Preparation method and application of environment-friendly CO2 enhanced burying and channeling sealing system
By preparing a combination of inorganic silicates containing metasilicate and acidic amino acids to generate a polysilicic acid structure, the problems of easy degradation and poor thermal stability of existing CO2 sealing systems in acidic formations are solved, achieving efficient and economical CO2 oil recovery and long-term storage.
Patent Information
- Application Number
- CN202510701931.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-28
- Publication Date
- 2025-09-23
AI Technical Summary
The existing CO2 sealing system is easily degraded in acidic formations, has poor thermal stability, is complex to prepare and has high costs, and is difficult to meet the needs of CO2 oil recovery and long-term storage.
A combination of inorganic silicates containing metasilicate, acidic amino acids, inorganic nanomaterials and thermosensitive sustained-release capsules is used to generate amine compounds and metasilicic acid precipitates through decarboxylation reaction, forming a polysilicic acid structure to prepare an environmentally friendly CO2 enhanced storage and sealing system.
The prepared sealing system has good injection performance, strong temperature resistance, low viscosity before curing, controllable curing time, high curing strength, and economical and reasonable price, meeting the needs of CO2 oil displacement and long-term sealing.
Smart Images

Figure CN120681975A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of carbon dioxide sequestration, and in particular to a preparation method and application of an environmentally friendly CO2 enhanced sequestration and sealing system. Background Art
[0002] CO2 capture, utilization, and storage are core technologies for China to achieve its "dual carbon" goals and are a global research hotspot. CO2 flooding not only improves oil production efficiency but also enables CO2 storage. However, during CO2 storage, reservoir heterogeneity can easily create advantageous channels for CO2 crossflow. Furthermore, the low viscosity and high mobility of CO2 in a supercritical state can easily lead to viscous fingering.
[0003] Currently, there are four main types of sealing systems that are most widely used on the market: gel sealing systems (delayed cross-linking polyacrylamide gel, pre-cross-linked gel particles, two-stage sealing gel systems, foam gel, etc.); resin sealing systems (phenolic resin systems, epoxy resin systems, polyester resin systems, urea-formaldehyde resin systems and some composite resin systems, etc.); intelligent sealing systems (CO2-responsive sealing systems, pH-responsive sealing systems, etc.); other sealing systems (cement sealing systems such as G-grade oil well high-resistance cement and ultrafine cement, sealing systems that generate precipitation by CO2 and sodium silicate solution, CO2 and high-concentration potassium silicate solution, and CO2 foam sealing systems, etc.). Gel-based sealing systems are prone to degradation in acidic formation environments caused by CO2, and gel-foam systems have poor thermal stability and the foam is prone to rupture. Although resin-based sealing systems have high strength and stability, their complex preparation process and high cost limit their widespread application in actual production. Although intelligent sealing systems have good injection performance and sealing capabilities, their preparation conditions are strict and the monomer cost is high, so a lot of research is still needed to verify their applicability on construction sites.
[0004] In view of this, it is very meaningful and necessary to develop an environmentally friendly sealing system with simple preparation, low cost, strong reservoir adaptability, strong stability, good injectivity and strong sealing ability. Summary of the Invention
[0005] One of the purposes of the present invention is to provide a method for preparing an environmentally friendly CO2 enhanced storage and sealing system. The CO2 enhanced storage and sealing system prepared by this method has the advantages of good injection performance, strong temperature resistance, and long temperature resistance period; and the system has low viscosity before solidification, controllable solidification time, and high solidification strength; on-site construction is simple and convenient; the price is economical and reasonable, and can meet the needs of CO2 oil displacement and long-term storage and sealing.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing an environmentally friendly CO2 enhanced storage and sealing system comprises the following steps:
[0008] a. Prepare the required raw materials: The raw materials are composed of the following raw materials according to weight percentage:
[0009] 25-45% of an inorganic silicate containing metasilicate, 12-22% of an acidic amino acid containing a carboxyl group at each end of the molecule, 0.15-0.3% of an anionic surfactant containing an aromatic ring, 1.5-3.0% of an inorganic nanomaterial containing silanol groups, 0.03% of an amino acid decarboxylase, and the balance being water; the amino acid decarboxylase is used as a core material and is wrapped inside a gelatin wall material, and the core and wall materials together constitute a temperature-sensitive sustained-release capsule;
[0010] b. Stir and mix the raw materials required in step a to form a mixed system. Control the temperature of the mixed system to 50-70° C. At this temperature, the following reactions occur in sequence:
[0011] The acidic amino acid undergoes a decarboxylation reaction with amino acid decarboxylase, and the carboxyl groups at both ends of the acidic amino acid molecule are broken to generate amine compounds and carbon dioxide;
[0012] The carbon dioxide released by the reaction reduces the pH of the mixed system. When the pH is less than 9, the metasilicate in the inorganic silicate reacts with the carbon dioxide to form metasilicate precipitation and orthosilicic acid.
[0013] The orthosilicic acid obtained by the reaction and the inorganic nanomaterial containing silanol groups work together to form a polysilicic acid structure. The amine compound is embedded in the polysilicic acid structure through hydrogen bonding, and then forms a semi-solid silica gel under the action of anionic surfactant.
[0014] In the above-mentioned preparation method of an environmentally friendly CO2 enhanced storage and sealing system, the inorganic silicate containing metasilicate is sodium silicate, asbestos, feldspar or glass.
[0015] In the above-mentioned preparation method of an environmentally friendly CO2 enhanced storage and sealing system, the acidic amino acid containing a carboxyl group at each end of the molecule is aspartic acid or glutamic acid.
[0016] In the above-mentioned preparation method of an environmentally friendly CO2 enhanced storage and sealing system, the anionic surfactant containing an aromatic ring is sodium dodecylbenzene sulfonate, linear alkylbenzene sulfonate, sodium lignin sulfonate or calcium lignin sulfonate.
[0017] In the above-mentioned preparation method of an environmentally friendly CO2 enhanced storage and sealing system, the inorganic nanomaterial containing silanol is nano-silicon dioxide.
[0018] The above-mentioned preparation method of the environmentally friendly CO2 enhanced storage and sealing system is to add temperature-sensitive sustained-release microcapsules to the mixed system. The temperature-sensitive sustained-release microcapsules include a wall material and a core material, the wall material is gelatin, and the core material is amino acid decarboxylase.
[0019] The above-mentioned preparation method of an environmentally friendly CO2 enhanced storage and sealing system, the preparation method of the temperature-sensitive sustained-release microcapsules is: add gelatin to deionized water at 45-55°C and stir and dissolve it thoroughly; after cooling the resulting solution to 30-40°C, add amino acid decarboxylase and mix evenly, drop the resulting mixed solution into vegetable oil, form an oil-in-water emulsion by stirring, and then transfer the oil-in-water emulsion to ice water and stir until the gelatin condenses, and obtain the temperature-sensitive sustained-release microcapsules after separation and drying.
[0020] In the above-mentioned preparation method of the environmentally friendly CO2 enhanced storage and sealing system, the temperature-sensitive sustained-release microcapsules begin to depolymerize and release amino acid decarboxylase at 60°C.
[0021] The above-mentioned preparation method of an environmentally friendly CO2 enhanced storage and sealing system, the raw material composition is: 35% of inorganic silicate containing metasilicate, 18% of acidic amino acid containing a carboxyl group at each end of the molecule, 0.2% of anionic surfactant containing an aromatic ring, 2% of inorganic nanomaterial containing silicone hydroxyl groups, 0.03% of amino acid decarboxylase, and the remainder is water.
[0022] Another object of the present invention is to provide an application of an environmentally friendly CO2 enhanced storage and sealing system, which is to mix an environmentally friendly CO2 enhanced storage and sealing system with temperature-sensitive sustained-release capsules and inject them into the oil reservoir, and continue to inject carbon dioxide after shutting down the well for 3 to 5 days.
[0023] Compared with the prior art, the present invention brings the following beneficial technical effects:
[0024] The present invention proposes a method for preparing an environmentally friendly CO2 enhanced storage and sealing system, which first undergoes a decarboxylation reaction between an acidic amino acid and an amino acid decarboxylase, breaking the carboxyl groups at both ends of the acidic amino acid molecule to generate an amine compound and carbon dioxide; wherein the amine compound can participate in the subsequent polysilicic acid structure, which can better complex the calcium and magnesium ions in the formation and improve the strength of the gel product. The carbon dioxide can lower the pH of the system and provide the metasilicate in the inorganic silicate to react with carbon dioxide to further generate metasilicic acid precipitate and orthosilicic acid. The orthosilicic acid undergoes a condensation reaction and acts together with an inorganic nanomaterial containing silanol to form a polysilicic acid structure; the polysilicic acid structure is cross-linked under the action of an anionic surfactant to finally obtain a silica gel. In the above preparation method, by improving the raw materials and combining the methods, a silica gel with high mechanical strength and high curing strength can be prepared.
[0025] The CO2 enhanced storage and sealing system prepared by the present invention has good injection performance, strong temperature resistance, and long effective temperature resistance period; low viscosity before solidification, controllable solidification time, and high solidification strength; simple and convenient on-site construction; economical and reasonable price, and meets the needs of CO2 oil displacement and long-term storage and sealing. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The present invention will be further described below with reference to the accompanying drawings:
[0027] Figure 1 Schematic diagram of the silica gel prepared by the present invention before and after curing;
[0028] Figure 2 This is a microscopic image of the silicic acid gel prepared by the present invention after curing;
[0029] Figure 3 This is the infrared spectrum of the silica gel prepared by the present invention;
[0030] Figure 4 This is a graph showing the curing time of the silica gel prepared in the present invention at different concentrations at 70°C;
[0031] Figure 5 This is a curve diagram showing the change in viscosity of the silica gel prepared by the present invention as a function of instantaneous temperature;
[0032] Figure 6 This is a schematic diagram of the one-dimensional tubular flow model required by the present invention;
[0033] Figure 7 This is a graph showing the relationship between the injection pressure of the silica gel prepared in the present invention and the injected pore volume;
[0034] Figure 8 This is a schematic diagram of the parallel artificial core flow model required by the present invention;
[0035] Figure 9 This is a graph showing the relationship between the injection pressure and diversion rate of the system of the present invention and the injected pore volume;
[0036] Figure 10 This is a graph showing the relationship between the residual resistance coefficient and the permeability of the system of the present invention;
[0037] Figure 11 This is a graph showing the relationship between the free water rate of the system of the present invention and time;
[0038] Figure 12 This is a graph showing the relationship between the residual resistance coefficient retention rate of the system of the present invention and time. DETAILED DESCRIPTION
[0039] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application.
[0040] In the description of this application, unless otherwise specified, " / " means "or". For example, A / B can mean A or B. "And / or" in this document is simply a description of the association relationship between related objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone.
[0041] The raw materials required for the present invention: inorganic silicate containing metasilicate, acidic amino acid containing a carboxyl group at each end of the molecule, anionic surfactant containing an aromatic ring, inorganic nanomaterial containing silanol, and amino acid decarboxylase can all be purchased through commercial channels.
[0042] Among them, inorganic silicates containing metasilicate groups include sodium silicate, asbestos, feldspar, and glass. Acidic amino acids containing a carboxyl group at each end of the molecule include aspartic acid or glutamic acid. Anionic surfactants containing aromatic rings include sodium dodecylbenzenesulfonate, linear alkylbenzenesulfonate, sodium ligninsulfonate, or calcium ligninsulfonate. Inorganic nanomaterials containing silanol groups include nanosilica.
[0043] In the drawings of the present invention, component A is an inorganic silicate containing metasilicate, component B is an acidic amino acid containing a carboxyl group at each end of the molecule, and component D is an inorganic nanomaterial containing silanol groups.
[0044] According to the different required components and contents (weight percentage), the present invention can obviously obtain a variety of system combinations, namely:
[0045] Combination 1: sodium silicate 25%, aspartic acid 12%, sodium dodecylbenzene sulfonate 0.15%, nano-silica 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0046] Combination 2: asbestos 45%, glutamic acid 22%, linear alkylbenzene sulfonate 0.3%, nano-silica 3%, amino acid decarboxylase 0.03%, and the balance is water.
[0047] Combination 3: glass 30%, aspartic acid 15%, sodium lignin sulfonate 0.2%, nano-silica 2%, amino acid decarboxylase 0.03%, and the balance is water.
[0048] Combination 4: feldspar 35%, glutamic acid 20%, sodium dodecylbenzene sulfonate 0.25%, nano-silica 1.8%, amino acid decarboxylase 0.03%, and the balance is water.
[0049] Combination 5: sodium silicate 25%, glutamic acid 18%, calcium lignin sulfonate 0.15%, nano-silicon dioxide 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0050] Combination six: sodium silicate 30%, glutamic acid 18%, calcium lignin sulfonate 0.15%, nano-silicon dioxide 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0051] Combination seven: sodium silicate 35%, glutamic acid 18%, calcium lignin sulfonate 0.15%, nano-silicon dioxide 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0052] Combination 8: sodium silicate 40%, glutamic acid 18%, calcium lignin sulfonate 0.15%, nano-silicon dioxide 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0053] Combination nine: sodium silicate 45%, glutamic acid 18%, calcium lignin sulfonate 0.15%, nano-silicon dioxide 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0054] Combination 10: sodium silicate 45%, aspartic acid 18%, calcium lignin sulfonate 0.15%, nano-silicon dioxide 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0055] The preparation method of the thermosensitive sustained-release microcapsules described in the present invention comprises: adding gelatin to deionized water at 45-55°C and stirring thoroughly to dissolve; cooling the resulting solution to 30-40°C, adding amino acid decarboxylase, and mixing thoroughly; dropping the resulting mixed solution into vegetable oil and stirring to form an oil-in-water emulsion; then transferring the oil-in-water emulsion to ice water and stirring until the gelatin condenses; separating and drying to obtain the thermosensitive sustained-release microcapsules. The resulting thermosensitive sustained-release microcapsules comprise a wall material made of gelatin and a core material made of amino acid decarboxylase. The thermosensitive sustained-release microcapsules begin to depolymerize at 60°C and release the amino acid decarboxylase.
[0056] Example 1:
[0057] In combination with different combinations of the above systems, the preparation method of silica gel in this embodiment includes the following steps:
[0058] Step 1: Prepare the required raw materials: 25% sodium silicate, 12% aspartic acid, 0.15% sodium dodecylbenzene sulfonate, 1.5% nano-silica, 0.03% amino acid decarboxylase, and the balance is water.
[0059] Step 2: Mix all the raw materials evenly to form a mixed system, add the temperature-sensitive sustained-release microcapsules to the mixed system, and control the temperature of the mixed system to 60°C. At this temperature, the temperature-sensitive sustained-release microcapsules begin to depolymerize and slowly release amino acid decarboxylase, and the following reactions occur in sequence:
[0060] Acidic amino acids undergo a decarboxylation reaction with amino acid decarboxylase, and the carboxyl groups at both ends of the acidic amino acid molecules are broken to generate amine compounds and carbon dioxide; among them, the amine compounds can be embedded in the subsequently formed polysilicate network through hydrogen bonding, and can complex calcium and magnesium ions in the formation, thereby increasing the strength of the silicate gel.
[0061] The inorganic silicate solution is strongly alkaline. As the amount of carbon dioxide released increases, the carbon dioxide reduces the pH of the mixed system. When the pH is less than 9, the metasilicate in the inorganic silicate reacts with carbon dioxide to generate metasilicate precipitation and orthosilicic acid. The reaction ion equations are shown in Equations (1) and (2):
[0062] 2OH - +2CO2+SiO3 2- →H2SiO3↓+2CO3 2- (1); 2OH - +CO2+SiO3 2- →SiO4 4- +CO3 2- +2H + (2);
[0063]
[0064] The resulting orthosilicic acid reacts with inorganic nanomaterials containing silanol groups to form a polysilicic acid structure. The amine compound is embedded in the polysilicic acid structure through hydrogen bonding, and then forms a semi-solid silica gel under the action of anionic surfactants. Equation (3) shows a schematic diagram of the system condensation reaction.
[0065] The silica gel prepared in this example is as follows Figure 1 As shown, Figure 1(a) shows the state before solidification, and (b) shows the state after solidification. The viscosity of the system is 2-5 mPa·s at room temperature. The viscosity before solidification is low, and after solidification, it becomes a large solid with high strength. Figure 2 As shown in the microscopic morphology of the silica gel after curing, it can be seen from the scanning results at the 500nm scale that the system gradually forms regular crystals. The holes between the crystals are left by the bound water, and the pore size is less than 1μm. This shows that the system has high mechanical strength. These crystals are combined with each other through surface contact to form aggregates with coral-like structures (3μm, 10μm). The aggregates interact to form an overall solid with a stable structure (50μm). Figure 3 As shown in the infrared spectrum of silica gel, it can be seen that there are many types of carboxylic acids, alcohols, phenols and other substances containing heteroatoms (such as C, N, O, Si, etc.) in the system. -1 There is an absorption peak in the region, which indicates that the system may contain amino groups; at 1447cm -1 and 1633cm -1 There is an absorption peak in the region, which indicates that the system may contain carboxylate ions; at 1104 cm -1 The absorption peak appears in the region, reflecting that the system contains silicon-oxygen-silicon bridge bonds. The curing time of silica gel at different concentrations at 70℃ is shown in the figure below. Figure 4 shown.
[0066] Example 2:
[0067] Step 1: Prepare the required raw materials: 25% sodium silicate, 18% glutamic acid, 0.15% calcium lignin sulfonate, 1.5% nano-silica, 0.03% amino acid decarboxylase, and the balance is water.
[0068] The preparation method is the same as that in Example 1.
[0069] Example 3:
[0070] Step 1: Prepare the required raw materials: 30% sodium silicate, 18% glutamic acid, 0.15% calcium lignin sulfonate, 1.5% nano-silica, 0.03% amino acid decarboxylase, and the balance is water.
[0071] The preparation method is the same as that in Example 1.
[0072] Example 4:
[0073] Step 1: Prepare the required raw materials: 35% sodium silicate, 18% glutamic acid, 0.15% calcium lignin sulfonate, 1.5% nano-silica, 0.03% amino acid decarboxylase, and the balance is water.
[0074] The preparation method is the same as that in Example 1.
[0075] Example 5:
[0076] Step 1: Prepare the required raw materials: sodium silicate 40%, glutamic acid 18%, calcium lignin sulfonate 0.15%, nano-silica 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0077] The preparation method is the same as that in Example 1.
[0078] Example 6:
[0079] Step 1: Prepare the required raw materials: sodium silicate 45%, glutamic acid 18%, calcium lignin sulfonate 0.15%, nano-silica 1.5%, amino acid decarboxylase 0.03%, and the balance is water.
[0080] The preparation method is the same as that in Example 1.
[0081] Example 7:
[0082] The difference from Example 1 is that no temperature-sensitive sustained-release microcapsules are added in step 2.
[0083] Amino acids and amino acid decarboxylase undergo decarboxylation reactions at room temperature. The resulting products can easily trigger premature condensation reactions and precipitation in the system, leading to a sharp decrease in injectability. Furthermore, this reaction process is difficult to effectively control, making it impossible to ensure precise release of the system under specific formation conditions, thus affecting the safety and controllability of the operation.
[0084] The injection performance and selective injection capability of the silica gel prepared in Examples 2 to 6 were tested, and the real-time viscosity of the system was measured with temperature using a Brookfield DV-II viscometer. Figure 5 As shown in the figure, the injection performance of the system is examined. The lower the viscosity, the easier it is to inject into the formation. The higher the concentration of component A, the higher the viscosity. However, reducing the concentration of A will lead to longer curing time and lower curing strength, so comprehensive consideration is required.
[0085] The injection performance of the system is investigated using a one-dimensional tubular flow model, such as Figure 6 As shown. The system is injected at a constant flow rate, and the injection pressure at different concentrations and different permeabilities is measured as a function of the injected pore volume multiple (PV), as shown in Figure 2. Figure 7 As shown, the test sample is the system before solidification. The lower the injection pressure, the better. The curve is the injection pressure of the 35wt% A+18wt% B system at different core permeabilities. The overall injection pressure is low, indicating that the system has good injectivity at different permeabilities.
[0086] The parallel artificial core flow model was used to investigate the selective injection capability of the system. Figure 8As shown. Inject the system at a constant flow rate, record the injection pressure and high and low core tube diversion volumes; draw the injection pressure and diversion rate curves with the injection pore volume multiple (PV) at different concentrations and different permeability extremes, as shown Figure 9 As shown, Figure 9 It is the diversion rate of the 35wt% A+18wt% B system when the permeability difference is 6. The higher the diversion rate of the high permeability core, the better. The diversion rate of the high permeability core is close to 90%, so the system has good selective injection performance.
[0087] The plugging ability of the silica gel prepared in Examples 2 to 6 was tested. The plugging ability of the system was investigated using a one-dimensional tubular flow model. An artificial core was placed in an oven, evacuated, and saturated with simulated groundwater. The system solution was injected at a constant flow rate. After the system was gelled, supercritical CO2 was injected at the same flow rate. The relationship between the residual resistance coefficient and the permeability at different concentrations was measured, as shown in FIG. Figure 10 As shown in Figure 1, residual resistance coefficient = permeability before plugging / permeability after plugging. The larger the value, the better the plugging effect. The 45wt% A + 18wt% B system has the best plugging effect at different permeabilities.
[0088] The aging stability of the silica gels prepared in Examples 2 to 6 above was tested. The systems with different concentrations were placed in a constant temperature box and aged for 120 days. The free water rate of the system was measured at intervals. The aging stability of the system was evaluated by plotting the relationship between the free water rate of the different concentration systems and time. Figure 11 As shown. Free water rate = precipitated water / total volume. Under the same aging time, the lower the free water rate, the better the stability. Using a one-dimensional tubular flow model, the relationship between the residual resistance coefficient retention rate of different concentration systems and time is plotted, as shown in Figure 12 As shown in the figure, the higher the residual resistance coefficient retention rate, the better the long-term plugging performance of the system.
[0089] In summary, the environmentally friendly CO2 enhanced storage and channel sealing system provided by the present invention exhibits excellent injection performance, selective injection capability, and sealing capabilities. Due to its low pre-curing viscosity, it causes less damage to the formation. Furthermore, the system offers strong heat resistance and a long effective heat resistance period; a controllable curing time and high curing strength; simple and convenient on-site construction; and an affordable price. These advantages meet the needs of CO2 oil recovery and long-term storage and channel sealing.
[0090] Parts not described in the present invention can be implemented by referring to the existing technology.
[0091] Those skilled in the art should recognize that the above embodiments are merely intended to illustrate the present application and are not intended to limit the present application. As long as they are within the spirit of the present application, appropriate changes and modifications to the above embodiments are within the scope of protection claimed in the present application.
Claims
1. A method for preparing an environmentally friendly CO2 enhanced storage and sealing system, characterized in that: The following steps are involved: a. Prepare the required raw materials: The raw materials are composed of the following raw materials according to weight percentage: 25-45% of an inorganic silicate containing metasilicate, 12-22% of an acidic amino acid containing a carboxyl group at each end of the molecule, 0.15-0.3% of an anionic surfactant containing an aromatic ring, 1.5-3.0% of an inorganic nanomaterial containing silanol groups, 0.03% of an amino acid decarboxylase, and the balance being water; the amino acid decarboxylase is used as a core material and is wrapped inside a gelatin wall material, and the core and wall materials together constitute a temperature-sensitive sustained-release capsule; b. Stir and mix the raw materials required in step a to form a mixed system. Control the temperature of the mixed system to 50-70° C. At this temperature, the following reactions occur in sequence: The acidic amino acid undergoes a decarboxylation reaction with the amino acid decarboxylase in the temperature-sensitive sustained-release microcapsule, and the carboxyl groups at both ends of the acidic amino acid molecule are broken to generate amine compounds and carbon dioxide; The carbon dioxide released by the reaction reduces the pH of the mixed system. When the pH is less than 9, the metasilicate in the inorganic silicate reacts with the carbon dioxide to form metasilicate precipitation and orthosilicic acid. The orthosilicic acid obtained by the reaction and the inorganic nanomaterial containing silanol groups work together to form a polysilicic acid structure. The amine compound is embedded in the polysilicic acid structure through hydrogen bonding, and then forms a semi-solid silica gel under the action of anionic surfactant.
2. The method for preparing an environmentally friendly CO2 enhanced storage and sealing system according to claim 1, characterized in that: Inorganic silicates containing metasilicate are sodium silicate, asbestos, feldspar or glass.
3. The method for preparing an environmentally friendly CO2 enhanced storage and sealing system according to claim 1, characterized in that: The acidic amino acids containing a carboxyl group at each end of the molecule are aspartic acid or glutamic acid.
4. The method for preparing an environmentally friendly CO2 enhanced storage and sealing system according to claim 1, characterized in that: The anionic surfactant containing an aromatic ring is sodium dodecylbenzenesulfonate, linear alkylbenzenesulfonate, sodium ligninsulfonate or calcium ligninsulfonate.
5. The method for preparing an environmentally friendly CO2 enhanced storage and sealing system according to claim 1, characterized in that: The inorganic nanomaterial containing silanol is nano-silicon dioxide.
6. The method for preparing an environmentally friendly CO2 enhanced storage and sealing system according to claim 5, characterized in that: The preparation method of the thermosensitive sustained-release microcapsules comprises the following steps: adding gelatin to deionized water at 45-55°C and stirring thoroughly to dissolve the resultant solution; cooling the resulting solution to 30-40°C, adding amino acid decarboxylase and mixing uniformly; dripping the resulting mixed solution into vegetable oil and stirring to form an oil-in-water emulsion; then transferring the oil-in-water emulsion into ice water and stirring until the gelatin condenses; and separating and drying the resulting mixture to obtain the thermosensitive sustained-release microcapsules.
7. The method for preparing an environmentally friendly CO2 enhanced storage and sealing system according to claim 6, characterized in that: The temperature-sensitive sustained-release microcapsules begin to depolymerize and release amino acid decarboxylase at 60°C.
8. The method for preparing an environmentally friendly CO2 enhanced storage and sealing system according to claim 1, characterized in that: The raw materials are composed of: 35% inorganic silicate containing metasilicate, 18% acidic amino acid containing a carboxyl group at each end of the molecule, 0.2% anionic surfactant containing an aromatic ring, 2% inorganic nanomaterial containing silanol, 0.03% amino acid decarboxylase, and the balance is water.
9. Application of an environmentally friendly CO2 enhanced storage and sealing system prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The application is to mix an environmentally friendly CO2 enhanced storage and sealing system with a temperature-sensitive slow-release capsule and inject it into the oil reservoir, and then continue to inject carbon dioxide after shutting down the well for 3 to 5 days.