obtain precision casting wax.
8. An application of a modified precision casting wax, characterized in that: The modified precision casting wax is prepared by the preparation method of a modified precision casting wax as described in claim 7, and the modified precision casting wax is used for preparing wax models of high-precision aviation casting structural parts.
Citation Information
Patent Citations
Preparation method of investment casting wax
CN108329701A
Quick-dry composite wax for investment casting
CN109265847A
Repairing wax for investment casting and preparation method of repairing wax
CN110205092A
Cited By
Casting wax pattern material and preparation method thereof
CN120842867A