Microbial remediation ceramsite and preparation method thereof
By modifying porous sustained release Ca2+ ceramics to load alkali-resistant microorganisms and wrapping them with a cement-based protective shell, the problems of insufficient strength and limited solid load in concrete are solved, and the mechanical properties of concrete and crack repair effect are improved.
Patent Information
- Application Number
- CN202510816525.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-06-18
- Publication Date
- 2025-08-26
AI Technical Summary
The existing microbial carriers have problems in concrete, such as insufficient strength, limited solid-load microbial mass and intimate connection with concrete, which affects the crack repair effect of cement-based materials and the mechanical properties of concrete.
Modified porous sustained release Ca2+ ceramic granules are used as carriers, and alkali-resistant microorganisms and nutrients are loaded through vacuum impregnation, and wrapped with cement-based protective shells to prepare microbial repair ceramic granules, combined with silanization and glutaraldehyde cross-linking modification to improve the microbial load and carrier stability, and epoxy resin is used to enhance the adhesion ability of ceramic granules to cement matrix.
It improves the microbial load and stability of microbial repair ceratops, enhances the interface adhesion between the ceratops and cement matrix, improves the mechanical properties and durability of concrete, and achieves efficient crack repair effect.
Smart Images

Figure CN120535227A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete crack repair, in particular to a microbial repair ceramsite and a preparation method thereof. Background Art
[0002] Due to its economical and practical nature, concrete has long been a crucial building material, both today and for a long time to come. However, due to inherent flaws such as brittleness, low tensile strength, and susceptibility to cracking, concrete inevitably develops cracks during use and under the influence of the surrounding environment. Penetrating water and harmful chemicals can degrade the matrix within a certain range and corrode embedded rebar, reducing the structure's service life at best and endangering its safety at worst. Traditional concrete repair methods rely primarily on regular maintenance and post-repair. This passive and ineffective approach is not only costly but also ineffective, failing to meet the demands placed on concrete materials by modern multifunctional and intelligent buildings. Therefore, there is an urgent need for technologies or methods that can proactively and automatically repair cracks and damaged areas, thereby restoring or even improving the concrete's strength and extending the service life of concrete structures.
[0003] Active self-repair technology can intervene and repair cracks in their early stages, preventing further development and preventing water damage to the concrete matrix. Microbial self-repair, as an active self-repair technology, has attracted the attention of numerous researchers due to its environmentally friendly, intelligent, and repeatable repair capabilities. Mineralizing microorganisms, along with the necessary substrates and calcium sources, are introduced into cement-based materials. When cracks form in the concrete, the microorganisms, under the influence of water and air invading the crack space, undergo metabolic activity, producing specific enzymes that catalyze the production of carbonate ions from the substrate. Using themselves as nucleation sites, they induce calcium carbonate crystallization, thus repairing the cracks.
[0004] However, the microbial repair method faces the problem of damage to microorganisms caused by the harsh conditions of the concrete matrix. Effective load protection methods can provide suitable conditions for the long-term preservation of microorganisms in concrete. Generally, functional components such as microorganisms used to repair cracks are called "repair components", and the functional materials used to carry repair components are called "carriers". A suitable carrier encapsulates microorganisms, which can not only protect microorganisms from the high alkaline environment of concrete, but also provide sufficient living space for microorganisms to survive, so that microorganisms can survive effectively in the matrix for a long time.
[0005] However, there are still some problems in the application of microbial carriers. The carriers have disadvantages such as being decomposed by organisms, complex immobilization methods, limited amount of immobilized microorganisms, loose connection with the concrete matrix, and significant impact on the mechanical properties of concrete. Summary of the Invention
[0006] The present invention addresses the current problems of insufficient microbial carrier matrix strength, limited immobilized microorganisms, and loose connection with concrete, which in turn affect the effect of repairing cracks in cement-based materials and the mechanical properties of concrete. The invention provides a microbial repair ceramsite and a preparation method thereof, which can not only efficiently repair cracks in cement-based materials, but also improve the mechanical properties of cement-based materials and enhance their durability.
[0007] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:
[0008] A microbial repair ceramsite, comprising microorganisms, modified porous slow-release Ca 2+ Ceramsite, nutrients and cement-based protective shell, microorganisms and nutrients are loaded on modified porous slow-release Ca 2+ In ceramsite, cement-based protective shell is wrapped in modified porous slow-release Ca 2+ The outer surface of ceramsite.
[0009] A preparation method for microbial remediation ceramsite, the specific steps of which are as follows:
[0010] S1: Prepare microorganisms and activate and culture the freeze-dried microorganism powder;
[0011] S2: Perform alkali resistance gradient acclimation on microorganisms and select enhanced alkaliphilic acclimated microorganisms that adapt to the high alkaline environment of concrete;
[0012] S3: Preparation of porous sustained-release Ca 2+ ceramsite;
[0013] S4: Porous sustained release Ca 2+ The surface of ceramsite is cross-linked and modified to obtain modified porous slow-release Ca 2+ ceramsite;
[0014] S5: Microorganisms and nutrients are loaded onto modified porous slow-release Ca2+ substrates using vacuum impregnation. 2+ ceramsite;
[0015] S6: Wrap the cement-based protective shell to obtain microbial repaired ceramsite.
[0016] The porous sustained-release Ca 2+ Ceramic granules are artificial ceramsites with porous slow release of Ca 2+ The specific preparation method of ceramsite is as follows:
[0017] Lime mud, fly ash and diatomaceous earth are directly mixed in a mass ratio of 3-5:3-5:1-2, and stirred in a mortar mixing pot for 10 minutes to obtain a mixture; calcium carbonate is the main component of lime mud and is used as a source of calcium oxide and also as a pore-forming material. After sintering, the crystal phases of calcium feldspar and wollastonite show good Ca 2+Slow-release ability. Calcite-type CaCO3 is obtained by microbial mineralization. The substrate for mineralization requires sufficient Ca 2+ Source, the ceramsite after lime mud burning replenishes Ca through slow release 2+ , ensuring Ca 2+ Adequate; fly ash contains sufficient SiO2 and Al2O3, which can make up for the disadvantage of low strength of lime mud as sintered ceramsite particles; diatomaceous earth contains a large number of micropores, which helps to form a porous structure and increase porosity.
[0018] The mixture is placed in a granulator, and 2% to 8% of water by mass of the mixture is added to the granulator to obtain wet ceramsite with a particle size of 2.36 to 4.75 mm;
[0019] Dry the wet ceramsite at room temperature for 2-3 days and then dry it in an oven at 105°C for 24 hours;
[0020] The dried ceramsite was placed in a sintering furnace and sintered at 800°C for 1 hour, and then at 1000°C, 1050°C, and 1100°C for 2 hours respectively. When the temperature was less than 800°C, the heating rate was 10°C / min, and when the temperature was above 800°C, the heating rate was 5°C / min.
[0021] Prepare 0.1 mol / L acetic acid solution and 1 mol / L sodium hydroxide solution, soak the sintered ceramsite in acetic acid solution and sodium hydroxide solution for 12 hours respectively, wash the soaked ceramsite with clean water and dry it to constant weight to obtain porous slow-release Ca 2+ expanded clay.
[0022] The porous sustained-release Ca 2+ The specific preparation method of ceramsite surface cross-linking modification is:
[0023] Weigh a certain amount of porous slow-release Ca 2+ The ceramsite was placed in a rotary evaporator with a concentration of 0.01mol / L-0.1mol / L HCl solution and vacuumed for 1 hour. The ceramsite was taken out and placed in a 5%-15% silane toluene solution, vacuumed, and rotated at room temperature overnight. The ceramsite was then placed in a 1%-5% glutaraldehyde solution and cross-linked and activated with magnetic stirring at room temperature for 1 hour to obtain a modified porous slow-release Ca 2+Ceramic. When ceramsite is exposed to strong acid, the hydrated calcium silicate gel (CSH) undergoes a hydroxylation reaction, increasing the number of hydroxyl groups and acidic centers on the ceramsite surface. This is beneficial for the ceramsite's reaction with silanization and glutaraldehyde. Silane coupling agents can simultaneously produce compounds with a certain binding force with polar and non-polar substances, promoting the reaction of silanols generated by hydrolysis with hydroxyl groups on the carrier surface to form stable silicon-oxygen bonds. After treatment with glutaraldehyde aqueous solution, active groups - aldehyde groups - are generated on the surface of the functionalized layer. The methyl groups (-CH3) on the surface of the silanized ceramsite undergo a bonding reaction with an aldehyde group (-CHO) in glutaraldehyde. The other aldehyde group in glutaraldehyde is used to fix biomolecules, thereby increasing the microbial load on the ceramsite surface.
[0024] The microorganisms and nutrients are loaded on the modified porous slow-release Ca 2+ The specific preparation method of ceramsite is:
[0025] Modified porous slow-release Ca 2+ The ceramsite and microbial solution were placed in a vacuum bottle and then pressurized to -0.7 bar for 1 h;
[0026] When modified porous slow-release Ca 2+ When the mass of the bacterial solution adsorbed by the ceramsite no longer increases, the excess bacterial solution is filtered and the modified porous slow-release Ca 2+ The expanded clay is air-dried until there is a small amount of moisture on the surface, and then the nutrients are coated on the expanded clay using a sugar coating machine.
[0027] The microorganisms are selected from one or more of Bacillus sphaericus, Bacillus pasteurianus, Bacillus cohnii, Bacillus cereus, and Bacillus licheniformis, and are preferably selected through gradient acclimation. In an indoor culture environment, a high alkaline environment inside concrete is simulated, and Bacillus sphaericus, Bacillus pasteurianus, Bacillus cohnii, Bacillus cereus, and Bacillus licheniformis are cultured. Microorganisms with good alkali resistance are selected from the microorganisms and subjected to gradient acclimation to obtain enhanced alkaliphilic acclimated microorganisms that are adapted to the high alkaline environment inside concrete, thereby improving the survival rate of the microorganisms.
[0028] The nutrient is a mixture of sucrose powder and yeast powder. The nutrient is embedded in the modified porous slow-release Ca 2+ Ceramic ceramsite can effectively prevent spores from germinating during the process of absorbing nutrients, providing a continuous source of nutrients for microorganisms.
[0029] The cement-based protective shell is composed of epoxy resin and mixed powder. The preparation steps of the cement-based protective shell are as follows:
[0030] Modified porous sustained release Ca 2+ The ceramsite is coated with cured epoxy resin and then immediately wrapped with mixed powder: After the epoxy resin is cured, the particles are repeatedly coated with epoxy resin and then wrapped with mixed powder.
[0031] The mixed powder includes sulphoaluminate cement and one or more of fly ash, silica fume and nano-silicon dioxide. 2+ Ceramic aggregate has strong bonding ability, but the outer surface of the ceramic aggregate is smooth after impregnation treatment, and the bonding force with mortar is weak. In order to further enhance the interfacial adhesion between the ceramic aggregate and the cement matrix, cement-based mixed powder is wrapped on the outside. Sulphoaluminate cement ensures the early strength of the ceramic aggregate, and fly ash, silica fume, nano-silica and other materials make the later strength of the ceramic aggregate continue to increase.
[0032] The beneficial effects of the present invention are as follows: the microorganisms used in the microbial repair ceramsite of the present invention are cultured by simulating the high alkaline environment inside the concrete in an indoor culture environment, and microorganisms with good alkali resistance are selected and gradient domesticated to obtain enhanced alkaliphilic domesticated microorganisms that can adapt to the high alkaline environment in the concrete. The microorganisms after gradient domestication show higher urease activity and induced mineralization deposition efficiency in the high alkaline environment, which will have a positive effect on improving the performance and self-healing ability of the bioconcrete; the carrier is a porous slow-release Ca 2+ Ceramsite, calcite-type CaCO3 is obtained by microbial mineralization, and substrate mineralization requires sufficient Ca 2+ Source, after sintering, the ceramsite replenishes Ca through slow release 2+ , ensuring Ca 2+ Fly ash contains sufficient SiO2 and Al2O3, which can make up for the disadvantage of low strength of lime mud as sintered ceramsite particles. Diatomaceous earth contains a large number of micropores, which helps to form a porous structure and increase porosity. Porous slow-release Ca 2+ Ceramsite in slow release of Ca 2+ Under the condition of good mechanical strength and pore structure, it has no effect on the strength and durability of concrete; the surface of the expanded clay is modified by the aggregation-cross-linking method, and the modified microbial expanded clay carrier has a larger microbial load and better stability under the dual effects of physical adsorption and valence bond binding, which further ensures the repair effect of the expanded clay on cracks; the cement-based protective shell adopts epoxy resin to improve the cylinder pressure strength of the expanded clay, and protects microorganisms and nutrients from being destroyed by the high alkaline environment; the cement-based mixed powder is used to enhance the interfacial adhesion between the expanded clay and cement concrete, the sulphoaluminate cement in the mixed powder ensures the early strength of the expanded clay, and the fly ash, silica fume, nano-silica and other materials make the later strength of the expanded clay continue to increase, further enhancing the structural density and the mechanical properties of the concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a schematic diagram of the microbial remediation ceramsite structure of the present invention;
[0034] In the figure: 1-microorganism; 2-modified porous slow-release Ca2+ Ceramic aggregate; 3-nutrients; 4-cement-based protective shell;
[0035] The following is a detailed description of the embodiments of the invention with reference to the accompanying drawings. DETAILED DESCRIPTION
[0036] The present invention will be further described below with reference to the accompanying drawings and examples:
[0037] Example 1
[0038] The microbial remediation ceramsite of the present invention is prepared according to the following method: comprising the following steps:
[0039] S1: Prepare microorganism 1 and activate and culture the freeze-dried microorganism powder;
[0040] 15 g of casein peptone, 5 g of soy peptone, and 20 g of urea were added to 1 L of distilled water to obtain 1 L of liquid culture medium, and then 220 μL of Bacillus pasteurianus freeze-dried powder was selected and activated, and cultured in the liquid culture medium at 30° C. for 24 hours to obtain a bacterial solution of microorganism 1;
[0041] S2: Perform gradient acclimation of microorganism 1 to improve its alkali resistance, and select enhanced alkaliphilic acclimated microorganism 1 that is adapted to the high alkaline environment of concrete;
[0042] The activated Bacillus pasteurianus was inoculated in an environment of pH = 7 and continuously cultured at a constant temperature of 30°C under an aerobic environment for 48 hours. The target colony was then selected with an inoculating loop and inoculated into a culture medium of the next alkalinity level (pH = 8). The above inoculation-culture-sampling process was repeated, gradually and systematically increasing the alkalinity of the culture environment. In the highly alkaline environment, the microorganism 1 with the outwardly protruding tip was selected to obtain the microorganism 1 that can stably grow in a highly alkaline environment of pH = 12;
[0043] S3: Preparation of porous sustained-release Ca 2+ ceramsite;
[0044] The lime mud, fly ash and diatomaceous earth are directly mixed in a mass ratio of 5:5:1, and stirred in a mortar stirring pot for 10 minutes to obtain a mixture; the mixture is placed in a granulator, and 2%-8% of water by mass of the mixture is added to obtain wet ceramsite with a particle size of 2.36-4.75 mm; the wet ceramsite is dried at room temperature for 2-3 days, and then placed in a 105°C oven for drying for 24 hours; the dried ceramsite is placed in a sintering furnace, sintered at 800°C for 1 hour, and sintered at 1000°C, 1050°C and 1100°C for 2 hours respectively, with a heating rate of 10°C / min when the temperature is less than 800°C and 5°C / min above 800°C; an acetic acid solution with a concentration of 0.1 mol / L and a sodium hydroxide solution with a concentration of 1 mol / L are prepared, and the sintered ceramsite is immersed in the acetic acid solution and the sodium hydroxide solution for 12 hours, washed with clean water and dried to constant weight to obtain porous slow-release Ca 2+ ceramsite;
[0045] S4: Porous sustained release Ca 2+ The surface of ceramsite is cross-linked and modified to obtain modified porous slow-release Ca 2+ Ceramsite 2;
[0046] Weigh a certain amount of porous slow-release Ca 2+ The ceramsite was placed in a rotary evaporator with a concentration of 0.05 mol / L HCl solution and vacuumed for 1 hour. The ceramsite was taken out and placed in a 10% silane toluene solution, vacuumed, and rotated at room temperature overnight. The ceramsite was then placed in a 0.5% glutaraldehyde solution and cross-linked and activated with magnetic stirring at room temperature for 1 hour to obtain a modified porous slow-release Ca 2+ Ceramsite 2;
[0047] S5: The microorganism 1 and the nutrient 3 are loaded onto the modified porous slow-release Ca2+ substrate by vacuum impregnation. 2+ Ceramsite 2;
[0048] Modified porous slow-release Ca 2+ Place the ceramsite 2 and the solution of the strongly alkaliphilic acclimated microorganism 1 into a vacuum bottle, then pressurize it to -0.7 bar for 1 hour. When the mass of the bacterial solution adsorbed by the ceramsite no longer increases, filter the excess bacterial solution. After the ceramsite is air-dried until a small amount of moisture remains on the surface, use a sugar coater to coat the nutrient 3 on the ceramsite, completing the loading of the microorganism 1 and nutrient 3.
[0049] S6: Wrap the cement-based protective shell 4 to obtain microbial remediation ceramsite:
[0050] The immobilized ceramsite is then coated with epoxy resin and immediately encased in a powder mix. The powder mix consists of the following components in a 4:4:1 ratio by weight: sulphoaluminate cement, fly ash, and nano-silica. After the epoxy resin cures, the particles are repeatedly coated with epoxy resin and then encased in the powder mix to create the microbially remediated ceramsite.
[0051] Concrete specimens were prepared using PO 42.5R ordinary Portland cement and ordinary sand with a fineness modulus of 2.6. The specimens were all 40 mm × 40 mm × 160 mm prisms. After forming, the specimens were left to rest for 48 hours before demolding. They were then cured for 7 days at a relative humidity of 85 ± 5% and a temperature of 22 ± 2°C. After pre-cracks were introduced, the specimens were cured to the specified age and tested for performance. The mix proportions are shown in Table 1.
[0052] Table 1 Concrete mix ratio kg / m 3
[0053]
[0054]
[0055] Example 2
[0056] The microbial remediation ceramsite of the present invention is prepared according to the following method: comprising the following steps:
[0057] S1: Prepare microorganism 1 and activate and culture the freeze-dried powder of the microorganism.
[0058] 15 g of casein peptone, 5 g of soy peptone, and 20 g of urea were added to 1 L of distilled water to obtain 1 L of liquid culture medium. Then, 220 μL of freeze-dried Bacillus pasteurianus powder was selected and activated, and cultured in the liquid culture medium at 30° C. for 24 hours to obtain a bacterial liquid of microorganism 1.
[0059] S2: Perform gradient acclimation of microorganism 1 to improve its alkali resistance, and select enhanced alkaliphilic acclimated microorganism 1 that is adapted to the high alkaline environment of concrete.
[0060] The activated Bacillus pasteurianus was inoculated in an environment at pH 7 and cultured continuously at a constant temperature of 30°C under aerobic conditions for 48 hours. The target colony was then selected with an inoculating loop and inoculated into a culture medium at the next alkalinity level (pH 8). The above inoculation-culture-sampling process was repeated, gradually and systematically increasing the alkalinity of the culture environment. In the highly alkaline environment, the outward-protruding tip of microorganism 1 was selected, resulting in microorganism 1 that could stably grow in a highly alkaline environment of pH 12.
[0061] S3: Preparation of porous sustained-release Ca 2+ ceramsite;
[0062] The lime mud, fly ash and diatomaceous earth are directly mixed in a mass ratio of 7:3:1, and stirred in a mortar stirring pot for 10 minutes to obtain a mixture; the mixture is placed in a granulator, and 2%-8% of water by mass of the mixture is added to obtain wet ceramsite with a particle size of 2.36-4.75 mm; the wet ceramsite is dried at room temperature for 2-3 days, and then placed in a 105°C oven for drying for 24 hours; the dried ceramsite is placed in a sintering furnace, sintered at 800°C for 1 hour, and sintered at 1000°C, 1050°C and 1100°C for 2 hours respectively, with a heating rate of 10°C / min when the temperature is less than 800°C and a heating rate of 5°C / min when the temperature is above 800°C; an acetic acid solution with a concentration of 0.1 mol / L and a sodium hydroxide solution with a concentration of 1 mol / L are prepared, and the sintered ceramsite is immersed in the acetic acid solution and the sodium hydroxide solution for 12 hours, washed with clean water and dried to constant weight to obtain porous slow-release Ca 2+ ceramsite;
[0063] S4: Porous sustained release Ca 2+ The surface of ceramsite is cross-linked and modified to obtain modified porous slow-release Ca 2+ Ceramsite 2;
[0064] Weigh a certain amount of porous slow-release Ca 2+ The ceramsite was placed in a rotary evaporator with a concentration of 0.05 mol / L HCl solution and vacuumed for 1 hour. The ceramsite was taken out and placed in a 10% silane toluene solution, vacuumed, and rotated at room temperature overnight. The ceramsite was then placed in a 0.5% glutaraldehyde solution and cross-linked and activated with magnetic stirring at room temperature for 1 hour to obtain a modified porous slow-release Ca 2+ Ceramic 2.
[0065] S5: The microorganism 1 and the nutrient 3 are loaded onto the modified porous slow-release Ca2+ matrix by vacuum impregnation. 2+ Ceramsite 2;
[0066] The modified porous sustained-release Ca 2+ Place the ceramsite 2 and the solution of strongly alkaliphilic acclimated microorganism 1 into a vacuum flask and pressurize it to -0.7 bar for 1 hour. When the mass of the bacterial solution adsorbed by the ceramsite no longer increases, filter the excess bacterial solution. Allow the ceramsite to air-dry until a small amount of moisture remains on the surface. Then, use a sugar coater to coat the ceramsite with nutrient 3, completing the loading of microorganism 1 and nutrient 3.
[0067] S6: Wrapping the cement-based protective shell 4 to obtain microbial remediation ceramsite;
[0068] The immobilized ceramsite is then coated with epoxy resin and immediately encased in a powder mix. The powder mix consists of the following components in a 4:4:1 ratio by weight: sulphoaluminate cement, fly ash, and nano-silica. After the epoxy resin cures, the particles are repeatedly coated with epoxy resin and then encased in the powder mix to create the microbially remediated ceramsite.
[0069] Concrete specimens were prepared using PO 42.5R ordinary Portland cement and ordinary sand with a fineness modulus of 2.6. The specimens were all 40 mm × 40 mm × 160 mm prisms. After forming, the specimens were left to rest for 48 hours before demolding. They were then cured for 7 days at a relative humidity of 85 ± 5% and a temperature of 22 ± 2°C. After pre-cracks were introduced, the specimens were cured to the specified age and tested for performance. The mix proportions are shown in Table 1.
[0070] Example 3
[0071] The microbial remediation ceramsite of the present invention is prepared according to the following method: comprising the following steps:
[0072] S1: Prepare microorganism 1 and activate and culture the freeze-dried powder of the microorganism.
[0073] 15 g of casein peptone, 5 g of soy peptone, and 20 g of urea were added to 1 L of distilled water to obtain 1 L of liquid culture medium. Then, 220 μL of freeze-dried Bacillus pasteurianus powder was selected and activated, and cultured in the liquid culture medium at 30° C. for 24 hours to obtain a bacterial liquid of microorganism 1.
[0074] S2: Perform gradient acclimation of microorganism 1 to improve its alkali resistance, and select enhanced alkaliphilic acclimated microorganism 1 that is adapted to the high alkaline environment of concrete.
[0075] The activated Bacillus pasteurianus was inoculated in an environment at pH 7 and cultured continuously at a constant temperature of 30°C under aerobic conditions for 48 hours. The target colony was then selected with an inoculating loop and inoculated into a culture medium at the next alkalinity level (pH 8). The above inoculation-culture-sampling process was repeated, gradually and systematically increasing the alkalinity of the culture environment. In the highly alkaline environment, the outward-protruding tip of microorganism 1 was selected, resulting in microorganism 1 that could stably grow in a highly alkaline environment of pH 12.
[0076] S3: Preparation of porous sustained-release Ca 2+ ceramsite;
[0077] The lime mud, fly ash and diatomaceous earth are directly mixed in a mass ratio of 5:5:1, and stirred in a mortar stirring pot for 10 minutes to obtain a mixture; the mixture is placed in a granulator, and 2%-8% of water by mass of the mixture is added to obtain wet ceramsite with a particle size of 2.36-4.75 mm; the wet ceramsite is dried at room temperature for 2-3 days, and then placed in a 105°C oven for drying for 24 hours; the dried ceramsite is placed in a sintering furnace, sintered at 800°C for 1 hour, and sintered at 1000°C, 1050°C and 1100°C for 2 hours respectively, with a heating rate of 10°C / min when the temperature is less than 800°C and a heating rate of 5°C / min when the temperature is above 800°C; an acetic acid solution with a concentration of 0.1 mol / L and a sodium hydroxide solution with a concentration of 1 mol / L are prepared, and the sintered ceramsite is immersed in the acetic acid solution and the sodium hydroxide solution for 12 hours, washed with clean water and dried to constant weight to obtain porous slow-release Ca 2+ expanded clay.
[0078] S4: Porous sustained release Ca 2+ The surface of ceramsite is cross-linked and modified to obtain modified porous slow-release Ca 2+ Ceramsite 2;
[0079] Weigh a certain amount of porous slow-release Ca 2+ The ceramsite was placed in a rotary evaporator with a concentration of 0.1 mol / L HCl solution and vacuumed for 1 hour. The ceramsite was taken out and placed in a 12% silane toluene solution, vacuumed, and rotated at room temperature overnight. The ceramsite was then placed in a 0.8% glutaraldehyde solution and cross-linked and activated with magnetic stirring at room temperature for 1 hour to complete the surface modification of the ceramsite.
[0080] S5: The microorganism 1 and the nutrient 3 are loaded onto the modified porous slow-release Ca2+ substrate by vacuum impregnation. 2+ Ceramsite 2;
[0081] Modified porous slow-release Ca 2+ Place the ceramsite 2 and the solution of strongly alkaliphilic acclimated microorganism 1 into a vacuum flask and pressurize it to -0.7 bar for 1 hour. When the mass of the bacterial solution adsorbed by the ceramsite no longer increases, filter the excess bacterial solution. Allow the ceramsite to air-dry until a small amount of moisture remains on the surface. Then, use a sugar coater to coat the ceramsite with nutrient 3, completing the loading of microorganism 1 and nutrient 3.
[0082] S6: Wrapping the cement-based protective shell 4 to obtain microbial remediation ceramsite;
[0083] The immobilized ceramsite is then coated with epoxy resin and immediately encased in a powder mix. The powder mix consists of the following components in a 4:4:1 ratio by weight: sulphoaluminate cement, fly ash, and nano-silica. After the epoxy resin cures, the particles are repeatedly coated with epoxy resin and then encased in the powder mix to create the microbially remediated ceramsite.
[0084] Concrete specimens were prepared using PO 42.5R ordinary Portland cement and ordinary sand with a fineness modulus of 2.6. The specimens were all 40 mm × 40 mm × 160 mm prisms. After forming, the specimens were left to rest for 48 hours before demolding. They were then cured for 7 days at a relative humidity of 85 ± 5% and a temperature of 22 ± 2°C. After pre-cracks were introduced, the specimens were cured to the specified age and tested for performance. The mix proportions are shown in Table 1.
[0085] Comparative Example 1
[0086] Compared with Example 1, the microbial remediation ceramsite prepared in this comparative example is the same as that in Example 1, except that Bacillus pasteurianus is directly used as microorganism 1 without alkali resistance gradient acclimation. The remaining steps are the same as those in Example 1.
[0087] Comparative Example 2
[0088] Compared with Example 1, the microbial remediation ceramsite prepared in this comparative example uses expanded perlite as the ceramsite carrier, and the remaining steps are the same as those in Example 1.
[0089] Comparative Example 3
[0090] Compared with Example 1, the microbial remediation ceramsite prepared in this comparative example has only porous slow-release Ca 2+ Ceramsite 2 was not cross-linked and modified, and the remaining steps were the same as those in Example 1.
[0091] Comparative Example 4
[0092] Compared with Example 1, the microbial remediation ceramsite prepared in this comparative example only uses epoxy resin for the ceramsite protective shell and does not further wrap the mixed powder. The remaining steps are the same as those in Example 1.
[0093] The properties of the repaired ceramsite prepared in Examples 1-3 and Comparative Examples 1-4 were tested, including the cylinder pressure strength, integrity, microbial load and Ca 2+ Slow-release capacity as well as compressive strength and crack repair effect of concrete.
[0094] Cylinder pressure strength: It is an important indicator for evaluating the strength of porous materials. The determination method refers to "Light aggregate and its test methods Part 2: Test methods for light aggregate" (GB / T 17431.2-2010) for cylinder pressure strength test. The arithmetic mean of the results of three tests is used as the measured value, and the calculation is accurate to 0.1MPa.
[0095] Integrity: When self-healing particles are added to mortar, the integrity of the particles is one of the factors that determine their ability to heal cracks later. The particles are added to the mortar at a specific dosage and mixed with cement, sand, and water in a cement mortar mixer. The mixing process follows the national standard (GB / T 17671). After mixing, the cement mortar is removed and placed in a container. The slurry is washed off with running water, the particle surface is observed, and the integrity rate is calculated. The integrity rate is calculated using Equation (1).
[0096]
[0097] Where: I-integrity rate; m-total mass of particles; m0-mass of particles with damaged coating.
[0098] Microbial load: This is an evaluation of the number of microorganisms present in the ceramsite. The microorganism-loaded ceramsite is placed in a liquid culture medium, left to stand for a period of time, and then ultrasonically vibrated for a few seconds. Flow cytometry technology is used to irradiate the cells in the flow suspension one by one to obtain the light scattering index parameters of the cell population and the number of microorganisms.
[0099] Ca 2+ Leaching concentration: Evaluation of Ca2+ in ceramsite remediation by microorganisms 2+ Sustained release capacity. 200 mL of deionized water and 4 g of porous slow-release Ca 2+ Ceramsite 2 was placed in a 250 mL conical flask for static leaching. The conical flask was placed in a 25°C water bath and then shaken at 150 r / min for 12 h. The Ca content of the test solution was 2+ concentration.
[0100] Compressive Strength: This study evaluated the effects of microbial-remediated ceramsite on the mechanical properties of concrete. The concrete compressive specimens were 100 mm cubes. Uniaxial ultimate compressive strength was measured using standard test methods at a loading rate of 6.75 kN / s with continuous loading. Three concrete specimens were tested.
[0101] Crack Repair Rate: This method evaluates the self-repairing ability of microbially remediated ceramsite. Pre-set cracks were applied to the specimen using a three-point method using an electro-hydraulic servo pressure testing machine. Crack observation points were set every 10 mm along the specimen cracks, and the initial crack widths were recorded. The specimens were then placed in a natural environment and watered for curing. The crack widths at these observation points were measured at 7, 14, 21, and 28 days. The repair rate at these crack markers was used to characterize the local repair effect.
[0102]
[0103] Where: η is the crack repair rate; w0 is the initial crack width at the observation point, mm; w t - Remaining crack width at the observation point, mm.
[0104] The test results of microbial remediation of ceramsite and concrete are shown in Table 2.
[0105] Table 2 Performance test table
[0106]
[0107]
[0108] The microbial repair ceramsite of Examples 1 to 3 showed good mechanical properties and microbial loading capacity, and also had a certain Ca 2+ The mechanical properties of concrete with added microorganisms to repair expanded clay did not show a significant decline, and the 28-day repair rate of 0.25mm cracks was as high as over 86%, showing good early repair response behavior and repair efficiency.
[0109] From the comparison between Example 1 and Comparative Example 1, it can be seen that in Comparative Example 1, the microorganisms were not acclimated to the alkali resistance gradient, and the cylinder pressure strength, integrity, microbial load, and Ca content of the microbial repaired ceramsite in Comparative Example 1 were 2+ The leaching concentration and concrete compressive strength are basically not much different from those in Example 1, but the alkaline environment of the concrete will partially inhibit the activity of microorganisms that have not been acclimated to alkali resistance, and may even cause the death of microorganisms, further leading to a decrease in the 28d crack repair rate of Comparative Example 1.
[0110] From the comparison between Example 1 and Comparative Example 2, it can be seen that in Comparative Example 2, natural zeolite is used as a microbial carrier. The microbial remediation ceramsite is better than natural zeolite in cylinder pressure strength, integrity, microbial load and Ca 2+ There is a significant performance improvement in terms of leaching concentration, which in turn improves the compressive strength and crack repair rate of concrete.
[0111] From the comparison between Example 1 and Comparative Example 3, it can be seen that Comparative Example 3 does not affect the porous sustained-release Ca 2+ The cross-linking modification of ceramsite 2 was carried out, and the cylinder pressure strength, integrity, Ca 2+ The leaching concentration and concrete compressive strength are basically not much different from those in Example 1, but the lack of cross-linking modification reduces the microbial load of the ceramsite, thereby reducing the 28d crack repair rate of Comparative Example 3.
[0112] From the comparison between Example 1 and Comparative Example 4, it can be seen that Comparative Example 3 does not continue to coat the ceramsite with mixed powder, and the integrity and Ca 2+ The leaching concentration and 28d crack repair rate were basically not significantly different from those in Example 1. However, the failure to continue coating the ceramsite with the mixed powder reduced the cylinder compressive strength of the ceramsite. At the same time, the lack of cement-based materials also weakened the bonding with concrete, thereby reducing the integrity of the ceramsite and the mechanical properties of the concrete.
[0113] From the above results, it can be seen that the microbial repair ceramsite provided by the present invention has good mechanical properties and microbial loading capacity, and has a certain Ca 2+ The slow-release ability can provide a continuous source of calcium for microorganisms, and when added to concrete, it has good early repair response behavior and repair efficiency, which solves the current shortcomings of limited solid loading capacity of microbial carriers, loose connection with concrete matrix, and significant impact on the mechanical properties of concrete.
[0114] In the description of the invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like to indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore should not be understood as a limitation on the invention.
[0115] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features being referred to. Thus, a feature specified as "first" or "second" may explicitly or implicitly include at least one such feature. In the description of an invention, "plurality" means at least two, such as two, three, etc., unless otherwise specifically defined.
[0116] In the present invention, unless otherwise expressly specified or limited, terms such as "mounted," "connected," "connect," and "fixed" should be interpreted broadly. For example, they may refer to fixed connections, detachable connections, or integration; mechanical connections, electrical connections, or communication between them; direct connections or indirect connections through an intermediate medium; and internal communication between two components or interaction between two components, unless otherwise expressly limited. Those skilled in the art will understand the specific meanings of the above terms in the present invention based on specific circumstances.
[0117] The invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the invention is not limited to the above-mentioned method. As long as various improvements are made using the method concept and technical solution of the invention, or they are directly applied to other occasions without improvement, they are all within the scope of protection of the invention.
Claims
1. A microbial remediation ceramsite, characterized in that: Including microorganisms (1), modified porous slow-release Ca 2+ Ceramsite (2), nutrients (3) and cement-based protective shell (4), microorganisms (1) and nutrients (3) are loaded on modified porous slow-release Ca 2+ In the ceramsite (2), the cement-based protective shell (4) is wrapped in the modified porous slow-release Ca 2+ The outer surface of the ceramsite (2).
2. The method for preparing a microbial remediation ceramsite according to claim 1, wherein: The specific steps are as follows: S1: preparing microorganisms (1), activating and culturing the freeze-dried powder of microorganisms; S2: performing gradient acclimation of the microorganisms (1) to alkaline resistance, and selecting enhanced alkaliphilic acclimated microorganisms (1) that are adapted to the high alkaline environment of concrete; S3: Preparation of porous sustained-release Ca 2+ ceramsite; S4: Porous sustained release Ca 2+ The surface of ceramsite is cross-linked and modified to obtain modified porous slow-release Ca 2+ Ceramsite (2); S5: The microorganisms (1) and nutrients (3) are loaded onto the modified porous slow-release Ca2+ substrate by vacuum impregnation. 2+ Ceramsite (2); S6: Wrapping the cement-based protective shell (4) to obtain microorganisms (1) to repair the ceramsite.
3. The method for preparing a microbial remediation ceramsite according to claim 2, wherein: The porous sustained-release Ca 2+ Ceramsite is fired ceramsite, porous slow release Ca 2+ The specific preparation method of ceramsite is as follows: Lime mud, fly ash, and diatomaceous earth are directly mixed in a mass ratio of 3-5:3-5:1-2, and stirred in a mortar mixing pot for 10 minutes to obtain a mixture; The mixture is placed in a granulator, and 2% to 8% of water by mass of the mixture is added to the granulator to obtain wet ceramsite with a particle size of 2.36 to 4.75 mm; Dry the wet ceramsite at room temperature for 2-3 days and then dry it in an oven at 105°C for 24 hours; The dried ceramsite was placed in a sintering furnace and sintered at 800°C for 1 hour, and then at 1000°C, 1050°C, and 1100°C for 2 hours respectively. When the temperature was less than 800°C, the heating rate was 10°C / min, and when the temperature was above 800°C, the heating rate was 5°C / min. Prepare 0.1 mol / L acetic acid solution and 1 mol / L sodium hydroxide solution, soak the sintered ceramsite in acetic acid solution and sodium hydroxide solution for 12 hours respectively, wash the soaked ceramsite with clean water and dry it to constant weight to obtain porous slow-release Ca 2+ expanded clay.
4. The method for preparing a microbial remediation ceramsite according to claim 2, wherein: The porous sustained-release Ca 2+ The specific preparation method of ceramsite surface cross-linking modification is: Weigh a certain amount of porous slow-release Ca 2+ The ceramsite was placed in a rotary evaporator with a concentration of 0.01mol / L-0.1mol / L HCl solution and vacuumed for 1 hour. The ceramsite was taken out and placed in a 5%-15% silane toluene solution, vacuumed, and rotated at room temperature overnight. The ceramsite was then placed in a 1%-5% glutaraldehyde solution and cross-linked and activated with magnetic stirring at room temperature for 1 hour to obtain a modified porous slow-release Ca 2+ Ceramic clay (2).
5. The method for preparing a microbial remediation ceramsite according to claim 2, wherein: The microorganisms (1) and nutrients (3) are loaded on the modified porous slow-release Ca 2+ The specific preparation method of ceramsite (2) is: Modified porous slow-release Ca 2+ The ceramsite (2) and microorganism (1) solution were placed in a vacuum bottle and then pressurized to -0.7 bar for 1 hour; When modified porous slow-release Ca 2+ When the mass of the bacterial solution adsorbed by the ceramsite (2) no longer increases, the excess bacterial solution is filtered and the modified porous slow-release Ca 2+ The ceramsite (2) is air-dried until a small amount of moisture remains on the surface, and then the nutrients (3) are coated on the ceramsite using a sugar coating machine.
6. The method for preparing a microbial remediation ceramsite according to claim 5, wherein: The microorganism (1) is selected from one or more of Bacillus sphaericus, Bacillus pasteurianus, Bacillus cohnii, Bacillus cereus, and Bacillus licheniformis, and is preferably subjected to gradient acclimation; The nutrient (3) is a mixture of sucrose powder and yeast powder.
7. The method for preparing a microbial remediation ceramsite according to claim 2, wherein: The cement-based protective shell (4) is composed of epoxy resin and mixed powder. The preparation steps of the cement-based protective shell (4) are as follows: Modified porous sustained release Ca 2+ The ceramsite (2) is coated with cured epoxy resin and then immediately wrapped with mixed powder: after the epoxy resin is cured, the particles are repeatedly coated with epoxy resin and then wrapped with mixed powder.
8. The method for preparing a microbial remediation ceramsite according to claim 7, wherein: The mixed powder comprises sulphoaluminate cement and one or more of fly ash, silica fume and nano silicon dioxide.
Citation Information
Cited By
Preparation method of fly ash-based soil improvement type slow-release organic fertilizer
CN121574024A
Preparation method of fly ash-based soil improvement type slow-release organic fertilizer
CN121574024B
A composite carrier for immobilizing functional bacteria and a preparation method and application thereof
CN122706674A