Lithium manganese iron phosphate positive electrode material and preparation method thereof
By coating the surface of the lithium manganese iron phosphate positive electrode material with an aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound and a NiOx buffer layer, the problems of poor conductivity and cycle stability of the lithium manganese iron phosphate positive electrode material are solved, achieving higher structural stability and improved battery performance.
Patent Information
- Application Number
- CN202511245218.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-02
- Publication Date
- 2025-10-03
- Estimated Expiration
- 2045-09-02
AI Technical Summary
Lithium manganese iron phosphate positive electrode material has poor conductivity and easily undergoes side reactions with the electrolyte, resulting in poor cycle stability, and manganese ions are easily dissolved, affecting the stability of the electrolyte.
An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is coated on the surface of lithium manganese iron phosphate particles as a coating layer, and a NiOx buffer layer is added in between to form dynamic interface protection, provide lithium ion and electron transmission channels, and reduce side reactions.
The structural stability and conductivity of the lithium manganese iron phosphate positive electrode material are improved, the cycle stability and high-rate performance are enhanced, and manganese dissolution and electrolyte corrosion are reduced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a lithium manganese iron phosphate positive electrode material and a preparation method thereof. Background Art
[0002] With the popularization of new energy vehicles around the world, the demand for power batteries is also continuing to grow. With the growth of public demand and the continuous iteration of technology, it is particularly urgent to develop a lithium-ion battery with high energy density, low cost, environmental friendliness, safety and stability.
[0003] As a crucial component of lithium-ion batteries, cathode materials are key to improving their performance. They not only determine the battery's energy density but also influence its cycle stability, safety, and cost. Common cathode materials currently include olivine-type lithium iron phosphate, layered lithium cobalt oxide, and lithium nickel oxide.
[0004] As a new type of lithium battery cathode material, lithium iron phosphate has higher energy density and low-temperature discharge capability than lithium iron phosphate cathode materials, and its safety performance is also relatively stable. However, lithium iron phosphate cathode materials have poor conductivity and poor cycle stability. The main reason is that during the charge and discharge cycle, the trivalent manganese ions in the lithium iron phosphate cathode material easily induce the Jahn-Teller effect, resulting in a distorted crystal structure. In addition, the trivalent manganese ions are prone to disproportionation reactions at high temperatures or high-rate cycling conditions to generate divalent manganese ions and tetravalent manganese ions. The divalent manganese ions easily dissolve in the electrolyte to form MnF2, while the tetravalent manganese ions may undergo redox reactions with substances in the electrolyte, thereby affecting the stability of the electrolyte.
[0005] In addition, since the voltage platform of the lithium iron manganese phosphate positive electrode material itself is close to the oxidation potential of the conventional electrolyte, it promotes the decomposition of the electrolyte. Moreover, the moisture and acidic substances in the electrolyte will corrode the lithium iron manganese phosphate positive electrode material, causing side reactions, thereby reducing the electrochemical activity of the lithium battery. Summary of the Invention
[0006] The purpose of the present invention is to provide a lithium manganese iron phosphate positive electrode material and a preparation method thereof, so as to solve the problem that the lithium manganese iron phosphate positive electrode material has poor conductivity and is prone to side reactions with the electrolyte.
[0007] The purpose of the present invention can be achieved through the following technical solutions: In a first aspect, the present invention provides a lithium iron manganese phosphate positive electrode material, which comprises at least lithium iron manganese phosphate particles and a coating layer coated on the outside of the lithium iron manganese phosphate particles; The raw materials of the coating layer include aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound.
[0008] Preferably, the weight of the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is 4-6 wt % of the lithium manganese iron phosphate particles.
[0009] Preferably, the molar ratio of lithium, manganese, iron and phosphorus in the lithium manganese iron phosphate particles is (0.95-1.05): (0.5-0.7): (0.3-0.5): 1.
[0010] Preferably, the lithium manganese iron phosphate particles are prepared by any one of a hydrothermal synthesis method, a sol-gel method, a co-precipitation method, and a high-temperature solid-phase method.
[0011] By adopting the above technical solution, a coating layer is coated on the outside of the lithium manganese iron phosphate particles, which can directly form a physical barrier, reduce the direct contact between the surface of the lithium manganese iron phosphate particles and the electrolyte, thereby reducing the reactivity of the lithium manganese iron phosphate positive electrode material and the electrolyte. In addition, the coating layer as a dense physical barrier can also reduce the possibility of manganese ions being dissolved due to oxidation or structural distortion, thereby improving the cycle stability of the positive electrode material.
[0012] The coating layer of the present invention adopts an aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound as a raw material, wherein the aluminum fluoride can serve as a chemical buffer between the electrolyte and the lithium iron manganese phosphate particles. Since the hydrofluoric acid generated by the hydrolysis of the electrolyte can corrode the lithium iron manganese phosphate positive electrode material, thereby causing the occurrence of side reactions, aggravating the dissolution of manganese and causing structural damage, the aluminum fluoride can preferentially react with the generated hydrofluoric acid to form a coordination compound, thereby reducing the direct corrosion of the hydrofluoric acid on the positive electrode material and significantly reducing the occurrence of side reactions between the lithium iron manganese phosphate positive electrode material and the electrolyte. At the same time, the aluminum fluoride can also enhance the overall structural stability of the positive electrode material by reducing oxygen vacancies on the surface of the lithium iron manganese phosphate particles and inhibiting the accumulation of structural stress.
[0013] However, directly coating the surface of the lithium iron manganese phosphate cathode material with aluminum fluoride is also problematic. Because aluminum fluoride is an insulator, its coating hinders the cross-interface transmission of electrons and lithium ions, resulting in a decrease in the high-rate performance of the cathode material. Furthermore, aluminum fluoride itself has no conductivity, and given the inherent poor conductivity of the lithium iron manganese phosphate material, direct coating with aluminum fluoride further restricts the electron transport path, accelerating polarization and capacity decay. Therefore, the present invention embeds aluminum fluoride in a polyethylene dioxythiophene-polystyrene sulfonate lithium compound.
[0014] Polyethylenedioxythiophene-polystyrene sulfonic acid is a highly conductive polymer whose three-dimensional network structure can provide a continuous electron transport path for the surface of lithium iron manganese phosphate particles, theoretically compensating for the insulating properties of aluminum fluoride. However, after aluminum fluoride was embedded in polyethylenedioxythiophene-polystyrene sulfonic acid, it was found that the sulfonic acid groups in polyethylenedioxythiophene-polystyrene sulfonic acid would form hydrogen bonds with the surface groups of aluminum fluoride, which not only affected the dispersibility of aluminum fluoride in polyethylenedioxythiophene-polystyrene sulfonic acid but also induced the hydrolysis of aluminum fluoride in polar water. Not only did it fail to provide a chemical buffering effect, it also produced new hydrofluoric acid, which corroded the lithium iron manganese phosphate cathode material. On the other hand, the strong polarity of the sulfonic acid group caused its protons to compete with lithium ions in the electrolyte for migration, significantly reducing the diffusion rate of lithium ions. As a result, the polyethylenedioxythiophene-polystyrene sulfonic acid, as a highly conductive polymer, combined with aluminum fluoride and coated on the surface of the lithium iron manganese phosphate cathode material had very limited improvement in electronic conductivity.
[0015] To address this problem, the present invention first performs a lithiation treatment on polyethylene dioxythiophene-polystyrene sulfonic acid, and then embeds aluminum fluoride. The hydrogen ions of the sulfonic acid groups in the polyethylene dioxythiophene-polystyrene sulfonic acid are replaced by lithium ions, which can directly eliminate the interference of protons on lithium ion transmission. In addition, the binding energy between lithium ions and sulfonic acid groups is higher than that between hydrogen ions, thereby forming a more stable ion transmission channel without affecting its conductive properties. Moreover, after the lithiation treatment, the pH value of the material can be regulated, and the hydrolysis reaction of aluminum fluoride can be inhibited. At the same time, the lithium ions can also form a passivation layer between the aluminum fluoride, blocking direct contact between aluminum fluoride and water, thereby reducing the occurrence of side reactions.
[0016] The finally obtained aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate compound is used as a coating layer raw material to coat the surface of lithium manganese iron phosphate particles, which can form dynamic interface protection, inhibit the dissolution of manganese and the corrosion of the electrolyte, polyethylene dioxythiophene-polystyrene sulfonate lithium provides an electron pathway, and aluminum fluoride optimizes the ion transmission selectivity. The formed coating layer can provide a more flexible transmission channel for lithium ions and electrons while physically blocking, thereby improving the structural stability of the obtained positive electrode material, enhancing the rate performance of the positive electrode material, and reducing the capacity attenuation rate.
[0017] Preferably, the raw materials of the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound include polystyrene sulfonate lithium, aluminum fluoride and 3,4-ethylene dioxythiophene in a molar ratio of 1: (0.8-1): (1.2-1.8).
[0018] Preferably, the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound is prepared according to the following method: S1. Dissolve polystyrene sulfonic acid in water to prepare a premix of 10 to 20% by mass; add a lithium salt to the premix, stir the reaction until no bubbles are generated, then add molecular sieves and let stand for 12 to 20 hours to obtain a lithium polystyrene sulfonate solution; S2. The aluminum fluoride is impregnated in a strong acid solution for 2 to 3 hours, then washed, neutralized, and dried to obtain pretreated aluminum fluoride; S3. Add pretreated aluminum fluoride to the lithium polystyrene sulfonate solution, ultrasonically disperse for 20 to 40 minutes, add 3,4-ethylenedioxythiophene, stir and disperse, then add the oxidant, continue stirring and react for 4 to 6 hours, and finally wash, spin dry and dry to obtain the product.
[0019] Preferably, the lithium salt includes a combination of one or more of lithium carbonate, lithium chloride, lithium nitrate and lithium sulfate; and the molar ratio of the lithium salt to the polystyrene sulfonic acid is (0.4-0.6):1.
[0020] Preferably, the strong acid solution includes any one of nitric acid, hydrochloric acid and sulfuric acid.
[0021] Preferably, the oxidant includes a combination of one or more of sodium persulfate, ammonium persulfate, ferric sulfate, ferric chloride and hydrogen peroxide; the added amount of the oxidant is 0.5 to 1% of the mass of 3,4-ethylenedioxythiophene.
[0022] By adopting the above technical solution, polystyrene sulfonic acid is first dissolved in water, and then a soluble lithium salt is added. At this time, an ion exchange reaction occurs between the lithium ions in the lithium salt and the polystyrene sulfonic acid, and the lithium ions are transferred to the polystyrene sulfonic acid. The formed lithium polystyrene sulfonate solution is mixed with the acidified aluminum fluoride. After the strong acid treatment, new polar groups such as carboxyl groups can be introduced on the surface of the aluminum fluoride, which can enhance the binding force between the aluminum fluoride and the lithium polystyrene sulfonate. A lithium polystyrene sulfonate adsorption layer is gradually formed on the surface of the aluminum fluoride. Then, 3,4-ethylenedioxythiophene monomer is added. Under the interaction of π-π attraction and van der Waals force, the monomer molecules are adsorbed on the surface of the aluminum fluoride. Then, under the action of an oxidant, the monomer molecules use the aluminum fluoride particles as a template and undergo in-situ oxidative polymerization on the surface to form a polyethylenedioxythiophene-polystyrene sulfonate lithium compound.
[0023] The prepared aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound can directly act as a physical barrier to inhibit manganese dissolution while reducing direct contact between internal lithium iron manganese phosphate particles and the electrolyte. It can also improve the ion transmission efficiency and electron transmission efficiency of the lithium iron manganese phosphate positive electrode material, improve the interface performance, optimize the binding force between aluminum fluoride and polyethylene dioxythiophene-polystyrene sulfonate, and solve the binding barrier between the two, thereby obtaining a lithium iron manganese phosphate positive electrode material with excellent performance.
[0024] Preferably, NiO is connected between the lithium manganese iron phosphate particles and the coating layer. x Buffer layer; the NiO x The buffer layer is made of NiO x Nanoparticle composition.
[0025] Preferably, NiO x The mass of the buffer layer is 2-4 wt% of the lithium manganese iron phosphate particles.
[0026] Preferably, NiO x The nanoparticles were prepared by dissolving a soluble nickel salt in water, adjusting the solution pH to 8-10, stirring and mixing for 30-60 minutes, and then washing by centrifugation, drying and calcining to obtain NiO x Nanoparticles; soluble nickel salts include one or more combinations of nickel sulfate hexahydrate, nickel chloride hexahydrate, nickel nitrate hexahydrate and nickel acetate tetrahydrate.
[0027] More preferably, NiO x The nanoparticles are nickel oxide vacancy nanoparticles; NiO x The nanoparticles are a mixture of NiO, NiOOH and Ni2O3. Due to the excess oxygen content, a large number of Ni vacancies exist, making NiO exist in a non-stoichiometric form.
[0028] By adopting the above technical solution, a layer of NiO is added between the lithium manganese iron phosphate particles and the coating layer formed by the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound. x Buffer layer. NiO x As a transition metal oxide, it can cooperate with the coating layer to inhibit the corrosion of the electrolyte on the positive electrode material and reduce the occurrence of interface side reactions. x NiO in the buffer layer x The porous structure of the nanoparticles can serve as a lithium ion pre-storage layer, shortening the diffusion distance of lithium ions from the electrolyte to the lithium iron manganese phosphate positive electrode material, thereby improving the rate performance and cycle performance of the obtained lithium iron manganese phosphate positive electrode material.
[0029] And NiO x The addition of the buffer layer can reduce the ability of the coating layer to induce oxygen vacancies and inhibit the increase of oxygen vacancy concentration during long-term charge and discharge cycles, thereby improving the structural stability. x The buffer layer can also form hydrogen bonds with the polar groups in the coating layer, thereby improving the adhesion of the coating layer to the surface of the lithium manganese iron phosphate particles, thereby improving the capacity retention rate and high-rate performance of the obtained lithium manganese iron phosphate positive electrode material.
[0030] In a second aspect, the present invention provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising the following process steps: An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is added to deionized water, stirred and dispersed, and then lithium manganese iron phosphate particles are added, soaked for 4 to 6 hours, and then heat-treated at 110 to 130° C. for 2 to 3 hours to form a coating layer to obtain a lithium manganese iron phosphate positive electrode material; Alternatively, NiO x The nanoparticles are dispersed in deionized water and then spin-coated on the surface of lithium manganese iron phosphate particles. They are heat-treated at 120-150°C for 30-40 minutes to form NiO x buffer layer to obtain pretreated lithium manganese iron phosphate particles.
[0031] An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is added to deionized water, stirred and dispersed, and then pretreated lithium manganese iron phosphate particles are added and soaked for 4 to 6 hours. Then, heat treatment is performed at 110 to 130° C. for 2 to 3 hours to form a coating layer to obtain a lithium manganese iron phosphate positive electrode material.
[0032] Preferably, the solid-liquid ratio of the aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound to deionized water is 1 g: (2-4) mL.
[0033] Preferably, the lithium manganese iron phosphate particles are not subjected to NiO x Nanoparticle pretreatment to form NiO x The buffer layer can also achieve the technical effects of this application.
[0034] By adopting the above technical solution, the soluble nickel salt is dissolved in water and then calcined to form NiO x Nanoparticles containing NiO x The solution of nanoparticles is spin-coated on the surface of lithium manganese iron phosphate particles and then heat-treated to form a stable NiO x The buffer layer is formed, and the obtained pretreated lithium manganese iron phosphate particles are then immersed in an aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound slurry to form a coating layer on the outermost layer to obtain a lithium manganese iron phosphate positive electrode material that can significantly inhibit manganese dissolution and electrolyte side reactions, and the positive electrode material also has good conductivity and cycle stability.
[0035] Beneficial effects of the present invention: 1. The surface of the lithium manganese iron phosphate positive electrode material of the present invention further comprises a coating layer, the raw materials of which include an aluminum fluoride-intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound. On the one hand, the coating layer can serve as a physical barrier, forming a dynamic interface protection, directly inhibiting the dissolution of manganese and the erosion of the electrolyte, and reducing the occurrence of side reactions between the electrolyte and the positive electrode material. On the other hand, the aluminum fluoride-intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound, after lithiation treatment and aluminum fluoride intercalation, can simultaneously provide a more flexible transmission channel for lithium ions and electrons, improving the lithium ion transmission efficiency while enhancing the conductivity of the positive electrode material, resulting in a lithium manganese iron phosphate positive electrode material with a stable structure, high rate performance, and cycle stability.
[0036] 2. The lithium manganese iron phosphate positive electrode material of the present invention further comprises a NiO layer between the lithium manganese iron phosphate particles and the coating layer. x The buffer layer can provide a path for lithium ion transmission, reduce the generation of oxygen vacancies, improve structural stability, and at the same time increase the bonding force between the lithium iron manganese phosphate particles and the coating layer, thereby improving the capacity retention rate of the lithium iron manganese phosphate positive electrode material. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present invention.
[0038] Preparation Example Preparation Example 1: An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound was prepared according to the following method: S1. Dissolve 50 mmol of polystyrene sulfonic acid in water to prepare a 15% mass fraction premix; add 25 mmol of lithium carbonate to the premix, stir until no bubbles are generated, then add silicon / aluminum molecular sieves and let stand for 12 to 20 hours to obtain a lithium polystyrene sulfonate solution; S2. 45 mmol of aluminum fluoride was impregnated with nitric acid for 2 h, then washed, neutralized, and dried to obtain pretreated aluminum fluoride; S3. Add pretreated aluminum fluoride to the lithium polystyrene sulfonate solution, ultrasonically disperse for 30 minutes, add 75 mmol of 3,4-ethylenedioxythiophene, stir and disperse, then add 0.1 g of ammonium persulfate, continue stirring and react for 5 hours, and finally wash, spin dry and dry to obtain the product.
[0039] Preparation Example 2: An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound was prepared according to the following method: S1. Dissolve 50 mmol of polystyrene sulfonic acid in water to prepare a 15% mass fraction premix; add 20 mmol of lithium carbonate to the premix, stir until no bubbles are generated, then add silicon / aluminum molecular sieves and let stand for 12 to 20 hours to obtain a lithium polystyrene sulfonate solution; S2. 40 mmol of aluminum fluoride was impregnated with nitric acid for 2 h, then washed, neutralized, and dried to obtain pretreated aluminum fluoride; S3. Add pretreated aluminum fluoride to the lithium polystyrene sulfonate solution, ultrasonically disperse for 30 minutes, add 60 mmol of 3,4-ethylenedioxythiophene, stir and disperse, then add 0.08 g of ammonium persulfate, continue stirring and react for 5 hours, and finally wash, spin dry and dry to obtain the product.
[0040] Preparation Example 3: An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound was prepared according to the following method: S1. Dissolve 50 mmol of polystyrene sulfonic acid in water to prepare a 15% mass fraction premix; add 30 mmol of lithium carbonate to the premix, stir until no bubbles are generated, then add silicon / aluminum molecular sieves and let stand for 12 to 20 hours to obtain a lithium polystyrene sulfonate solution; S2. 50 mmol of aluminum fluoride was impregnated with nitric acid for 2 h, then washed, neutralized, and dried to obtain pretreated aluminum fluoride; S3. Add pretreated aluminum fluoride to the lithium polystyrene sulfonate solution, ultrasonically disperse for 30 minutes, add 90 mmol of 3,4-ethylenedioxythiophene, stir and disperse, then add 0.1 g of ammonium persulfate, continue stirring and react for 5 hours, and finally wash, spin dry and dry to obtain the product.
[0041] Preparation Example 4, an aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound, is different from Preparation Example 1 only in that the amount of aluminum fluoride added is 30 mmol.
[0042] Preparation Example 5, an aluminum fluoride-embedded polyethylenedioxythiophene-polystyrenesulfonate lithium compound, is different from Preparation Example 1 only in that the amount of aluminum fluoride added is 60 mmol.
[0043] Preparation Example 6: An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonic acid compound was prepared according to the following method: S1. 45 mmol of aluminum fluoride was impregnated with nitric acid for 2 h, then washed, neutralized, and dried to obtain pretreated aluminum fluoride; S2. Dissolve 50 mmol of polystyrene sulfonic acid in water to prepare a premix with a mass fraction of 15%. Add pretreated aluminum fluoride to the premix and ultrasonically disperse for 30 minutes. Add 75 mmol of 3,4-ethylenedioxythiophene and stir to disperse. Then, add 0.1 g of ammonium persulfate and continue stirring for 5 hours. Finally, wash, spin dry, and dry to obtain the product.
[0044] Preparation Example 7: A polyethylenedioxythiophene-polystyrene sulfonate lithium compound was prepared according to the following method: S1. Dissolve 50 mmol of polystyrene sulfonic acid in water to prepare a 15% mass fraction premix; add 25 mmol of lithium carbonate to the premix, stir until no bubbles are generated, then add silicon / aluminum molecular sieves and let stand for 12 to 20 hours to obtain a lithium polystyrene sulfonate solution; S2. Add 75 mmol of 3,4-ethylenedioxythiophene to the lithium polystyrene sulfonate solution, stir and disperse, then add 0.1 g of ammonium persulfate, continue stirring and react for 5 hours, and finally wash, spin dry and dry to obtain the product.
[0045] Preparation Example 8: An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound was prepared according to the following method: S1. Dissolve 50 mmol of polystyrene sulfonic acid in water to prepare a 15% mass fraction premix; add 25 mmol of lithium carbonate to the premix, stir until no bubbles are generated, then add silicon / aluminum molecular sieves and let stand for 12 to 20 hours to obtain a lithium polystyrene sulfonate solution; S2. Add 45 mmol of aluminum fluoride to the lithium polystyrene sulfonate solution and disperse it ultrasonically for 30 minutes. Then add 75 mmol of 3,4-ethylenedioxythiophene and disperse it with stirring. Then add 0.1 g of ammonium persulfate and continue stirring and reacting for 5 hours. Finally, wash, spin dry, and dry to obtain the product.
[0046] Example Example 1: A lithium manganese iron phosphate cathode material is prepared according to the following method: The aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 was added to deionized water, wherein the solid-liquid ratio of the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound to deionized water was 1 g:3 mL; After stirring and dispersing, lithium iron manganese phosphate particles obtained by hydrothermal synthesis are added, wherein the molar ratio of lithium, manganese, iron and phosphorus in the lithium iron manganese phosphate particles is 1:0.7:0.3:1, and the mixture is soaked for 5 hours, and then heat-treated at 120°C for 2 hours to form a coating layer. The mass of the aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is controlled to be 5wt% of the lithium iron manganese phosphate particles to obtain a lithium iron manganese phosphate positive electrode material.
[0047] Example 2, a lithium iron manganese phosphate positive electrode material, which differs from Example 1 only in that the molar ratio of lithium, manganese, iron and phosphorus in the lithium iron manganese phosphate particles is 1.05:0.5:0.5:1; the mass of the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is controlled to be 4wt% of the lithium iron manganese phosphate particles.
[0048] Example 3, a lithium iron manganese phosphate positive electrode material, which differs from Example 1 only in that the molar ratio of lithium, manganese, iron and phosphorus in the lithium iron manganese phosphate particles is 0.95:0.6:0.4:1; the mass of the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is controlled to be 6wt% of the lithium iron manganese phosphate particles.
[0049] Example 4, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is replaced by an equal amount of the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 2.
[0050] Example 5, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is replaced by an equal amount of the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 3.
[0051] Example 6, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 4 is used to replace the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1.
[0052] Example 7, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is replaced by an equal amount of the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 5.
[0053] Example 8, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 8 is used to replace the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1.
[0054] Example 9, a lithium iron manganese phosphate positive electrode material, differs from Example 1 only in that the mass of the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is controlled to be 2wt% of the lithium iron manganese phosphate particles.
[0055] Example 10, a lithium iron manganese phosphate positive electrode material, differs from Example 1 only in that the mass of the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is controlled to 8wt% of the lithium iron manganese phosphate particles.
[0056] Example 11: A lithium manganese iron phosphate positive electrode material is prepared according to the following method: Nickel sulfate hexahydrate was dissolved in water, the pH value of the solution was adjusted to 8.5, and the mixture was stirred for 60 minutes. Then, NiO was obtained by centrifugal washing, drying and calcination. x Nanoparticles; The NiO obtained above x The nanoparticles were dispersed in deionized water and then spin-coated on the surface of lithium manganese iron phosphate particles, where the molar ratio of lithium, manganese, iron and phosphorus in the lithium manganese iron phosphate particles was 1:0.7:0.3:1, and heat-treated at 140°C for 40 minutes to form NiO x Buffer layer, control NiO x The mass of the buffer layer is 3 wt % of the lithium iron manganese phosphate particles, to obtain pretreated lithium iron manganese phosphate particles; The aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate compound prepared in Preparation Example 1 was added to deionized water, wherein the solid-liquid ratio of the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate compound to deionized water was 1 g:3 mL; after stirring and dispersing, the pretreated lithium manganese iron phosphate particles were added, infiltrated for 6 hours, and then heat treated at 120°C for 2 hours to form a coating layer, and the mass of the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate compound prepared in Preparation Example 1 was controlled to be 5wt% of the lithium manganese iron phosphate particles, to obtain a lithium manganese iron phosphate positive electrode material.
[0057] Example 12, a lithium manganese iron phosphate positive electrode material, which is different from Example 11 only in that the NiO x The mass of the buffer layer is 2 wt% of the lithium manganese iron phosphate particles.
[0058] Example 13, a lithium manganese iron phosphate positive electrode material, which is different from Example 11 only in that the NiO x The mass of the buffer layer is 4 wt% of the lithium manganese iron phosphate particles.
[0059] Comparative Example Comparative Example 1, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonic acid compound prepared in Preparation Example 6 is used to replace the aluminum fluoride intercalated polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1.
[0060] Comparative Example 2, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is replaced by an equal amount of the polyethylene dioxythiophene-polystyrene sulfonic acid compound prepared in Preparation Example 7.
[0061] Comparative Example 3, a lithium manganese iron phosphate positive electrode material, differs from Example 1 only in that the aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound prepared in Preparation Example 1 is replaced by an equal amount of aluminum fluoride.
[0062] Comparative Example 4: A lithium manganese iron phosphate positive electrode material was prepared according to the following method: Nickel sulfate hexahydrate was dissolved in water, the pH value of the solution was adjusted to 8.5, and the mixture was stirred for 60 minutes. Then, NiO was obtained by centrifugal washing, drying and calcination. x Nanoparticles; The NiO obtained above x The nanoparticles were dispersed in deionized water and then spin-coated on the surface of lithium manganese iron phosphate particles, where the molar ratio of lithium, manganese, iron and phosphorus in the lithium manganese iron phosphate particles was 1:0.7:0.3:1, and heat-treated at 140°C for 40 minutes to form NiO x Buffer layer, control NiO x The mass of the buffer layer is 3wt% of the lithium manganese iron phosphate particles, and a lithium manganese iron phosphate positive electrode material is obtained.
[0063] Performance testing According to the relevant records in GB / T 31467.3-2015 "Safety Requirements and Test Methods for Lithium-ion Power Battery Packs and Systems for Electric Vehicles", sample batteries were prepared using the lithium manganese iron phosphate positive electrode material obtained in the examples and comparative examples as the positive electrode material.
[0064] Then, the sample battery was tested at room temperature and 1C rate for the first discharge capacity and after 500 cycles, and the capacity retention rate was calculated. At the same time, the sample battery was tested at room temperature and 3C rate before and after 200 cycles, and the capacity retention rate was calculated.
[0065] The above experimental results are shown in Table 1: Table 1 Performance test results
[0066] Combining Example 1 and Example 8, it can be seen that the high rate performance and cycle performance of Example 8 are lower than those of Example 1. The reason is that during the preparation process of the aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound in Example 8, aluminum fluoride was not subjected to acidification treatment, resulting in a significant decrease in the polar group content on the surface of aluminum fluoride. In the process of compounding with polyethylene dioxythiophene-polystyrene sulfonate lithium, the interface bonding force is poor, aluminum fluoride is easy to agglomerate, and it is also easy to fall off during long-term circulation and enter the electrolyte, inducing side reactions, which is not conducive to improving the stability of the battery.
[0067] Combining Example 1 and Example 11, it can be seen that the various properties of Example 11 are improved compared with Example 1. The reason is that NiO is added to the lithium manganese iron phosphate positive electrode material obtained in Example 11. x The buffer layer can optimize the performance of the coating layer and provide a lithium ion transmission path, thereby improving the rate performance and cycle performance of the lithium manganese iron phosphate positive electrode material.
[0068] Combining Example 1 and Comparative Example 1, it can be seen that the high-rate performance and cycle performance of Comparative Example 1 are lower than those of Example 1. The reason is that the polyethylene dioxythiophene-polystyrene sulfonic acid in Comparative Example 1 has not been subjected to lithiation treatment, and the highly polar sulfonic acid groups contained therein will reduce the diffusion rate of lithium ions, affecting the performance of the embedded aluminum fluoride, and the improvement of the conductive performance is not obvious, resulting in a decrease in the performance of the lithium-ion battery.
[0069] Combining Example 1 and Comparative Example 2, it can be seen that the cycle performance of Comparative Example 2 is lower than that of Example 1. The reason is that the raw material of the coating layer in Comparative Example 2 is a polyethylene dioxythiophene-polystyrene sulfonate lithium compound, and there is no embedded aluminum fluoride. Its first discharge specific capacity does not change much, because the polyethylene dioxythiophene-polystyrene sulfonate lithium coating layer has a certain conductivity, which can make up for the poor conductivity of the lithium manganese iron phosphate positive electrode material. However, there is a lack of aluminum fluoride, that is, there is a lack of a chemical buffer between the positive electrode material and the electrolyte. The erosion of the electrolyte on the positive electrode material is enhanced compared to Example 1, resulting in a decrease in cycle performance and high-rate performance.
[0070] Combining Example 1, Comparative Example 3 and Comparative Example 4, it can be seen that the various properties of Comparative Example 3 and Comparative Example 4 are significantly reduced compared with Example 1. The reason is that the aluminum fluoride coating layer and NiO in Comparative Example 3 x The buffer layer has poor conductivity and limited effect on improving the structural stability of the material, resulting in a decrease in the performance of the resulting lithium-ion battery.
[0071] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.
[0072] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. A lithium manganese iron phosphate positive electrode material, characterized in that: The lithium iron manganese phosphate positive electrode material at least comprises lithium iron manganese phosphate particles and a coating layer coated on the lithium iron manganese phosphate particles; The raw material of the coating layer includes aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound.
2. The lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that The mass of the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is 4-6 wt % of the lithium manganese iron phosphate particles.
3. The lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that The raw materials of the aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound include polystyrene sulfonate lithium, aluminum fluoride and 3,4-ethylene dioxythiophene in a molar ratio of 1: (0.8-1): (1.2-1.8).
4. The lithium iron manganese phosphate positive electrode material according to claim 3, characterized in that The aluminum fluoride embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is prepared according to the following method: S1. Dissolve polystyrene sulfonic acid in a solvent to prepare a premix with a mass fraction of 10 to 20%; add a lithium salt to the premix, stir the reaction until no bubbles are generated, then add molecular sieves and let stand for 12 to 20 hours to obtain a lithium polystyrene sulfonate solution; S2. The aluminum fluoride is impregnated in a strong acid solution for 2 to 3 hours, then washed, neutralized, and dried to obtain pretreated aluminum fluoride; S3. Add pretreated aluminum fluoride to the lithium polystyrene sulfonate solution, ultrasonically disperse for 20 to 40 minutes, add 3,4-ethylenedioxythiophene, stir and disperse, then add the oxidant, continue stirring and react for 4 to 6 hours, and finally wash, spin dry and dry to obtain the product.
5. The lithium manganese iron phosphate positive electrode material according to claim 4, characterized in that The lithium salt includes a combination of one or more of lithium carbonate, lithium chloride, lithium nitrate and lithium sulfate; the molar ratio of the lithium salt to polystyrene sulfonic acid is (0.4-0.6):
1.
6. The lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that The molar ratio of lithium, manganese, iron and phosphorus in the lithium manganese iron phosphate particles is (0.95-1.05): (0.5-0.7): (0.3-0.5):
1.
7. The lithium manganese iron phosphate positive electrode material according to claim 1, characterized in that NiO is also connected between the lithium manganese iron phosphate particles and the coating layer. x Buffer layer; the NiO x The buffer layer is made of NiO x Nanoparticle composition.
8. The lithium iron manganese phosphate positive electrode material according to claim 7, characterized in that The NiO x The mass of the buffer layer is 2-4 wt% of the lithium manganese iron phosphate particles.
9. The lithium iron manganese phosphate positive electrode material according to claim 7, characterized in that The NiO x The nanoparticles were prepared according to the following method: Dissolve soluble nickel salt in water, adjust the solution pH to 8-10, stir and mix for 30-60 minutes, then centrifuge, wash, dry and calcine to obtain NiO x Nanoparticles; the soluble nickel salt includes a combination of one or more of nickel sulfate hexahydrate, nickel chloride hexahydrate, nickel nitrate hexahydrate and nickel acetate tetrahydrate.
10. A method for preparing a lithium manganese iron phosphate positive electrode material, characterized in that: The process steps include: The aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate compound is added to deionized water, stirred and dispersed, and then lithium manganese iron phosphate particles are added and soaked for 4 to 6 hours, and then heat-treated at 110 to 130° C. for 2 to 3 hours to form a coating layer to obtain the lithium manganese iron phosphate positive electrode material according to any one of claims 1 to 6; Alternatively, NiO x The nanoparticles are dispersed in deionized water and then spin-coated on the surface of lithium manganese iron phosphate particles. They are heat-treated at 120-150°C for 30-40 minutes to form NiO x buffer layer, obtaining pretreated lithium manganese iron phosphate particles; An aluminum fluoride-embedded polyethylene dioxythiophene-polystyrene sulfonate lithium compound is added to deionized water, stirred and dispersed, and then pretreated lithium manganese iron phosphate particles are added and soaked for 4 to 6 hours, and then heat-treated at 110 to 130° C. for 2 to 3 hours to form a coating layer to obtain the lithium manganese iron phosphate positive electrode material according to any one of claims 7 to 9.
Citation Information
Patent Citations
Composite lithium ion battery positive electrode material with high rate performance and preparation method of material
CN104218233A
Preparation method of aluminum fluoride coated lithium vanadium phosphate cathode material
CN109935809A
Positive pole piece, secondary battery and electric device
CN118843960A
Lithium manganese iron phosphate coated lithium manganate positive electrode material and preparation method thereof
CN118908285A
Metal fluoride coated lithium intercalation material and methods of making same and uses thereof
US20180233770A1
Cited By
Lithium ion battery coating diaphragm as well as preparation method and application thereof
CN121663109A
A negative electrode material, its preparation method, and a battery
CN122370372A