Composite collecting agent and preparation method and application thereof

Through the preparation method of the composite collector, the synergistic effect of thiocarbamate and mercaptobenzothiazole derivatives is utilized to destroy the Zn-S shielding layer, improve the silver recovery rate, solve the problems of low fine silver recovery rate and environmental pollution, and achieve efficient and low-cost silver recovery.

CN120733884APending Publication Date: 2025-10-03CHINA UNIV OF MINING & TECH (BEIJING)
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202510984346.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-17
Publication Date
2025-10-03

AI Technical Summary

Technical Problem

Existing technologies make it difficult to effectively recover fine silver particles with a particle size of less than 10μm. Traditional collectors have poor selectivity and are unstable under alkaline conditions, resulting in a silver recovery rate of less than 60% and environmental pollution problems.

Method used

A composite collector, including a main agent, an auxiliary agent and a synergist, is used. By compounding thiocarbamate and mercaptobenzothiazole derivatives in a specific ratio, the Zn-S shielding layer is destroyed, the silver recovery rate is enhanced, the foam stability is improved, and the selectivity is increased.

Benefits of technology

The silver recovery rate was significantly increased to over 84%, the dosage of reagents was reduced, environmental pollution was reduced, flotation efficiency was improved, and costs were reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120733884A_ABST
    Figure CN120733884A_ABST
Patent Text Reader

Abstract

The invention discloses a composite collecting agent and a preparation method and application thereof, and relates to the technical field of solid waste recycling. The composite collecting agent comprises a main agent, an auxiliary agent and a synergist, and the mass ratio of the main agent to the auxiliary agent is (3-1): (1-2). The mass of the synergist is 0.1%-2.5% of the total mass of the composite collecting agent; the structural formula of the main agent is as shown in formula (I): R-O-C (= S)-NH-R '(I); in the formula (I), R is alkyl, and R'is 3-chloro-1, 2-epoxypropane; the auxiliary agent is a mercaptobenzothiazole derivative. The thiocarbamate and the mercaptobenzothiazole derivative are compounded according to a specific proportion for the first time, a Zn-S shielding layer is destroyed through an intermolecular synergistic effect, and the silver recovery rate is increased; the preparation method is simple and easy to operate, facilitates reduction of the dosage of a single agent and reduces environmental pollution. The foam stability is improved, the flotation efficiency is improved, the selective collection efficiency of the silver-zinc ore is remarkably improved, and the flotation index is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid waste resource utilization, and in particular to a composite collector and a preparation method and application thereof. Background Art

[0002] During the non-ferrous metal smelting process, zinc slag, as a byproduct, contains a variety of valuable metals. Silver, among them, is a key precious metal resource with significant economic value. Traditional silver recovery methods include pyrometallurgical and hydrometallurgical processes, but these methods often suffer from high energy consumption and severe environmental pollution.

[0003] Flotation is an important mineral separation technology and is widely used in the field of non-ferrous metal recovery. Currently, the thiosulfate and xanthate collectors commonly used in industry mainly achieve mineral flotation by forming coordination bonds between sulfur atoms and metal ions. These traditional collectors have good recovery effects on silver minerals of conventional particle size, but when processing fine silver particles with a particle size of less than 10μm, they are unable to effectively destroy [Ag] in zinc slag due to their molecular size and activity limitations. + -Zn 2+ ]The Zn-S bonding layer of the solid solution results in a silver recovery rate generally less than 60%.

[0004] While mercaptobenzothiazole collectors exhibit a certain degree of selectivity for silver and can form stable complexes with silver ions, their applicability is strictly limited by the pH of the solution. Under alkaline conditions, these collectors undergo hydrolysis and become ineffective. Conventional flotation processes typically require an alkaline environment, which severely limits their application in industrial practice. Furthermore, factors such as the ionic composition and temperature of the slurry during flotation can also affect the stability of these collectors.

[0005] Under current technological conditions, the efficient recovery of fine-particle silver from zinc smelting solid solution slag still faces significant challenges. This requires overcoming the poor selectivity of conventional collectors for fine-particle silver, while also addressing the stability of specific collectors under conventional process conditions.

[0006] In view of this, the present invention is proposed. Summary of the Invention

[0007] The purpose of the present invention is to provide a composite collector and its preparation method and application to solve the above technical problems.

[0008] The present invention is achieved in that: In a first aspect, an embodiment of the present invention provides a composite collector, comprising a main agent, an auxiliary agent, and a synergist; wherein the mass ratio of the main agent to the auxiliary agent is (3-1):(1-2); the mass of the synergist is 0.1%-2.5% of the total mass of the composite collector; The structural formula of the main agent is shown in formula (I): ROC(=S)-NH-R' (I); in formula (I), R is an alkyl group, and R' is a 3-chloro-1,2-epoxypropylene group; The auxiliary agent is a mercaptobenzothiazole derivative.

[0009] In a second aspect, an embodiment of the present invention provides a method for preparing the composite collector as described above, comprising the following steps: The main agent, auxiliary agent and synergist are reacted in alcohol solution in proportion to prepare a composite collector; wherein the reaction temperature is 45°C-55°C and the reaction time is 1.5h-3h.

[0010] In a third aspect, an embodiment of the present invention provides a use of the aforementioned composite collector or the composite collector prepared by the aforementioned preparation method in the flotation of silver-zinc ore.

[0011] The present invention has the following beneficial effects: The composite collector provided by the embodiments of the present invention, as well as its preparation method and application, is the first to compound thiocarbamate and mercaptobenzothiazole derivatives in a specific ratio, thereby destroying the Zn-S shielding layer through the intermolecular synergistic effect and improving the silver recovery rate. The preparation method is simple and easy to operate, which helps to reduce the dosage of a single reagent and reduce environmental pollution. It improves foam stability, increases flotation efficiency, significantly enhances the selective collection efficiency of silver-zinc ore, and improves flotation indicators. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without paying any creative work.

[0013] Figure 1 This is a schematic diagram of the flotation process of silver-zinc ore. DETAILED DESCRIPTION

[0014] To make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, all are conventional products that can be purchased commercially.

[0015] In a first aspect, an embodiment of the present invention provides a composite collector, comprising a main agent, an auxiliary agent, and a synergist; wherein the mass ratio of the main agent to the auxiliary agent is (3-1):(1-2); the mass of the synergist is 0.1%-2.5% of the total mass of the composite collector; The structural formula of the main agent is shown in formula (I): ROC(=S)-NH-R' (I); in formula (I), R is an alkyl group, and R' is a 3-chloro-1,2-epoxypropylene group; The auxiliary agent is a mercaptobenzothiazole derivative.

[0016] It should be noted that the Zn-S bonded shielding layer on the surface of silver-zinc ore is a key obstacle to capture. The composite collector used in the embodiments of the present invention has the following characteristics: it synergistically destroys the Zn-S shielding layer, enhancing silver capture; improves selectivity and reduces gangue inclusions; reduces the dosage of a single reagent, reducing environmental pollution; and improves flotation stability and enhances flotation efficiency.

[0017] The main agent has the structural formula of ROC(=S)-NH-R', which belongs to thiocarbamate. The main agent thiocarbamate is biodegradable, and the auxiliary agent mercaptobenzothiazole derivative has low toxicity, which can reduce the impact of the agent residue on eutrophication of water bodies. The synergist is through the complexation of Zn 2+ Inhibit its Ag + Competitive interference with adsorption. The researchers behind this invention, for the first time, compounded the main agent, auxiliary agent, and synergist in a specific ratio, significantly improving the selective capture efficiency of silver-zinc ore, improving flotation indicators (such as recovery rate and grade), and reducing reagent costs and environmental impact; the silver recovery rate is >84%.

[0018] Specifically, the -SH in the auxiliary mercaptobenzothiazole derivatives and Zn 2+ Forming a stable complex, adsorbing on the ZnS surface through π-π stacking, preferentially occupying the Zn 2+ The coordination sites of the shielding layer are destroyed, exposing the wrapped Ag active sites; the -C(=S)-NH- group in the main agent thiocarbamate has a strong affinity for silver. + A stable bidentate chelate ring is formed to achieve direct capture of silver.

[0019] In an optional embodiment, the mass ratio of the main agent to the auxiliary agent can be selected from any one of 3:2, 3:1, 2:1, 2:2 and 1:2, or other values ​​within the range of (3-1): (1-2) according to actual needs.

[0020] In an optional embodiment, in the main agent, R is n-butyl and R' is 3-chloro-2-hydroxypropyl.

[0021] In an optional embodiment, the mercaptobenzothiazole derivative is at least one selected from 2-mercaptobenzothiazole, 4-mercaptobenzothiazole, 5-mercaptobenzothiazole and 2-mercapto-6-methylbenzothiazole.

[0022] Mercaptobenzothiazole derivatives are highly effective collectors in the flotation of silver-zinc ores. The sulfur atom in the mercapto group (-SH) has a lone pair of electrons, forming stable chelates with metal ions such as silver (Ag) and zinc (Zn). These chelates preferentially adsorb on the surface of silver-zinc ores, enhancing their hydrophobicity and making them more easily attached to bubbles for flotation enrichment. This enhances the capture of difficult-to-float silver-zinc ores. They also accelerate the mineral-bubble bonding process, shortening flotation time and significantly improving production efficiency and metal recovery in silver-zinc concentrates. They are particularly effective for fine-grained ores with high oxidation rates. Furthermore, their low toxicity can reduce the impact of residual reagents on water eutrophication.

[0023] In the most preferred embodiment, the mercaptobenzothiazole derivative is 2-mercaptobenzothiazole.

[0024] In an optional embodiment, the synergist is selected from at least one of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) and methyl cellulose (MC).

[0025] It should be noted that the synergists in this embodiment are all environmentally friendly, low-cost, and readily available. In silver-zinc ore flotation, synergists improve flotation efficiency by adjusting mineral surface properties, improving solution dispersibility, or selectively inhibiting gangue minerals, thereby synergizing with collectors.

[0026] Among them, the PVP molecular chain contains polar pyrrolidone ring (-CO-N-) and methylene (-CH2-), and its core function is to regulate the surface properties of minerals through electrostatic adsorption and steric hindrance. Specifically, the pyrrole ring of PVP contains lone pairs of electrons, which can react with Ca on the surface of gangue. 2+ Mg 2+ or Si 4+ Formation of weak coordination bonds (such as PVP-Ca 2+ ), covering the active sites on the gangue surface, reducing the non-selective adsorption of the adjuvant on the gangue, thereby inhibiting the floating of the gangue; it can also combine with metal cations through electrostatic attraction to stabilize the adsorption layer of the adjuvant on the silver-zinc ore surface, enhance the hydrophobicity of the mineral, slow down the rising speed of bubbles, prolong the contact time between bubbles and minerals, and improve the capture probability.

[0027] The PVA molecular chain contains a large number of hydroxyl groups (-OH), which are mainly used for hydrogen bonding and surface modification. Silver-zinc ore often contains clay. The hydroxyl groups on the clay surface combine with the hydroxyl groups of PVA through hydrogen bonds to form a stable hydration film, which hinders the contact between clay particles and collectors and inhibits the adsorption of clay on collectors. In addition, the long-chain hydroxyl groups of PVA can form hydrogen bonds with water molecules in the hydration film on the surface of bubbles, delaying bubble rupture, prolonging the attachment time of bubbles and minerals, and improving the ability of foam to load minerals.

[0028] The MC molecular chain contains methoxy (-OCH3) and hydroxyl (-OH) groups, and its effects are characterized by steric hindrance and film-forming properties. The long chain structure of MC can be adsorbed on the surface of fine mud particles through a "bridging" effect, forming a steric hindrance layer, preventing fine mud from agglomerating and fully exposing the target minerals. It also enhances the stability of the hydrophobic film and regulates the rheological properties of the slurry, which facilitates synergistic enhancement of collectors and improves collection efficiency.

[0029] The mass of the synergist is 0.1%-1.5% of the total mass of the composite collector; it can be selected from any one of 0.1%, 0.3%, 0.4%, 0.5%, 0.7%, 0.9%, 1.0% and 1.5%, or other values ​​within the range of 0.1%-1.5%.

[0030] If too much synergist is used, the target mineral will be over-suppressed, resulting in a sharp drop in recovery rate. This will lead to a surge in reagent costs, reduced economic viability, and increased environmental and health risks. If too little is used, gangue suppression will fail, resulting in a drop in concentrate grade. Collector efficiency will also decrease, leading to a drop in recovery rate.

[0031] In a second aspect, an embodiment of the present invention provides a method for preparing the composite collector as described above, comprising the following steps: The main agent, auxiliary agent and synergist are reacted in alcohol solution in proportion to prepare a composite collector; wherein the reaction temperature is 45°C-55°C and the reaction time is 1.5h-3h.

[0032] It should be noted that the preparation process of the composite collector of the present invention, while shortening the time and reducing energy consumption, balances the solvent loss or equipment requirements caused by the temperature increase, and reasonably selects the reaction temperature and time. It can be reasonably adjusted according to the actual amount of material to be processed. In order to make the reaction more complete, during the preparation process, the preparation system can be stirred or ultrasonically assisted.

[0033] The present invention does not impose any particular restrictions on the type of alcohol solution; ethanol, methanol, and the like may be selected based on actual needs. Specifically, in the embodiments of the present invention, an ethanol solution is used. Alcohols possess both polar and non-polar groups (such as hydroxyl groups and alkyl groups) and can dissolve most organic compounds. They also possess strong solubility, mild reaction conditions, environmental compliance, and biodegradability.

[0034] The preparation of the composite collector is carried out in an inert atmosphere, which can be nitrogen, argon, helium, or the like, as desired. Specifically, in embodiments of the present invention, nitrogen is used as the inert gas. Preparing the composite collector in an inert atmosphere helps isolate reactive gases such as oxygen and water vapor, inhibits side reactions such as oxidation and hydrolysis, and ensures the chemical integrity and thermodynamic stability of the product. This also helps improve preparation yield and purity, reduces reagent waste, and lowers industrial application costs.

[0035] In an optional embodiment, the main agent is prepared by the following steps: An intermediate is prepared by mixing an alkylamine and carbon disulfide in a molar ratio of 1:(1.0-1.2) and reacting them at a temperature of 35°C-45°C for 1.5h-3h. The intermediate is mixed with epichlorohydrin at a molar ratio of 1:(1.0-5.42), and refluxed at 55-65°C for 3-5 hours to obtain the main agent.

[0036] It should be noted that the molar ratio setting is related to the structural formula of the materials. Selecting an appropriate excess of one of the substances can shift the equilibrium toward the product, thereby increasing the conversion rate and yield of the target product. This ensures sufficient reaction in the reaction system and the rational utilization of materials without waste. The specific reaction temperature and time can be adjusted appropriately based on the actual material quantities.

[0037] The main agent prepared is thiocarbamate.

[0038] In a third aspect, an embodiment of the present invention provides a use of the aforementioned composite collector or the composite collector prepared by the aforementioned preparation method in the flotation of silver-zinc ore.

[0039] In an optional embodiment, the flotation of silver-zinc ore includes: adopting a "two coarsening, three fine, two sweeping" flotation operation process; during which 100g / t-300g / t of a composite collector and 20g / t-40g / t of a frother are added, and the pH of the system is controlled at 6.3-6.7.

[0040] The flotation process of "two roughing, three cleaning and two scavenging" belongs to a type of cascade flotation. In the embodiment of the present invention, it specifically refers to two roughing, three cleaning and two scavenging. Figure 1 Schematic diagram of the silver-zinc ore flotation operation process.

[0041] It should be noted that in addition to the composite collector, other reagents such as sulfuric acid, hydrochloric acid, pine oil, and sodium sulfide are added to the "two coarsening, three fine, two sweeping" flotation process. These reagents, in synergy with the composite collector, can significantly improve flotation selectivity, recovery, and concentrate grade. Sulfuric acid can precisely adjust pH, control mineral surface electrical properties and collector dissociation, and inhibit gangue interference; hydrochloric acid removes surface oxides; pine oil facilitates the generation of stable foam, improving the flotation efficiency of target minerals and ensuring separation accuracy; and sodium sulfide can be used to activate difficult-to-float oxidized ores or suppressed minerals, expanding the flotation range and reducing collector consumption.

[0042] The phased addition of composite collectors facilitates "demand-based allocation and precise control." Through the synergistic effects of the collector components at each stage, the entire flotation process is efficiently operated, characterized by efficient recovery, precise enrichment, and low costs. In the roughing stage, composite collectors can rapidly adsorb target minerals, avoiding excessive reagent waste and reducing costs. In the cleaning stage, composite collectors enhance selective adsorption. In the scavenging stage, useful minerals not captured in the roughing stage (such as fine-grained and suppressed minerals) are recovered, reducing metal loss.

[0043] The dosage of the composite collector and the foaming agent can be reasonably adjusted according to the actual amount of mineral processed. The dosage of the composite collector can be any one of 100g / t, 150g / t, 180g / t, 200g / t, 280g / t and 300g / t, or other values ​​within the range of 100g / t-300g / t; the dosage of the foaming agent can be any one of 20g / t, 25g / t, 30g / t, 35g / t, 38g / t and 40g / t, or other values ​​within the range of 20g / t-40g / t.

[0044] The present invention does not particularly limit the type of the foaming agent, and the foaming agent may be selected from pine oil, eucalyptus oil, diethylhexanol, polypropylene alcohol or methyl isobutyl carbinol (MIBC) according to actual needs.

[0045] The pH of the system is controlled by adding Na2CO3-NaOH buffer solution to the system. The raw materials of the buffer solution are all inorganic compounds and are non-biotoxic. If excessive discharge occurs, the environmental impact can be reduced by natural neutralization (such as reaction with acidic substances in the soil) or simple treatment (such as dilution). Its buffering effect mainly depends on CO3 2- , can avoid greenhouse gas emissions; in addition, the cost of the raw materials of the buffer solution is low and the industrial applicability is strong. In other embodiments of the present invention, reasonable replacements can be made according to actual needs.

[0046] In an optional embodiment, the aeration volume in the roughing stage is 0.8m 3 / (m 2·min)-1.2m 3 / (m 2 ·min), the roughing time is 6min-10min, and the total flotation operation time is ≤15min.

[0047] It should be noted that the amount of aeration during the roughing stage is a key parameter affecting bubble generation and contact between minerals and bubbles. The rising bubbles drive the slurry into a circulating flow, promoting the diffusion and adsorption of the collector on the mineral surface. This also ensures that the surface activity of the frother is evenly distributed, stabilizing the foam layer.

[0048] Too much or too little aeration can cause reagents to be carried away before they can fully function (the slurry flow rate is too fast when the aeration volume is too high) or to be locally over-concentrated (the slurry stagnates when the aeration volume is too low), both of which reduce reagent utilization efficiency and increase reagent consumption. Specifically, if the aeration volume is insufficient, the bubbles generated are small and large, resulting in a limited number of mineral particles that can adhere to the bubble surface. A large amount of useful minerals cannot contact the bubbles in time and are lost with the tailings (reduced recovery rate). If the aeration volume is too large, the bubbles are too numerous but too small, and they tend to aggregate into large bubbles and burst quickly. At the same time, the stability of the foam layer decreases (the bubbles merge and burst frequently), and useful minerals may fall off the surface of the burst bubbles, resulting in "secondary losses." In addition, excessive bubbles dilute the slurry concentration, reducing the effective collision frequency between mineral particles and bubbles.

[0049] Controlling the roughing time is beneficial to controlling the recovery integrity of useful minerals. Too short will lead to "tail running", too long will lead to "grade reduction". It is necessary to balance the recovery rate and concentrate quality.

[0050] Controlling the total flotation time is beneficial to coordinating the rhythm of the entire process and needs to match the ore properties (multi-metal separation, differences in mineral flotation speeds) and economic goals.

[0051] Silver-zinc ore flotation also includes: raw material pretreatment; ball milling the silver-zinc slag to D90 = 30μm-45μm; after the pH reaches 1.0-2.0, acid leaching is performed, and the liquid-solid ratio in the acid leaching treatment is controlled to (3-5):1.

[0052] It should be noted that, in the embodiment of the present invention, microwave-assisted activation pretreatment of the raw materials is used in the raw material pretreatment stage to improve the flotation efficiency.

[0053] The raw material pretreatment adopts stage grinding, which can effectively avoid energy waste caused by over-grinding, improve separation efficiency and product quality, and reduce the burden of subsequent operations.

[0054] During the raw material pretreatment, water glass and citric acid are used as composite inhibitors, which have the characteristics of synergistically inhibiting gangue minerals, improving selectivity; improving slurry properties, optimizing the sorting environment; reducing the amount of reagents used, and saving costs.

[0055] The features and performance of the present invention are further described in detail below with reference to the embodiments.

[0056] Example 1 This embodiment provides a composite collector, the preparation method of which includes the following steps: (1) Under nitrogen protection, n-butylamine and carbon disulfide were reacted at a molar ratio of 1:1.2 at 40°C for 2 h to generate the intermediate NH2-CS-SH; (2) The intermediate was mixed with epichlorohydrin at a molar ratio of 1:1.05 and refluxed at 60°C for 4 h to obtain a crude thiocarbamate product, i.e., the main agent; (3) The crude thiocarbamate product and 2-mercaptobenzothiazole in a mass ratio of 2:1 and a synergist (PVP) accounting for 0.5% of the total mass of the composite collector were mixed in an ethanol solution, stirred at 50°C for 2 h, and distilled under reduced pressure to obtain an orange-red oily complex, i.e., the composite collector, with a yield of 89.3%.

[0057] This embodiment also provides a test of using a composite collector in a silver-zinc ore flotation process (for specific flotation process, see Figure 1 ), the relevant data are as follows: (1) Raw material pretreatment: A smelting slag containing 195.6 g / t silver and 22.8% zinc was ground to D90 = 38 μm and leached with hydrochloric acid (pH = 1.5) to remove surface oxides. The liquid-to-solid ratio in the acid leaching treatment was 4:1.

[0058] It should be noted that, in this stage, microwave-assisted activation treatment was used to activate the raw materials, wherein the microwave treatment power was 800 W and the time was 4 min.

[0059] (2) Flotation operation process: adopt the flotation operation process of "two roughing, three fine and two sweeping".

[0060] Dosage of reagents: composite collector 200g / t, foaming agent MIBC 30g / t, wherein, the stages of adding composite collector are: roughing I 150g / t, scavenging I 20g / t, scavenging II 30g / t.

[0061] pH control: Na2CO3-NaOH buffer system was used to maintain pH=6.3-6.7; Flotation time: The air volume in the roughing stage is 0.8m 3 / (m 2 ·min), roughing time is 8min, cleaning time is 3 times, and the total flotation operation time is 13min. The final concentrate had a silver grade of 4120 g / t, a recovery rate of 89.7%, and the tailings contained only 0.8% zinc.

[0062] Example 2 This embodiment provides a composite collector, the preparation method of which differs from that of Example 1 only in that: In the preparation method of the composite collector, (3) the crude thiocarbamate product and 2-mercaptobenzothiazole in a mass ratio of 2:1 and PVP accounting for 1.5% of the total mass of the composite collector are mixed in an ethanol solution, stirred at 60°C for 2h, and the composite collector is obtained after reduced pressure distillation (the yield is 98.68%).

[0063] This embodiment also provides a test of using a composite collector in a silver-zinc ore flotation process (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: The final concentrate silver grade was 3859 g / t, with a recovery rate of 80.26%, and the tailings contained only 1.26% zinc.

[0064] Example 3 This embodiment provides a composite collector, which differs from Example 1 only in that: The composite collector was used in the experiment of silver-zinc ore flotation process. (2) Flotation process: the flotation process of "one coarse, three fine and two sweep" was adopted.

[0065] Dosage of reagents: composite collector 200g / t, foaming agent MIBC 30g / t, wherein, the stages of adding composite collector are: roughing I 150g / t, scavenging I 20g / t, scavenging II 30g / t.

[0066] The final concentrate silver grade is 4026 g / t, the recovery rate is 87.79%, and the tailings contain only 1.02% zinc.

[0067] Example 4 This embodiment provides a composite collector, the preparation method of which differs from that of Example 1 only in that: In the preparation method of the composite collector, (1) under nitrogen protection, n-butylamine and carbon disulfide (molar ratio 1:1.15) are reacted at 35°C for 2.5h to generate the intermediate NH2-CS-SH; This embodiment also provides a test of using a composite collector in a silver-zinc ore flotation process (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: The final concentrate silver grade is 4003 g / t, with a recovery rate of 86.59%, and the tailings contain only 1.15% zinc.

[0068] Example 5 This embodiment provides a composite collector, the preparation method of which differs from that of Example 1 only in that: In the preparation method of the composite collector, (2) the intermediate and epichlorohydrin (molar ratio 1:3.59) are refluxed at 60°C for 3.5h to obtain a crude thiocarbamate product, i.e., the main agent; This embodiment also provides a test of using a composite collector in a silver-zinc ore flotation process (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: The final concentrate silver grade was 4102 g / t, with a recovery rate of 88.89%, and the tailings contained only 0.92% zinc.

[0069] Example 6 This embodiment provides a composite collector, the preparation method of which differs from that of Example 1 only in that: In the preparation method of the composite collector, (2) the intermediate and epichlorohydrin (molar ratio 1:4.03) are refluxed at 65°C for 4 h to obtain a crude thiocarbamate product, i.e., the main agent; This embodiment also provides a test of using a composite collector in a silver-zinc ore flotation process (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: The final concentrate silver grade was 3968 g / t, with a recovery rate of 85.69%, and the tailings contained only 1.01% zinc.

[0070] Example 7 This embodiment provides a composite collector, the preparation method of which differs from that of Example 1 only in that: In the preparation method of the composite collector, (2) the intermediate and epichlorohydrin (molar ratio 1:5.42) are refluxed at 60°C for 5 h to obtain a crude thiocarbamate product, i.e., the main agent; This embodiment also provides a test of using a composite collector in a silver-zinc ore flotation process (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: The final concentrate silver grade is 3959 g / t, the recovery rate is 84.60%, and the tailings contain only 1.18% zinc.

[0071] Comparative Example 1 This comparative example provides a test of using a composite collector in the flotation process of silver-zinc ore (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: (2) Flotation operation process: The collector used is butyl xanthate, and the dosage is 300g / t.

[0072] The final concentrate silver grade was 3791 g / t, the concentrate silver recovery rate was only 72.3%, and the concentrate contained as much as 5.5% zinc.

[0073] Comparative Example 2 This comparative example provides a test of using a composite collector in the flotation process of silver-zinc ore (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: (2) Flotation operation process: The collector used is butyl xanthate + black medicine, and the dosage is 400g / t.

[0074] The final concentrate silver grade was 3799 g / t, the concentrate silver recovery rate was only 75.68%, and the concentrate contained as much as 5.1% zinc.

[0075] Comparative Example 3 This comparative example provides a test of using a composite collector in the flotation process of silver-zinc ore (for specific flotation process, see Figure 1 ), the differences between the relevant data and Example 1 are as follows: (2) Flotation operation process: The collector used is black medicine, and the dosage is 350g / t.

[0076] The final concentrate silver grade was 3669 g / t, the concentrate silver recovery rate was only 70.23%, and the concentrate contained as much as 5.9% zinc.

[0077] In summary, the present invention is the first to compound thiocarbamate and mercaptobenzothiazole derivatives in a specific ratio. The benzothiazole ring of the mercaptobenzothiazole derivative is adsorbed on the ZnS surface through π-π stacking, exposing the wrapped Ag sites; the -CS-NH- group of the thiocarbamate and the Ag + A bidentate chelate ring is formed to achieve direct capture of silver; through the intermolecular synergistic effect, the selective capture efficiency of silver-zinc ore can be significantly improved, flotation indicators (such as recovery rate and grade) can be improved, and the reagent cost and environmental load can be reduced; among them, the silver recovery rate is >84%.

[0078] The foregoing description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Those skilled in the art will readily appreciate that various modifications and variations of the present invention are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present invention are intended to be within the scope of protection of the present invention.

Claims

1. A composite collector, characterized in that: The composite collector comprises a main agent, an auxiliary agent and a synergist; wherein the mass ratio of the main agent to the auxiliary agent is (3-1): (1-2); the mass of the synergist is 0.1%-2.5% of the total mass of the composite collector; The structural formula of the main agent is shown in formula (I): ROC(=S)-NH-R' (I); in formula (I), R is an alkyl group, and R' is a 3-chloro-1,2-epoxypropylene group; The auxiliary agent is a mercaptobenzothiazole derivative.

2. The composite collector according to claim 1, characterized in that In the main agent, R is n-butyl; R' is 3-chloro-2-hydroxypropyl.

3. The composite collector according to claim 1, characterized in that The mercaptobenzothiazole derivative is at least one selected from 2-mercaptobenzothiazole, 4-mercaptobenzothiazole, 5-mercaptobenzothiazole and 2-mercapto-6-methylbenzothiazole.

4. The composite collector according to claim 1, characterized in that The synergist is selected from at least one of polyvinyl pyrrolidone, polyvinyl alcohol and methyl cellulose.

5. A method for preparing a composite collector according to any one of claims 1 to 4, characterized in that: The steps include: The main agent, auxiliary agent and synergist are reacted in alcohol solution in proportion to prepare a composite collector; wherein the reaction temperature is 45°C-55°C and the reaction time is 1.5h-3h.

6. The preparation method according to claim 5, characterized in that The main agent is prepared by the following steps: An intermediate is prepared by mixing an alkylamine and carbon disulfide in a molar ratio of 1:(1.0-1.2) and reacting them at a temperature of 35°C-45°C for 1.5h-3h. The intermediate is mixed with epichlorohydrin at a molar ratio of 1:(1.0-5.42), and the mixture is refluxed at a temperature of 55° C.-65° C. for 3 h-5 h to obtain the main agent.

7. Use of the composite collector according to any one of claims 1 to 4 or the composite collector prepared by the preparation method according to any one of claims 5 to 6 in the flotation of silver-zinc ore.

8. The use according to claim 7, characterized in that The silver-zinc ore flotation comprises: The flotation process of "two coarsening, three refining and two sweeping" is adopted; during the process, 100g / t-300g / t of composite collector and 20g / t-40g / t of frother are added, and the pH of the system is controlled at 6.3-6.

7.

9. The use according to claim 8, characterized in that The aeration volume in the roughing stage is 0.8m 3 / (m 2 ·min)-1.2m 3 / (m 2 ·min), the roughing time is 6min-10min, and the total flotation operation time is ≤15min.

10. The use according to claim 7, characterized in that The silver-zinc ore flotation further includes: raw material pretreatment; ball milling the silver-zinc slag to a D90 of 30 μm-45 μm; after the pH value reaches 1.0-2.0, acid leaching is performed, and the liquid-solid ratio in the acid leaching is controlled to be (3-5):1.

Citation Information

Cited By

  • Method for recovering tungsten from tungsten ore tailings

    CN121178314A

  • A method for recovering tungsten from tungsten mine tailings

    CN121178314B