Flame-retardant heat-insulating fabric for fire-fighting clothes and preparation process thereof
Through modified polyester fiber wire and chemical modification treatment, fire-fighting clothing fabrics with flame-retardant outer layer, heat-insulating core layer and antibacterial inner layer were prepared, which solved the problems of flammable polyester fibers and insufficient antibacterial properties of cotton fabrics, and achieved efficient flame-retardant, heat-insulating and antibacterial comprehensive performance.
Patent Information
- Application Number
- CN202510477287.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-16
- Publication Date
- 2025-07-08
- Estimated Expiration
- 2045-04-16
AI Technical Summary
The polyester fibers in existing fire-fighting clothing are flammable and have poor flame retardancy, and the cotton fabrics have insufficient antibacterial and durability, which affects service life and comfort.
Modified polyester fiber wire braided flame-retardant outer layer fabric, synthetic fiber and aramid fiber blended with heat-insulating core fabric, and modified ε-polylysine hydrochloride treated cotton grey fabric to make an antibacterial inner layer fabric, and the compatibility and binding force between each layer is improved through specific chemical modification.
It improves the flame retardant performance, thermal stability and antibacterial durability of flame retardant insulation fabrics, extends the service life of fire-fighting clothing and improves comfort.
Smart Images

Figure CN120269888A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fire-fighting fabrics, and particularly relates to a flame-retardant and heat-insulating fabric for fire-fighting clothing and a preparation process thereof. Background Art
[0002] Fire is a disaster that poses a serious threat to human life, property and social order. Firefighters need to face extreme high-temperature environments during fire extinguishing and rescue operations. Therefore, the flame-retardant and heat-insulating performance of fire-fighting clothing is crucial.
[0003] Due to its excellent heat insulation, wear resistance and wrinkle resistance, polyester fiber fabric can withstand the friction and mechanical stress during fire-fighting operations, and is not easily deformed after washing, which can ensure the long-term structural integrity of fire-fighting clothing. Therefore, it can be applied to fire-fighting clothing. Ordinary polyester fiber is flammable, and usually needs to add a flame retardant to improve its flame-retardant performance. Ammonium polyphosphate is an inorganic phosphorus-based compound flame retardant containing both P and N elements. It has good heat resistance and flame retardancy, and no harmful gases are generated during combustion. It can replace halogen-based and organophosphorus-based flame retardants in polymer materials. However, when ammonium polyphosphate is used alone, it has poor dispersibility, is easy to precipitate, and has poor compatibility with the matrix. Therefore, directly adding ammonium polyphosphate to polyester fiber fabric is difficult to ensure its flame retardancy.
[0004] In addition, cotton fabric has good moisture absorption and air permeability. Using it as the inner layer material of fire-fighting clothing can improve the comfort of fire-fighting clothing. When firefighters carry out long-term rescue operations, the heat and sweat generated by the body itself are easy to breed bacteria, reducing the wearing comfort. And cotton fabric usually does not have antibacterial properties. To make cotton fabric have antibacterial properties, it usually needs to be subjected to antibacterial finishing. However, currently, the principle of antibacterial finishing of cotton fabric is that the antibacterial agent is adsorbed on the surface of cotton fabric through van der Waals force or hydrogen bond, etc. But the adsorption amount will be significantly reduced after washing, resulting in poor antibacterial persistence of cotton fabric.
[0005] Based on this, we propose a flame-retardant and heat-insulating fabric for fire-fighting clothing with antibacterial persistence and a preparation process thereof to extend the service life of fire-fighting clothing. Summary of the Invention
[0006] Aiming at the deficiencies of the existing technology, the purpose of the present invention is to provide a flame-retardant and heat-insulating fabric for fire-fighting clothing and a preparation process thereof.
[0007] A flame-retardant and heat-insulating fabric for fire-fighting clothing includes a flame-retardant outer layer fabric, a heat-insulating core layer fabric and an antibacterial inner layer fabric;
[0008] The flame-retardant outer layer fabric is woven from modified polyester fiber filaments. Among them, the preparation raw materials of the modified polyester fiber filaments include polyester powder, coated modified ammonium polyphosphate, modified expanded perlite and polyester chips;
[0009] The heat-insulating core layer fabric is made by blending synthetic fiber and aramid fiber in a mass ratio of 1:(2 - 3). Among them, the raw materials for preparing the synthetic fiber include polyvinyl chloride, ethylene-propylene rubber, sodium stearate, bamboo charcoal powder, sepiolite nanofibers, KH-550 coupling agent, cellulose ester, and sodium alginate;
[0010] The antibacterial inner layer fabric is made by soaking cotton grey cloth with a modified treatment solution. Among them, the raw materials for preparing the modified treatment solution include ε-polylysine hydrochloride, epoxidized linseed oil, sodium hydroxide solution, Tween 80, glacial acetic acid, citric acid, and deionized water.
[0011] A preparation process of a flame-retardant and heat-insulating fabric for fire-fighting clothing is characterized by including the following steps:
[0012] S1: Prepare coated modified ammonium polyphosphate
[0013] Disperse ammonium polyphosphate in deionized water, then add polyethyleneimine for preliminary coating, and then add a solution of hydroxyethylidene diphosphonic acid for reaction to obtain coated modified ammonium polyphosphate;
[0014] S2: Modify expanded perlite
[0015] Dissolve γ-aminopropyltriethoxysilane in an ethanol solution, then add expanded perlite for reaction, and then add dimethyl hydroxymethylphosphonate for reaction to obtain modified expanded perlite;
[0016] S3: Prepare the flame-retardant outer layer fabric
[0017] Mix polyester powder, the above-mentioned coated modified ammonium polyphosphate, and the above-mentioned modified expanded perlite and granulate them to make a modified polyester masterbatch, then make modified polyester fiber filaments with polyester chips, and then carry out plain weave to make the flame-retardant outer layer fabric;
[0018] S4: Prepare the heat-insulating core layer fabric
[0019] Mix polyvinyl chloride, ethylene-propylene rubber, sodium stearate, bamboo charcoal powder, and sepiolite nanofibers evenly and heat them to a molten state, then add KH-550 coupling agent, cellulose ester, and sodium alginate and continue to mix evenly and extrude to obtain synthetic fiber, and then blend the synthetic fiber with aramid fiber to obtain the heat-insulating core layer fabric;
[0020] S5: Prepare the antibacterial inner layer fabric
[0021] Prepare an ε-polylysine hydrochloride solution and an epoxidized linseed oil emulsion respectively, then mix and heat them for reaction to obtain modified ε-polylysine hydrochloride. After dissolving, add citric acid and treat the cotton grey cloth to obtain the antibacterial inner layer fabric;
[0022] S6: Bonding
[0023] The flame-retardant outer layer fabric, the heat-insulating core layer fabric and the antibacterial inner layer fabric are sequentially bonded to obtain the flame-retardant heat-insulating fabric.
[0024] Furthermore, S1 specifically includes the following steps:
[0025] S1.1: Add ammonium polyphosphate into deionized water at a solid-liquid ratio of 1 g: (20-30) mL, disperse by ultrasonic for 20-30 min, and then add 0.1 mol / L dilute hydrochloric acid to adjust the pH to 5-6 to obtain an ammonium polyphosphate dispersion;
[0026] S1.2: Add polyethyleneimine to the above ammonium polyphosphate dispersion and stir at a constant temperature of 50-60°C for 2-3 hours to obtain a preliminary coated ammonium polyphosphate mixed solution;
[0027] S1.3: Dissolve hydroxyethylidene diphosphonic acid in deionized water at a solid-liquid ratio of 1g: (30-40)mL to obtain a hydroxyethylidene diphosphonic acid solution, then add the hydroxyethylidene diphosphonic acid solution to the above-mentioned preliminary coated ammonium polyphosphate mixed solution, and add 0.1mol / L dilute hydrochloric acid to adjust the pH to 4-5, then continue to keep warm and stir for 3-4h, and obtain the coated modified ammonium polyphosphate after centrifugation, filtration, washing and drying.
[0028] Furthermore, S2 specifically includes the following steps:
[0029] S2.1: Add γ-aminopropyltriethoxysilane to 60% ethanol solution at a solid-liquid ratio of 1 g: (10-12) mL, stir thoroughly to dissolve, and then add acetic acid to adjust the pH to 4-5 to obtain a γ-aminopropyltriethoxysilane solution;
[0030] S2.2: The expanded perlite is ultrasonically cleaned with deionized water and dried to constant weight, and then added to the above-mentioned γ-aminopropyltriethoxysilane solution at a solid-liquid ratio of 1g:(5-6)mL, and heated and stirred at 70-80°C for 3-4h to obtain an amination expanded perlite solution;
[0031] S2.3: Add dimethyl hydroxymethylphosphonate to the above-mentioned amino expanded perlite solution at a solid-liquid ratio of 1g:(12-16)mL, and add 0.1mol / L hydrochloric acid to adjust the pH to 2-3, heat and stir at 80-90℃ for 10-12h, cool, centrifuge, wash to neutrality and dry to obtain modified expanded perlite.
[0032] Furthermore, S3 specifically includes the following steps:
[0033] S3.1: Evenly mix the polyester powder, the coated modified ammonium polyphosphate obtained in step S1.3 and the modified expanded perlite obtained in step S2.3, and extrude and granulate them through a twin-screw extruder to obtain a modified polyester masterbatch;
[0034] S3.2: Mix the above-mentioned modified polyester masterbatch and polyester chips according to a mass ratio of 1:(5 - 7) for spinning to obtain modified polyester fiber filaments, and then perform plain weaving to obtain a flame-retardant outer fabric.
[0035] Further, S5 specifically includes the following steps:
[0036] S5.1: Add ε-polylysine hydrochloride to deionized water according to a solid-liquid ratio of 1 g:(10 - 20) mL, stir well to dissolve, and then add 0.1 mol / L sodium hydroxide solution to adjust the pH to 10 - 11 to obtain an ε-polylysine hydrochloride solution;
[0037] S5.2: Add Tween 80 to deionized water according to a mass ratio of 1:(10 - 15), stir well to dissolve, then add epoxidized linseed oil with an epoxy value of 6 - 8% according to an oil-water ratio of 1:(4 - 6), and stir and emulsify at 1000 - 1500 r / min for 20 - 30 min to obtain an epoxidized linseed oil emulsion;
[0038] S5.3: Add the above-mentioned epoxidized linseed oil emulsion to the above-mentioned ε-polylysine hydrochloride solution according to a mass ratio of 1:(6 - 8), heat and stir at 50 - 60 °C for 4 - 6 h, then add glacial acetic acid to adjust the pH to neutral, and after dialysis purification and freeze-drying, obtain modified ε-polylysine hydrochloride;
[0039] S5.4: Dissolve the above-mentioned modified ε-polylysine hydrochloride in deionized water to prepare a solution with a mass fraction of 1 - 3%, and then add 0.2 - 0.3 wt% citric acid catalyst, stir and mix evenly to obtain a modified treatment liquid;
[0040] S5.5: Immerse the cotton grey fabric in the above-mentioned modified treatment liquid according to a bath ratio of 1:(15 - 25), heat and soak at 50 - 60 °C for 1 - 2 h, take it out, wash and dry it to obtain an antibacterial inner fabric.
[0041] Further, the addition amount of polyethyleneimine is 15 - 20% of the mass of ammonium polyphosphate.
[0042] Further, the addition amount of hydroxyethylidene diphosphonic acid is 40 - 50% of the mass of polyethyleneimine.
[0043] Further, the mass ratio of polyester powder, coated and modified ammonium polyphosphate and modified expanded perlite is (35 - 45):(3 - 5):1.
[0044] Furthermore, by mass, the raw materials of the synthetic fiber include: 30-40 parts of polyvinyl chloride, 10-20 parts of ethylene-propylene rubber, 2-3 parts of sodium stearate, 3-5 parts of bamboo charcoal powder, 2-4 parts of sepiolite nanofibers, 2-4 parts of KH-550 coupling agent, 1-2 parts of cellulose ester, and 1-2 parts of sodium alginate.
[0045] Compared with the prior art, the present invention has at least the following beneficial effects:
[0046] 1. The flame-retardant and heat-insulating fabric for fire-fighting clothing of the present invention is bonded by a flame-retardant outer fabric, a heat-insulating core fabric, and an antibacterial inner fabric. Among them, by first dispersing ammonium polyphosphate in deionized water and adding polyethyleneimine under acidic conditions, the amino group on polyethyleneimine first undergoes an ion exchange reaction with the ammonium ion of ammonium polyphosphate to preliminarily coat ammonium polyphosphate, and then adding a solution of hydroxyethylidene diphosphonic acid for a salt-forming reaction to prepare coated and modified ammonium polyphosphate with a core-shell structure. Since ammonium polyphosphate is modified by hydroxyethylidene diphosphonic acid and polyethyleneimine, the compatibility of ammonium polyphosphate with the polyester matrix can be effectively improved, and the problem of the reduction of the flame-retardant performance of the flame-retardant outer fabric caused by the precipitation of ammonium polyphosphate can be improved. Therefore, after mixing and granulating the coated and modified ammonium polyphosphate with polyester powder and then making it into a flame-retardant outer fabric, the flame-retardant performance of the flame-retardant outer fabric can be effectively improved.
[0047] 2. In the present invention, by first surface-modifying expanded perlite with γ-aminopropyltriethoxysilane to introduce amino groups on its surface, and then adding dimethyl hydroxymethylphosphonate. On the one hand, the phosphonate group in dimethyl hydroxymethylphosphonate undergoes electrostatic attraction with the protonated amino group on the surface of amino-functionalized expanded perlite in an acidic environment. On the other hand, the hydroxymethyl group in dimethyl hydroxymethylphosphonate forms a hydrogen bond network with the hydroxyl group on the surface of expanded perlite, thereby grafting dimethyl hydroxymethylphosphonate on the surface of expanded perlite to modify it, and further achieving the effect of improving the dispersibility of expanded perlite in the polyester matrix and preventing agglomeration. In addition, after mixing and granulating the modified expanded perlite with polyester powder and then making it into modified polyester fiber filaments, not only can the thermal stability of the modified polyester fiber filaments be effectively improved, but also the flame-retardant and heat-insulating properties of the obtained flame-retardant outer fabric can be further improved.
[0048] 3. In the present invention, by first separately preparing an ε-polylysine hydrochloride solution and an epoxidized linseed oil emulsion, then adding the epoxidized linseed oil emulsion to the ε-polylysine hydrochloride solution, heating and stirring for reaction, using one epoxy group in the epoxidized linseed oil to react with the amino group of the ε-polylysine hydrochloride to modify the ε-polylysine hydrochloride, and treating the cotton grey fabric with the modified ε-polylysine hydrochloride, the remaining epoxy groups of the epoxy linseed oil in the modified ε-polylysine hydrochloride react with the hydroxyl groups of the cotton fibers to generate ether bonds and hydroxyl groups, forming a crosslinked network, thereby improving the binding force between the antibacterial ε-polylysine hydrochloride and the cotton grey fabric, and further achieving the effect of improving the antibacterial persistence of the prepared antibacterial inner layer fabric. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] The accompanying drawings incorporated herein and constituting a part of the specification illustrate embodiments of the present disclosure and, together with the specification, are further used to explain the principles of the present disclosure and enable those skilled in the relevant art to implement and use the present disclosure.
[0050] Figure 1 It is a process flow chart of the preparation of the flame retardant and heat insulation fabric for fire fighting clothing adopted in the embodiments of the present invention. DETAILED DESCRIPTION OF THE EMBODIMENTS
[0051] The following describes in detail a flame retardant and heat insulation fabric for fire fighting clothing and its preparation process provided by the present invention with reference to the accompanying drawings and specific embodiments.
[0052] Example 1
[0053] A preparation process of a flame retardant and heat insulation fabric for fire fighting clothing, as Figure 1 shown, includes the following steps:
[0054] S1: Prepare coated ammonium polyphosphate
[0055] S1.1: Add ammonium polyphosphate to deionized water according to a solid-liquid ratio of 1 g: 20 mL, ultrasonically disperse for 20 min, and then add 0.1 mol / L dilute hydrochloric acid to adjust the pH to 5 to obtain an ammonium polyphosphate dispersion;
[0056] S1.2: Add polyethyleneimine to the above ammonium polyphosphate dispersion and stir at a constant temperature of 50 °C for 2 h to obtain a preliminarily coated ammonium polyphosphate mixture, wherein the addition amount of polyethyleneimine is 15% of the mass of ammonium polyphosphate;
[0057] S1.3: Dissolve hydroxyethylidene diphosphonic acid in deionized water at a solid-liquid ratio of 1g:30mL to obtain a hydroxyethylidene diphosphonic acid solution, then add the hydroxyethylidene diphosphonic acid solution to the above-mentioned preliminary coated ammonium polyphosphate mixed solution, and add 0.1mol / L dilute hydrochloric acid to adjust the pH to 4, then continue to keep warm and stir for 3h, centrifuge, filter, wash and dry to obtain a coated modified ammonium polyphosphate, wherein the amount of hydroxyethylidene diphosphonic acid added is 40% of the mass of polyethyleneimine;
[0058] S2: Modified expanded perlite
[0059] S2.1: Add γ-aminopropyltriethoxysilane to 60% ethanol solution at a solid-liquid ratio of 1 g:10 mL, stir thoroughly to dissolve, and then add acetic acid to adjust the pH to 4 to obtain a γ-aminopropyltriethoxysilane solution;
[0060] S2.2: The expanded perlite is ultrasonically cleaned with deionized water and dried to constant weight, and then added to the above-mentioned γ-aminopropyltriethoxysilane solution at a solid-liquid ratio of 1g:5mL, and heated and stirred at 70°C for 3-4h to obtain an amination expanded perlite solution;
[0061] S2.3: Add dimethyl hydroxymethylphosphonate to the above-mentioned amino expanded perlite solution at a solid-liquid ratio of 1g:12mL, and add 0.1mol / L hydrochloric acid to adjust the pH to 2, heat and stir at 80°C for 10h, cool, centrifuge, filter, wash to neutrality and dry to obtain modified expanded perlite;
[0062] S3: Preparation of flame retardant outer fabric
[0063] S3.1: uniformly mixing polyester powder, the coated modified ammonium polyphosphate obtained in step S1.3 and the modified expanded perlite obtained in step S2.3 in a mass ratio of 35:3:1, and extruding and granulating through a twin-screw extruder to obtain a modified polyester masterbatch;
[0064] S3.2: The modified polyester masterbatch and the polyester chips are mixed in a mass ratio of 1:5 and spun to obtain modified polyester fiber yarn, which is then plain woven to obtain a flame retardant outer fabric;
[0065] S4: Preparation of thermal insulation core fabric
[0066] 30 parts by mass of polyvinyl chloride, 10 parts by mass of ethylene-propylene rubber, 2 parts by mass of sodium stearate, 3 parts by mass of bamboo charcoal powder and 2 parts by mass of sepiolite nanofibers are mixed uniformly and heated to a molten state, and then 2 parts by mass of KH-550 coupling agent, 1 part by mass of cellulose ester and 1 part by mass of sodium alginate are added, and the mixture is continued to be mixed uniformly and extruded to obtain synthetic fibers, and then the synthetic fibers are blended with aramid fibers at a mass ratio of 1:2 to obtain a heat-insulating core fabric;
[0067] S5: Prepare the antibacterial inner fabric
[0068] S5.1: Add ε-polylysine hydrochloride into deionized water according to the solid-liquid ratio of 1 g: 10 mL, stir well to dissolve, and then add 0.1 mol / L sodium hydroxide solution to adjust the pH to 10 to obtain an ε-polylysine hydrochloride solution;
[0069] S5.2: Add Tween 80 into deionized water according to the mass ratio of 1:10, stir well to dissolve, then add epoxidized linseed oil with an epoxy value of 6% according to the oil-water ratio of 1:4, and stir and emulsify at 1000 r / min for 20 min to obtain an epoxidized linseed oil emulsion;
[0070] S5.3: Add the above epoxidized linseed oil emulsion into the above ε-polylysine hydrochloride solution according to the mass ratio of 1:6, heat and stir at 50 °C for 4 h, then add glacial acetic acid to adjust the pH to neutral, and after dialysis purification and freeze-drying, obtain modified ε-polylysine hydrochloride;
[0071] S5.4: Dissolve the above modified ε-polylysine hydrochloride in deionized water to prepare a solution with a mass fraction of 1%, and then add 0.2 wt% catalyst citric acid, stir and mix evenly to obtain a modified treatment solution;
[0072] S5.5: Immerse the cotton grey fabric in the above modified treatment solution according to the bath ratio of 1:15, heat and soak at 50 °C for 1 h, take it out, wash with water and dry to obtain the antibacterial inner fabric;
[0073] S6: Bonding
[0074] Bond the above flame-retardant outer fabric, heat-insulating core fabric and antibacterial inner fabric in sequence to obtain a flame-retardant and heat-insulating fabric.
[0075] Example 2
[0076] A preparation process of a flame-retardant and heat-insulating fabric for fire-fighting clothing, as Figure 1 shown, includes the following steps:
[0077] S1: Prepare coated and modified ammonium polyphosphate
[0078] S1.1: Add ammonium polyphosphate into deionized water according to the solid-liquid ratio of 1 g: 25 mL, ultrasonically disperse for 25 min, and then add 0.1 mol / L dilute hydrochloric acid to adjust the pH to 5.5 to obtain an ammonium polyphosphate dispersion;
[0079] S1.2: Add polyethyleneimine to the above ammonium polyphosphate dispersion and stir at a constant temperature of 55 °C for 2.5 h to obtain a preliminarily coated ammonium polyphosphate mixture, wherein the addition amount of polyethyleneimine is 17.5% of the mass of ammonium polyphosphate;
[0080] S1.3: Dissolve hydroxyethane diphosphonic acid in deionized water according to a solid-liquid ratio of 1 g: 35 mL to obtain a hydroxyethane diphosphonic acid solution. Then add the hydroxyethane diphosphonic acid solution to the above-mentioned preliminarily coated ammonium polyphosphate mixture, and add 0.1 mol / L dilute hydrochloric acid to adjust the pH to 4.5. Then continue to keep warm and stir for 3.5 h, and after centrifugation, filtration, washing and drying, obtain coated and modified ammonium polyphosphate, wherein the addition amount of hydroxyethane diphosphonic acid is 45% of the mass of polyethyleneimine;
[0081] S2: Modified expanded perlite
[0082] S2.1: Add γ-aminopropyltriethoxysilane to a 60% ethanol solution according to a solid-liquid ratio of 1 g: 11 mL, stir well to dissolve, and then add acetic acid to adjust the pH to 4.5 to obtain a γ-aminopropyltriethoxysilane solution;
[0083] S2.2: Ultrasonically clean the expanded perlite with deionized water and dry it to a constant weight, and then add it to the above-mentioned γ-aminopropyltriethoxysilane solution according to a solid-liquid ratio of 1 g: 5.5 mL, and heat and stir at 75 °C for 3.5 h to obtain an amino-functionalized expanded perlite solution;
[0084] S2.3: Add dimethyl hydroxymethylphosphonate to the above-mentioned amino-functionalized expanded perlite solution according to a solid-liquid ratio of 1 g: 14 mL, and add 0.1 mol / L hydrochloric acid to adjust the pH to 2.5, and heat and stir at 85 °C for 11 h. After cooling, centrifuge, filter, wash to neutrality and dry to obtain modified expanded perlite;
[0085] S3: Prepare a flame-retardant outer fabric
[0086] S3.1: Uniformly mix polyester powder, the coated and modified ammonium polyphosphate prepared in step S1.3 and the modified expanded perlite prepared in step S2.3 according to a mass ratio of 40: 4: 1, and extrude and pelletize through a twin-screw extruder to obtain a modified polyester masterbatch;
[0087] S3.2: Mix the above-mentioned modified polyester masterbatch and polyester chips according to a mass ratio of 1: 6 for spinning to obtain modified polyester fiber filaments, and then perform plain weaving to obtain a flame-retardant outer fabric;
[0088] S4: Prepare a heat-insulating core fabric
[0089] Mix 35 parts by mass of polyvinyl chloride, 15 parts by mass of ethylene-propylene rubber, 2.5 parts by mass of sodium stearate, 4 parts by mass of bamboo charcoal powder and 3 parts by mass of sepiolite nanofibers evenly and heat to the molten state, then add 3 parts by mass of KH-550 coupling agent, 1.5 parts by mass of cellulose ester and 1.5 parts by mass of sodium alginate, continue to mix evenly and extrude to obtain synthetic fibers, and then blend the synthetic fibers and aramid fibers according to the mass ratio of 1:2.5 to obtain the heat-insulating core layer fabric;
[0090] S5: Prepare the antibacterial inner layer fabric
[0091] S5.1: Add ε-polylysine hydrochloride to deionized water according to the solid-liquid ratio of 1 g:15 mL, stir well to dissolve, and then add 0.1 mol / L sodium hydroxide solution to adjust the pH to 10.5 to obtain an ε-polylysine hydrochloride solution;
[0092] S5.2: Add Tween 80 to deionized water according to the mass ratio of 1:12.5, stir well to dissolve, then add epoxidized linseed oil with an epoxy value of 7% according to the oil-water ratio of 1:5, and stir and emulsify at 1250 r / min for 25 min to obtain an epoxidized linseed oil emulsion;
[0093] S5.3: Add the above epoxidized linseed oil emulsion to the above ε-polylysine hydrochloride solution according to the mass ratio of 1:7, heat and stir at 55 °C for 5 h, then add glacial acetic acid to adjust the pH to neutral, and obtain modified ε-polylysine hydrochloride through dialysis purification and freeze-drying;
[0094] S5.4: Dissolve the above modified ε-polylysine hydrochloride in deionized water to prepare a solution with a mass fraction of 2%, and then add 0.25 wt% catalyst citric acid, stir and mix evenly to obtain a modified treatment solution;
[0095] S5.5: Immerse the cotton grey fabric in the above modified treatment solution according to the bath ratio of 1:20, heat and soak at 55 °C for 1.5 h, take it out, wash and dry to obtain the antibacterial inner layer fabric;
[0096] S6: Bonding
[0097] Bond the above flame-retardant outer layer fabric, heat-insulating core layer fabric and antibacterial inner layer fabric in sequence to obtain the flame-retardant and heat-insulating fabric.
[0098] Example 3
[0099] A preparation process of a flame-retardant and heat-insulating fabric for fire-fighting clothing, as Figure 1 shown, includes the following steps:
[0100] S1: Prepare coated modified ammonium polyphosphate
[0101] S1.1: Add ammonium polyphosphate into deionized water at a solid-liquid ratio of 1 g:30 mL, disperse by ultrasonic for 30 min, and then add 0.1 mol / L dilute hydrochloric acid to adjust the pH to 6 to obtain an ammonium polyphosphate dispersion;
[0102] S1.2: Add polyethyleneimine to the above ammonium polyphosphate dispersion and stir at a constant temperature of 60°C for 3 hours to obtain a preliminary coated ammonium polyphosphate mixed solution, wherein the amount of polyethyleneimine added is 20% of the mass of the ammonium polyphosphate;
[0103] S1.3: Dissolve hydroxyethylidene diphosphonic acid in deionized water at a solid-liquid ratio of 1g:40mL to obtain a hydroxyethylidene diphosphonic acid solution, then add the hydroxyethylidene diphosphonic acid solution to the above-mentioned preliminary coated ammonium polyphosphate mixed solution, and add 0.1mol / L dilute hydrochloric acid to adjust the pH to 5, then continue to keep warm and stir for 4h, centrifuge, filter, wash and dry to obtain a coated modified ammonium polyphosphate, wherein the amount of hydroxyethylidene diphosphonic acid added is 50% of the mass of polyethyleneimine;
[0104] S2: Modified expanded perlite
[0105] S2.1: Add γ-aminopropyltriethoxysilane to 60% ethanol solution at a solid-liquid ratio of 1 g:12 mL, stir thoroughly to dissolve, and then add acetic acid to adjust the pH to 5 to obtain a γ-aminopropyltriethoxysilane solution;
[0106] S2.2: The expanded perlite is ultrasonically cleaned with deionized water and dried to constant weight, and then added to the above-mentioned γ-aminopropyltriethoxysilane solution at a solid-liquid ratio of 1g:6mL, and heated and stirred at 80°C for 4h to obtain an amination expanded perlite solution;
[0107] S2.3: Add dimethyl hydroxymethylphosphonate to the above-mentioned amino expanded perlite solution at a solid-liquid ratio of 1g:16mL, and add 0.1mol / L hydrochloric acid to adjust the pH to 3, heat and stir at 90°C for 12h, cool, centrifuge, filter, wash to neutrality and dry to obtain modified expanded perlite;
[0108] S3: Preparation of flame retardant outer fabric
[0109] S3.1: Evenly mix the polyester powder, the coated modified ammonium polyphosphate obtained in step S1.3, and the modified expanded perlite obtained in step S2.3 in a mass ratio of 45:5:1, and extrude and granulate them through a twin-screw extruder to obtain a modified polyester masterbatch;
[0110] S3.2: The modified polyester masterbatch and the polyester chips are mixed in a mass ratio of 1:7 and spun to obtain modified polyester fiber yarn, which is then plain woven to obtain a flame retardant outer fabric;
[0111] S4: Preparation of thermal insulation core fabric
[0112] 40 parts by mass of polyvinyl chloride, 20 parts by mass of ethylene-propylene rubber, 3 parts by mass of sodium stearate, 5 parts by mass of bamboo charcoal powder and 4 parts by mass of sepiolite nanofibers are mixed uniformly and heated to a molten state, and then 4 parts by mass of KH-550 coupling agent, 2 parts by mass of cellulose ester and 2 parts by mass of sodium alginate are added, and the mixture is continued to be mixed uniformly and extruded to obtain synthetic fibers, and then the synthetic fibers are blended with aramid fibers at a mass ratio of 1:3 to obtain a heat-insulating core fabric;
[0113] S5: Preparation of antibacterial inner fabric
[0114] S5.1: Add ε-polylysine hydrochloride to deionized water at a solid-liquid ratio of 1 g:20 mL, stir thoroughly to dissolve, and then add 0.1 mol / L sodium hydroxide solution to adjust the pH to 11 to obtain an ε-polylysine hydrochloride solution;
[0115] S5.2: Tween 80 is added to deionized water at a mass ratio of 1:15, and the mixture is stirred and dissolved, and then epoxidized linseed oil with an epoxide value of 8% is added at an oil-water ratio of 1:6, and the mixture is stirred and emulsified at 1500 r / min for 30 min to obtain an epoxidized linseed oil emulsion;
[0116] S5.3: adding the epoxidized linseed oil emulsion to the ε-polylysine hydrochloride solution at a mass ratio of 1:8, heating and stirring at 60° C. for 6 h, then adding glacial acetic acid to adjust the pH to neutral, dialysis purification and freeze drying to obtain modified ε-polylysine hydrochloride;
[0117] S5.4: dissolving the modified ε-polylysine hydrochloride in deionized water to prepare a solution with a mass fraction of 3%, adding 0.3wt% of catalyst citric acid, stirring and mixing to obtain a modified treatment solution;
[0118] S5.5: Immerse the cotton grey fabric in the above-mentioned modified treatment solution at a bath ratio of 1:25, and heat and soak it at 60°C for 2 hours. After taking it out, wash it with water and dry it to obtain the antibacterial inner layer fabric;
[0119] S6: Bonding
[0120] The flame-retardant outer layer fabric, the heat-insulating core layer fabric and the antibacterial inner layer fabric are sequentially bonded to obtain the flame-retardant heat-insulating fabric.
[0121] Comparative Example 1
[0122] The difference between this comparative example 1 and example 1 is that step S1 is removed, and the coated modified ammonium polyphosphate in step S3.1 is replaced by an equal amount of ammonium polyphosphate.
[0123] Comparative Example 2
[0124] The difference between Comparative Example 2 and Example 1 is that step S2 is removed, and the modified expanded perlite in step S3.1 is removed.
[0125] Comparative Example 3
[0126] The difference between Comparative Example 3 and Example 1 is that step S2 is removed, and the modified expanded perlite in step S3.1 is replaced with an equal amount of expanded perlite.
[0127] Comparative Example 4
[0128] The difference between Comparative Example 4 and Example 1 is that steps S5.1 - 5.3 are removed, and the modified ε - polylysine hydrochloride in step S5.4 is replaced with an equal amount of ε - polylysine hydrochloride.
[0129] Test Example
[0130] Test 1: According to GB / T5454 - 1997, the limiting oxygen index of the flame - retardant outer fabric prepared in Examples 1 - 3 and Comparative Examples 1 - 2 was tested, and the results are shown in Table 1.
[0131] Table 1: Test results of the limiting oxygen index of the flame - retardant outer fabric
[0132] Limiting oxygen index (%) Example 1 36.2 Example 2 36.1 Example 3 36.4 Comparative Example 1 29.5 Comparative Example 3 33.8
[0133] As shown in Table 1, in Comparative Example 1, after the ammonium polyphosphate was not surface - coated and modified, the ammonium polyphosphate was directly added to the polyester powder to make a polyester masterbatch, which was then mixed and spun with polyester chips to make polyester fiber filaments, and then made into a flame - retardant outer fabric. The limiting oxygen index of the obtained flame - retardant outer fabric was much lower than that of Example 1. Thus, it can be seen that after modifying the ammonium polyphosphate with hydroxyethylidene diphosphonic acid and polyethyleneimine, not only can the compatibility between the ammonium polyphosphate and the polyester matrix be effectively improved, and the problem of the reduction of the flame - retardant performance of the flame - retardant outer fabric caused by the precipitation of ammonium polyphosphate be improved, but also the flame - retardant performance of the flame - retardant outer fabric can be further improved;
[0134] In addition, in Comparative Example 3, after the expanded perlite was not modified, the limiting oxygen index of the obtained flame - retardant outer fabric was also lower than that of Example 1, indicating that grafting dimethyl hydroxymethylphosphonate on the surface of the expanded perlite and modifying it can further improve the flame - retardant performance of the obtained flame - retardant outer fabric.
[0135] Test 2: According to GA10 - 2014, the dimensional change rate of the flame - retardant outer fabric prepared in Examples 1 - 3 and Comparative Example 2 was tested to reflect its thermal stability, and the results are shown in Table 2.
[0136] Table 2: Test results of the dimensional change rate of the flame - retardant outer fabric
[0137] Dimensional change rate (%) Example 1 0.76 Example 2 0.74 Example 3 0.73 Comparative Example 2 1.24
[0138] As shown in Table 2, the dimensional change rate of the flame-retardant outer fabric prepared without adding modified expanded perlite in Comparative Example 2 is higher than that in Example 1, indicating that the addition of modified expanded perlite can effectively improve the thermal stability of the flame-retardant outer fabric.
[0139] Test 3: The clo values of the flame-retardant and heat-insulating fabrics prepared in Examples 1-3 and Comparative Examples 2-3 were measured in accordance with GB / T 11048-2018, and the results are shown in Table 3.
[0140] Table 3: Test results of clo values of flame-retardant and heat-insulating fabrics
[0141] <![CDATA[Clo value (m 2 ·C / W)]]> Example 1 1.163 Example 2 1.168 Example 3 1.171 Comparative Example 2 0.903 Comparative Example 3 1.026
[0142] As shown in Table 3, when no modified expanded perlite is added to the flame-retardant outer fabric in Comparative Example 2, the clo value of the prepared flame-retardant and heat-insulating fabric is lower than that in Example 1. Thus, it can be seen that after adding modified expanded perlite, the heat-insulating performance of the flame-retardant outer fabric can be improved, and further the heat-insulating performance of the flame-retardant and heat-insulating fabric can be improved. When the expanded perlite is not modified in Comparative Example 3, the clo value of the prepared flame-retardant and heat-insulating fabric is also lower than that in Example 1, indicating that after modifying the expanded perlite with dimethyl hydroxymethyl phosphonate, the dispersibility of the expanded perlite can be effectively improved, and further the heat-insulating performance of the flame-retardant and heat-insulating fabric can be improved.
[0143] Test 4: Referring to GB / T 20944.3—2008, the initial antibacterial rate and antibacterial rate after 50 washes of the antibacterial inner fabrics prepared in Examples 1-3 and Comparative Example 4 were tested. The test bacteria were Staphylococcus aureus. Each group of experiments was repeated three times, and the average value was taken. The results are shown in Table 4.
[0144] Table 4: Test results of initial antibacterial rate and antibacterial rate after 50 washes of antibacterial inner fabrics
[0145] Initial antibacterial rate (%) Antibacterial rate after 50 times of washing (%) Example 1 99.89 95.86 Example 2 99.93 95.83 Example 3 99.95 95.91 Comparative Example 4 99.72 58.77
[0146] As shown in Table 4, after the ε-polylysine hydrochloride is not modified with epoxidized linseed oil in Comparative Example 4, the antibacterial rate of the prepared antibacterial inner fabric decreases significantly after 50 washes, while the antibacterial rate of the antibacterial inner fabrics prepared in Examples 1-3 is above 95% after 50 washes. Thus, it can be seen that by modifying the ε-polylysine hydrochloride with epoxidized linseed oil and then treating the cotton grey fabric with the modified ε-polylysine hydrochloride, the binding force between the antibacterial ε-polylysine hydrochloride and the cotton grey fabric can be improved, and further the antibacterial persistence of the prepared antibacterial inner fabric can be achieved.
[0147] The above embodiments are only illustrative of the principles and effects of the present invention and are not intended to limit the present invention. Any person familiar with this technology can modify or change the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the technical field without departing from the spirit and technical idea disclosed by the present invention should still be covered by the claims of the present invention.
Claims
1. A flame-retardant and heat-insulating fabric for fire-fighting clothing, characterized in that, It includes a flame-retardant outer fabric, a heat-insulating core fabric, and an antibacterial inner fabric; The flame-retardant outer fabric is woven from modified polyester fiber filaments. Among them, the raw materials for preparing the modified polyester fiber filaments include polyester powder, coated modified ammonium polyphosphate, modified expanded perlite, and polyester chips; The heat-insulating core fabric is spun from synthetic fiber and aramid fiber in a mass ratio of 1:(2 - 3). Among them, the raw materials for preparing the synthetic fiber include polyvinyl chloride, ethylene-propylene rubber, sodium stearate, bamboo charcoal powder, sepiolite nanofibers, KH-550 coupling agent, cellulose ester, and sodium alginate; The antibacterial inner fabric is made by soaking cotton greige with a modified treatment liquid. Among them, the raw materials for preparing the modified treatment liquid include ε-polylysine hydrochloride, epoxidized linseed oil, sodium hydroxide solution, Tween 80, glacial acetic acid, citric acid, and deionized water.
2. The preparation process of the flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 1, characterized in that, It includes the following steps: S1: Prepare coated modified ammonium polyphosphate Disperse ammonium polyphosphate in deionized water, then add polyethyleneimine for preliminary coating, and then add hydroxyethylidene diphosphonic acid solution for reaction to obtain coated modified ammonium polyphosphate; S2: Modify expanded perlite Dissolve γ-aminopropyltriethoxysilane in ethanol solution, then add expanded perlite for reaction, and then add dimethyl hydroxymethylphosphonate for reaction to obtain modified expanded perlite; S3: Prepare the flame-retardant outer fabric Mix and granulate polyester powder, the above-mentioned coated modified ammonium polyphosphate, and the above-mentioned modified expanded perlite to make a modified polyester masterbatch, then make modified polyester fiber filaments with polyester chips, and then perform plain weave to make the flame-retardant outer fabric; S4: Prepare the heat-insulating core fabric Mix polyvinyl chloride, ethylene-propylene rubber, sodium stearate, bamboo charcoal powder, and sepiolite nanofibers evenly and heat to a molten state, then add KH-550 coupling agent, cellulose ester, and sodium alginate and continue to mix evenly and extrude to obtain synthetic fiber, and then blend the synthetic fiber with aramid fiber to obtain the heat-insulating core fabric; S5: Prepare the antibacterial inner fabric Prepare ε-polylysine hydrochloride solution and epoxidized linseed oil emulsion respectively, then mix and heat for reaction to obtain modified ε-polylysine hydrochloride. After dissolving, add citric acid and treat the cotton greige to obtain the antibacterial inner fabric; S6: Bonding Bond the above-mentioned flame-retardant outer fabric, heat-insulating core fabric, and antibacterial inner fabric in sequence to obtain the flame-retardant and heat-insulating fabric.
3. The preparation process of the flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 2, characterized in that, S1 specifically includes the following steps: S1.1: Add ammonium polyphosphate to deionized water according to a solid-liquid ratio of 1 g:(20 - 30) mL, ultrasonically disperse for 20 - 30 min, and then add 0.1 mol / L dilute hydrochloric acid to adjust the pH to 5 - 6 to obtain an ammonium polyphosphate dispersion; S1.2: Add polyethyleneimine to the above-mentioned ammonium polyphosphate dispersion and stir at a constant temperature of 50 - 60 °C for 2 - 3 h to obtain a preliminarily coated ammonium polyphosphate mixture; S1.3: Dissolve hydroxyethylidene diphosphonic acid in deionized water according to a solid-liquid ratio of 1 g : (30 - 40) mL to obtain a hydroxyethylidene diphosphonic acid solution. Then add the hydroxyethylidene diphosphonic acid solution to the above-mentioned preliminarily coated ammonium polyphosphate mixture, and add 0.1 mol / L dilute hydrochloric acid to adjust the pH to 4 - 5. Then continue to keep warm and stir for 3 - 4 h, and after centrifugation, filtration, washing and drying, obtain coated and modified ammonium polyphosphate.
4. The preparation process of the flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 3, characterized in that, S2 specifically includes the following steps: S2.1: Add γ-aminopropyltriethoxysilane to a 60% ethanol solution according to a solid-liquid ratio of 1 g : (10 - 12) mL, stir well to dissolve, and then add acetic acid to adjust the pH to 4 - 5 to obtain a γ-aminopropyltriethoxysilane solution; S2.2: Ultrasonically clean expanded perlite with deionized water and dry it to a constant weight, and then add it to the above-mentioned γ-aminopropyltriethoxysilane solution according to a solid-liquid ratio of 1 g : (5 - 6) mL, and heat and stir at 70 - 80 °C for 3 - 4 h to obtain an aminated expanded perlite solution; S2.3: Add dimethyl hydroxymethylphosphonate to the above-mentioned aminated expanded perlite solution according to a solid-liquid ratio of 1 g : (12 - 16) mL, and add 0.1 mol / L hydrochloric acid to adjust the pH to 2 - 3, and heat and stir at 80 - 90 °C for 10 - 12 h. After cooling, centrifuge, filter, wash to neutral and dry to obtain modified expanded perlite.
5. The preparation process of the flame retardant and heat insulating fabric for fire fighting clothing according to claim 4, characterized in that, S3 specifically includes the following steps: S3.1: Uniformly mix polyester powder, the coated and modified ammonium polyphosphate prepared in step S1.3 and the modified expanded perlite prepared in step S2.3, and extrude and granulate through a twin-screw extruder to obtain a modified polyester masterbatch; S3.2: Mix the above-mentioned modified polyester masterbatch and polyester chips according to a mass ratio of 1 : (5 - 7) for spinning to obtain modified polyester fiber filaments, and then perform plain weaving to obtain a flame-retardant outer fabric.
6. The preparation process of the flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 5, characterized in that, S5 specifically includes the following steps: S5.1: Add ε-polylysine hydrochloride to deionized water according to a solid-liquid ratio of 1 g : (10 - 20) mL, stir well to dissolve, and then add 0.1 mol / L sodium hydroxide solution to adjust the pH to 10 - 11 to obtain an ε-polylysine hydrochloride solution; S5.2: Add Tween 80 to deionized water according to a mass ratio of 1 : (10 - 15), stir well to dissolve, and then add epoxidized linseed oil with an epoxy value of 6 - 8% according to an oil-water ratio of 1 : (4 - 6), and stir and emulsify at 1000 - 1500 r / min for 20 - 30 min to obtain an epoxidized linseed oil emulsion; S5.3: Add the above-mentioned epoxidized linseed oil emulsion to the above-mentioned ε-polylysine hydrochloride solution according to a mass ratio of 1 : (6 - 8), heat and stir at 50 - 60 °C for 4 - 6 h, then add glacial acetic acid to adjust the pH to neutral, and after dialysis purification and freeze-drying, obtain modified ε-polylysine hydrochloride; S5.4: Dissolve the above-mentioned modified ε-polylysine hydrochloride in deionized water to prepare a solution with a mass fraction of 1 - 3%, and then add 0.2 - 0.3 wt% catalyst citric acid, stir and mix evenly to obtain a modified treatment solution; S5.5: Immerse the cotton grey fabric in the above-mentioned modified treatment liquid at a liquor ratio of 1:(15 - 25), heat and soak it at 50 - 60 °C for 1 - 2 h. After taking it out, wash it with water and dry it to obtain the antibacterial inner fabric.
7. The preparation process of the flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 3, characterized in that, The addition amount of polyethyleneimine is 15 - 20% of the mass of ammonium polyphosphate.
8. The preparation process of the flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 3, characterized in that, The addition amount of hydroxyethylidene diphosphonic acid is 40 - 50% of the mass of polyethyleneimine.
9. The preparation process of the flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 5, characterized in that, The mass ratio of polyester powder, coated modified ammonium polyphosphate and modified expanded perlite is (35 - 45):(3 - 5):
1.
10. The preparation process of a flame-retardant and heat-insulating fabric for fire-fighting clothing according to claim 2, characterized in that, By mass, the raw materials of the synthetic fiber include: 30 - 40 parts of polyvinyl chloride, 10 - 20 parts of ethylene-propylene rubber, 2 - 3 parts of sodium stearate, 3 - 5 parts of bamboo charcoal powder, 2 - 4 parts of sepiolite nanofibers, 2 - 4 parts of KH-550 coupling agent, 1 - 2 parts of cellulose ester and 1 - 2 parts of sodium alginate.
Citation Information
Cited By
Heat-insulating flame-retardant fabric and preparation method thereof
CN121381354A
Heat-insulation fireproof protective clothing and preparation method thereof
CN121606840A
Industrial flame-retardant antistatic fabric and preparation method thereof
CN121826920A
Industrial flame-retardant antistatic fabric and preparation method thereof
CN121826920B
Fireproof heat-insulation heat-preservation composite material as well as preparation method and application thereof
CN122275378A