Adhesive containing epoxy-terminated polyurethane epoxy resin as well as preparation method and application of adhesive

Through the preparation method of epoxy-terminated polyurethane epoxy resin, flexible chain segments and thermally conductive fillers are introduced to solve the problems of high heat release and insufficient toughness of epoxy resin adhesives, achieving high strength, high toughness and stability, and suitable for aerospace, electronic appliances and other fields.

CN120795268APending Publication Date: 2025-10-17JIANGSU CHANGNENG ENERGY SAVING NEW MATERIALS SCI & TECH

Patent Information

Application Number
CN202511110588.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-08
Publication Date
2025-10-17

AI Technical Summary

Technical Problem

Traditional epoxy resin adhesives have problems such as thermal stress, material defects, and poor toughness caused by high exothermic peaks during the curing process, and NCO residues cause foaming problems. Existing improvement technologies have limited effects.

Method used

Epoxy-terminated polyurethane epoxy resin is used. By reacting polyurethane prepolymer with epoxy resin, small molecule epoxy compounds are added to eliminate NCO, flexible chain segments are introduced, and thermal conductive fillers are combined to reduce the crosslinking rate and heat accumulation, forming a flexible bridged rigid network.

Benefits of technology

Significantly reduce the exothermic peak, improve toughness and impact resistance, avoid foaming, maintain high strength and stability, and adapt to harsh scenarios such as aerospace, electronics and electrical appliances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005539752730000031
    Figure BDA0005539752730000031
  • Figure BDA0005539752730000051
    Figure BDA0005539752730000051
  • Figure BDA0005539752730000071
    Figure BDA0005539752730000071
Patent Text Reader

Abstract

The invention discloses an adhesive containing epoxy-terminated polyurethane epoxy resin as well as a preparation method and application of the adhesive. The adhesive comprises the following components in parts by weight: 10-15 parts of epoxy resin, 70-75 parts of epoxy-terminated polyurethane epoxy resin, 19-21 parts of an amine curing agent and 8-15 parts of heat-conducting filler, wherein the epoxy-terminated polyurethane epoxy resin is obtained by reacting a polyurethane prepolymer and epoxy resin, NCO of the polyurethane prepolymer and hydroxyl of the epoxy resin are subjected to an addition reaction, and after the reaction is finished, NCO of a system is eliminated by adopting a small-molecule epoxy compound; the polyurethane prepolymer is obtained by reaction of isocyanate and polyether polyol with flexible chain segments. According to the adhesive, the curing heat release peak value is reduced, the toughness is improved, meanwhile, the high strength is kept, the foaming problem is avoided, the defects that a traditional epoxy adhesive is high in heat release and poor in toughness are overcome, and the adhesive is suitable for the fields such as aerospace and electronic and electric appliances which have strict performance requirements.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of adhesives, in particular to an adhesive containing epoxy-terminated polyurethane epoxy resin and a preparation method and application thereof. BACKGROUND

[0002] Epoxy resin adhesives are widely used in aerospace, electronics, mechanical manufacturing and many other fields due to their high strength, good chemical stability and excellent bonding performance. However, traditional epoxy resin adhesives have two significant defects: first, a high exothermic peak value is generated during the curing process. Due to the rapid increase in crosslinking density when epoxy resin reacts with amine curing agent, a large amount of reaction heat accumulates in a short time, resulting in a sharp rise in local temperature (usually up to 120-150℃). The thermal stress generated during the curing process can cause cracks, pores and other defects in the material, and may also cause thermal damage to the bonded heat-sensitive materials (such as electronic components, polymer composites, etc.), affecting their performance and service life, thereby reducing the mechanical properties and durability of the materials. In addition, for large-size products, the rapid reaction exotherm can easily cause local temperature to be too high and the curing to be uneven, thereby affecting the quality consistency of the products; second, the molecular chain of epoxy resin itself is rigid and has high crosslinking density, resulting in poor toughness of the cured material, with an elongation at break usually less than 5%. When subjected to stress caused by impact, vibration or temperature change, the adhesive is prone to brittle fracture, leading to bonding failure.

[0003] To solve the above problems, the existing technology mainly uses the methods of adding toughening agents or changing the curing system. For example, although adding rubber elastomers, thermoplastic resins and other toughening agents can improve the toughness to some extent, it often leads to a decrease in strength and may cause phase separation problems, affecting the comprehensive performance of the adhesive; adjusting the type or ratio of the curing agent to reduce the exothermic peak value has limited effect and may prolong the curing time, reducing the production efficiency.

[0004] In addition, Patent CN 116285831 A (Application No: 202211513435.7) discloses a polyurethane-modified epoxy resin adhesive and a preparation method thereof. The EP-PU grafted IPNs structure is generated by the reaction of epoxy resin and polyurethane prepolymer, which improves the toughness and fatigue resistance of the adhesive, and improves the storage capacity and foaming problem in the construction process. However, the technology still has the following shortcomings: first, when the polyurethane prepolymer reacts with the epoxy resin, the NCO group may not be completely consumed, thereby forming potential reactive sites in the system, and the foaming problem cannot be fundamentally solved; second, although the technology optimizes the energy consumption by reducing the reaction temperature and shortening the reaction time, the control effect of the exothermic peak is limited, and the problem of local heat accumulation cannot be completely avoided; third, although the elongation at break is improved (more than 6.55%), further improvement is still needed for some high-toughness application scenarios.

[0005] Therefore, the exothermic peak of the epoxy resin adhesive needs to be reduced, the toughness needs to be improved, and the foaming problem caused by NCO residue needs to be solved. SUMMARY

[0006] The first object of the present application is to provide an epoxy-terminated polyurethane epoxy resin that eliminates NCO residue and has a slow crosslinking speed during reaction with an amine curing agent. The second object of the present application is to provide a preparation method of the epoxy-terminated polyurethane epoxy resin. The third object of the present application is to provide an adhesive containing the epoxy-terminated polyurethane epoxy resin that reduces the exothermic peak, improves the toughness, and avoids the foaming problem caused by NCO residue. The fourth object of the present application is to provide a preparation method of the adhesive. The fifth object of the present application is to provide an application of the adhesive.

[0007] The epoxy-terminated polyurethane epoxy resin of the present application is obtained by the reaction of a polyurethane prepolymer and an epoxy resin, wherein the NCO of the polyurethane prepolymer and the hydroxyl of the epoxy resin undergo an addition reaction, and a small molecule epoxy compound is used to eliminate the NCO of the system after the reaction. The polyurethane prepolymer is obtained by the reaction of isocyanate and chain segment flexible polyether polyol.

[0008] The NCO content of the polyurethane prepolymer is 5-6%. In the reaction of the polyurethane prepolymer and the epoxy resin, the amount of NCO added to the system is 2-3%.

[0009] In the epoxy-terminated polyurethane epoxy resin of the present application, the NCO of the polyurethane prepolymer only reacts with the hydroxyl group in the epoxy resin and does not react with the epoxy group, the integrity of all the epoxy groups of the epoxy resin is preserved, pure epoxy reserves are provided for the subsequent epoxy-termination reaction of glycidol, the side reaction of ring opening of the epoxy group (such as the formation of ether bond or tertiary amine) is avoided, and finally the structure of the resin is clearly controllable, the clear block structure of "polyurethane flexible chain" and "epoxy rigid end group" is realized, and the ideal topology of "flexible bridging rigid network" is formed after curing with the curing agent.

[0010] Preferably, the chain segment flexible polyether polyol is at least one of polypropylene oxide polyol (PPG), polytetramethylene oxide polyol (PTMEG) or polyethylene oxide-propylene oxide copolymer polyol.

[0011] The epoxy resin is at least one of bisphenol A type epoxy resin and bisphenol F type epoxy resin.

[0012] Preferably, the small molecule epoxy compound is glycidol.

[0013] Preferably, the isocyanate is toluene diisocyanate (TDI-80) or isophorone diisocyanate (IPDI).

[0014] The preparation method of the epoxy-terminated polyurethane epoxy resin of the present application comprises the following steps:

[0015] (1) The chain segment flexible polyether polyol is dehydrated, and then reacted with isocyanate at 70-80℃ under the protection of inert gas for 2-3 hours to obtain a polyurethane prepolymer;

[0016] (2) The epoxy resin is added to the polyurethane prepolymer and reacted at 60-70℃ for 2-3 hours; the small molecule epoxy compound is added dropwise, and the organic tin catalyst is added, and reacted at 50-55℃ until the NCO group disappears completely to obtain the epoxy-terminated polyurethane epoxy resin. The synthesis route is as follows:

[0017]

[0018] Preferably, in step (1), the dehydrating conditions of the polyether polyol are as follows: dehydrated at 110-120℃ under a vacuum degree of-0.095MPa for 2-3 hours.

[0019] In step (2), the bisphenol A epoxy resin is first reacted with the polyurethane prepolymer at 60-70℃ for 2-3 hours to prevent ring opening of the epoxy and consume part of the -NCO groups of the polyurethane prepolymer to complete molecular chain extension; the small molecule epoxy compound is slowly added to completely consume the -NCO groups of the polyurethane prepolymer to complete epoxy capping; and the organic tin catalyst is added to promote the reaction of the small molecule compound with the -NCO groups, and the reaction is carried out at 50-55℃ to control the selectivity at low temperature.

[0020] Preferably, in step (2), the organic tin catalyst is at least one of dibutyltin dilaurate (DBTDL) or stannous octoate.

[0021] The adhesive containing the epoxy-capped polyurethane epoxy resin of the present application comprises the following components by weight: 10-15 parts of epoxy resin, 70-75 parts of epoxy-capped polyurethane epoxy resin, 19-21 parts of amine curing agent, and 8-15 parts of heat-conducting filler.

[0022] The epoxy resin is at least one of bisphenol A epoxy resin and bisphenol F epoxy resin.

[0023] Preferably, the heat-conducting filler is at least one of aluminum oxide, aluminum hydroxide, or aluminum nitride.

[0024] Preferably, the amine curing agent is at least one of isophorone diamine (IPDA), cyclohexanediamine (CHDA), m-phenylenediamine (MPDA), or p-phenylenediamine (PPDA).

[0025] The preparation method of the adhesive of the present application comprises the following steps:

[0026] (1) uniformly mixing the epoxy resin, the epoxy-capped polyurethane epoxy resin, and the heat-conducting filler;

[0027] (2) adding the amine curing agent, mixing at a vacuum degree of ≤-100 kPa and a rotation speed of 1200 RPM for 30 seconds to obtain the adhesive.

[0028] The adhesive of the present application is applied in the fields of aerospace, electronics, and mechanical manufacturing.

[0029] Invention mechanism:

[0030] The flexible chain segments are introduced into the epoxy-capped polyurethane epoxy resin of the present application, which can delay the crosslinking reaction during the reaction of the epoxy-capped polyurethane epoxy resin with the amine curing agent, and the flexible polyether polyols have excellent flexibility and suppleness, which can break the constraints of the rigid crosslinking structure of the original epoxy resin after being introduced into the epoxy resin network. In addition, the residual -NCO groups in the system are completely eliminated in the epoxy-capped polyurethane epoxy resin of the present application.

[0031] The epoxy-terminated polyurethane epoxy resin is introduced into the adhesive of the present application. The polyether flexible chain segment in the epoxy-terminated polyurethane epoxy resin hinders the rapid crosslinking of the epoxy resin during the curing process, reduces the crosslinking reaction rate, delays the heat release, and thus reduces the exothermic peak. The addition of the thermally conductive filler in the adhesive can effectively conduct the heat generated by the curing reaction, avoid local heat accumulation, and further reduce the exothermic peak of the system. The introduction of the flexible chain segment in the epoxy-terminated polyurethane epoxy resin breaks the restraint of the rigid crosslinking structure of the original epoxy resin. When the adhesive is stretched by external force, the flexible chain segment can absorb energy through the stretching and slipping of the molecular chain, thereby significantly improving the extension capacity of the material. The epoxy-terminated polyurethane epoxy resin of the present application completely eliminates the residual -NCO groups in the system through the chemical termination process, and fundamentally solves the material foaming problem. In addition, the epoxy-terminated polyurethane epoxy resin and the epoxy resin are simultaneously introduced into the adhesive, and the polyurethane chain segment is firmly connected to the epoxy resin network through chemical bonds by the reaction of the epoxy groups with the curing agent, avoiding the phase separation problem caused by simple physical blending. The flexible chain segment in the epoxy-terminated polyurethane resin can improve the brittleness of the epoxy resin and improve the impact resistance and flexibility of the material. The rigid structure of the epoxy resin maintains the tensile strength and hardness of the material, avoids excessive softening, and ensures that the adhesive maintains high bonding strength and stability while improving toughness.

[0032] Advantages: Compared with the prior art, the present application has the following advantages:

[0033] (1) The epoxy-terminated polyurethane epoxy resin of the present application breaks the restraint of the rigid crosslinking structure of the original epoxy resin, delays the crosslinking reaction speed with the amine curing agent, and completely eliminates the residual -NCO groups in the system;

[0034] (2) The preparation method of the epoxy-terminated polyurethane epoxy resin of the present application is simple and easy to industrialize;

[0035] (3) The adhesive containing the epoxy-terminated polyurethane epoxy resin of the present application reduces the exothermic peak, reduces the exothermic peak by 25-50℃, avoids thermal damage and uneven curing of heat-sensitive materials, and improves the quality consistency of large-size products; significantly improves the toughness: the elongation at break is greater than 7%, solves the problem of brittle fracture of traditional epoxy resin, enhances the impact and vibration resistance of the adhesive, and adapts to dynamic stress scenarios; maintains high strength: the tensile strength is maintained at more than 66.9 MPa, realizes the balance of "high toughness-high strength", and overcomes the disadvantage of strength reduction caused by toughening agent; eliminates the foaming hazard: the chemical termination process completely consumes the NCO groups, avoids foaming from the root, and integrates the polyurethane and the epoxy resin through chemical bonds to prevent phase separation and improve stability;

[0036] (4) The adhesive containing the epoxy-terminated polyurethane epoxy resin of the present application has the following advantages: process adaptability: raw material selection is flexible (polyether, heat-conducting filler, etc. can be adjusted), simple process, suitable for large-scale production, and meets the needs of harsh performance requirements in aerospace, electronics, and other fields. DETAILED DESCRIPTION

[0037] The present application will be further described below in conjunction with specific examples.

[0038] The relevant information of the raw materials used in the present application is shown in Table 1.

[0039]

[0040] Example 1

[0041] The adhesive containing the epoxy-terminated polyurethane epoxy resin described in the present application has the following steps in its preparation method:

[0042] (1) Put PTMEG-2000 into a reaction kettle, dehydrate for 3 hours at 110°C and a vacuum degree of -0.095 MPa to remove water from the raw materials and prevent side reactions between water and isocyanate. According to the weight fraction, take 100 parts of dehydrated PTMEG-2000, then add 24 parts of TDI-80, protect with nitrogen, stir at 80°C for 2 hours, and prepare a polyurethane prepolymer with an NCO content of 6%.

[0043] (2) According to the weight fraction, add 70 parts of E-44 (the NCO content of the system after addition is 3%) to the above-mentioned 20 parts of polyurethane prepolymer, react at 60°C for 3 hours; slowly add 10 parts of glycidol at a speed of 50 mg / min, and add 0.05 parts of DBTDL at the same time, react at 50°C until the NCO of the system disappears, and prepare an epoxy-terminated polyurethane epoxy resin.

[0044] (3) According to the weight fraction, take 75 parts of the synthesized epoxy-terminated polyurethane epoxy resin, 10 parts of bisphenol A epoxy resin E-44, and 15 parts of filler aluminum oxide, mix at a speed of 700 RPM for 10 seconds to form component A, add 19 parts of isophorone diamine to component A, vacuumize to a pressure of -100 kPa or below, and mix at a speed of 1200 RPM for 30 seconds to prepare an epoxy-terminated polyurethane epoxy adhesive.

[0045] Example 2

[0046] This example is the same as Example 1, and the difference is that PPG-2000 is used instead of PTMEG-2000 ((the NCO content of the system after addition is 6%).

[0047] Example 3

[0048] The same as example 1 is not described, the difference is that the input amount of epoxy terminated polyurethane epoxy resin, epoxy resin E-44, aluminum oxide, isophorone diamine is respectively: 70 parts, 15 parts, 15 parts, 19 parts.

[0049] Example 4

[0050] The same as example 1 is not described, the difference is that the input amount of epoxy terminated polyurethane epoxy resin, epoxy resin E-44, aluminum oxide, isophorone diamine is respectively: 75 parts, 10 parts, 8 parts, 19 parts.

[0051] Example 5

[0052] The same as example 1 is not described, the difference is that the input amount of epoxy terminated polyurethane epoxy resin, epoxy resin E-44, aluminum oxide, isophorone diamine is respectively: 75 parts, 10 parts, 8 parts, 19 parts.

[0053] Example 6

[0054] The same as example 1 is not described, the difference is that the input amount of epoxy terminated polyurethane epoxy resin, epoxy resin E-44, aluminum oxide, isophorone diamine is respectively: 75 parts, 10 parts, 8 parts, 19 parts.

[0055] Example 7

[0056] The same as example 1 is not described, the difference is that the input amount of epoxy terminated polyurethane epoxy resin, epoxy resin E-44, aluminum oxide, isophorone diamine is respectively: 75 parts, 10 parts, 8 parts, 19 parts.

[0057] Comparative example 1

[0058] According to the weight fraction, bisphenol A epoxy resin E-44 85 parts, isophorone diamine 19 parts, under the condition of vacuum extraction to the pressure below-100kPa, under the condition of 1200RPM rotation speed, high speed mixing for 30s, epoxy resin adhesive is prepared.

[0059] Comparative example 2

[0060] According to the weight fraction, epoxy resin CYDF-170 85 parts, isophorone diamine 21 parts, under the condition of vacuum extraction to the pressure below-100kPa, under the condition of 1200RPM rotation speed, high speed mixing for 30s, epoxy resin adhesive is prepared.

[0061] Comparative example 3

[0062] On the basis of example 1, in step (2), without using glycidol for capping, some NCO groups are reserved, and the rest of the conditions are unchanged, epoxy resin adhesive is prepared.

[0063] Comparative example 4

[0064] On the basis of Example 1, in step (2), 70 parts of E-44 was added to the above 20 parts of polyurethane prepolymer, and reacted at 90°C until the system NCO disappeared.

[0065] Comparative Example 5

[0066] On the basis of Example 1, in step (1), the flexible polyether PTMEG-2000 was replaced by the non-flexible polyether 670BA.

[0067] Comparative Example 6

[0068] On the basis of Example 1, in step (3), the input amount of epoxy-terminated polyurethane epoxy resin, epoxy resin E-44, alumina, isophorone diamine was 85 parts, 0 parts, 15 parts, 19 parts, respectively.

[0069] Performance Test

[0070] The samples obtained in Examples 1-7 and Comparative Examples 1-6 were tested for performance, including tensile strength, elongation at break, viscosity, exothermic peak, and the test methods are as follows.

[0071] Tensile strength: 25°C cured for 7 days, tested according to GB / T 528-2009.

[0072] Elongation at break: 25°C cured for 7 days, tested according to GB / T 528-2009.

[0073] Exothermic peak: The accurate exothermic peak was obtained by DSC test (heating rate 10°C / min).

[0074] Foaming phenomenon: Group A was exposed to air for 48 hours, and visually observed whether bubbles were generated

[0075] The test results of each sample are shown in Table 1.

[0076] Table 1 Test results of each sample

[0077]

[0078] The adhesives of Examples 1-7 all have a strength ≥66.9 MPa, a toughness ≥7%, an exotherm ≤115°C, and no foaming phenomenon. This is because the performance of the epoxy adhesive is comprehensively optimized by epoxy-terminated polyurethane modification and the introduction of heat-conducting fillers, achieving the synergistic optimization of high strength, high toughness, and low exotherm, overcoming the contradiction of strength decline or excessive exotherm in traditional toughening technology. The chemical capping process ensures complete consumption of NCO groups, avoiding foaming problems.

[0079] Compared with Examples 1-7, the comparative examples do not use modified epoxy resin and thermal conductive filler, and the cross-linking reaction of the epoxy resin is violent, the heat release is concentrated, and the peak is high. The heat release peak of Examples 1-7 is 80-115°C, which is significantly lower than that of Comparative Example 1 (130°C) and Comparative Example 2 (140°C). The higher the thermal conductivity of the thermal conductive filler, the better the heat release control (aluminum nitride > aluminum oxide > aluminum hydroxide). Among them, the heat release peak of Example 6 using aluminum nitride (high thermal conductivity 150-220 W / (m·K)) is the lowest (80°C), indicating that the thermal conductive filler can effectively conduct heat, and the flexible segment of the epoxy-terminated polyurethane can hinder rapid cross-linking, thereby reducing the heat release peak.

[0080] The elongation at break of Examples 1-7 is 7.0%-10%, which is much higher than that of Comparative Example 1 (4%) and Comparative Example 2 (3%). The flexible segment of the polyether is embedded in the epoxy network through a chemical bond, and the flexible segment can absorb stress, thereby improving the elongation at break. The comparative examples have poor toughness due to the rigid structure of the epoxy resin.

[0081] Compared with Comparative Example 1, the tensile strength of Examples 1-6 is 66.9-67.5 MPa, which is close to that of Comparative Example 1 (68 MPa). This indicates that the epoxy termination process does not sacrifice strength while improving toughness, and avoids phase separation through chemical bonding.

[0082] Compared with Example 1, Comparative Examples 3-4 use glycidol to react with NCO to introduce epoxy groups, forming a "polyurethane-epoxy block" structure, and the terminal is an active epoxy group. When reacting with amine, the epoxy group ring-opening forms a three-dimensional cross-linked network, while retaining the flexibility of the polyurethane segment, resulting in good mechanical properties. In Comparative Example 3, glycidol is not used for termination, and a certain amount of NCO is retained in the system, which increases the elongation but decreases the strength and is accompanied by foaming. In Comparative Example 4, glycidol is not used for termination, and the polyurethane prepolymer reacts with the hydroxyl and epoxy groups of E-44 to form a random copolymer. The epoxy group is not directionally terminated, and when reacting with amine, the cross-linking points are randomly distributed, resulting in a decrease in the mechanical properties of the material.

[0083] Compared with Example 1, Comparative Example 5 uses a non-flexible polyether, which decreases the elongation at break of the material and increases the heat release peak temperature, indicating that the flexible polyether plays a key role in increasing the elongation at break of the epoxy adhesive and plays an important role in delaying the cross-linking reaction speed of the epoxy resin and amine curing agent.

[0084] Comparative Example 6 has a large amount of polyurethane segments (flexible) in the epoxy-terminated polyurethane epoxy resin, resulting in less rigid crosslinking points (epoxy groups), and if used alone, the crosslinked network after curing is too loose and the strength is insufficient, so the epoxy-terminated polyurethane epoxy resin still needs to be used in combination with conventional epoxy resins (such as bisphenol A type and bisphenol F type) to ensure crosslinking density and mechanical strength.

Claims

1. An epoxy-terminated polyurethane epoxy resin, characterized in that The polyurethane prepolymer is obtained by reacting a polyurethane prepolymer with an epoxy resin, wherein the NCO of the polyurethane prepolymer and the hydroxyl of the epoxy resin undergo an addition reaction, and after the reaction, a small molecule epoxy compound is used to eliminate the NCO of the system; the polyurethane prepolymer is obtained by reacting an isocyanate with a polyether polyol with a flexible chain segment.

2. The epoxy-terminated polyurethane epoxy resin according to claim 1, characterized in that The polyether polyol with flexible chain segments is at least one of polyoxypropylene polyol, polytetramethylene oxide polyol or polyoxyethylene-oxypropylene copolymer polyol.

3. The epoxy-terminated polyurethane epoxy resin according to claim 1, characterized in that The small molecule epoxy compound is glycidol.

4. A method for preparing the epoxy-terminated polyurethane epoxy resin according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Dehydrating a polyether polyol having a flexible chain segment, and then reacting it with an isocyanate at 70 to 80° C. under an inert gas protection for 2 to 3 hours to obtain a polyurethane prepolymer; (2) adding epoxy resin to the polyurethane prepolymer and reacting at 60-70° C. for 2-3 hours; adding a small molecule epoxy compound dropwise, adding an organic tin catalyst, and reacting at 50-55° C. until the NCO group completely disappears, thereby obtaining an epoxy-terminated polyurethane epoxy resin.

5. The method for preparing the epoxy-terminated polyurethane epoxy resin according to claim 4, wherein: The organic tin catalyst is at least one of dibutyltin dilaurate and stannous octoate.

6. An adhesive containing the epoxy-terminated polyurethane epoxy resin according to any one of claims 1 to 3, characterized in that: The invention comprises the following components in parts by weight: 10 to 15 parts of epoxy resin, 70 to 75 parts of epoxy-terminated polyurethane epoxy resin, 19 to 21 parts of amine curing agent and 8 to 15 parts of thermal conductive filler.

7. The adhesive according to claim 6, characterized in that The thermally conductive filler is at least one of aluminum oxide, aluminum hydroxide or aluminum nitride.

8. The adhesive according to claim 6, characterized in that The amine curing agent is at least one of isophorone diamine, ethylenediamine, m-phenylenediamine or p-phenylenediamine.

9. A method for preparing the adhesive according to any one of claims 6 to 8, characterized in that: The following steps are involved: (1) uniformly mixing epoxy resin, epoxy-terminated polyurethane epoxy resin and thermal conductive filler; (2) Add an amine curing agent, mix, and prepare an adhesive.

10. Use of the adhesive according to any one of claims 6 to 8 in the fields of aerospace, electronics or machinery manufacturing.

Citation Information

Patent Citations

  • A preparation method of a polyurethane / epoxy resin composite material

    CN103524703A

  • Room temperature curing ultralow temperature epoxy sealant and preparation method thereof

    CN105001824A

  • Mercapto-terminated polyurethane modified epoxy mortar and preparation method thereof

    CN111960726A

  • Epoxy structure adhesive film for bonding aviation organic glass and preparation method of epoxy structure adhesive film

    CN114672271A

  • Polyurethane modified epoxy resin adhesive and preparation method thereof

    CN116285831A

Cited By

  • Quick-curing polyurethane seamless expansion joint material for roads and preparation method thereof

    CN121022087A

  • End-capped polyurethane flexibilizer, epoxy resin composition and preparation method of epoxy resin composition

    CN121108441A

  • Wear-resistant network cable with high shielding effectiveness and preparation method thereof

    CN121537778A