Anti-corrosion composite furnace lining material for fluidizing chlorination of zircon sand and preparation method of anti-corrosion composite furnace lining material

By using a composite structure of high-purity electromelting corundum aggregate and anti-permeable chlorine protective layer in the zircon sand boiling chlorination furnace lining material, the performance of the zircon sand boiling chlorination furnace lining material in high temperature, chlorine corrosion, mechanical wear and thermal shock is solved, and efficient reduction of chlorine permeability and extension of the material life is achieved.

CN120574056AActive Publication Date: 2025-09-02LIAONING HUAXIANG NEW MATERIAL CO LTD

Patent Information

Application Number
CN202511079747.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-04
Publication Date
2025-09-02
Estimated Expiration
2045-08-04

AI Technical Summary

Technical Problem

The existing zircon sand boiling chlorination furnace lining materials have insufficient performance in high temperature, chlorine corrosion, mechanical wear, thermal shock and impurity penetration, resulting in a short life and does not meet the requirements of high-temperature chemical inertia, wear resistance, thermal shock stability and structural compactness.

Method used

The composite structure of high-purity electromelting corundum aggregate, fine powder matrix layer and anti-permeable chlorine protective layer is adopted. Through the coating solution of aluminum dihydrogen phosphate glue, chromium trichloride hexahydrate and spinel powder, a spinel blended chromium corundum structure is formed, and combined with the chlorine-annealing process, the denseness and chlorine resistance of the material are improved.

Benefits of technology

Significantly reduce chlorine permeability, improve the thermal stability and wear resistance of the material, extend the furnace lining life, reduce impurity content, and improve the product purity and cost-effectiveness of the zircon sand boiling chlorination process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an anti-corrosion composite furnace lining material for zircon sand fluidizing chlorination and a preparation method thereof.The anti-corrosion composite furnace lining material comprises a base body layer and an anti-chlorine-seepage protection layer, and the preparation method comprises the steps of base body layer preparation, coating liquid preparation, base body layer surface coating, coating curing, high-temperature firing, chlorine seepage treatment and annealing. According to the method, the specially-made coating liquid is adopted for enhancing the surface of the high-purity corundum furnace lining for the first time, the permeability of the coating liquid to a base body layer is improved by means of matched dissolution-sedimentation of chromium chloride and phosphoric acid, pores are blocked by means of expansion caused by dehydration and oxidation of CrCl3. 6H2O, densification of surface layer Cr2O3, spinel and phosphate and surface layer pore blocking are achieved, the porosity is greatly reduced, and the porosity of the high-purity corundum furnace lining is improved. The chlorine permeability is reduced, and the core problems of high permeability and short service life of the material in a high-temperature chlorine corrosion environment are solved; according to the invention, a chlorination-annealing self-cleaning process is matched to realize deep removal of impurities, so that the product purity of the chlorination process is improved, and the purification cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of industrial furnace lining materials, and in particular to a corrosion-resistant composite furnace lining material for zircon sand boiling chlorination and a preparation method thereof. Background Art

[0002] The zircon sand boiling chlorination process converts zircon sand (ZrSiO4) into zirconium tetrachloride (ZrCl4). The product, zirconium tetrachloride, serves as a key intermediate in the production of high-end materials such as metallic zirconium / hafnium and zirconium dioxide. The core reaction involves a gas-solid reaction between zircon sand, chlorine (Cl2), and a reducing agent (petroleum coke) at 1000-1200°C in a high-temperature fluidized bed reactor. ZrSiO4+4Cl2+4C→ZrCl4↑+SiCl4↑+4CO↑ The reaction has the characteristics of strong endothermicity, violent gas evolution, and fluidized motion. The process includes the following steps: 1) Raw material pretreatment: Zircon sand and petroleum coke are mixed in proportion, usually C:ZrSiO4≈4:1, and crushed to 80-200μm.

[0003] 2) Boiling chlorination: The mixed material is added from the bottom of the fluidized bed, and high-temperature chlorine is introduced from the bottom of the bed to form a "boiling bed".

[0004] The particles tumble violently under the support of the airflow, becoming fluidized and achieving efficient gas-solid contact.

[0005] 3) Product separation: Gaseous products (ZrCl4, SiCl4, CO, etc.) are discharged from the top of the furnace and solid ZrCl4 is obtained through condensation and graded purification; the residue (unreacted coke, FeCl3 and other impurities) is discharged from the bottom.

[0006] The traditional zircon sand boiling chlorination furnace may encounter the following problems during the production process: 1) High temperature (>1000℃) may cause material softening, sintering, and increased thermal stress; 2) Highly reactive chlorine (Cl2) may corrode metals / oxides and generate volatile chlorides (such as AlCl3, FeCl3, etc.); 3) Fluidized particle scouring may cause mechanical wear of the furnace lining and accelerate material spalling; 4) The reaction releases gas violently, causing pressure fluctuations in the furnace and exacerbating chlorine penetration; 5) Impurities (Fe, Ca) may form low-melting-point chlorides (such as CaCl2), which penetrate into the furnace lining and destroy its structure.

[0007] Zircon sand boiling chlorination furnaces generally require linings with high-temperature corrosion, mechanical wear, and thermal shock resistance. Traditional lining materials mainly include the following types: 1) High-purity corundum bricks (Al2O3>99%) have high high-temperature strength (>1500℃), good wear resistance and low cost, but chlorine penetrates through the grain boundaries and reacts with Al2O3: Al2O3+3Cl2+3C→2AlCl3↑+3CO↑ It causes intergranular corrosion, resulting in material loosening and even peeling and failure, and the service life is usually only 3-6 months.

[0008] 2) Chrome corundum brick (Al2O3-Cr2O3), which forms a Cr2O3 protective film by doping Cr, has better chlorine corrosion resistance than pure corundum, but the thermal expansion coefficient of Cr2O3 is high and the thermal shock stability is insufficient. However, when the Cr content is too high, Cr 3+ May be converted into toxic Cr in high temperature oxidizing atmosphere 6+ , causing environmental problems.

[0009] 3) Silicon carbide bricks (SiC) have good thermal conductivity and excellent thermal shock stability, but react in high temperature chlorine: SiC+2Cl2→SiCl4↑+C It causes rapid weight loss and is only suitable for low temperature areas (<800℃).

[0010] By comparison, the existing boiling chlorination furnace lining materials still cannot meet the following performance requirements: 1) Extreme resistance to chlorine penetration: Prevents Cl2 from penetrating into the material, avoiding the formation of volatile chlorides (such as AlCl3) that cause structural collapse; 2) High temperature chemical inertness: does not react with Cl2, SiCl4, CO, etc., and no low melting point phase is generated; 3) High wear resistance: resists continuous erosion of boiling sand-coke mixture; 4) Excellent thermal shock stability: Withstands sudden temperature changes caused by furnace start-up and shutdown or operating condition fluctuations (ΔT>200°C); 5) Structural density: The furnace lining material needs to have low porosity (<15%) to reduce the chlorine gas penetration path. Summary of the Invention

[0011] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a corrosion-resistant composite furnace lining material for boiling chlorination of zircon sand and a preparation method thereof.

[0012] In order to achieve the above object, the present invention adopts the following technical solutions: Anti-corrosion composite furnace lining material for zircon sand boiling chlorination, comprising a base layer and a chlorine-resistant protective layer; The matrix layer is sintered by high-purity fused corundum aggregate and fine powder (Al2O3 content ≥99%), supplemented by a small amount of sintering agent (such as kaolin); The chlorine-resistant protective layer is prepared by mixing, coating, high-temperature firing, chlorine-infiltrating treatment and annealing the following components in parts by weight: 100 parts of aluminum dihydrogen phosphate (Al(H2PO4)3) glue, used as a high-temperature binder and film-forming matrix; 45-50 parts of chromium chloride hexahydrate (CrCl3·6H2O) participates in the formation of a dense chromium oxide / phosphate layer at high temperature, effectively blocking the penetration of chloride ions; 40-50 parts of an aqueous phosphoric acid solution, wherein the weight concentration of phosphoric acid is 40-50wt%; 35-40 parts of spinel powder (MgAl2O4) provide excellent chemical inertness and resistance to chlorine corrosion. Too high a dosage will cause the coating liquid to easily settle, while too low a dosage will cause the surface density and structural thermal stability to decrease.

[0013] The present invention also provides a method for preparing the aforementioned corrosion-resistant composite furnace lining material, comprising the following steps: 1) Preparation of substrate layer: The chromium corundum bricks made of high-purity fused white corundum (Al2O3 content ≥99%), chromium oxide and other auxiliary materials are used as the base layer; 2) Preparation of coating solution: The method is prepared by mixing aluminum dihydrogen phosphate gel, chromium trichloride hexahydrate, phosphoric acid aqueous solution and spinel powder; 3) Surface coating of substrate layer: Applying a coating liquid on the surface of a dry base layer having an apparent porosity p of 5-10%; 4) Coating curing: In an air atmosphere, the substrate layer coated with the coating liquid was cured in an infrared oven at 300°C for 15 minutes to obtain a dry body A. For example, the apparent porosity of the substrate layer decreased from 7.3% to 3.9%, indicating that the cured coating had a significant pore-blocking effect, especially for larger pores. During the initial infrared baking, white smoke (atomized gas formed by HCl and water in the air, likely generated by the reaction of phosphoric acid and chromium chloride) permeated the surface. After 10 minutes of baking, no smoke was generated on the surface, resulting in a dry body A. The choice of 300°C as the curing temperature was influenced by previous research, which showed that the use of spinel is beneficial to the curing of aluminum phosphate. At this temperature, chromium chloride oxidizes to chromium oxide and releases HCl. The oxidation process involves expansion, which can block the pores on the surface of the substrate layer, thereby significantly reducing the porosity. 5) High temperature firing: In air atmosphere, the dry body A is placed in a muffle furnace and slowly heated to 400℃ at 5℃ / min, and kept warm for 30min; then slowly heated to 1350-1420℃ at 10℃ / min, and sintered at 1350-1420℃ for 12-18h to obtain the primary brick B; at about 400℃, phosphoric acid and aluminum dihydrogen phosphate dehydrate to form a continuous phosphoric acid film, which acts as a bond to the various phases of corundum and chromium salts, while reducing porosity and increasing density; at a temperature greater than 800℃, the surfaces of spinel, chromium oxide and aluminum oxide react with phosphoric acid to produce magnesium phosphate, chromium and aluminum phosphate, and at the same time, the excess Cl in the system is - The residue may occupy the O vacancy of AlPO4 to produce AlPO3Cl; the temperature is ≥1200℃, and the impurity ions in the system (such as Na + , K + ) will volatilize with Cl, remove impurities, and create molecular-level nano-mesopores. AlPO3Cl will also decompose and dechlorinate to form more stable cristobalite-type AlPO4 (C-AlPO4); ≥1300℃, chromium and aluminum react to form chromium-aluminum solid solution oxides, forming a chromium corundum structure inside to improve the strength of the brick. The surface spinel and chromium oxide, aluminum oxide, and phosphate interpenetrate to form a spinel-mixed chromium corundum structure. According to previous studies, the surface may be spinel phase and Mg x Cr y Al 1-x-y The cristobalite phase of the PO4 solid solution maintains the dense passivation film characteristics of chromium oxide. Therefore, the dry body A with an apparent porosity of 3.9% becomes the primary brick B with an apparent porosity of 2.5% after calcination. The porosity is further reduced, further reducing the risk of chlorine penetration. The unreacted spinel phase can greatly improve the surface hardness and wear resistance, and the high surface smoothness makes the alkali resistance higher. The part of the surface that penetrates into the internal chromium corundum phase may be Mg generated by the reaction. x Cr y Al 1-x-y PO4 solid solution, the basic structure is still cristobalite phase, thus filling and protecting the original pores of the main chrome corundum, eliminating the risk of cracking after corrosion of the main brick.

[0014] 6) Chlorination treatment: Although during the sintering process in step 5), there may be volatile impure metal chlorides due to the residual chlorine inside the dry body A, the impurity metals (mainly low-melting-point Na, K and their oxides) in the primary brick B are still relatively high (>0.5%). Therefore, a further chlorination treatment is adopted to remove impurities, as follows: Place the primary brick B in a tube furnace, introduce a mixture of Cl2 and N2, with a volume ratio of Cl2 to N2 of 1:4, heat to 900-950℃, keep warm for 2-4h, and then -The AlPO3Cl phase is embedded into the lattice vacancies; then the temperature is lowered to 600℃ and the pure N2 purge is switched to remove the residual chlorine to obtain the chlorine-infiltrated brick C; 7) Annealing: The chlorine-permeable brick C is sprayed with water for curing at room temperature for 10-15 hours, and after drying, is placed in a muffle furnace. In an air atmosphere, the temperature is rapidly increased to 1200°C at 30°C / min, and kept warm for 2-3 hours until the tail gas does not contain chlorides. The brick is cooled with the furnace to obtain a corrosion-resistant composite furnace lining material, the surface of which is a chlorine-permeable protective layer.

[0015] Preferably, the preparation process of the matrix layer in 1) is as follows: High-purity fused white corundum (Al2O3 content ≥99%), chromium oxide, calcined α-alumina powder (Al2O3 content ≥99%), kaolin, aluminum dihydrogen phosphate, carboxylated cellulose and water are mixed at a weight ratio of 100:15:10:5:2:3:5 at 90°C for 1 hour. After cooling at room temperature, the resulting mud is poured into a mold and formed by vibration press, hydraulic pressure or isostatic pressing using a friction brick press. The dried brick is sintered at 1400-1500°C for 2 days to obtain a brick-shaped base layer with a porosity of 7.3%. The appropriate porosity is about 5-10%. If the porosity is too high, the chlorine permeability resistance will be reduced. If too little binder (kaolin, aluminum dihydrogen phosphate, carboxylated cellulose) is used, although the porosity is low, the strength of the brick is too low, and the compressive strength of the base layer after calcination is also low.

[0016] Preferably, the preparation process of the coating liquid in 2) is as follows: Add part of chromium trichloride hexahydrate to the aluminum dihydrogen phosphate gel, stir until gray-green flocs are formed, add phosphoric acid aqueous solution dropwise until the solution is clear; continue to add chromium trichloride hexahydrate and stir until gray-green flocs are formed, add phosphoric acid aqueous solution dropwise until the solution is clear, repeat this operation 5-6 times until all the chromium trichloride hexahydrate and phosphoric acid aqueous solution are added to form a green transparent viscous liquid; add spinel powder and stir to form a light green milky slurry, which is the coating liquid.

[0017] Furthermore, the preparation process of aluminum dihydrogen phosphate gel is as follows: Aluminum hydroxide was added to a phosphoric acid aqueous solution with a mass concentration of 85 wt%, the P / A1 molar ratio was controlled to be 3.1:1, and the mixture was heated to 110°C and refluxed for 10-15 minutes until the solution became transparent and clear. The heating was stopped and the solution was naturally cooled to room temperature to obtain aluminum dihydrogen phosphate gel.

[0018] Furthermore, the preparation process of spinel powder is as follows: Aluminum hydroxide and magnesium hydroxide powders were weighed separately according to an Al / Mg molar ratio of 2:1, and the powder to grinding ball mass ratio was 2:1. The mixture was ball-milled with zirconia balls for 8 hours, and then the temperature was slowly increased to 1300°C at 5°C / min in a muffle furnace and sintered at high temperature for 1 hour. After crushing, ball milling and sieving, spinel powder with a particle size of <10μm was obtained.

[0019] Preferably, the coating thickness of the coating liquid in 3) is T, T=p×5mm, where p is the apparent porosity of the uncoated substrate layer. For example, for a corundum brick body with an apparent porosity of 7.3%, the average coating thickness of the coating liquid is 0.365mm, i.e., the coating is 365μm thick.

[0020] Compared with the prior art, the present invention has the following beneficial effects: 1. This invention is the first to use a special coating liquid to enhance the surface of the existing high-purity corundum furnace lining. The aluminum dihydrogen phosphate glue in the coating liquid forms a continuous phosphate film after solidification and sintering, which acts as a bond for the various phases of corundum and chromium salts; the spinel powder and chromium oxide and aluminum oxide interpenetrate to form a spinel-mixed chromium corundum structure, which improves the surface hardness and thermal stability; the surface spinel and chromium oxide, aluminum oxide, and phosphate interpenetrate to form a spinel-mixed chromium corundum structure. According to previous research, the surface layer may be a spinel phase and Mg x Cr y Al 1-x-y The cristobalite phase of PO4 solid solution maintains the dense passivation film characteristics of chromium oxide, that is, it maintains high thermal stability (derived from spinel and cristobalite phosphate) while ensuring density, greatly improving the chlorine permeability resistance (≤3.2×10 -5 g / cm 2 h); The coordinated dissolution and precipitation of chromium chloride and phosphoric acid can improve the permeability of the coating liquid into the substrate layer, and utilize the expansion and pore plugging of CrCl3·6H2O dehydration oxidation, coupled with the densification and surface pore plugging of surface Cr2O3, spinel and phosphate, to significantly reduce the porosity and chlorine permeability.

[0021] 2. The present invention also adopts a chlorination-annealing self-cleaning process, utilizing the lattice occupancy effect of Cl2 and phosphate. Cl2 gas carries low-melting-point NaCl / KCl (melting point 801°C / 770°C) to volatilize, simultaneously removing impurities at the grain boundaries, achieving deep removal of impurities (Na / K ≤ 0.04%), thereby improving the product purity of the chlorination process and reducing purification costs.

[0022] 3. In summary, the present invention realizes the triple synergistic mechanism of "expansion plugging - nano-filling - self-cleaning and impurity removal", solving the core problem of high permeability and short life of materials in high-temperature chlorine corrosion environment. The process parameters (such as coating thickness T = p × 5mm, 35-40 parts of spinel, and 900℃ chlorine permeation) constitute a precise control window, providing new ideas for the design of special refractory materials. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0024] The method for preparing the corrosion-resistant composite furnace lining material comprises the following steps: 1) Preparation of substrate layer: High-purity fused white corundum (Al2O3 content ≥99%), chromium oxide, calcined α-alumina powder (Al2O3 content ≥99%), kaolin, aluminum dihydrogen phosphate, carboxylated cellulose and water are mixed at a weight ratio of 100:15:10:5:2:3:5 at 90°C for 1 hour. After cooling at room temperature, the resulting mud is poured into a mold and formed by vibration press, hydraulic pressure or isostatic pressing using a friction brick press. The dried brick is sintered at 1400-1500°C for 2 days to obtain a brick-shaped base layer with a porosity of 7.3%. The appropriate porosity is about 5-10%. If the porosity is too high, the chlorine permeability resistance will be reduced. If too little binder (kaolin, aluminum dihydrogen phosphate, carboxylated cellulose) is used, although the porosity is low, the strength of the brick is too low, and the compressive strength of the base layer after calcination is also low.

[0025] 2) Preparation of coating solution: Add part of chromium trichloride hexahydrate to the aluminum dihydrogen phosphate gel, stir until gray-green flocs are formed, add phosphoric acid aqueous solution dropwise until the solution is clear; continue to add chromium trichloride hexahydrate and stir until gray-green flocs are formed, add phosphoric acid aqueous solution dropwise until the solution is clear, repeat this operation 5-6 times until all the chromium trichloride hexahydrate and phosphoric acid aqueous solution are added to form a green transparent viscous liquid; add spinel powder and stir to form a light green milky slurry, which is the coating liquid.

[0026] 3) Surface coating of substrate layer: The coating liquid is applied on the surface of a dry base layer with an apparent porosity p of 5-10%. The coating thickness is T, where T=p×5mm, where p is the apparent porosity of the uncoated base layer. For example, for a corundum brick body with an apparent porosity of 7.3%, the average coating thickness of the coating liquid is 0.365mm, i.e., the coating is 365μm thick.

[0027] 4) Coating curing: In an air atmosphere, the substrate layer coated with the coating liquid was cured in an infrared oven at 300°C for 15 minutes to obtain a dry body A. For example, the apparent porosity of the substrate layer decreased from 7.3% to 3.9%, indicating that the cured coating had a significant pore-blocking effect, especially for larger pores. During the initial infrared baking, white smoke (atomized gas formed by HCl and water in the air, likely generated by the reaction of phosphoric acid and chromium chloride) permeated the surface. After 10 minutes of baking, no smoke was generated on the surface, resulting in a dry body A. The choice of 300°C as the curing temperature was influenced by previous research, which showed that the use of spinel is beneficial to the curing of aluminum phosphate. At this temperature, chromium chloride oxidizes to chromium oxide and releases HCl. The oxidation process involves expansion, which can block the pores on the surface of the substrate layer, thereby significantly reducing the porosity. 5) High temperature firing: In air atmosphere, the dry body A is placed in a muffle furnace and slowly heated to 400℃ at 5℃ / min, and kept warm for 30min; then slowly heated to 1350-1420℃ at 10℃ / min, and sintered at 1350-1420℃ for 12-18h to obtain the primary brick B; at about 400℃, phosphoric acid and aluminum dihydrogen phosphate dehydrate to form a continuous phosphoric acid film, which acts as a bond to the various phases of corundum and chromium salts, while reducing porosity and increasing density; at a temperature greater than 800℃, the surfaces of spinel, chromium oxide and aluminum oxide react with phosphoric acid to produce magnesium phosphate, chromium and aluminum phosphate, and at the same time, the excess Cl in the system is - The residue may occupy the O vacancy of AlPO4 to produce AlPO3Cl; the temperature is ≥1200℃, and the impurity ions in the system (such as Na + , K + ) will volatilize with Cl, remove impurities, and create molecular-level nano-mesopores. AlPO3Cl will also decompose and dechlorinate to form more stable cristobalite-type AlPO4 (C-AlPO4); ≥1300℃, chromium and aluminum react to form chromium-aluminum solid solution oxides, forming a chromium corundum structure inside to improve the strength of the brick. The surface spinel and chromium oxide, aluminum oxide, and phosphate interpenetrate to form a spinel-mixed chromium corundum structure. According to previous studies, the surface may be spinel phase and Mg x Cr y Al 1-x-y The cristobalite phase of the PO4 solid solution maintains the dense passivation film characteristics of chromium oxide. Therefore, the dry body A with an apparent porosity of 3.9% becomes the primary brick B with an apparent porosity of 2.5% after calcination. The porosity is further reduced, further reducing the risk of chlorine penetration. The unreacted spinel phase can greatly improve the surface hardness and wear resistance, and the high surface smoothness makes the alkali resistance higher. The part of the surface that penetrates into the internal chromium corundum phase may be Mg generated by the reaction. x Cr y Al 1-x-yPO4 solid solution, the basic structure is still cristobalite phase, thus filling and protecting the original pores of the main chrome corundum, eliminating the risk of cracking after corrosion of the main brick.

[0028] 6) Chlorination treatment: Although during the sintering process in step 5), there may be volatile impure metal chlorides due to the residual chlorine inside the dry body A, the impurity metals (mainly low-melting-point Na, K and their oxides) in the primary brick B are still relatively high (>0.5%). Therefore, a further chlorination treatment is adopted to remove impurities, as follows: Place the primary brick B in a tube furnace, introduce a mixture of Cl2 and N2, with a volume ratio of Cl2 to N2 of 1:4, heat to 900-950℃, keep warm for 2-4h, and then - The AlPO3Cl phase is embedded into the lattice vacancies; then the temperature is lowered to 600℃ and the pure N2 purge is switched to remove the residual chlorine to obtain the chlorine-infiltrated brick C; 7) Annealing: The chlorine-permeable brick C is sprayed with water for curing at room temperature for 10-15 hours, and after drying, is placed in a muffle furnace. In an air atmosphere, the temperature is rapidly increased to 1200°C at 30°C / min, and kept warm for 2-3 hours until the tail gas does not contain chlorides. The brick is cooled with the furnace to obtain a corrosion-resistant composite furnace lining material, the surface of which is a chlorine-permeable protective layer.

[0029] Wherein, the preparation process of aluminum dihydrogen phosphate gel is as follows: Aluminum hydroxide was added to a phosphoric acid aqueous solution with a mass concentration of 85 wt%, the P / A1 molar ratio was controlled to be 3.1:1, and the mixture was heated to 110°C and refluxed for 10-15 minutes until the solution became transparent and clear. The heating was stopped and the solution was naturally cooled to room temperature to obtain aluminum dihydrogen phosphate gel.

[0030] The preparation process of spinel powder is as follows: Aluminum hydroxide and magnesium hydroxide powders were weighed separately according to an Al / Mg molar ratio of 2:1, and the powder to grinding ball mass ratio was 2:1. The mixture was ball-milled with zirconia balls for 8 hours, and then the temperature was slowly increased to 1300°C at 5°C / min in a muffle furnace and sintered at high temperature for 1 hour. After crushing, ball milling and sieving, spinel powder with a particle size of <10μm was obtained.

[0031] According to the above steps, the embodiments and comparative examples are designed as follows: Example 1

[0032] 1. Matrix layer: 100 parts of high-purity fused corundum with an Al2O3 purity of 99.2%, 15 parts of chromium oxide, 10 parts of α-alumina micropowder, 5 parts of kaolin, 2 parts of aluminum dihydrogen phosphate, 3 parts of carboxylated cellulose, and 5 parts of water. Sintered at 1400°C for 48 hours, the apparent porosity is 7.3%.

[0033] 2. Coating liquid: 100 parts of aluminum dihydrogen phosphate gel prepared at a P / Al ratio of 3.1:1, 45 parts of CrCl3·6H2O, 40 parts of 50wt% phosphoric acid, and 40 parts of spinel powder with a particle size of 8μm.

[0034] 3. Preparation method of corrosion-resistant composite furnace lining material: coating thickness 365μm → 300℃ infrared curing for 15min (the apparent porosity of the cured product is 3.9%) → 1420℃ sintering for 12h (the apparent porosity of the sintered product is 2.5%) → chlorination treatment at 950℃×3h according to Cl2 / N2=1:4 → 1200℃ annealing for 2h.

[0035] Result: Mg is formed on the surface 0.25 Cr 0.28 Al 0.47 PO4 solid solution, chlorine permeability reduced by 98%.

[0036] Example 2

[0037] 1. Base layer: The formula is the same as that of Example 1, sintered at 1500°C for 48 hours, and the apparent porosity is 7.0%.

[0038] 2. Coating liquid: 100 parts of aluminum dihydrogen phosphate gel prepared at a P / Al ratio of 3.1:1, 50 parts of CrCl3·6H2O, 50 parts of 40wt% phosphoric acid, and 37 parts of spinel powder with a particle size of 8μm.

[0039] 3. Preparation method of corrosion-resistant composite furnace lining material: coating thickness 350μm → 300℃ infrared curing for 15min (the apparent porosity of the cured product is 3.5%) → 1420℃ sintering for 12h (the apparent porosity of the sintered product is 2.4%) → chlorination treatment at 950℃×3h according to Cl2 / N2=1:4 → 1200℃ annealing for 2h.

[0040] Results: The density of the surface layer was improved probably due to the increase of Cr2O3, but the risk of sedimentation of the coating liquid increased, and the stirring needed to be accelerated.

[0041] Example 3

[0042] 1. Base layer: The formula is the same as that of Example 1. Sintered at 1450°C for 48 hours, the apparent porosity of the base layer is 7.1%.

[0043] 2. Coating liquid: 100 parts of aluminum dihydrogen phosphate gel prepared at a P / Al ratio of 3.1:1, 48 parts of CrCl3·6H2O, 42 parts of 45wt% phosphoric acid, and 35 parts of spinel powder with a particle size of 8μm.

[0044] 3. Preparation method of corrosion-resistant composite furnace lining material: coating thickness 355μm → 300℃ infrared curing for 15min (the apparent porosity of the cured product is 3.7%) → 1420℃ sintering for 12h (the apparent porosity of the sintered product is 2.4%) → chlorination treatment at 950℃×3h according to Cl2 / N2=1:4 → 1200℃ annealing for 2h.

[0045] Example 4

[0046] The formula of the base layer is the same as that of Example 1. The sintering temperature of the base layer is reduced to 1350° C. and kept warm for 18 hours. The rest is the same as that of Example 1.

[0047] Results: The apparent porosity was 2.8%, the chromium-aluminum solid solution was insufficiently formed, and the compressive strength was reduced by 15%.

[0048] Example 5

[0049] The chlorination conditions were changed to: 900°C × 4h → direct annealing after N2 purging, and the rest were the same as in Example 1.

[0050] Results: The impurity Na / K content was reduced from 0.09% in Example 1 to 0.04%, the AlPO3Cl conversion rate was improved, and the thermal stability was higher than that in Example 1.

[0051] Comparative Example 1 Base layer: 100 parts of high-purity fused corundum with an Al2O3 purity of 99.2%, 15 parts of chromium oxide, 10 parts of α-alumina powder, 5 parts of kaolin, 2 parts of aluminum dihydrogen phosphate, 6 parts of carboxylated cellulose, and 5 parts of water. Sintered at 1400°C for 48 hours, the apparent porosity of the base layer is 9.8%, and the corresponding coating thickness increases to 490 μm. The rest is the same as in Example 1.

[0052] Results: The apparent porosity of the cured product was 4.1%, the apparent porosity of the sintered product after final curing was 3.0%, and the chlorine barrier efficiency was lower than that of Example 1.

[0053] Comparative Example 2 Base layer: 100 parts of high-purity fused corundum with an Al2O3 purity of 99.2%, 15 parts of chromium oxide, 10 parts of α-alumina powder, 5 parts of kaolin, 2 parts of aluminum dihydrogen phosphate, 1 part of carboxylated cellulose, and 5 parts of water. Sintered at 1400°C for 48 hours, the apparent porosity of the base layer was 5.0%, and the corresponding coating thickness was reduced to 250 μm. The rest was the same as in Example 1.

[0054] Results: The apparent porosity of the sintered product after final solidification was 2.1%, but the thermal shock resistance was slightly reduced, and microcracks appeared after 50 cycles of reaction.

[0055] Comparative Example 3 Coating liquid: 100 parts of aluminum dihydrogen phosphate gel prepared at a P / Al ratio of 3.1:1, 48 parts of CrCl3·6H2O, 42 parts of 45wt% phosphoric acid, and 60 parts of spinel powder with a particle size of 8μm.

[0056] The coating liquid needs to be stirred at high speed before coating, and the rest is the same as in Example 1.

[0057] Results: The coating slurry had serious sedimentation, resulting in uneven coating, which further caused the local porosity of the sintered product to be greater than 5% after solidification and a significant decrease in chlorine corrosion resistance.

[0058] Comparative Example 4 The infrared curing temperature was changed to 250° C. for 15 min, and the rest was the same as in Example 1.

[0059] Results: HCl was not completely released during the curing process, the coating adhesion was poor, and the protective layer peeled off after sintering.

[0060] Comparative Example 5 The chlorine treatment was omitted and the primary brick B was directly annealed. The rest was the same as in Example 1.

[0061] Results: After final solidification, the residual Na / K impurities in the sintered product were 0.48%, and the intergranular corrosion was aggravated after long-term use.

[0062] Comparative Example 6 Cr2O3 was used in place of CrCl3·6H2O in the coating liquid formula to make the Cr element content the same as that of the coating liquid in Example 1. The rest of the formula and steps were the same as in Example 1.

[0063] Results: During the infrared curing process, there was a lack of dehydration and expansion effect of chromium chloride. The apparent porosity of the sintered product after curing was only reduced to 6.1%, and the chlorine barrier efficiency was low.

[0064] The data is shown in Table 1: Group Apparent porosity (%) Chlorine permeability (g / cm²·h) Compressive strength (MPa) Impurities (Na / K,%) Chlorination process impurity content (wt%) Example 1 2.5 <![CDATA[3.2×10 -5 ]]> 148 0.09 <0.02 Example 2 2.4 <![CDATA[2.8×10 -5 ]]> 152 0.08 <0.02 Example 3 2.4 <![CDATA[2.9×10 -5 ]]> 150 0.10 <0.02 Example 4 2.8 <![CDATA[5.1×10 -5 ]]> 126 0.12 0.021 Example 5 2.3 <![CDATA[2.5×10 -5 ]]> 145 0.04 <0.01 Comparative Example 1 3.0 <![CDATA[1.8×10 -4 ]]> 135 0.15 0.030 Comparative Example 2 2.1 <![CDATA[4.0×10 -5 ]]> 138 0.11 <0.02 Comparative Example 3 5.3 <![CDATA[1.2×10 -4 ]]> 98 0.10 <0.02 Comparative Example 4 4.9 <![CDATA[2.2×10 -4 ]]> 105 0.18 0.049 Comparative Example 5 2.7 <![CDATA[3.0×10 -5 ]]> 142 0.48 0.128 Comparative Example 6 6.1 <![CDATA[3.5×10 -4 ]]> 118 0.13 0.028 It should be noted that the apparent porosity in Table 1 refers to the apparent porosity of the final product - the corrosion-resistant composite furnace lining material; the impurity content in the chlorination process refers to applying the corrosion-resistant composite furnace lining materials in Examples 1-5 or Comparative Examples 1-6 to the zircon sand boiling chlorination process, and detecting the chloride impurity content in the gas product other than ZrCl4 and SiCl4, and the chloride impurities are mainly NaCl, KCl and AlCl3.

[0065] Comparing Examples 1-5 horizontally, the apparent porosity of the protective layer of Example 1-3 is ≤2.5%, and the chlorine permeability is as low as 10 -5 The pores may be blocked by the dehydration, oxidation and expansion of CrCl3·6H2O at 300℃; spinel and phosphate form a Mg-Cr-Al-PO4 solid solution at high temperature, namely cristobalite phase, which forms nano-filled micropores.

[0066] In contrast, the substrate porosity of Comparative Example 1 was 9.8%, resulting in the coating being unable to completely cover the deep pores → the final porosity was 3.0%, and the chlorine permeability increased by 5.6 times.

[0067] Comparative Example 5 does not contain CrCl3 and lacks dehydration expansion effect. After curing, the porosity is reduced to only 6.1%, and the chlorine barrier fails.

[0068] In Example 1, spinel reacts with phosphate to form a continuous dense layer with a surface hardness of HV1200. However, in Comparative Example 3, excessive spinel is used, which causes the coating liquid slurry to settle and the coating liquid viscosity to increase from 850 mPa·s to 2100 mPa·s, resulting in uneven coating. In addition, excessive spinel may hinder the oxidation expansion of CrCl3, resulting in a local porosity of >5%, a significant decrease in chlorine corrosion resistance, and a decrease in strength.

[0069] Example 5 further improves the chlorination-annealing process, chlorination at 900℃×4h, so that the O vacancies in AlPO4 are replaced by Cl - AlPO3Cl is generated, and AlPO3Cl decomposes and removes Cl when annealed at 1200℃ - And take away Na + / K +, The impurity content was reduced to 0.04%, while that of Example 1 was 0.09%.

[0070] In Comparative Example 4, the chlorination process is omitted, and the Na / K residue is 0.48%. Low-melting-point NaCl or KCl is formed at high temperature. The melting points of NaCl and KCl are 801°C and 770°C, respectively. On the one hand, it causes intergranular corrosion, and on the other hand, it increases the impurity content of the chlorination process, thereby increasing the purification cost.

[0071] Comparing Example 1 with Example 4, the sintering temperature of Example 1 is 1420°C, at which temperature the chromium-aluminum solid solution is fully formed, thereby increasing the compressive strength to 148 MPa, while the sintering temperature of Example 4 is 1350°C, at which temperature the solid solution is insufficiently formed, the compressive strength drops to 126 MPa, and the porosity increases to 2.8%, which indirectly indicates that expansion plugging + solid solution nanofilling is the core of achieving ultra-low porosity (≤2.5%).

[0072] The above description is only a preferred specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, who makes equivalent replacements or changes based on the technical solution and inventive concept of the present invention, should be covered by the scope of protection of the present invention.

Claims

1. Anti-corrosion composite furnace lining material for boiling chlorination of zircon sand, characterized in that: It includes a base layer and a chlorine-resistant protective layer; The matrix layer is formed by sintering high-purity fused corundum aggregate and fine powder with a small amount of sintering agent; The anti-chlorine permeation protective layer is prepared by mixing, coating, high-temperature firing, chlorine permeation treatment and annealing the following components in parts by weight: 100 parts of aluminum dihydrogen phosphate gel; 45-50 parts of chromium trichloride hexahydrate; 40-50 parts of an aqueous phosphoric acid solution, wherein the weight concentration of phosphoric acid is 40-50wt%; 35-40 parts of spinel powder.

2. The method for preparing the corrosion-resistant composite furnace lining material for boiling chlorination of zircon sand according to claim 1, characterized in that: The following steps are involved: 1) Preparation of substrate layer: The chrome corundum bricks made of high-purity fused white corundum, chromium oxide and other auxiliary materials are used as the base layer; 2) Preparation of coating liquid: The method is prepared by mixing aluminum dihydrogen phosphate gel, chromium trichloride hexahydrate, phosphoric acid aqueous solution and spinel powder; 3) Surface coating of substrate layer: Applying a coating liquid on the surface of a dry base layer having an apparent porosity p of 5-10%; 4) Coating curing: In an air atmosphere, the base layer coated with the coating liquid is baked and cured in an infrared baking machine at 300° C. for 15 minutes to obtain a dry body A. 5) High temperature firing: In air atmosphere, the dried body A was placed in a muffle furnace and slowly heated to 400°C at 5°C / min and kept at this temperature for 30 minutes; then slowly heated to 1350-1420°C at 10°C / min and sintered at 1350-1420°C for 12-18 hours to obtain a primary brick B; 6) Chlorination treatment: Place the primary brick B in a tube furnace, introduce a mixture of Cl2 and N2, with a volume ratio of Cl2 to N2 of 1:4, heat to 900-950℃, keep warm for 2-4h, and then - The AlPO3Cl phase is embedded into the lattice vacancies; then the temperature is lowered to 600℃ and the pure N2 purge is switched to remove the residual chlorine to obtain the chlorine-infiltrated brick C; 7) Annealing: The chlorine-permeable brick C is sprayed with water for curing at room temperature for 10-15 hours, and after drying, is placed in a muffle furnace. In an air atmosphere, the temperature is rapidly increased to 1200°C at 30°C / min, and kept warm for 2-3 hours until the tail gas does not contain chlorides. The brick is cooled with the furnace to obtain a corrosion-resistant composite furnace lining material, the surface of which is a chlorine-permeable protective layer.

3. The method for preparing the corrosion-resistant composite furnace lining material for boiling chlorination of zircon sand according to claim 2, characterized in that: The preparation process of the substrate layer in 1) is as follows: High-purity fused white corundum, chromium oxide, calcined α-alumina powder, kaolin, aluminum dihydrogen phosphate, carboxylated cellulose and water are mixed at a weight ratio of 100:15:10:5:2:3:5 at 90°C for 1 hour. After cooling at room temperature, the obtained mud is poured into a mold and formed by vibration press, hydraulic pressure or isostatic pressing using a friction brick press. The dried bricks are sintered at 1400-1500°C for 2 days to obtain a brick-shaped base layer.

4. The method for preparing the corrosion-resistant composite furnace lining material for boiling chlorination of zircon sand according to claim 2, characterized in that: The preparation process of the coating liquid in 2) is as follows: Add part of chromium trichloride hexahydrate to the aluminum dihydrogen phosphate gel, stir until gray-green flocs are formed, add phosphoric acid aqueous solution dropwise until the solution is clear; continue to add chromium trichloride hexahydrate and stir until gray-green flocs are formed, add phosphoric acid aqueous solution dropwise until the solution is clear, repeat this operation 5-6 times until all the chromium trichloride hexahydrate and phosphoric acid aqueous solution are added to form a green transparent viscous liquid; add spinel powder and stir to form a light green milky slurry, which is the coating liquid.

5. The method for preparing the corrosion-resistant composite furnace lining material for boiling chlorination of zircon sand according to claim 4, characterized in that: The preparation process of the aluminum dihydrogen phosphate gel is as follows: Aluminum hydroxide was added to a phosphoric acid aqueous solution with a mass concentration of 85 wt%, the P / A1 molar ratio was controlled to be 3.1:1, and the mixture was heated to 110°C and refluxed for 10-15 minutes until the solution became transparent and clear. The heating was stopped and the solution was naturally cooled to room temperature to obtain aluminum dihydrogen phosphate gel.

6. The method for preparing the corrosion-resistant composite furnace lining material for boiling chlorination of zircon sand according to claim 4, characterized in that: The preparation process of the spinel powder is as follows: Aluminum hydroxide and magnesium hydroxide powders were weighed separately according to an Al / Mg molar ratio of 2:1, and the powder to grinding ball mass ratio was 2:

1. The mixture was ball-milled with zirconia balls for 8 hours, and then the temperature was slowly increased to 1300°C at 5°C / min in a muffle furnace and sintered at high temperature for 1 hour. After crushing, ball milling and sieving, spinel powder with a particle size of <10μm was obtained.

7. The method for preparing the corrosion-resistant composite furnace lining material for boiling chlorination of zircon sand according to claim 2, characterized in that: The coating thickness of the coating liquid in the above 3) is T, where T=p×5 mm, where p is the apparent porosity of the uncoated substrate layer.

Citation Information

Patent Citations

  • Aeronautic glass formula and preparation method of aeronautic glass

    CN110156319A

  • Method for improving performance of SiC MOSFET device by using chlorine-containing post-oxidation annealing technology

    CN113223940A

  • Water-coal-slurry gasification furnace lining material based on high-chromium castable and preparation method of water-coal-slurry gasification furnace lining material

    CN119059828A

  • Composite wear-resistant and fire-resistant corundum brick and preparation method thereof

    CN120349199A

Cited By

  • Micro-nano structure ceramic coating and its application in zircon sand boiling chlorination method reaction furnace

    CN122380818A

  • Micro-nano structure ceramic coating and its application in zircon sand boiling chlorination method reaction furnace

    CN122380818B