Modified separation membrane as well as preparation method and application thereof

By ultrasonic exfoliation and cross-linking modification of kaolinite and montmorillonite nanosheets, a highly efficient modified separation membrane was prepared, which solved the problem of magnesium-lithium ion separation in salt lake brine, achieved high selectivity and high throughput separation effect, and improved the extraction efficiency and purity of lithium resources.

CN120961001AActive Publication Date: 2025-11-18CENT SOUTH UNIV

Patent Information

Application Number
CN202511499850.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-21
Publication Date
2025-11-18
Estimated Expiration
2045-10-21

AI Technical Summary

Technical Problem

In existing methods for treating salt lake brine, the separation membrane materials have insufficient retention rates and low separation coefficients in the selective separation of magnesium and lithium ions, making it impossible to achieve efficient separation of magnesium and lithium ions. Furthermore, traditional methods suffer from environmental pollution and high costs.

Method used

Kaolinite and montmorillonite nanosheets are used as raw materials. Single-layer or few-layer nanosheets are formed by ultrasonic liquid phase exfoliation and combined with crosslinking agents. These nanosheets are then loaded onto microporous aqueous filter membranes to form modified separation membranes. The separation performance is improved by utilizing the specific interactions of the nanosheets and the modifying effect of the crosslinking agents.

Benefits of technology

It significantly improves the separation effect of lithium and magnesium ions, achieving high separation coefficient, high rejection rate and high throughput, thereby improving the extraction efficiency and purity of lithium resources and meeting the needs of salt lake brine treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120961001A_ABST
    Figure CN120961001A_ABST
Patent Text Reader

Abstract

The invention provides a modified separation membrane as well as a preparation method and application thereof, the preparation method of the modified separation membrane comprises the following steps: obtaining a mixed system of a mineral aggregate and a polar solvent, performing ultrasonic liquid phase stripping on the mixed system to obtain a to-be-treated liquid, and the mass volume ratio of the mineral aggregate to the polar solvent is (50-100) mg: (30-60) ml; performing centrifugal treatment on the to-be-treated liquid, and collecting supernatant liquid to obtain nano suspension liquid; a cross-linking agent is mixed with the nano suspension to obtain modified liquid, the modified liquid contains the modified nanosheets, and the mass of the cross-linking agent is 2%-30% of the mass of the mineral aggregate; the modified liquid is filtered through a filter membrane, the modified nanosheets are evenly loaded on the surface of the filter membrane, and the modified separation membrane is prepared. The modified separation membrane prepared by the invention is a modified separation membrane material with high separation coefficient, high rejection rate and high flux, and has excellent performance.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of membrane separation, and particularly relates to a modified separation membrane and a preparation method and application thereof. BACKGROUND

[0002] As an important resource, salt lake brine contains rich lithium, magnesium and other metal ions. With the rapid development of new energy industry, the demand for lithium resources is increasing, and the extraction of lithium from salt lake brine has become one of the important ways to obtain lithium resources. However, salt lake brine usually contains high concentration of magnesium ions, and magnesium and lithium ions have similar properties. How to realize efficient and selective separation of magnesium and lithium ions has become a key technical problem in the extraction of lithium resources from salt lake brine. In the existing methods for treating salt lake brine, there are many limitations. The traditional chemical precipitation method consumes a large amount of chemical reagents, which not only increases the treatment cost, but also may introduce new impurities and pollute the environment. Although the solvent extraction method has a certain selectivity, the organic solvents used are often toxic, and the extraction process is complex, the equipment investment is large, and the operation cost is high. In the ion exchange method, the adsorption capacity of ion exchange resin is limited, and the regeneration process is complicated, which is difficult to meet the demand of large-scale industrial treatment of salt lake brine.

[0003] Membrane separation technology, as a new separation technology, has attracted widespread attention in the field of salt lake brine treatment due to its advantages of high efficiency, energy saving, no pollution, etc. However, the existing separation membrane materials still have deficiencies in the selective separation of magnesium and lithium ions. The ordinary separation membrane has a poor difference in the retention rate of magnesium and lithium ions, and a low separation coefficient, which cannot realize efficient separation of magnesium and lithium ions.

[0004] Therefore, it is necessary to provide a modified separation membrane material with high separation coefficient, high retention rate and high flux to alleviate or solve the above problems. SUMMARY

[0005] To solve the technical problem that the above conventional technologies cannot realize effective and selective separation of ions in wastewater such as salt lake brine while maintaining high retention rate and high flux, the application provides a preparation method of a modified separation membrane, comprising the following steps: obtaining a mixed system of a mineral material and a polar solvent, the mixed system being subjected to ultrasonic liquid phase stripping to obtain a to-be-treated liquid, and the mass-volume ratio of the mineral material to the polar solvent being 50-100 mg:30-60 ml; centrifuging the to-be-treated liquid to collect supernatant to obtain a nanosuspension; mixing a crosslinking agent with the nanosuspension to obtain a modified liquid, the modified liquid containing modified nanosheets, and the mass of the crosslinking agent being 2%-30% of the mass of the mineral material; The modified liquid is filtered through a filter membrane, so that the modified nanosheets are uniformly loaded on the surface of the filter membrane, and a modified separation membrane is prepared.

[0006] Further, the mineral material includes kaolinite and / or montmorillonite, and the polar solvent includes one or more of water, ethanol and propylene glycol.

[0007] Further, the cross-linking agent includes one or more of 1,3-propanediamine, 1,6-hexanediamine, 1,9-nonanediamine and 1,12-diaminododecane.

[0008] Further, the ultrasonic condition in the ultrasonic liquid phase exfoliation process is that the ultrasonic power is 300-500 W, and the exfoliation time is 4-24 h.

[0009] Further, the filtration mode includes vacuum filtration, and the vacuum filtration negative pressure is 0-0.1 MPa.

[0010] Further, the filter membrane includes a microporous water-based filter membrane, and the pore size of the filter membrane is 0.15-0.3 microns. The loading amount of the modified nanosheet on the filter membrane is 0.6-1.4 mg / cm 2 .

[0011] Further, the mass of the cross-linking agent is 2.5%-20% of the mass of the mineral material.

[0012] The application provides a modified separation membrane prepared by the preparation method of the modified separation membrane.

[0013] The application provides an application of the modified separation membrane in salt lake brine treatment.

[0014] Further, the concentration of magnesium ions in the salt lake brine is 0.01-0.5 mol / L, and the concentration of lithium ions in the salt lake brine is 0.01-0.5 mol / L. The modified separation membrane has a lithium ion retention rate of not less than 90%, a magnesium ion separation rate of not less than 95%, and a separation coefficient greater than 1.5.

[0015] Compared with the prior art, the application has at least the following advantages: The application successfully optimizes the separation performance of the separation membrane by the originality design of the steps and raw materials, cooperates the structural characteristics of the raw materials, ultrasonic exfoliation, cross-linking modification and filter membrane loading and other technical features, significantly improves the lithium-magnesium ion separation effect, and prepares a modified separation membrane material with high separation coefficient, high retention rate and high flux. Correlation between raw material structure and separation performance. Kaolinite and montmorillonite have typical two-dimensional layered structure and high stacking degree. This structure makes the nanosheets formed after subsequent treatment have large specific surface area and abundant surface active sites. These active sites can interact specifically with lithium and magnesium ions during the separation process; the large specific surface area also increases the contact opportunity between ions and separation membranes, which is beneficial to improve the ion retention rate and separation coefficient.

[0016] Optimization of separation effect by ultrasonic exfoliation. Kaolinite and montmorillonite are effectively exfoliated into single-layer or few-layer nanosheets after ultrasonic treatment. Single-layer or few-layer nanosheets have thinner thickness and greater flexibility, which can be more closely arranged on the surface of the filter membrane during the preparation of the separation membrane to form more uniform ion channels. For lithium and magnesium ions, due to the differences in ion radius and charge properties, they will be hindered to different degrees when passing through these ion channels, thereby improving the selectivity (separation coefficient) of the separation membrane to lithium and magnesium ions. At the same time, uniform ion channels also help to improve the ion retention rate and reduce the disordered permeation of ions.

[0017] Significant improvement of separation performance by cross-linking modification. New peaks appear in the infrared spectrum after adding different cross-linking agents, confirming that the cross-linking agent is successfully grafted between the layers. After the grafting of the cross-linking agent, the surface chemical properties and spatial structure of the nanosheets are changed. First, the specific functional groups carried by the cross-linking agent can interact with lithium and magnesium ions, and due to the differences in ion properties, the interaction strength and mode are different, thereby strengthening the selective recognition and separation ability of the ions and improving the separation coefficient. Second, cross-linking promotes the closer connection between nanosheets, building a more stable separation membrane structure. This stable structure can effectively block the disordered permeation of ions and improve the retention rate of lithium and magnesium ions.

[0018] Guarantee of separation effect by filter membrane loading. The surface of the microporous aqueous filter membrane is smooth and has no cross-sectional layered structure, and water molecules and salt ions can freely permeate. After uniformly loading the modified nanosheets on it, the smooth surface reduces the ion transmission resistance, helping the ions to smoothly reach the modified nanosheet layer and fully exert their selective separation function. At the same time, the good permeability of the filter membrane guarantees the ion transmission efficiency, avoiding the influence of the separation effect due to its own hindrance. This loading method ensures that the modified nanosheets stably exert their separation performance and continuously improve the high selectivity (separation coefficient), retention rate, and flux of the separation membrane to lithium and magnesium ions. BRIEF DESCRIPTION OF DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the accompanying drawings needed to be used in the embodiments or prior art description will be briefly introduced. Obviously, the accompanying drawings in the following description only constitute some embodiments of the present application, and for those skilled in the art, other drawings can also be obtained from the structures shown in the drawings without any creative effort.

[0020] Figure 1 (a) is a SEM morphology of kaolinite applied in the embodiment 1 of the present application, Figure 1 (b) is a SEM morphology of montmorillonite applied in the embodiment 5 of the present application.

[0021] Figure 2 (a), Figure 2 (b) and Figure 2 (c) are the morphologies of kaolinite nanosheets after exfoliation in the embodiment 1 of the present application; wherein, Figure 2 (a) is the distribution state of kaolinite nanosheets under 20000 times; Figure 2 (b) is the morphology of kaolinite nanosheets under 10000 times; Figure 2 (c) is the microstructure of kaolinite nanosheets under 100000 times, and the inset in the upper right corner is the corresponding selected area electron diffraction (SAED) pattern.

[0022] Figure 2 (d), Figure 2 (e) and Figure 2 (f) are the TEM morphologies of montmorillonite nanosheets after exfoliation in the embodiment 5 of the present application; Figure 2 (d) is the overall distribution of montmorillonite nanosheets under 20000 times; Figure 2 (e) is the image of montmorillonite nanosheets under 10000 times; Figure 2 (f) is the morphology of montmorillonite nanosheets under 100000 times, and the inset in the upper right corner is the corresponding SAED pattern.

[0023] Figure 3 (a) is the infrared spectrogram of the kaolinite modified separation membrane prepared in the embodiments 1-4 of the present application; Figure 3 (b) is the infrared spectrogram of the montmorillonite modified separation membrane in the embodiments 5-8 of the present application.

[0024] Figure 4 are the SEM of the microporous water system filter membrane used in each embodiment and the comparative example of the present application and the SEM of the modified separation membrane in the embodiment 1 and the embodiment 7; wherein, Figure 4 (a) is the SEM of the front surface (water permeable surface) of the microporous water system filter membrane; Figure 4 (b) is the SEM of the surface of the modified separation membrane in the embodiment 1; Figure 4(c) is a SEM image of the side (end surface) of the modified separation membrane in Example 1; Figure 4 (d) is a SEM image of the side (end surface) of the microporous water-based filter membrane; Figure 4 (e) is a SEM image of the surface of the modified separation membrane in Example 7; Figure 4 (f) is a SEM image of the side (end surface) of the modified separation membrane in Example 7. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present application will be clearly and completely described below with reference to the drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work fall within the scope of protection of the present application.

[0026] In addition, the technical solutions of the various embodiments of the present application can be combined with each other, but it must be based on the fact that a person skilled in the art can realize it. When the combination of technical solutions contradicts each other or cannot be realized, it should be considered that the combination of technical solutions does not exist and is not within the scope of protection required by the present application.

[0027] When the embodiments give numerical ranges, it should be understood that, unless otherwise stated by the present application, both endpoints of each numerical range and any number between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present application are used by those skilled in the art in the present technical field and in the description of the present application. Any method, equipment and material of the prior art similar or equivalent to the method, equipment and material of the embodiments of the present application can also be used to realize the present application.

[0028] The present application provides a preparation method of a modified separation membrane, comprising the steps of: S1. obtaining a mixed system of a mineral material and a polar solvent, wherein the mixed system is subjected to ultrasonic liquid phase exfoliation to obtain a to-be-treated liquid.

[0029] In the present application, the mineral material includes kaolinite and / or montmorillonite. Kaolinite and montmorillonite are natural two-dimensional layered clay minerals, and the nanosheet layers are connected by weak interaction forces such as hydrogen bonds or van der Waals forces. Ultrasonic waves are mechanical waves that can propagate in a liquid. By causing rapid expansion and collapse of tiny bubbles in the liquid between the nanosheet layers, the mutual separation between the layers is accelerated, the nanosheet is exfoliated, and single-layer or few-layer nanosheet materials are produced. In some embodiments, the mineral material can be passed through a 200-mesh sieve before being mixed with the polar solvent.

[0030] In the present application, the polar solvent includes one or more of water, ethanol and propylene glycol.

[0031] In the present application, the mass-volume ratio of the mineral material to the polar solvent can be 50-100 mg: 30-60 ml; for example, 50-80:30-40, or 60-70:30-50.

[0032] In the present application, the ultrasonic liquid phase exfoliation can be performed in an ultrasonic cleaner. In some embodiments, the ultrasonic conditions in the ultrasonic liquid phase exfoliation process are: ultrasonic power 300-500 W, exfoliation time 4-24 h; more specifically, the ultrasonic power can be 400-500 W, and the exfoliation time can be 16-24 h.

[0033] S2. Centrifugal treatment is performed on the mixed system, and the supernatant is collected to obtain a nanosuspension.

[0034] In the present application, the device used for centrifugal treatment can be a centrifuge. In some embodiments, the centrifuge speed in the centrifugal treatment process can be 3500-4000 rpm, and the time can be 2-5 minutes. For example, in the case of a speed of 3500 rpm, the time can be 3 minutes; in the case of a speed of 4000 rpm, the time can be 3 minutes.

[0035] S3. The crosslinking agent is mixed with the nanosuspension to obtain a modified liquid, the modified liquid containing modified nanosheets, and the mass of the crosslinking agent being 2%-30% of the mass of the mineral material.

[0036] In the present application, the crosslinking agent can be one or more of 1,3-propanediamine (TN), 1,6-hexanediamine (HDM), 1,9-nonanediamine (NMD), and 1,12-diaminododecane (DMD).

[0037] In some embodiments, the mass of the crosslinking agent can also be 2.5-20% of the mass of the mineral material; For example, the mass of the crosslinking agent can also be 2.5-5 wt%, or 2.5-7.5 wt%, or 2.5-10 wt%, or 2.5-15 wt%, or 5-15 wt%, or 5-20 wt%, or 10-20 wt%, or 2.5-20 wt% of the mass of the mineral material.

[0038] For example, the mass of the crosslinking agent can also be 2-3 wt%, or 4-6 wt%, or 7-8 wt%, or 9-11 wt%, or 14-16 wt%, or 19-21 wt% of the mass of the mineral material.

[0039] In some embodiments, after the crosslinking agent is mixed with the suspension, it can be placed on a magnetic stirrer to ensure successful crosslinking. In some specific embodiments, the speed of the magnetic stirring can be 200-400 rpm, and the time can be 0.5-2 h.

[0040] The Zeta potential of the modified nanosheet surface changes, the Zeta potential of the modified kaolinite nanosheet surface changes in the range of -48 mV to -19 mV, the Zeta potential of the modified montmorillonite nanosheet surface changes in the range of -39 mV to -23 mV, the surface potential of the unmodified kaolinite nanosheet is -52 mV, and the surface potential of the unmodified montmorillonite nanosheet is -42 mV.

[0041] S4. The modification liquid is filtered through a filter membrane, so that the modified nanosheet is uniformly loaded on the surface of the filter membrane to prepare a modified separation membrane.

[0042] In the present application, the filtration method can be vacuum filtration, and the negative pressure of the vacuum filtration is 0-0.1 MPa. In some specific embodiments, the detailed operation steps of the vacuum filtration method include: placing the filter membrane on the mouth of the filtration bottle, vacuum filtering to 0.1 MPa of negative pressure in the bottle, and pouring the nanosuspension into the bottle. Under the action of hydrogen bonding and electrostatic interaction force, the modified kaolinite / montmorillonite nanosheet is stacked layer by layer to prepare a layered modified separation membrane with good layered structure.

[0043] In the present application, the filter membrane can be a microporous water-based filter membrane.

[0044] In some embodiments, the pore size of the filter membrane can be 0.15-0.3 μm, such as 0.2-0.25 μm. For example, the pore size can be 0.22 μm.

[0045] In some embodiments, the material of the microporous water-based filter membrane can be mixed cellulose, and the diameter thereof can be 20-80 mm, such as 40-60 mm.

[0046] In some embodiments, the ratio between the mass of the modified nanosheet and the diameter of the microporous water-based filter membrane can satisfy 8-12 mg:50 mm.

[0047] In some embodiments, the loading amount of the modified nanosheet on the filter membrane can be 0.6-1.4 mg / cm 2 , such as 0.8-1.4 mg / cm 2 , or 0.6-1.2 mg / cm 2 , or 0.8-1.2 mg / cm 2 . It should be noted that the definition of the loading amount here is the ratio between the mass of the modified nanosheet and the effective loading area; wherein, the effective loading area is not equal to the area of the microporous water-based filter membrane, and the definition of the effective loading area is the effective membrane forming area of the mouth of the filtration bottle in the vacuum filtration device.

[0048] In other embodiments, the effective loading area of the modified separation membrane prepared by the present application can be 10-20 cm 2 , such as 12-13 cm 2; correspondingly, the mass of the nanosheets in the nanosuspension can be 6-28 mg.

[0049] The microporous water-based filter membrane applied in all embodiments of the present application is purchased from Tianjin Keyilong Experimental Equipment Co., Ltd.

[0050] The present application provides a modified separation membrane prepared by the preparation method of the modified separation membrane according to any one of the embodiments.

[0051] In the present application, the modified separation membrane comprises a filter membrane and modified nanosheets loaded thereon.

[0052] In some embodiments, the pore size of the filter membrane can be 0.15-0.3 μm, such as 0.2-0.25 μm. For example, the pore size can be 0.22 μm.

[0053] In some embodiments, the material of the microporous water-based filter membrane can be mixed cellulose, and the diameter thereof can be 20-80 mm, such as 40-60 mm.

[0054] In some embodiments, the ratio between the mass of the modified nanosheets and the diameter of the microporous water-based filter membrane can satisfy 8-12 mg: 50 mm.

[0055] In some embodiments, the loading amount of the modified nanosheets on the filter membrane can be 0.6-1.4 mg / cm 2 , such as 0.8-1.4 mg / cm 2 , or 0.6-1.2 mg / cm 2 , or 0.8-1.2 mg / cm 2 . It should be noted that the definition of the loading amount here is the ratio between the mass of the modified nanosheets and the effective loading area; wherein, the effective loading area is not equal to the area of the microporous water-based filter membrane, and the definition of the effective loading area is the effective membrane forming area of the bottle mouth of the vacuum filtration device.

[0056] In other embodiments, the effective loading area of the modified separation membrane prepared by the present application can be 10-20 cm 2 , such as 12-13 cm 2 ; correspondingly, the mass of the nanosheets in the nanosuspension can be 6-28 mg.

[0057] It should be noted that the filter membrane diameter, pore size, effective microporous water system filter membrane loading area of the modified separation membrane, and nanosheet mass in the above embodiments are only examples of a specific implementation. In actual applications, these parameters are not fixed and can be reasonably adjusted and optimized according to specific separation requirements, raw material characteristics, and actual production conditions. It has been verified in practice that as long as the preparation method of the present application is followed, the modified separation membrane prepared under different parameter combinations can also exhibit excellent separation performance and effectively separate target ions.

[0058] The present application provides a modified separation membrane prepared by the preparation method of the modified separation membrane as described above for application in salt lake brine treatment.

[0059] The present application provides a modified separation membrane for application in salt lake brine treatment.

[0060] In the present application, the salt lake brine can be treated by forward osmosis or reverse osmosis. In practice, both forward / reverse osmosis can be used. However, reverse osmosis has high energy consumption and poor ion retention effect. The modified separation membrane prepared in the present application has good forward osmosis performance; therefore, it is recommended to apply the modified separation membrane in the present application to forward osmosis, i.e., to separate wastewater by forward osmosis.

[0061] In some embodiments, the forward osmosis can be carried out by the following steps: injecting raw material liquid on one side of the U-shaped tube and injecting driving liquid on the other end. The modified separation membrane is placed in the middle membrane to separate them, the raw material liquid contacts one side of the modified separation membrane, and the other side of the modified separation membrane contacts the driving liquid. During the contact process, the osmotic pressure of the raw material liquid is lower than that of the driving liquid, and water molecules penetrate the modified separation membrane under the push of the osmotic pressure difference, but the interlayer structure of the membrane has different blocking effects on ions of different sizes / charge intensities, which provides a basis for selective separation of ions in wastewater.

[0062] In the present application, the concentration of magnesium ions in the salt lake brine can be 0.01-0.5 mol / L, such as 0.01-0.3 mol / L or 0.01-0.4 mol / L or 0.1-0.5 mol / L; the concentration of lithium ions in the salt lake brine can be 0.01-0.5 mol / L, such as 0.01-0.3 mol / L or 0.01-0.4 mol / L or 0.1-0.5 mol / L.

[0063] Compared with seawater desalination, there is no need to specially treat magnesium and lithium ions in the salt lake brine, there is no need to optimize the separation coefficient, and there is no technical problem to be solved in the present application, and the specific reasons are as follows: The difference in ion concentration is huge: the molar concentration of magnesium ions in seawater is usually not more than 50 mmol / L, and the molar concentration of lithium ions is usually not more than 0.01 mmol / L. The concentration of magnesium ions in salt lake brine is 0.01-0.5 mol / L, and the concentration of lithium ions is 0.01-0.5 mol / L. It can be seen that the concentration of lithium and magnesium ions in seawater is much lower than that in salt lake brine. In the process of seawater desalination, the main goal of which is to remove a large amount of salt to obtain fresh water, the content of lithium and magnesium ions in the numerous ions is extremely small, and even if the magnesium and lithium ions are not specially treated, the impact on the yield and quality of fresh water is minimal. However, the concentration of magnesium and lithium ions in salt lake brine is relatively high, and the separation of magnesium and lithium is the key to obtaining valuable lithium resources, so special treatment is required.

[0064] The core goal of seawater desalination is to significantly reduce the salt content (sodium chloride content) in seawater to meet the salinity, hardness and other indicators of fresh water. Magnesium and lithium ions are not the key focus of seawater desalination, and there is no problem of not being able to meet the production standards of fresh water due to the mutual influence of magnesium and lithium ions. However, in the field of lithium extraction from salt lake brine, due to the similar properties of magnesium and lithium ions, the presence of magnesium ions can seriously interfere with the extraction efficiency and purity of lithium in the process of extracting lithium, so it is necessary to optimize the separation coefficient of magnesium and lithium to solve this problem, which is one of the key technical problems to be solved by the present application.

[0065] In the present application, the modified separation membrane has a retention rate for lithium ions of not less than 90% and a separation rate for magnesium ions of not less than 95%, and the separation coefficient is greater than 1.5. The present application optimizes the separation coefficient of magnesium and lithium, which can on the one hand improve the extraction efficiency of lithium resources: in lithium-containing resource systems such as salt lake brine, magnesium and lithium ions often coexist and have similar properties, making separation difficult. Increasing the separation coefficient means that lithium ions can be more effectively separated from the magnesium-lithium mixed system, reducing the loss of lithium ions in the separation process, and allowing more lithium ions to enter the product phase, thereby improving the extraction efficiency of lithium resources and increasing the yield of lithium.

[0066] On the other hand, it can significantly improve the purity of lithium products: magnesium ions are one of the main impurity ions that affect the purity of lithium products. After the separation coefficient is increased, magnesium ions and lithium ions can be more completely separated, significantly reducing the content of magnesium ions in lithium products, meeting the strict requirements of high-end lithium products for high purity, and improving the application performance and market competitiveness of lithium products in the fields of batteries, pharmaceuticals and other fields.

[0067] It should be noted that the separation coefficient is usually used to measure the separation ability of the separation process for two different components, and the more it deviates from 1, the better the separation effect of the two components. In the present application, the separation coefficient is The calculation formula is: That is, for lithium ions and magnesium ions, if the retention rate of the membrane to magnesium ions is higher than that to lithium ions, it means that the relative content of lithium ions will increase and the relative content of magnesium ions will decrease on the permeation side, so will be greater than , and the separation coefficient will be greater than 1.

[0068] In order to facilitate those skilled in the art to further understand the present application, examples are given as follows: Example 1 Preparation of modified separation membrane: S1. 80 mg of kaolinite was added to 40 ml of water to obtain a mixed system; wherein the kaolinite was previously ground with a three-head grinder and passed through a 200-mesh fine sieve. The SEM morphology of the kaolinite is shown in Figure 1 (a), which has a significant laminar stacking structure.

[0069] The mixed system was subjected to ultrasonic liquid phase exfoliation to obtain a treated liquid; the ultrasonic power was set to 450 W, the exfoliation time was 20 h, and the uniform shaking interval was 2 h.

[0070] The TEM morphology of the kaolinite nanosheets after exfoliation is shown in Figure 2 (a), Figure 2 (b), and Figure 2 (c). Among them, Figure 2 (a) shows the distribution state of kaolinite nanosheets at a lower magnification, and a large number of nanosheets can be observed scattered in the field of view, showing irregular flaky morphology with certain size differences; Figure 2 (b) is the morphology of a single kaolinite nanosheet at a higher magnification, and the outline of the nanosheet can be clearly seen, with slightly irregular edges and a certain texture on the surface, indicating that the kaolinite has been successfully exfoliated into single-layer or few-layer nanosheets. Figure 2 (c) further magnifies the microstructure of the kaolinite nanosheet, and the inset in the upper right corner is the selected area electron diffraction (SAED) pattern, which shows regular diffraction spots, confirming that the kaolinite nanosheet has a good crystal structure and the exfoliation process has not seriously damaged its crystal integrity.

[0071] S2. The treated liquid was centrifuged using a freeze-drying centrifuge at a speed of 3500 rpm for 3 minutes, the wall residue was discarded, and the upper layer of nanosuspension with obvious Tyndall effect was taken. The mass concentration was calibrated using a UV spectrophotometer to establish a concentration-absorbance standard curve.

[0072] S4. 1,3-propanediamine (TN) was added to the nanosheet suspension and placed on a magnetic stirrer for 1 h of magnetic stirring to ensure successful crosslinking, obtaining a modified liquid, and the mass of the modified nanosheets in the modified liquid was 12 mg.

[0073] The experimental groups with cross-linking agent dosage of 2.5 wt%, 5 wt%, 7.5 wt% and 10 wt% of kaolinite respectively were set, and the application effects of the modified separation membranes prepared in each group were shown in Table 1.

[0074] S5. The modified liquid was filtered through the filter membrane by vacuum filtration method, and the modified nanosheets were uniformly loaded on the circular microporous water-based filter membrane to obtain the modified separation membrane.

[0075] The base membrane material was mixed cellulose with a diameter of 50 mm and a pore size of 0.22 μm, which was purchased from Tianjin Keyilong Experimental Equipment Co., Ltd., and the effective loading area of the membrane was 12.56 cm 2 , and the loading amount of the modified nanosheets on the filter membrane was about 12 mg.

[0076] Application of the modified separation membrane: The prepared modified separation membrane was subjected to a 4h forward osmosis experiment in a U-tube, and the water flux and the rejection rate of Li + , Mg 2+ ions were measured, and the separation coefficient was calculated: one side of the modified separation membrane was 100 ml of 0.1 mol / L LiCl and MgCl2 mixed solution (simulating salt lake brine) with the same concentration, and the other side was 100 mL of deionized water.

[0077] The modified separation membrane under the same preparation conditions was taken, and 100 mL of deionized water was filtered through the modified separation membrane from top to bottom under the condition of vacuum pump filtration, and the filtration flux of the modified separation membrane for water was measured, wherein the negative pressure in the bottle was 0.1 MPa.

[0078] Table 1 Ion rejection and water flux performance table of the modified separation membrane prepared under different cross-linking agent dosages Example 2 In this embodiment, only 1, 6-hexanediamine (HDM) was replaced by 1, 3-propanediamine (TN) compared with Example 1, and other conditions remained unchanged. The test results corresponding to different concentrations of 1, 6-hexanediamine (HDM) in this embodiment were shown in the following table: Table 2 Ion rejection and water flux performance table of the modified separation membrane prepared under different cross-linking agent dosages Example 3 In this embodiment, only 1, 9-nonanediamine (NMD) was replaced by 1, 3-propanediamine (TN) compared with Example 1, and other conditions remained unchanged. The test results corresponding to different concentrations of 1, 9-nonanediamine (NMD) in this embodiment were shown in the following table: Table 3. Ion rejection and water flux performance of modified separation membranes prepared at different dosages of cross-linking reagent Example 4 In this example, only 1,3-propanediamine (TN) was replaced by 1,12-diaminododecane (DMD) compared with Example 1, and other conditions remained unchanged. The corresponding test results of different concentrations of 1,12-diaminododecane (DMD) in this example are shown in the following table: Table 4. Ion rejection and water flux performance of modified separation membranes prepared at different dosages of cross-linking reagent The infrared spectrum images of the kaolinite modified separation membranes of Examples 1-4 are shown in Figure 3 (a).

[0079] Example 5 In this example, only kaolinite was replaced by montmorillonite compared with Example 1, and the reagent system was adjusted, and other conditions remained unchanged. The SEM morphology of montmorillonite is shown in Figure 1 (b), the TEM morphology of the exfoliated montmorillonite nanosheets is shown in Figure 2 (d), Figure 2 (e), Figure 2 (f). Figure 2 (d) shows the overall distribution of the montmorillonite nanosheets at a relatively low magnification, and it can be seen that the nanosheets are uniformly dispersed, and the morphology is also irregular sheet-shaped. Figure 2 (e) is an image of a single montmorillonite nanosheet at a higher magnification, and the detailed features of the nanosheet can be observed, and its surface is relatively flat, but there are some slight undulations, reflecting the structural characteristics of the montmorillonite nanosheet. Figure 2 (f) is the morphology of the montmorillonite nanosheet at a higher magnification, and the inset in the upper right corner is the corresponding SAED pattern, and the diffraction spots are clearly distinguishable, indicating that the exfoliated montmorillonite nanosheet still maintains a good crystal structure, and successfully realizes the exfoliation to a single layer or few-layer nanosheet.

[0080] In this example, different concentrations of 1,3-propanediamine (TN) were used, and the corresponding test results are shown in the following table: Table 5. Ion rejection and water flux performance of modified separation membranes prepared at different dosages of cross-linking reagent Example 6 In this example, only 1,3-propanediamine (TN) was replaced by 1,6-hexanediamine (HDM) compared with Example 5, and other conditions remained unchanged.

[0081] The corresponding test results of different concentrations of 1,6-hexamethylenediamine (HDM) in this embodiment are shown in the following table: Table 6 Ion rejection and water flux performance table of modified separation membranes prepared under different cross-linking agent dosages Example 7 In this embodiment, only 1,3-propanediamine (TN) is replaced by 1,9-nonanediamine (NMD) compared with Example 5, and other conditions remain unchanged. The corresponding test results of different concentrations of 1,9-nonanediamine (NMD) in this embodiment are shown in the following table: Table 7 Ion rejection and water flux performance table of modified separation membranes prepared under different cross-linking agent dosages Example 8 In this embodiment, only 1,3-propanediamine (TN) is replaced by 1,12-diaminododecane (DMD) compared with Example 5, and other conditions remain unchanged. The corresponding test results of different concentrations of 1,12-diaminododecane (DMD) in this embodiment are shown in the following table: Table 8 Ion rejection and water flux performance table of modified separation membranes prepared under different cross-linking agent dosages The infrared spectrum images of the montmorillonite modified separation membranes of Examples 5-8 are shown in Figure 3 (b).

[0082] Comparative Example 1 In this comparative example, no modified separation membrane is prepared (steps 1-4 are deleted), and the modified separation membrane is replaced by a microporous water system filter membrane, and other conditions remain unchanged.

[0083] The corresponding test results of the microporous water system filter membrane in this comparative example are shown in the following table: Table 9 Ion rejection and water flux performance table of microporous water system filter membranes Comparative Example 2 In this comparative example, no cross-linking agent is added in step 4 compared with Example 1, and other conditions remain unchanged.

[0084] The corresponding test results of the pure kaolinite membrane in this comparative example are shown in the following table: Table 10 Ion rejection and water flux performance table of pure kaolinite membranes Comparative Example 3 In this comparative example, no cross-linking agent is added in step 4 compared with Example 5, and other conditions remain unchanged.

[0085] The test results corresponding to the pure montmorillonite membrane in the present comparative example are shown in the following table: Table 11 Ion rejection and water flux performance table of pure montmorillonite membrane Comparative Example 4 In the present comparative example, only the crosslinking agent 1,3-propanediamine (TN) added in the fourth step in Example 1 was replaced by polyethyleneimine (PEI), and other conditions remained unchanged. The test results corresponding to different concentrations of polyethyleneimine (PEI) in the present comparative example are shown in the following table: Table 12 Ion rejection and water flux performance table of modified separation membrane prepared under different PEI dosages Comparative Example 5 In the present comparative example, only the crosslinking agent 1,3-propanediamine (TN) added in the fourth step in Example 5 was replaced by polyethyleneimine (PEI), and other conditions remained unchanged. The test results corresponding to different concentrations of polyethyleneimine (PEI) in the present comparative example are shown in the following table: Table 13 Ion rejection and water flux performance table of modified separation membrane prepared under different PEI dosages Analysis Example 1 It can be seen that: Figure 1 Kaolin and montmorillonite have typical two-dimensional layered structure and high stacking degree.

[0086] It can be seen that: Figure 2 After ultrasonic treatment, kaolin and montmorillonite are effectively exfoliated to obtain single-layer or few-layer nanosheets.

[0087] It can be seen that: Figure 3 After adding different crosslinking agents, new peaks appear on the infrared spectrum, indicating that the crosslinking agent is successfully grafted between the layers, and the modified separation membrane is successfully prepared.

[0088] It can be seen that: Figure 4 The surface of the microporous aqueous filter membrane is very smooth, the pore size is about 0.22 μm, and there is no layered structure on the cross section. Water molecules and salt ions can pass through freely. By depositing 12 mg of nanosheets on the base membrane, kaolin and montmorillonite membranes with thicknesses of 5.2 μm and 7.9 μm, respectively, can be prepared. Figure 4 SEM images of the microporous aqueous filter membrane used in each example and comparative example of the present application, and SEM images of the modified separation membranes in Example 1 and Example 7; Among them, Figure 4 (a) is the SEM image of the front surface (water permeable surface) of the microporous aqueous filter membrane; Figure 4(d) is the SEM image of the side surface (end surface) of the microporous water system filter membrane; (b) is the SEM image of the surface of the modified separation membrane in Example 1; Figure 4 (c) is the SEM image of the side surface (end surface) of the modified separation membrane in Example 1; Figure 4 (e) is the SEM image of the surface of the modified separation membrane in Example 7; Figure 4 (f) is the SEM image of the side surface (end surface) of the modified separation membrane in Example 7.

[0089] Through the test data in Examples 1-8, and comparing the data in Comparative Examples 1-5, it can be seen that: After adding different types and amounts of crosslinking agents, the flux, retention rate and separation coefficient of the kaolinite / montmorillonite modified separation membrane are different from those of the microporous water system filter membrane and the pure mineral membrane. Among them, the modified separation membrane added with 1,3-propanediamine (TN) and 1,6-hexanediamine (HDM) has a larger flux; the modified separation membrane added with 1,9-nonanediamine (NMD) and 1,12-diaminododecane (DMD) has a certain inhibition on the flux. The retention rate of all modified separation membranes for ions is more than 90%, which has good retention effect and is significantly improved compared with the retention rate in the comparative examples. The separation coefficient has a large difference in the examples, the kaolinite modified separation membrane has a maximum of 2.17 and a minimum of 1.66; the montmorillonite modified separation membrane has a maximum of 3.91 and a minimum of 2.29, which is significantly increased compared with the separation coefficient in the comparative examples, and lithium and magnesium ions can be efficiently separated.

[0090] In the above technical scheme of the present application, the above is only the preferred embodiment of the present application, and does not limit the patent scope of the present application, and any equivalent structural transformation made under the technical concept of the present application, or direct / indirect application in other related technical fields is included in the patent protection scope of the present application.

Claims

1. A method for preparing a modified separation membrane, characterized in that, Including the following steps: A mixture of mineral material and polar solvent is obtained, and the mixture is subjected to ultrasonic liquid phase exfoliation to obtain a liquid to be treated. The mass-volume ratio of the mineral material to the polar solvent is 50-100 mg: 30-60 ml. The liquid to be treated is centrifuged, and the supernatant is collected to obtain a nano suspension; The crosslinking agent is mixed with the nano suspension to obtain a modified liquid containing modified nanosheets, wherein the mass of the crosslinking agent is 2%-30% of the mass of the mineral material. The modified liquid is filtered through a filter membrane to uniformly load the modified nanosheets onto the surface of the filter membrane, thereby obtaining a modified separation membrane.

2. The method for preparing the modified separation membrane according to claim 1, characterized in that, The mineral material includes kaolinite and / or montmorillonite, and the polar solvent includes one or more of water, ethanol, and propylene glycol.

3. The method for preparing the modified separation membrane according to claim 1, characterized in that, The crosslinking agent includes one or more of 1,3-propanediamine, 1,6-hexanediamine, 1,9-nonanediamine, and 1,12-diaminododecane.

4. The method for preparing the modified separation membrane according to claim 1, characterized in that, The ultrasonic conditions during the ultrasonic liquid phase stripping process are: ultrasonic power 300-500W, stripping time 4-24h.

5. The method for preparing the modified separation membrane according to claim 1, characterized in that, The filtration method includes vacuum filtration, with a negative pressure of 0-0.1 MPa.

6. The method for preparing the modified separation membrane according to claim 1, characterized in that, The filter membrane includes a microporous aqueous filter membrane; the pore size of the filter membrane is 0.15-0.3 micrometers; The modified nanosheets were loaded onto the filter membrane at a rate of 0.6-1.4 mg / cm³. 2 .

7. The method for preparing the modified separation membrane according to claim 1, characterized in that, The mass of the crosslinking agent is 2.5%-20% of the mass of the mineral material.

8. A modified separation membrane, characterized in that, It is prepared by the method for preparing the modified separation membrane as described in any one of claims 1-7.

9. The application of the modified separation membrane as described in claim 8 in the treatment of salt lake brine.

10. The application of the modified separation membrane according to claim 9 in the treatment of salt lake brine, characterized in that, The concentration of magnesium ions in the salt lake brine is 0.01-0.5 mol / L, and the concentration of lithium ions in the salt lake brine is 0.01-0.5 mol / L. The modified separation membrane has a lithium ion rejection rate of not less than 90%, a magnesium ion separation rate of not less than 95%, and a separation coefficient greater than 1.5.

Citation Information

Patent Citations

  • Membrane additive, seawater desalination membrane as well as preparation method and application of seawater desalination membrane

    CN116116234A

  • Modifier, modified permeable membrane, and preparation method and application thereof

    CN116272391A

  • Two-dimensional montmorillonite modified film for extracting lithium from salt lake original brine as well as preparation method and application of two-dimensional montmorillonite modified film

    CN119075706A

Cited By

  • Preparation method of membrane, membrane, and method, device and method for measuring air inlet value of membrane

    CN121715067A