Method for in-situ growth of SiOx in carbon nanotube cluster by using liquid phase method and application
By in-situ growing SiOx within carbon nanotube clusters using a liquid-phase method, CNTs@SiOx-F@C composite materials were prepared, solving the problems of poor conductivity and volume change in carbon anode materials and achieving a significant improvement in the performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202511094266.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-06
- Publication Date
- 2025-11-11
AI Technical Summary
Existing carbon anode materials in lithium-ion batteries suffer from poor conductivity, large volume changes, severe material pulverization, and low initial coulombic efficiency. The design of carbon nanotube/SiOx composite structures is complex and difficult to realize.
SiOx was grown in situ within carbon nanotube clusters using a liquid-phase method. The CNTs@SiOx-F@C composite material was prepared by mixing, aging, drying, and pyrolyzing a silane with a carbon nanotube dispersion. The silane crosslinking effect was used to form a cluster structure, and SiOx grew on the carbon nanotube wall.
It improves the conductivity of the material and alleviates volume expansion, thereby enhancing the overall electrochemical performance of lithium-ion batteries and making it suitable for industrial-scale preparation of silicon-oxygen-carbon composite materials.
Smart Images

Figure CN120933330A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional materials technology, and specifically relates to a method for in-situ growth of SiO2 within carbon nanotube clusters using a liquid-phase method. x The methods and their applications in the field of lithium-ion batteries. Background Technology
[0002] In recent years, clean technologies have developed rapidly, and the clean energy market has grown globally. The widespread adoption of electric vehicles has led to a strong demand for efficient energy conversion and storage devices. Compared to other rechargeable batteries, LIBs have a mature production system, offering high power density and energy density, as well as excellent cycle stability. However, carbon's theoretical specific capacity is relatively low (372 mAh g / g). -1 However, this cannot meet the demand for high energy density. Silicon materials have a much higher theoretical specific capacity than carbon (4200 mAh g⁻¹). -1 SiO₂ has a low discharge plateau and has attracted considerable attention as a promising alternative to carbon anodes. However, it often undergoes large volume changes during lithiation / delithiation, leading to loss of electrical contact between the electrode and the current collector. Unstable SEI films tend to re-form as fresh surfaces are continuously exposed to the electrolyte during cycling, ultimately resulting in low initial coulombic efficiency (ICE) and deterioration of reversible capacity. Compared to Si-based materials, SiO₂... x The material exhibits low volume expansion and high cycling stability, and some silicon composite structures can further enhance these properties by replacing some oxygen atoms with carbon atoms, thereby generating a certain degree of rigidity. However, these substituents still have some significant drawbacks, such as poor conductivity, non-negligible volume changes, severe material pulverization, and low ICE (internal conductivity). Carbon nanotubes, as excellent conductive structural materials, and SiO₂... x Material compositing can significantly improve the poor intrinsic conductivity of carbon nanotubes and alleviate the severe volume expansion during charging and discharging. However, designing stable carbon nanotube / SiO₂ composites remains a challenge. x The development of composite structures and the typically complex composite processes have limited their potential. Summary of the Invention
[0003] Based on the problems existing in the background technology, the present invention provides a method for in-situ growth of SiO2 within carbon nanotube clusters using a liquid phase method. x This method involves simply dissolving two silanes (VTES and TFPS) in a conventional hydrochloric acid solvent, then mixing and stirring with a carbon nanotube dispersion, aging, drying, and pyrolytic carbonization to obtain CNTs@SiO. x -F@C composite material; This method has the advantages of mild reaction conditions and easy control of silicon-oxygen-carbon ratio, and is expected to be used for industrial preparation of silicon-oxygen-carbon composite materials, which can be applied in the energy field, especially in the field of lithium-ion batteries.
[0004] To solve the above-mentioned technical problems, one technical solution adopted by the present invention is: an in-situ growth of SiO2 within carbon nanotube clusters using a liquid-phase method. x The method includes the following steps:
[0005] Step 1: Dissolve silane A and silane B in hydrochloric acid solution and react at room temperature to obtain a mixed silane solution;
[0006] Step 2: Disperse carboxylated carbon nanotubes in deionized water and ultrasonically disperse to obtain a carbon nanotube dispersion.
[0007] Step 3: Add the carbon nanotube dispersion to the silane mixed solution, stir and mix, then age at room temperature, collect the precipitate, and dry to obtain the dried product;
[0008] Step four: The dried product is pyrolyzed and carbonized at high temperature under an inert gas atmosphere to obtain CNTs@SiO. x -F@C composite material, where x is 1-2.
[0009] In further detail, in step one, silane A is vinyltris(2-methoxyethoxy)silane, silane B is trimethoxy(3,3,3-trifluoropropyl)silane, and the amounts of silane A and silane B are in a volume ratio of 1:(1-2).
[0010] To elaborate further, in step one, the concentrations of silane A and silane B in the hydrochloric acid solution are 0.1-0.5 mol / L.
[0011] To elaborate further, the concentration of the hydrochloric acid solution in step one is 1-5M.
[0012] To elaborate further, the concentration of the carbon nanotube dispersion in step two is 0.05-2 mg / ml.
[0013] Furthermore, in step three, the amount of carbon nanotubes used accounts for 10%-50% of the total amount of silane A and silane B.
[0014] To elaborate further, the aging time in step three is 24 hours, and the drying conditions are vacuum drying at 80°C for 10 hours.
[0015] To elaborate further, the high-temperature pyrolysis in step four takes place at a temperature of 500-1000℃ for 1-5 hours.
[0016] Furthermore, the heating rate of the high-temperature pyrolysis in step four is 2-5℃ / min.
[0017] Furthermore, the CNTs@SiO x -F@C composite material is used in the negative electrode of lithium-ion batteries.
[0018] The beneficial effects of the present invention include at least the following:
[0019] 1. This invention only requires mixing and dissolving two silanes (VTES, TFPS) in a conventional hydrochloric acid solvent, then mixing and stirring with a carbon nanotube dispersion, aging, drying, and pyrolysis carbonization to obtain CNTs@SiO. x -F@C composite material; in the obtained material, carbon nanotubes intertwine to form cluster structures due to the cross-linking effect of silane, SiO x It grows on the walls of carbon nanotubes within clusters. This unique structure provides a rapid electron-ion conduction channel, and the internal voids can alleviate the stress on SiO₂. x The volume expansion during cycling improves the overall electrochemical performance of silicon-oxygen anodes in lithium-ion batteries.
[0020] 2. The preparation method of the present invention has the advantages of mild reaction conditions and easy control of the silicon-oxygen-carbon ratio, and is expected to be used for industrial preparation of silicon-oxygen-carbon composite materials, which can be applied in the energy field, especially in the field of lithium-ion batteries. Attached Figure Description
[0021] The accompanying drawings are provided to further explain the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings:
[0022] Figure 1 CNTs@SiO in Embodiment 1 of the present invention x Scanning electron microscope image of the -F@C composite material;
[0023] Figure 2 CNTs@SiO in Embodiment 1 of the present invention x Transmission electron microscopy image of the -F@C composite material;
[0024] Figure 3 CNTs@SiO in Embodiment 1 of the present invention x XRD pattern of -F@C composite material;
[0025] Figure 4 CNTs@SiO in Embodiment 1 of the present invention x -F@C composite material as a negative electrode material for lithium-ion batteries half-cell cycle diagram;
[0026] Figure 5 CNTs@SiO in Embodiment 1 of the present invention x -F@C composite material-based batteries in 1Ag -1 Graph of 200 charge-discharge cycles at current density;
[0027] Figure 6 CNTs@SiO in Embodiment 1 of the present inventionx Rate performance of batteries made from -F@C composite materials. Detailed Implementation
[0028] The technical solution of the present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments.
[0029] Example 1:
[0030] Step 1: Vinyltris(2-methoxyethoxy)silane (VTES) and trimethoxy(3,3,3-trifluoropropyl)silane (TFPS) are dissolved in a conventional hydrochloric acid solvent at a volume ratio of 1:1 and reacted at room temperature for 5 min to obtain a silane mixed solution.
[0031] Step 2: Disperse carboxylated carbon nanotubes in deionized water and sonicate for 10 min to obtain a carbon nanotube mixed solution;
[0032] Step 3: Add the carbon nanotube dispersion to the silane mixture, mix and stir for 5 minutes, then age at room temperature for 24 hours. Collect the precipitate and vacuum dry at 80°C for 10 hours.
[0033] Step four: The dried product is heat-treated at 900℃ under a nitrogen atmosphere at a heating rate of 5℃ / min for 2 hours for pyrolysis and carbonization to obtain CNTs@SiO. x -F@C composite material.
[0034] Example 2:
[0035] Compared with Example 1, with other steps remaining unchanged, the volume ratio of vinyltris(2-methoxyethoxy)silane (VTES) and trimethoxy(3,3,3-trifluoropropyl)silane (TFPS) in step 1 is 1:2.
[0036] Example 3:
[0037] Compared with Example 1, the nitrogen atmosphere in step 4 is replaced with an argon atmosphere while keeping other steps unchanged.
[0038] Example 4:
[0039] Compared with Example 1, the heat treatment temperature in step 4 is 1000°C, while keeping other steps unchanged.
[0040] Example 5:
[0041] Compared with Example 1, the heat treatment time in step 4 is 4 hours, while keeping other steps unchanged.
[0042] Examples 1-5 all yielded the following results: Figure 1 The CNTs@SiO shownx -F@C composite material, made from Figure 1 The overall size of the product can be seen to be on the micrometer scale, SiO x They are evenly distributed within CNT clusters.
[0043] Comparative Example 1
[0044] The difference from Example 1 is that the two silane mixed dispersions are replaced with SiOx powder dispersions, while the other steps are the same.
[0045] Test case
[0046] Figure 1 and Figure 2 CNTs@SiO in Embodiment 1 of the present invention x Scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the -F@C composite material, from Figure 1 Scanning electron microscope images and Figure 2 As can be seen from the transmission electron microscopy image, the CNTs@SiO prepared in Example 1 of this invention... x -F@C composite materials possess CNT cluster structures, SiO2 x The carbon nanotubes grow on the walls of the clusters and are relatively evenly distributed, while the clusters also possess abundant porous structures. This unique structure can alleviate the stress on SiO₂. x The volume expansion during cycling increases the electron transport rate, providing abundant channels for lithium-ion transport.
[0047] Figure 3 CNTs@SiO in Embodiment 1 of the present invention x The XRD pattern of the -F@C composite material clearly shows that the composite material contains CNTs and SiO2. x .
[0048] Application examples
[0049] The composite materials prepared in Examples 1-5 and Comparative Example 1 were used as active materials to fabricate coin-type half-cells: the active material, SuperP, and polyacrylic acid binder were mixed in a mass ratio of 8:1:1 to form a uniform slurry; the obtained slurry was adhered to copper foil and vacuum dried in an oven at 80°C for 12 hours, and then the copper foil was stamped into a disc. The half-cells were assembled in an argon-filled glove box, using pure lithium foil as the counter electrode and a porous membrane (Celgard 2400) as the separator. The electrolyte was purchased from Duoduo Chemical Reagent Network, model LX-025.
[0050] The prepared coin cell was subjected to electrochemical testing at room temperature within a voltage window of 0.01–1.5 volts.
[0051] Table 1 shows the electrochemical performance test results of the batteries prepared from the composite materials of Examples 1-5 and Comparative Example 1.
[0052] Table 1
[0053]
[0054] Figure 4 CNTs@SiO in Embodiment 1 of the present invention x The battery prepared from the -F@C composite material was tested at 0.2Ag. -1 The graph shows 100 charge-discharge cycles at current density. The graph also shows CNTs@SiO2. x -F@C composite cathode at 0.2Ag -1 It is very stable under current density cycling.
[0055] Figure 5 CNTs@SiO in Embodiment 1 of the present invention x -F@C composite material-based batteries in 1Ag -1 The graph shows 200 charge-discharge cycles at current density. The graph also shows CNTs@SiO2. x -F@C composite cathode at 1Ag -1 Even after 200 cycles at high current density, the capacity remains very stable.
[0056] Figure 6 CNTs@SiO in Embodiment 1 of the present invention x The rate performance diagram of the battery prepared by the -F@C composite material is shown, where the current density is 0.2Ag. -1 0.5Ag -1 0.8Ag -1 1Ag -1 2Ag -1 In 2Ag -1 CNTs@SiO at current density x The -F@C cathode still exhibits high reversible capacity, and the current density recovers to 0.2Ag. -1 At the same time, the capacity can also be restored to over 800mAh / g, demonstrating the performance of CNTs@SiO. x -F@C composite materials have excellent rate performance.
[0057] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made based on the content of the present invention specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A method for in-situ growth of SiO2 within carbon nanotube clusters using a liquid-phase method x The method is characterized by, Includes the following steps: Step 1: Dissolve silane A and silane B in hydrochloric acid solution and react at room temperature to obtain a mixed silane solution; Step 2: Disperse carboxylated carbon nanotubes in deionized water and ultrasonically disperse to obtain a carbon nanotube dispersion. Step 3: Add the carbon nanotube dispersion to the silane mixed solution, stir and mix, then age at room temperature, collect the precipitate, and dry to obtain the dried product; Step four: The dried product is pyrolyzed and carbonized at high temperature under an inert gas atmosphere to obtain CNTs@SiO. x -F@C composite material, where x is 1-2.
2. The method according to claim 1, characterized in that, In step one, silane A is vinyltris(2-methoxyethoxy)silane, and silane B is trimethoxy(3,3,3-trifluoropropyl)silane. The volume ratio of silane A to silane B is 1:(1-2).
3. The method according to claim 1, characterized in that, In step one, the concentrations of silane A and silane B in the hydrochloric acid solution are 0.1-0.5 mol / L.
4. The method according to claim 1, characterized in that, The concentration of the hydrochloric acid solution in step one is 1-5M.
5. The method according to claim 1, characterized in that, In step two, the concentration of the carbon nanotube dispersion is 0.05-2 mg / ml.
6. The method according to claim 1, characterized in that, In step three, the amount of carbon nanotubes used accounts for 10%-50% of the total amount of silane A and silane B.
7. The method according to claim 1, characterized in that, In step three, the aging time is 24 hours, and the drying conditions are vacuum drying at 80℃ for 10 hours.
8. The method according to claim 1, characterized in that, In step four, the high-temperature pyrolysis temperature is 500-1000℃, and the time is 1-5 hours.
9. The method according to claim 1, characterized in that, The heating rate of high-temperature pyrolysis in step four is 2-5℃ / min.
10. The method according to claim 1, characterized in that, The CNTs@SiO x -F@C composite material is used in the negative electrode of lithium-ion batteries.
Citation Information
Cited By
SiOx-coated CNTs composite material for seawater desalination as well as preparation method and application of SiOx-coated CNTs composite material
CN121449075A