Novel cement product
By using a composite mineral-chemical synergistic modification technology, a combination of sulfoaluminate cement clinker, nano-silica aerogel, silicon carbide whiskers, modified attapulgite clay, graphene oxide dispersion, and shape memory polymer microspheres was used to solve the problems of high brittleness, poor crack resistance, and high thermal conductivity of traditional cement products, resulting in cement products with high strength, low thermal conductivity, and self-healing capabilities.
Patent Information
- Application Number
- CN202511133002.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-13
- Publication Date
- 2025-11-04
AI Technical Summary
Traditional cement products are brittle, have poor crack resistance, and high thermal conductivity. They are also prone to structural deterioration due to the propagation of microcracks during long-term use. In existing technologies, fiber reinforcement may cause local stress concentration, polymer modification is costly and may reduce fire resistance, and self-healing processes are complex or require harsh conditions.
The composite mineral-chemical synergistic modification technology is adopted, which combines sulfoaluminate cement clinker, nano-silica aerogel, silicon carbide whiskers, modified attapulgite clay and graphene oxide dispersion and shape memory polymer microspheres, and combines hydrochloric acid activation, ultrasonic dispersion, vacuum vibration molding and graded curing process to form a multi-level reinforcement network and self-healing function.
It significantly improves the mechanical properties and durability of cement products, reduces thermal conductivity, achieves early strength and self-healing ability, increases crack resistance by 62%, reduces thermal conductivity to 0.09 W/(m·K), and achieves compressive strength of 91.7 MPa.
Abstract
Description
Technical Field
[0001] This invention relates to the field of building materials technology, and in particular to a novel cement product. It is suitable for use in building walls, floors, and precast components. This cement product improves the mechanical properties and durability of traditional cement products. Background Technology
[0002] Traditional cement products generally suffer from high brittleness, poor crack resistance, and high thermal conductivity, and are prone to structural deterioration due to the propagation of microcracks during long-term use. Existing technologies typically improve performance by adding fiber reinforcement or polymer modification; however, uneven fiber dispersion can lead to localized stress concentration, while polymers are costly and may reduce fire resistance. Furthermore, some self-healing cements rely on microorganisms or encapsulated repair agents, which involve complex processes or demanding repair conditions. To address these issues, this invention proposes a composite mineral-chemical synergistic modification technology, achieving performance breakthroughs through raw material innovation and process optimization. Summary of the Invention
[0003] In view of this, in order to solve the problems existing in the technical background, the present invention proposes a novel cement product, specifically including the following:
[0004] A novel cement product, by weight proportions, comprises the following raw materials:
[0005] 40-60 parts of sulfoaluminate cement clinker, 5-10 parts of nano-silica aerogel, 3-8 parts of silicon carbide whiskers, 10-15 parts of modified attapulgite, 2-5 parts of graphene oxide dispersion, and 1-3 parts of shape memory polymer microspheres.
[0006] In one embodiment of the present invention, the sulfoaluminate cement clinker comprises 4 parts, nano-silica aerogel comprises 5 parts, silicon carbide whiskers comprises 3 parts, modified attapulgite clay comprises 10 parts, graphene oxide dispersion comprises 2 parts, and shape memory polymer microspheres comprises 1 part.
[0007] In one embodiment of the present invention, the following components are used: 50 parts of sulfoaluminate cement clinker, 8 parts of nano-silica aerogel, 6 parts of silicon carbide whiskers, 12 parts of modified attapulgite clay, 4 parts of graphene oxide dispersion, and 2 parts of shape memory polymer microspheres.
[0008] In one embodiment of the present invention, the components are: 60 parts of sulfoaluminate cement clinker, 10 parts of nano-silica aerogel, 8 parts of silicon carbide whiskers, 15 parts of modified attapulgite clay, 5 parts of graphene oxide dispersion, and 3 parts of shape memory polymer microspheres.
[0009] A new manufacturing process for cement products includes the following steps:
[0010] Step 1: After activating the attapulgite with hydrochloric acid, dry-modify it with a silane coupling agent to improve the interfacial bonding force; disperse silicon carbide whiskers in an ethanol solution with ultrasonic assistance and then blend them with graphene oxide.
[0011] Step 2: The cement clinker, nano-aerogel and pretreated reinforcing phase are ball-milled under an inert atmosphere until the particle size D90 < 50 μm;
[0012] Step 3: Add an aqueous solution containing water-reducing agent and shape memory microspheres, and stir to form a fluidized slurry;
[0013] Step 4: After vacuum vibration molding, first steam curing at 80℃ for 6 hours to activate early strength, then transfer to 20℃ saturated lime water for curing for 7 days.
[0014] In one embodiment of the present invention, in step four, the parameters are controlled as follows: vacuum degree ≥ 0.08 MPa and vibration frequency 50 Hz ± 5%.
[0015] In one embodiment of the present invention, the nano-aerogel reduces the thermal conductivity while providing nano-nucleation sites, and silicon carbide whiskers and attapulgite form a micron- to millimeter-level multi-level reinforcement network; graphene oxide enhances the early hydration rate; and shape memory polymer microspheres trigger expansion above 60°C to achieve self-repair of cracks.
[0016] In one embodiment of the present invention, in step one, attapulgite is activated in 1 mol / L hydrochloric acid for 2 hours, washed until neutral, and then dry modified with 2 wt% silane coupling agent. Silicon carbide whiskers and graphene oxide are ultrasonically dispersed in ethanol solution (power 800W, time 30min) to form a uniform suspension.
[0017] The above technical solution has the following beneficial effects:
[0018] This invention utilizes sulfoaluminate cement clinker combined with nano-silica aerogel to reduce thermal conductivity and provide nucleation sites. Silicon carbide whiskers and modified attapulgite form a multi-level reinforcing network, graphene oxide accelerates early hydration, and shape memory polymer microspheres achieve self-healing functionality triggered at 60°C. During preparation, attapulgite is activated with hydrochloric acid and modified with a silane coupling agent. Silicon carbide whiskers and graphene oxide are ultrasonically dispersed and ball-milled under an inert atmosphere until D90 < 50 μm to ensure uniform material dispersion. Vacuum vibration molding and graded curing processes are employed to achieve products with both high early strength and excellent durability. Detailed Implementation
[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] Example 1: A novel cement product, comprising the following raw materials by weight ratio: 4 parts of the sulfoaluminate cement clinker, 5 parts of nano-silica aerogel, 3 parts of silicon carbide whiskers, 10 parts of modified attapulgite clay, 2 parts of graphene oxide dispersion, and 1 part of shape memory polymer microspheres.
[0021] A new manufacturing process for cement products includes the following steps:
[0022] Step 1: After activating the attapulgite with hydrochloric acid, dry-modify it with a silane coupling agent to improve the interfacial bonding force; disperse silicon carbide whiskers in an ethanol solution with ultrasonic assistance and then blend them with graphene oxide.
[0023] Step 2: The cement clinker, nano-aerogel and pretreated reinforcing phase are ball-milled under an inert atmosphere until the particle size D90 < 50 μm;
[0024] Step 3: Add an aqueous solution containing water-reducing agent and shape memory microspheres, and stir to form a fluidized slurry;
[0025] Step 4: After vacuum vibration molding, first steam curing at 80℃ for 6 hours to activate early strength, then transfer to 20℃ saturated lime water for curing for 7 days.
[0026] In this embodiment, in step four, the parameters are controlled as follows: vacuum degree ≥ 0.08 MPa, vibration frequency 50 Hz ± 5%. The nano-aerogel reduces the thermal conductivity while providing nano-nucleation sites. Silicon carbide whiskers and attapulgite form a micron-millimeter level multi-level reinforcement network. Graphene oxide enhances the early hydration rate. Shape memory polymer microspheres trigger expansion above 60°C to achieve self-repair of cracks. In step one, attapulgite is activated in 1 mol / L hydrochloric acid for 2 hours, washed to neutral, and then dry modified with 2 wt% silane coupling agent. Silicon carbide whiskers and graphene oxide are ultrasonically dispersed in ethanol solution (power 800 W, time 30 min) to form a uniform suspension.
[0027] Example 2: A novel cement product, comprising the following raw materials by weight ratio: 50 parts of sulfoaluminate cement clinker, 8 parts of nano-silica aerogel, 6 parts of silicon carbide whiskers, 12 parts of modified attapulgite clay, 4 parts of graphene oxide dispersion, and 2 parts of shape memory polymer microspheres.
[0028] A new manufacturing process for cement products includes the following steps:
[0029] Step 1: After activating the attapulgite with hydrochloric acid, dry-modify it with a silane coupling agent to improve the interfacial bonding force; disperse silicon carbide whiskers in an ethanol solution with ultrasonic assistance and then blend them with graphene oxide.
[0030] Step 2: The cement clinker, nano-aerogel and pretreated reinforcing phase are ball-milled under an inert atmosphere until the particle size D90 < 50 μm;
[0031] Step 3: Add an aqueous solution containing water-reducing agent and shape memory microspheres, and stir to form a fluidized slurry;
[0032] Step 4: After vacuum vibration molding, first steam curing at 80℃ for 6 hours to activate early strength, then transfer to 20℃ saturated lime water for curing for 7 days.
[0033] In step four, the parameters are controlled with a vacuum degree ≥0.08MPa and a vibration frequency of 50Hz±5%. The nano-aerogel reduces the thermal conductivity while providing nano-nucleation sites. Silicon carbide whiskers and attapulgite form a micron-millimeter-level multi-level reinforcement network. Graphene oxide enhances the early hydration rate. Shape memory polymer microspheres trigger expansion at temperatures above 60℃ to achieve self-repair of cracks. In step one, attapulgite is activated in 1mol / L hydrochloric acid for 2 hours, washed to neutral, and then dry-modified with 2wt% silane coupling agent. Silicon carbide whiskers and graphene oxide are ultrasonically dispersed in ethanol solution (power 800W, time 30min) to form a uniform suspension.
[0034] Example 3: A novel cement product, comprising the following raw materials by weight ratio: 60 parts of the sulfoaluminate cement clinker, 10 parts of nano-silica aerogel, 8 parts of silicon carbide whiskers, 15 parts of modified attapulgite clay, 5 parts of graphene oxide dispersion, and 3 parts of shape memory polymer microspheres.
[0035] A new manufacturing process for cement products includes the following steps:
[0036] Step 1: After activating the attapulgite with hydrochloric acid, dry-modify it with a silane coupling agent to improve the interfacial bonding force; disperse silicon carbide whiskers in an ethanol solution with ultrasonic assistance and then blend them with graphene oxide.
[0037] Step 2: The cement clinker, nano-aerogel and pretreated reinforcing phase are ball-milled under an inert atmosphere until the particle size D90 < 50 μm;
[0038] Step 3: Add an aqueous solution containing water-reducing agent and shape memory microspheres, and stir to form a fluidized slurry;
[0039] Step 4: After vacuum vibration molding, first steam curing at 80℃ for 6 hours to activate early strength, then transfer to 20℃ saturated lime water for curing for 7 days.
[0040] In step four, the parameters are controlled with a vacuum degree ≥0.08MPa and a vibration frequency of 50Hz±5%. The nano-aerogel reduces the thermal conductivity while providing nano-nucleation sites. Silicon carbide whiskers and attapulgite form a micron-millimeter-level multi-level reinforcement network. Graphene oxide enhances the early hydration rate. Shape memory polymer microspheres trigger expansion at temperatures above 60℃ to achieve self-repair of cracks. In step one, attapulgite is activated in 1mol / L hydrochloric acid for 2 hours, washed to neutral, and then dry-modified with 2wt% silane coupling agent. Silicon carbide whiskers and graphene oxide are ultrasonically dispersed in ethanol solution (power 800W, time 30min) to form a uniform suspension.
[0041] index Example 1 Example 2 Example 3 3D compressive strength (MPa) 28.5 34.2 38.6 28-day compressive strength (MPa) 76.8 85.3 91.7 Thermal conductivity (W / m·K) 0.14 0.11 0.09 Freeze-thaw loss rate (%) 1.2 0.8 0.5
[0042] Analysis revealed that the rapid hardening properties of sulfoaluminate cement clinker, as the matrix material, complement the nano-nucleation effect of nano-silica aerogel. In Example 2, the addition of 8 parts of aerogel increased the early hydration rate by 35%, confirming its promoting effect on strength development. Example 3 exhibited optimal crack resistance, with crack propagation resistance increased by 62% compared to ordinary cement. Ultrasonic dispersion (800W / 30min) ensured uniform distribution of silicon carbide whiskers and graphene oxide, and SEM images showed that the dispersion of the reinforcing phase reached over 95%. Vacuum vibration molding (≥0.08MPa, 50Hz) reduced the porosity to 3.8%, significantly better than conventional vibration compaction (7.2%).
[0043] Shape memory microspheres expand at 60°C. Test in Example 2 showed a 92% repair rate for 0.25mm cracks, and the impermeability was restored to 89% of the initial value after repair.
[0044] This invention enhances the performance of cement products through the synergistic effect of its various raw material components. Sulfoaluminate cement clinker, as the matrix material, provides early strength assurance due to its rapid hardening properties. The addition of nano-silica aerogel not only significantly reduces thermal conductivity, but its abundant silanol groups also serve as nucleation sites for cement hydration, accelerating the formation of hydration products. Silicon carbide whiskers and modified attapulgite form a multi-scale reinforcing network. The attapulgite, activated by hydrochloric acid and modified with a silane coupling agent, improves the interfacial bonding with the cement matrix, while the silicon carbide whiskers prevent microcrack propagation through bridging. The synergy of these two components improves crack resistance. Graphene oxide, with its ultra-large specific surface area and oxygen-containing functional groups, promotes early hydration reactions and enhances impermeability through physical barrier effects. Shape memory polymer microspheres, as a smart repair component, can expand and fill cracks upon temperature triggering, achieving the material's self-healing function.
[0045] Example 1, using the basic formulation, achieved a 28-day compressive strength of 76.8 MPa, significantly superior to conventional cement products. Example 2, by optimizing the proportions of each component, particularly increasing the nano-aerogel to 8 parts and adjusting the silicon carbide whiskers to 6 parts, reduced the thermal conductivity to 0.11 W / (m·K) while increasing the compressive strength to 85.3 MPa, demonstrating the best cost-performance balance. Example 3, using the upper limit formulation, although increasing material costs, achieved an ultra-high strength of 91.7 MPa and an extremely low thermal conductivity of 0.09 W / (m·K), making it particularly suitable for special engineering projects with stringent performance requirements. This invention, through the functional complementarity of each component and process optimization, achieves a synergistic improvement in mechanical properties, durability, and intelligent characteristics. The data from each example verify the feasibility and reliability of the technical solution.
[0046] The basic principles and main features of the present invention have been described above. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are only illustrative of the principles of the present invention. Various changes and modifications can be made to the present invention without departing from the spirit and scope of the present invention. All such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the invention is defined by the appended claims and their equivalents.
Claims
1. A novel cement product, characterized in that, According to the weight ratio, the following raw materials are included: 40-60 parts of sulfoaluminate cement clinker, 5-10 parts of nano-silica aerogel, 3-8 parts of silicon carbide whiskers, 10-15 parts of modified attapulgite, 2-5 parts of graphene oxide dispersion, and 1-3 parts of shape memory polymer microspheres.
2. The novel cement product according to claim 1, characterized in that, The composition includes 4 parts of sulfoaluminate cement clinker, 5 parts of nano-silica aerogel, 3 parts of silicon carbide whiskers, 10 parts of modified attapulgite clay, 2 parts of graphene oxide dispersion, and 1 part of shape memory polymer microspheres.
3. A novel cement product according to claim 1, characterized in that, 50 parts of sulfoaluminate cement clinker, 8 parts of nano-silica aerogel, 6 parts of silicon carbide whiskers, 12 parts of modified attapulgite clay, 4 parts of graphene oxide dispersion, and 2 parts of shape memory polymer microspheres.
4. A novel cement product according to claim 1, characterized in that, The composition includes 60 parts of sulfoaluminate cement clinker, 10 parts of nano-silica aerogel, 8 parts of silicon carbide whiskers, 15 parts of modified attapulgite clay, 5 parts of graphene oxide dispersion, and 3 parts of shape memory polymer microspheres.
5. A novel manufacturing process for cement products, characterized in that, Includes the following steps: Step 1: After activating the attapulgite clay with hydrochloric acid, dry-modify it with a silane coupling agent to improve the interfacial bonding force; disperse silicon carbide whiskers in an ethanol solution with ultrasonic assistance and then blend them with graphene oxide. Step 2: The cement clinker, nano-aerogel and pretreated reinforcing phase are ball-milled under an inert atmosphere until the particle size D90 < 50 μm; Step 3: Add an aqueous solution containing water-reducing agent and shape memory microspheres, and stir to form a fluidized slurry; Step 4: After vacuum vibration molding, first steam curing at 80℃ for 6 hours to activate early strength, then transfer to 20℃ saturated lime water for curing for 7 days.
6. The manufacturing process of a novel cement product according to claim 5, characterized in that, In step four, the parameters are controlled as follows: vacuum degree ≥ 0.08 MPa and vibration frequency 50 Hz ± 5%.
7. The manufacturing process of a novel cement product according to claim 5, characterized in that, The nano-aerogel reduces thermal conductivity while providing nano-nucleation sites, and silicon carbide whiskers and attapulgite form a micron- to millimeter-level multi-level reinforcement network; graphene oxide enhances the early hydration rate; and shape memory polymer microspheres trigger expansion above 60°C to achieve self-repair of cracks.
8. The manufacturing process of a novel cement product according to claim 5, characterized in that, In step one, attapulgite is activated in 1 mol / L hydrochloric acid for 2 hours, washed until neutral, and then dry modified with 2 wt% silane coupling agent. Silicon carbide whiskers and graphene oxide are ultrasonically dispersed in ethanol solution (power 800W, time 30min) to form a uniform suspension.