Imprinted porous polymer adsorption material as well as preparation method and application thereof
Through the preparation method of nano-TiO2/Fe3O4 composite carrier and crown ether-cuvette aromatic hydrocarbon combined functional monomer, the problem of poor selectivity of existing adsorbents is solved, and efficient separation and rapid separation of rubidium ions is achieved, which is suitable for industrial production.
Patent Information
- Application Number
- CN202510819804.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-19
- Publication Date
- 2025-07-18
- Estimated Expiration
- 2045-06-19
AI Technical Summary
The existing adsorbents have poor selectivity for rubidium, making it difficult to achieve efficient separation and enrichment in complex systems, and the existing methods have problems such as high cost and high environmental pollution risks.
NanoTiO2/Fe3O4 is used as a composite carrier, and the ionic blotting polymerization is coordinated with rubidium ions through silanization modification and crown ether-cuvette aromatic hydrocarbon combined functional monomer, combined with crosslinking agent and initiator, to prepare the blot porous polymer adsorption material, and achieve rapid separation under an external magnetic field.
It realizes high selectivity and high capacity adsorption of rubidium ions, can efficiently separate and enrich rubidium in complex systems, and has a simple preparation method and low cost, which is suitable for industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of adsorption materials, and particularly relates to an imprinted porous polymer adsorption material, a preparation method thereof, and an application thereof. Background Art
[0002] As a rare and precious metal element, rubidium shows broad application prospects and important commercial value in the fields of electronic devices, energy, aviation, chemical catalysis, medicine, etc. Although the reserves of rubidium in nature are very rich, there are no minerals with rubidium as the main component. Rubidium often exists in an associated form in minerals such as lepidolite and pollucite, or exists in salt lake brines, coexisting with a large number of metal ions such as potassium, sodium, magnesium, calcium, and impurities such as organic substances. Since rubidium ions have extremely high use value, it is an urgent problem to extract and separate them from mineral or salt lake brine systems containing various components and impurities.
[0003] At present, common methods for separating and enriching rubidium include precipitation method, extraction method, adsorption method, etc. The precipitation method has high costs, some process procedures are relatively complex, and the stability of the precipitate is not high. In the extraction method, the extractant is expensive and easy to lose, a large amount of water needs to be treated during the extraction process, the corrosion is relatively large, and pollution is easily caused during the production process. Compared with other methods, the adsorption method has the advantages of simple process, high recovery rate, environmental friendliness, etc. The core principle of the adsorption method is to selectively adsorb rubidium ions by using an adsorbent. After adsorption saturation, the enrichment of rubidium and the regeneration of the adsorbent are achieved through elution. However, at present, there is less research and development on rubidium adsorbents, and the existing adsorbents have poor selectivity for rubidium and are difficult to adapt to the efficient separation and enrichment of rubidium in complex systems. Summary of the Invention
[0004] In view of this, the present invention provides an imprinted porous polymer adsorption material, a preparation method thereof, and an application thereof. The imprinted porous polymer adsorption material provided by the present invention has high selectivity for rubidium ions, and at the same time has the advantages of high capacity and high stability, and can achieve the efficient separation and enrichment of rubidium in complex systems.
[0005] In order to achieve the above-mentioned invention purposes, the present invention provides the following technical solutions: A preparation method of an imprinted porous polymer adsorption material, comprising the following steps: Mix a divalent iron salt, a trivalent iron salt, a titanium source, ammonia water, and water to carry out a coprecipitation reaction to obtain a coprecipitation product; calcine the coprecipitation product to obtain a nano-TiO2 / Fe3O4 composite support; Mix the nano-TiO2 / Fe3O4 composite support, 3-aminopropyltriethoxysilane, and a solvent to carry out a surface silanization reaction to obtain a silanized composite support; Mix the silanized composite support, 18-crown-6-acrylate, an activator, and a solvent to carry out a condensation reaction to obtain a crown-etherified composite support; Mix the crown-etherified composite support, sulfonated calix[4]arene and a solvent for self-assembly to obtain a crown-ether-arene-composite support; Mix the crown-ether-arene-composite support and a rubidium salt solution for template pre-assembly to obtain a pre-assembled complex; Mix the pre-assembled complex, methacrylic acid, a cross-linking agent and an initiator for ionic imprint polymerization to obtain a polymer; Elute Rb in the polymer + to obtain an imprinted porous polymer adsorbent material.
[0006] Preferably, the molar ratio of the divalent iron salt to the trivalent iron salt is 1:2 to 2.5; the titanium source is titanium tetrachloride; the total molar amount of the divalent iron salt and the trivalent iron salt and the molar ratio of the titanium source is 1:4 to 6; The temperature of the coprecipitation reaction is 50 to 70 °C, the time is 5 to 7 h, and the pH value is 10 to 11; Preferably, the calcination temperature is 400 to 600 °C and the time is 1 to 3 h.
[0007] Preferably, the dosage ratio of the nano-TiO2 / Fe3O4 composite support to 3-aminopropyltriethoxysilane is 5 g:1 to 3 mL; the temperature of the surface silanization reaction is 70 to 90 °C and the time is 7 to 9 h.
[0008] Preferably, the mass ratio of the nano-TiO2 / Fe3O4 composite support to 18-crown-6-acrylate is 5:0.1 to 0.2; the activator includes carbodiimide and N-hydroxysuccinimide; the temperature of the condensation reaction is 50 to 70 °C and the time is 10 to 15 h.
[0009] Preferably, the molar ratio of 18-crown-6-acrylate to sulfonated calix[4]arene is 1:0.2 to 3, and the self-assembly time is 20 to 30 h.
[0010] Preferably, the concentration of the rubidium salt solution is 0.1 to 0.3 mol / L; the pH value of the template pre-assembly is 7 to 8 and the time is 10 to 15 h; The dosage ratio of the nano-TiO2 / Fe3O4 composite support to methacrylic acid is 1 g:0.1 to 0.2 mL; The volume ratio of methacrylic acid to the cross-linking agent is 1:3 to 5; the cross-linking agent is ethylene glycol dimethacrylate; the initiator is an azo initiator; The eluent used for elution is an acid solution; the elution is carried out under ultrasonic oscillation conditions. The present invention also provides an imprinted porous polymer adsorbent material prepared by the preparation method described in the above scheme.
[0011] The present invention also provides an application of the imprinted porous polymer adsorbent material described in the above solution in rubidium ion adsorption.
[0012] The present invention also provides a method for separating and enriching rubidium from the solution after extracting lithium from lepidolite, comprising the following steps: Mix the solution after extracting lithium from lepidolite and the imprinted porous polymer adsorbent material described in the above solution for rubidium ion adsorption.
[0013] The present invention provides a preparation method of an imprinted porous polymer adsorbent material, comprising the following steps: Mix a divalent iron salt, a trivalent iron salt, a titanium source, ammonia water and water for coprecipitation reaction to obtain a coprecipitation product; Calcinate the coprecipitation product to obtain a nano-TiO2 / Fe3O4 composite support; Mix the nano-TiO2 / Fe3O4 composite support, 3-aminopropyltriethoxysilane and a solvent for surface silanization reaction to obtain a silanized composite support; Mix the silanized composite support, 18-crown-6-acrylate, an activator and a solvent for condensation reaction to obtain a crown etherified composite support; Mix the crown etherified composite support, sulfonated calix[4]arene and a solvent for self-assembly to obtain a crown ether-arene-composite support; Mix the crown ether-arene-composite support and a rubidium salt solution for template pre-assembly to obtain a pre-assembled complex; Mix the pre-assembled complex, methacrylic acid, a crosslinking agent and an initiator for ion imprinting polymerization reaction to obtain a polymer; Elute the Rb + from the polymer to obtain the imprinted porous polymer adsorbent material. The present invention uses nano-TiO2 / Fe3O4 as a composite support. On the one hand, the property of high specific surface area of nano-TiO2 can provide a large number of active sites, enhancing the adsorption capacity. At the same time, using the magnetic property of Fe3O4, the adsorbent material of the present invention can be recovered under the action of an external magnetic field, realizing the rapid separation between the adsorbent and the adsorbed solution. The present invention uses crown ether-calixarene as a combined functional monomer to coordinate with the template (Rb + ) Compared with a single functional monomer, the dual coordination of crown ether-calixarene can form cavity complementarity and multiple force synergy, thereby improving the selectivity of the adsorbent material for rubidium ions, and the adsorption capacity is also greatly improved. In summary, the imprinted porous polymer adsorbent material prepared by the present invention has high selectivity, high capacity and high stability, and can realize the efficient separation and enrichment of rubidium in a complex system; at the same time, the preparation method provided by the present invention has a simple process, low cost, strong operability, and is suitable for industrial production. Specific Embodiments
[0014] The present invention provides a preparation method of an imprinted porous polymer adsorbent material, comprising the following steps: Mix a ferrous salt, a ferric salt, a titanium source, ammonia water and water to carry out a coprecipitation reaction to obtain a coprecipitation product; calcine the coprecipitation product to obtain a nano-TiO₂ / Fe₃O₄ composite support; Mix the nano-TiO₂ / Fe₃O₄ composite support, 3-aminopropyltriethoxysilane and a solvent to carry out a surface silanization reaction to obtain a silanized composite support; Mix the silanized composite support, 18-crown-6 acrylate, an activator and a solvent to carry out a condensation reaction to obtain a crown etherified composite support; Mix the crown etherified composite support, sulfonated calix[4]arene and a solvent to carry out self-assembly to obtain a crown ether-arene-composite support; Mix the crown ether-arene-composite support and a rubidium salt solution to carry out template pre-assembly to obtain a pre-assembled complex; Mix the pre-assembled complex, methacrylic acid, a crosslinking agent and an initiator to carry out an ion-imprinting polymerization reaction to obtain a polymer; Remove Rb in the polymer + by elution to obtain an imprinted porous polymer adsorbent material.
[0015] In the present invention, a ferrous salt, a ferric salt, a titanium source, ammonia water and water are mixed to carry out a coprecipitation reaction to obtain a coprecipitation product; the coprecipitation product is calcined to obtain a nano-TiO₂ / Fe₃O₄ composite support. In the present invention, the ferrous salt is preferably ferrous chloride, and the ferric salt is preferably ferric chloride; the molar ratio of the ferrous salt to the ferric salt is preferably 1:2 to 2.5, more preferably 1:2; the titanium source is preferably titanium tetrachloride; the total molar amount of the ferrous salt and the ferric salt and the molar ratio of the titanium source are preferably 1:4 to 6, more preferably 1:5; the water is preferably deoxygenated water, the temperature of the coprecipitation reaction is preferably 50 to 70 °C, more preferably 60 °C, the reaction time is preferably 5 to 7 h, more preferably 6 h, and the pH value is preferably 10 to 11. In a specific embodiment of the present invention, it is preferred to first dissolve the ferrous salt and the ferric salt in water, then add the titanium source, then add ammonia water to adjust the pH value to 10 to 11, and then raise the temperature to the above temperature for the coprecipitation reaction; the coprecipitation product is specifically a hydroxide precursor of the composite support; after the coprecipitation reaction is completed, it is preferred in the present invention to carry out solid-liquid separation on the obtained product liquid, wash the obtained coprecipitation product, and then carry out calcination.
[0016] In the present invention, the calcination temperature is preferably 400 - 600 °C, more preferably 500 °C, and the calcination time is preferably 1 - 3 h, more preferably 2 h; during the calcination process, the hydroxide precursor forms a stable crystalline oxide to obtain a nano-TiO2 / Fe3O4 composite support; the nano-TiO2 / Fe3O4 composite support includes Fe3O4 and TiO2 nanoparticles coated on the surface of the Fe3O4.
[0017] After obtaining the nano-TiO2 / Fe3O4 composite support, the present invention mixes the nano-TiO2 / Fe3O4 composite support, 3-aminopropyltriethoxysilane (APTES) and a solvent to carry out a surface silanization reaction to obtain a silanized composite support (denoted as NH2-TiO2 / Fe3O4). In the present invention, the dosage ratio of the nano-TiO2 / Fe3O4 composite support to 3-aminopropyltriethoxysilane is preferably 5 g: 1 - 3 mL; the solvent used for the surface silanization reaction is preferably toluene; the temperature of the surface silanization reaction is preferably 70 - 90 °C, more preferably 80 °C. In a specific embodiment of the present invention, the surface silanization reaction is preferably carried out under reflux conditions; the time of the surface silanization reaction is preferably 7 - 9 h, more preferably 8 h, and the surface silanization reaction is preferably carried out under a protective gas, and the protective gas is preferably nitrogen; after the surface silanization reaction is completed, the present invention preferably magnetically separates the obtained product liquid, washes the solid product and then dries it to obtain the silanized composite support. The washing is preferably carried out successively with toluene, ethanol and deionized water, and the drying temperature is preferably 60 °C.
[0018] After obtaining the silylated composite support, the present invention mixes the silylated composite support, 18-crown-6 acrylate, an activator, and a solvent to carry out a condensation reaction to obtain a crown etherified composite support (denoted as crown ether-TiO2 / Fe3O4). The present invention has no special requirements for the source of the 18-crown-6 acrylate, and it can be either a commercially available product or prepared by methods well-known to those skilled in the art; in a specific embodiment of the present invention, the 18-crown-6 acrylate can be prepared by the following method: mixing 18-crown-6, acryloyl chloride, and DMF to carry out an esterification reaction to obtain 18-crown-6 acrylate; the molar ratio of 18-crown-6 to acryloyl chloride is preferably 1:1.2; the temperature of the esterification reaction is preferably 60 °C, and the time is preferably 12 h. The mass ratio of the TiO2 / Fe3O4 composite support to 18-crown-6 acrylate is preferably 5:0.1 to 0.2, and specifically can be 5:0.19; the activator preferably includes N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride (EDC) and N-hydroxysuccinimide (NHS); the dosage ratio of 18-crown-6 acrylate, EDC, and NHS is preferably 0.5 mmol:0.05 to 0.15 g:0.05 to 0.1 g, and specifically can be 0.5 mmol:0.1 g:0.06 g; the solvent used in the condensation reaction is preferably N,N-dimethylformamide (DMF); the temperature of the condensation reaction is preferably 50 to 70 °C, more preferably 60 °C, and the time of the condensation reaction is preferably 10 to 15 h, more preferably 12 h; the present invention modifies 18-crown-6 acrylate on the surface of the composite support through the condensation reaction.
[0019] After obtaining the crown etherified composite support, the present invention mixes the crown etherified composite support, sulfonated calix[4]arene, and a solvent to carry out self-assembly to obtain a crown ether-arene-composite support (denoted as crown ether-arene-TiO2 / Fe3O4). In the present invention, the solvent used for the self-assembly is preferably an alcohol, specifically methanol; the molar ratio of 18-crown-6 acrylate to sulfonated calix[4]arene is preferably 1:0.2 to 3, specifically can be 1:1 or 1:2, the time of the self-assembly is preferably 20 to 30 h, specifically can be 24 h, and the self-assembly can be carried out at room temperature; during the self-assembly process, electrostatic self-assembly occurs between the amino group in the crown etherified composite support and the sulfonic acid group in the sulfonated calix[4]arene to obtain a crown ether-arene-composite support.
[0020] After obtaining the crown ether-arene composite support, the present invention mixes the crown ether-arene composite support and a rubidium salt solution for template pre-assembly to obtain a pre-assembled complex. In the present invention, the rubidium salt in the rubidium salt solution is preferably RbNO3; the concentration of the rubidium salt solution is preferably 0.1 - 0.3 mol / L, more preferably 0.1 mol / L; the solvent of the rubidium salt solution is preferably an acetonitrile-water mixed solvent, and the volume ratio of acetonitrile to water in the acetonitrile-water mixed solvent is preferably 3 - 5:1, more preferably 4:1; the dosage ratio of the nano-TiO2 / Fe3O4 composite support to the rubidium salt solution is preferably 1 g:5 - 15 mL, more preferably 1 g:10 mL; the pH value of the template pre-assembly is preferably 7 - 8, and the time of the template pre-assembly is preferably 10 - 15 h, specifically it can be 12 h; the template pre-assembly can be carried out at room temperature; in a specific embodiment of the present invention, it is preferred to ultrasonically disperse the crown ether-arene composite support and the rubidium salt solution, then adjust the pH value of the system to 7 - 8, and then carry out the template pre-assembly under static conditions.
[0021] After obtaining the pre-assembled complex, the present invention mixes the pre-assembled complex, methacrylic acid (MAA), a cross-linking agent, and an initiator to carry out an ion-imprinting polymerization reaction to obtain a polymer (denoted as Rb + -IIP@TiO2 / Fe3O4). In the present invention, the dosage ratio of the nano-TiO2 / Fe3O4 composite support to methacrylic acid is preferably 1 g:0.1 - 0.2 mL; the cross-linking agent is preferably ethylene glycol dimethacrylate (EGDMA); the volume ratio of methacrylic acid to the cross-linking agent is preferably 1:3 - 5, more preferably 1:4; the initiator is preferably an azo initiator, specifically it can be azobisisobutyronitrile (AIBN); the dosage ratio of methacrylic acid to the initiator is preferably 0.1 mL:0.01 - 0.02 g; in a specific embodiment of the present invention, after the template pre-assembly is completed, without any treatment, directly add methacrylic acid, a cross-linking agent, and an initiator to the feed liquid for polymerization reaction; the temperature of the polymerization reaction is preferably 50 - 70 °C, more preferably 60 °C, and the time is preferably 20 - 30 h, more preferably 24 h; the polymerization reaction is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen. After the polymerization reaction is completed, the present invention preferably magnetically separates the product, washes it 3 times with acetonitrile, and then dries it at 60 °C to obtain the polymer.
[0022] After obtaining the polymer, the present invention removes the Rb in the polymer +Elute to obtain the imprinted porous polymer adsorbent material. In the present invention, the eluent used for elution is preferably an acid solution, specifically a nitric acid solution or a hydrochloric acid solution; the concentration of the acid solution is preferably 0.1 - 0.2 mol / L, more preferably 0.1 mol / L; the number of elution times is preferably 1 - 3 times, and the single elution time is preferably 1 - 2 h; the elution is preferably carried out under ultrasonic oscillation conditions; in the present invention, elution under ultrasonic oscillation conditions can improve the elution efficiency of rubidium ions. After elution is completed, in the present invention, the obtained product liquid is preferably centrifuged and washed with water until neutral, and then vacuum dried to obtain the imprinted porous polymer adsorbent material.
[0023] In the present invention, during the template pre-assembly process, the functional monomers (18-crown-6-acrylate and sulfonated calix[4]arene) and the template ion (Rb + ) assemble to form a complex, and then through a polymerization reaction, a porous polymer is formed, and then the template ion is eluted to obtain an imprinted porous polymer adsorbent material with rubidium ion imprinting.
[0024] The present invention also provides an imprinted porous polymer adsorbent material prepared by the preparation method described in the above solution.
[0025] The present invention also provides the application of the imprinted porous polymer adsorbent material described in the above solution in the adsorption of rubidium ions. In the present invention, the adsorption capacity of the imprinted porous polymer adsorbent material for rubidium ions is 1.8 - 2.2 mmol / g.
[0026] The present invention also provides a method for separating and enriching rubidium from the solution after extracting lithium from lepidolite, comprising the following steps: Mix the solution after extracting lithium from lepidolite and the imprinted porous polymer adsorbent material described in the above solution for rubidium ion adsorption.
[0027] In the present invention, the solution after extracting lithium from lepidolite is specifically the mother liquor remaining after extracting lithium from lepidolite; in the present invention, the solution after extracting lithium from lepidolite contains rubidium ions and impurity ions, and the impurity ions can specifically be one or more of Li + , Na + , K + and Cs + ; the adsorption time is preferably 1 h - 8 h; the adsorption can be carried out at room temperature; during the adsorption process, the cavities in the imprinted porous polymer adsorbent material selectively capture Rb + through size screening and chemical coordination, and repel other ions, thereby realizing the selective adsorption of Rb + .
[0028] After adsorption, the present invention preferably desorbs the imprinted porous polymer adsorbent after adsorption. The desorption preferably includes: using an eluent to desorb Rb from the imprinted porous polymer adsorbent after adsorption + to restore the activity of the cavity, and recycling the imprinted porous polymer adsorbent after elution; the eluent and specific elution conditions are the same as those for eluting Rb + ions during the preparation of the imprinted porous polymer adsorbent, which will not be elaborated here. The imprinted porous polymer adsorbent provided by the present invention can be repeatedly adsorbed and desorbed. After 10 cycles, the retention rate of the adsorption capacity is greater than 90%.
[0029] Next, the technical solutions in the present invention will be clearly and completely described in conjunction with the embodiments in the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments in the present invention without creative efforts belong to the protection scope of the present invention.
[0030] In the following examples and comparative examples: The preparation method of the nano-TiO2 / Fe3O4 composite carrier is as follows: Dissolve FeCl2 and FeCl3 in water at a molar ratio of 1:2, add TiCl4, and control the molar ratio of the total molar amount of FeCl2 and FeCl3 to TiCl4 to be 1:5. Slowly add ammonia water to adjust the pH to 10. React at 60 °C for 6 h, perform solid-liquid separation on the obtained product liquor, wash the obtained coprecipitation product, and calcine it at 500 °C for 2 h to obtain the nano-TiO2 / Fe3O4 composite carrier.
[0031] Example 1 Disperse 5 g of pre-synthesized nano-TiO2 / Fe3O4 composite support in 100 mL of toluene, add 2 mL of APTES, and reflux at 80 °C for 8 h under nitrogen protection. Perform magnetic separation, wash successively with toluene, ethanol, and deionized water, and dry in vacuum at 60 °C to obtain NH2-TiO2 / Fe3O4. Then disperse 0.5 mmol (0.19 g) of 18-crown-6 acrylate and NH2-TiO2 / Fe3O4 in 50 mL of DMF, add 0.1 g of EDC and 0.06 g of NHS, and react at 60 °C for 12 h. Perform magnetic separation and wash 3 times with DMF to obtain crown ether-TiO2 / Fe3O4. Disperse 0.5 mmol (0.43 g) of sulfonated calix[4]arene and crown ether-TiO2 / Fe3O4 in 50 mL of methanol, stir at room temperature for 24 h. Perform magnetic separation and wash with methanol to obtain crown ether-arene-TiO2 / Fe3O4 (the molar ratio of the functional monomer 18-crown-6 acrylate to sulfonated calix[4]arene is 1:1). Disperse crown ether-arene-TiO2 / Fe3O4 in 50 mL of acetonitrile / water (the volume ratio of acetonitrile to water is 4:1) solution containing 0.1 M RbNO3, ultrasonicate for 30 min, adjust the pH to 8.0, and let stand at 25 °C for 12 h. Add 0.5 mL of methacrylic acid (MAA), 2 mL of EGDMA (crosslinking agent), 0.05 g of AIBN, purge with nitrogen to remove oxygen, and polymerize in a water bath at 60 °C for 24 h. Perform magnetic separation, wash 3 times with acetonitrile, and dry at 60 °C to obtain Rb + -IIP@TiO2 / Fe3O4. Immerse Rb + -IIP@TiO2 / Fe3O4 in 0.1 M HNO3, perform oscillating ultrasonic treatment for 1 h, repeat 3 times, wash with deionized water until neutral, and dry in vacuum to obtain a blank imprinted porous polymer adsorbent material.
[0032] Adsorption experiment: Take 5 g of the blank imprinted porous polymer adsorbent material and add it to 500 mL of the solution after lithium extraction from lepidolite. Stir at 25 °C for 6 h. After magnetic separation, measure the Rb + concentration and other impurity concentrations in the supernatant, and calculate the adsorption capacity of rubidium ions. Among them, the adsorption capacity Q t of the adsorbent material for rubidium ions at time t is calculated by the following equation: Q t =(C0 - C t )V / W In the formula: the initial concentration of rubidium ions is C0 (mg / L), the concentration of rubidium ions after adsorption is C t (mg / L); W is the mass (g) of the imprinted porous polymer adsorbent material; V is the volume (L) of the solution after lithium extraction.
[0033] The ion concentrations in the solution after lithium extraction before and after adsorption are shown in Table 1.
[0034] Cyclic stability experiment: The adsorbed imprinted porous polymer adsorbent was immersed in 0.1 M HNO3, sonicated with shaking for 1 h, repeated 3 times, washed with deionized water until the eluent was neutral, and dried in vacuum. The desorbed imprinted porous polymer adsorbent was repeatedly subjected to the adsorption test under the same adsorption conditions as above. After testing, after 10 repeated adsorption-desorption cycles, the retention rate of the adsorption capacity of the adsorbent was 92%.
[0035] Comparative Example 1 0.5 mmol (0.19 g) of 18-crown-6 acrylate was dispersed in 50 mL of DMF and reacted at 60 °C for 12 h to obtain a crown ether coordination monomer. Subsequently, the monomer was dispersed in 50 mL of an acetonitrile-water (4:1, volume ratio) solution containing 0.1 M RbNO3, sonicated for 30 min, the pH was adjusted to 8.0, and left standing at 25 °C for 12 h. 0.5 mL of methacrylic acid (MAA), 2 mL of EGDMA (crosslinking agent), and 0.05 g of AIBN were added, degassed with nitrogen, and polymerized in a water bath at 60 °C for 24 h. Washed 3 times with acetonitrile and dried at 60 °C to obtain Rb + -IIP. The material was immersed in 0.1 M HNO3, sonicated with shaking for 1 h, repeated 3 times, washed with deionized water until neutral, and dried in vacuum to obtain a blank imprinted adsorbent.
[0036] Adsorption test: 5 g of the blank imprinted adsorbent was added to 500 mL of the solution after lithium extraction from lepidolite, stirred at 25 °C for 6 h, and after magnetic separation, the Rb + concentration and other impurity concentrations in the supernatant were measured, and the adsorption capacity of rubidium ions was calculated. The calculation method was the same as in Example 1. The ion concentrations in the solution after lithium extraction before and after adsorption are shown in Table 1.
[0037] Cyclic stability experiment: The adsorption-desorption cycle experiment was carried out in the same manner as in Example 1. The results showed that after 10 repeated adsorption-desorption cycles, the retention rate of the adsorption capacity of the adsorbent was 80%.
[0038] Table 1 Ion concentrations in the solution after lithium extraction before and after adsorption in Example 1 and Comparative Example 1
[0039] It can be seen from the data in Table 1 that the adsorbent in Example 1 has higher selectivity for rubidium and a larger adsorption capacity.
[0040] Example 2 Disperse 5 g of pre-synthesized nano-TiO2 / Fe3O4 composite support in 100 mL of toluene, add 2 mL of APTES, and reflux at 80 °C for 8 h under nitrogen protection. Perform magnetic separation, wash successively with toluene, ethanol, and deionized water, and dry in vacuum at 60 °C to obtain NH2-TiO2 / Fe3O4. Then disperse 0.5 mmol (0.19 g) of 18-crown-6 acrylate and NH2-TiO2 / Fe3O4 in 50 mL of DMF, add 0.1 g of EDC and 0.06 g of NHS, and react at 60 °C for 12 h. Perform magnetic separation and wash 3 times with DMF to obtain crown ether-TiO2 / Fe3O4. Disperse 1 mmol (0.86 g) of sulfonated calix[4]arene and crown ether-TiO2 / Fe3O4 in 50 mL of methanol, stir at room temperature for 24 h. Perform magnetic separation and wash with methanol to obtain crown ether-arene-TiO2 / Fe3O4 (the molar ratio of the functional monomer 18-crown-6 acrylate to sulfonated calix[4]arene is 1:2). Disperse crown ether-arene-TiO2 / Fe3O4 in 50 mL of acetonitrile-water solution containing 0.1 M RbNO3 (the volume ratio of acetonitrile to water is 4:1), ultrasonicate for 30 min, adjust the pH to 8.0, and let stand at 25 °C for 12 h. Add 0.5 mL of methacrylic acid (MAA), 2 mL of EGDMA (crosslinking agent), and 0.05 g of AIBN, purge with nitrogen to remove oxygen, and polymerize in a water bath at 60 °C for 24 h. Perform magnetic separation, wash 3 times with acetonitrile, and dry at 60 °C to obtain Rb + -IIP@TiO2 / Fe3O4. Immerse Rb + -IIP@TiO2 / Fe3O4 in 0.1 M HNO3, perform oscillating ultrasonic treatment for 1 h, repeat 3 times, wash with deionized water until neutral, and dry in vacuum to obtain a blank imprinted porous polymer adsorbent material.
[0041] Adsorption experiment: Take 5 g of the blank imprinted porous polymer adsorbent material and add it to 500 mL of the solution after lithium extraction from lepidolite. Stir at 25 °C for 6 h, perform magnetic separation, and then measure the Rb + concentration and other impurity concentrations in the supernatant, and calculate the adsorption capacity of rubidium ions. The calculation method is the same as in Example 1. The ion concentrations in the solution after lithium extraction before and after adsorption are shown in Table 2.
[0042] Cyclic stability experiment: Perform the adsorption-desorption cycle experiment in the same manner as in Example 1. The results show that after repeating the adsorption-desorption cycle 10 times, the retention rate of the adsorption capacity of the adsorbent material is 90%.
[0043] Comparative Example 2 Disperse 0.5 mmol (0.43 g) of sulfonated calix[4]arene in 50 mL of methanol and stir at room temperature for 24 h to obtain the arene coordination monomer. Subsequently, disperse the monomer in 50 mL of an acetonitrile-water (volume ratio of acetonitrile to water is 4:1) solution containing 0.1 M RbNO3, ultrasonicate for 30 min, adjust the pH to 8.0, and let stand at 25 °C for 12 h. Add 0.5 mL of methacrylic acid (MAA), 2 mL of EGDMA (crosslinking agent), and 0.05 g of AIBN, purge with nitrogen to remove oxygen, and polymerize in a water bath at 60 °C for 24 h. Wash three times with acetonitrile and dry at 60 °C to obtain Rb + -IIP. Immerse the material in 0.1 M HNO3, shake and ultrasonicate for 1 h, repeat three times, wash with deionized water until neutral, and dry in vacuo to obtain the blank imprinted adsorption material.
[0044] Adsorption experiment: Take 5 g of the blank imprinted adsorption material and add it to 500 mL of the solution after lithium extraction from lepidolite. Stir at 25 °C for 6 h, perform magnetic separation, and then measure the Rb + concentration and other impurity concentrations in the supernatant, and calculate the adsorption capacity of rubidium ions. The calculation method is the same as that in Example 1. The ion concentrations in the solution after lithium extraction before and after adsorption are shown in Table 2.
[0045] Cyclic stability experiment: Perform the adsorption-desorption cycle experiment in the same manner as in Example 1. The results show that after repeating the adsorption-desorption cycle 10 times, the retention rate of the adsorption capacity of the adsorption material is 84%.
[0046] Table 2 Ion concentrations in the solution after lithium extraction before and after adsorption in Example 2 and Comparative Example 2
[0047] It can be seen from the data in Table 2 that the adsorption material in Example 2 has higher selectivity for rubidium and a larger adsorption capacity.
[0048] In summary, the present invention uses rubidium ions as template ions, nano-TiO2 / Fe3O4 as a composite carrier, through silanization surface modification, uses crown ether-calixarene as a combined functional monomer to coordinate with the template ions, and then undergoes a polymerization reaction through a crosslinking agent and an initiator. After that, template elution and post-treatment are carried out to obtain the imprinted porous polymer adsorption material, which can selectively absorb rubidium ions efficiently. The preparation method provided by the present invention is simple to operate, the obtained adsorption material has a large specific surface area and a stable structure. Through dual coordination synergy, the adsorption sites of the material are increased, and the adsorption performance and repeatability of the material are improved. At the same time, the adsorption material can be recovered under the action of an external magnetic field to achieve rapid separation between the adsorbent and the adsorbed solution.
[0049] The above are only the preferred embodiments of the present invention. It should be noted that for those of ordinary skill in the art, without departing from the principle of the present invention, several improvements and refinements can be made, and these improvements and refinements should also be regarded as the protection scope of the present invention.
Claims
1. A preparation method of an imprinted porous polymer adsorbent material, characterized in that, It includes the following steps: Mix a ferrous salt, a ferric salt, a titanium source, ammonia water and water for coprecipitation reaction to obtain a coprecipitation product; calcine the coprecipitation product to obtain a nano-TiO₂ / Fe₃O₄ composite support; Mix the nano-TiO₂ / Fe₃O₄ composite support, 3-aminopropyltriethoxysilane and a solvent for surface silanization reaction to obtain a silanized composite support; Mix the silanized composite support, 18-crown-6-acrylate, an activator and a solvent for condensation reaction to obtain a crown-etherified composite support; Mix the crown-etherified composite support, sulfonated calix[4]arene and a solvent for self-assembly to obtain a crown-ether-arene-composite support; Mix the crown-ether-arene-composite support and a rubidium salt solution for template pre-assembly to obtain a pre-assembled complex; Mix the pre-assembled complex, methacrylic acid, a crosslinking agent and an initiator for ion-imprinting polymerization reaction to obtain a polymer; Elute Rb in the polymer + to obtain an imprinted porous polymer adsorbent material.
2. The preparation method according to claim 1, characterized in that, The molar ratio of the ferrous salt to the ferric salt is 1:2 to 2.5; the titanium source is titanium tetrachloride; the total molar amount of the ferrous salt and the ferric salt and the molar ratio of the titanium source is 1:4 to 6; The temperature of the coprecipitation reaction is 50 to 70 °C, the time is 5 to 7 h, and the pH value is 10 to 11.
3. The preparation method according to claim 1, characterized in that, The temperature of the calcination is 400 to 600 °C, and the time is 1 to 3 h.
4. The preparation method according to claim 1, characterized in that, The dosage ratio of the nano-TiO₂ / Fe₃O₄ composite support to 3-aminopropyltriethoxysilane is 5 g:1 to 3 mL; the temperature of the surface silanization reaction is 70 to 90 °C, and the time is 7 to 9 h.
5. The preparation method according to claim 1, characterized in that, The mass ratio of the nano-TiO₂ / Fe₃O₄ composite support to 18-crown-6-acrylate is 5:0.1 to 0.2; the activator includes carbodiimide and N-hydroxysuccinimide; the temperature of the condensation reaction is 50 to 70 °C, and the time is 10 to 15 h.
6. The preparation method according to claim 1, characterized in that, The molar ratio of 18-crown-6-acrylate to sulfonated calix[4]arene is 1:0.2 to 3, and the time of self-assembly is 20 to 30 h.
7. The preparation method according to claim 1, characterized in that, The concentration of the rubidium salt solution is 0.1 to 0.3 mol / L; the pH value of the template pre-assembly is 7 to 8, and the time is 10 to 15 h; The dosage ratio of the nano-TiO₂ / Fe₃O₄ composite support to methacrylic acid is 1 g:0.1 to 0.2 mL; The volume ratio of methacrylic acid to the crosslinking agent is 1:3 to 5; the crosslinking agent is ethylene glycol dimethacrylate; the initiator is an azo initiator; The eluent used for elution is an acid solution; the elution is carried out under ultrasonic oscillation conditions.
8. An imprinted porous polymer adsorbent material prepared by the preparation method according to any one of claims 1 to 7.
9. Application of the imprinted porous polymer adsorbent material according to claim 8 in rubidium ion adsorption.
10. A method for separating and enriching rubidium from the solution after extracting lithium from lepidolite, characterized in that, It includes the following steps: Mix the lithium mica lithium-extracted post-liquid and the imprinted porous polymer adsorbent material according to claim 8 for rubidium ion adsorption.
Citation Information
Patent Citations
Ag-modified ZnO nanorod substrate self-cleaning sensor, and preparation method and applications thereof
CN106970065A
Preparation method and application of double-imprinted porous silicon film
CN108404854A
Preparation method and application of imprinted porous adsorption lithium / rubidium ion material
CN109174049A
Preparation and application method of titanium dioxide / ferriferrous oxide / active carbon nanometer wastewater treating agent
CN109772328A
Cited By
Preparation method of surface ion imprinting functionalized magnetic nano adsorbent
CN121550980A