Process for preparing pure iron from red mud

Pure iron was prepared by leaching red mud with hydrochloric acid and oxalic acid, followed by photocatalysis and electrolysis. This method solved the problems of the complexity and environmental pollution associated with iron extraction from red mud, and achieved efficient, low-energy-consumption, and high-purity pure iron preparation.

CN121023588APending Publication Date: 2025-11-28ZHEJIANG INST OF ADVANCED MATERIALS SHU
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510968333.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-14
Publication Date
2025-11-28

AI Technical Summary

Technical Problem

Existing technologies for extracting iron from red mud suffer from problems such as high complexity, low extraction efficiency, high energy consumption, high cost, and serious environmental pollution.

Method used

Using Bayer red mud as raw material, pure iron is prepared through acid leaching with hydrochloric acid and oxalic acid, photocatalytic reaction, calcination and electrolysis. The process includes acid leaching, photocatalysis, thermal decomposition and electrolysis steps, and the iron element is separated and extracted.

Benefits of technology

It achieves simple, efficient, low-energy and low-cost extraction of iron from red mud, reduces environmental pollution, improves resource utilization, and the purity of pure iron can reach over 99 wt%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121023588A_ABST
    Figure CN121023588A_ABST
Patent Text Reader

Abstract

The invention relates to a process for preparing pure iron by using red mud, which is characterized in that the red mud is Bayer process red mud, i.e., solid waste residue formed by solid-liquid separation after aluminum oxide is dissolved out from bauxite through high temperature, high pressure and strong alkali in the process of producing aluminum oxide by adopting a Bayer process, so that the environmental burden caused by the Bayer process red mud can be solved; the method is beneficial for reducing carbon emission in the aspect of iron element extraction and promoting development of a green metallurgical technology, and is characterized by comprising the following steps: taking Bayer process red mud as a raw material, carrying out acid leaching on the Bayer process red mud to obtain a ferrous oxalate extract, calcining the ferrous oxalate to obtain iron oxide, and recycling the iron oxide. And dissolving the ferric oxide into a sulfuric acid solution to obtain a ferric sulfate solution, taking the ferric sulfate solution as an electrolyte in an electrolysis device, and obtaining electrolytic iron through the electrolysis device, so that the pure iron is prepared from the red mud.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of resource recycling, in particular to a process for preparing pure iron from red mud, wherein the red mud is the red mud produced by the Bayer process, i.e. the solid waste formed during the solid-liquid separation after the high-temperature high-pressure strong-alkali leaching of bauxite to produce alumina by the Bayer process, which is conducive to solving the environmental burden caused by the red mud and reducing carbon emissions and promoting the development of green metallurgical technology in the extraction of iron from red mud. BACKGROUND

[0002] Red mud is a strong alkaline solid waste produced in the process of alumina production, containing a large amount of valuable metal elements such as iron, aluminum, titanium, and scandium. Among them, iron is one of the metal elements with a higher content in red mud, which has great potential for recycling. The methods for preparing pure iron from red mud mainly include physical separation, reduction-magnetic separation, and wet extraction.

[0003] Physical separation method: This method usually includes magnetic separation and flotation technology, which separates iron minerals from other substances through physical action. This method is simple to operate and has low cost, but the separation effect is limited by the particle size and dissociation degree of iron minerals in red mud.

[0004] Reduction-magnetic separation method: This method reduces the iron oxide in red mud to magnetite by a reducing agent, and then separates the iron minerals by magnetic separation. This method can effectively improve the recovery rate of iron and the grade of iron concentrate, but requires high energy consumption and reducing agent consumption.

[0005] Wet extraction method: Wet extraction method uses acid or alkaline solution to leach red mud, so that iron elements are dissolved into the solution, and then iron is recovered by solvent extraction, ion exchange or precipitation. Wet extraction method can effectively treat red mud with low iron content.

[0006] Electrolysis method, as one of the wet preparation methods, has attracted widespread attention due to its simple process, low cost, less pollution, high purity of prepared iron, and low energy consumption. SUMMARY

[0007] The present application provides a process for preparing pure iron from red mud, wherein the red mud is the red mud produced by the Bayer process, i.e. the solid waste formed during the solid-liquid separation after the high-temperature high-pressure strong-alkali leaching of bauxite to produce alumina by the Bayer process, which is conducive to solving the environmental burden caused by the red mud and reducing carbon emissions and promoting the development of green metallurgical technology in the extraction of iron from red mud.

[0008] The technical solution of the present application is as follows:

[0009] The application discloses a process for preparing pure iron by using red mud, and belongs to the technical field of red mud utilization.

[0010] The process comprises the following steps:

[0011] Step 1, first-stage acid immersion: red mud obtained by a Bayer process is subjected to acid immersion pretreatment by using hydrochloric acid; after the acid immersion reaction is completed, the acid immersion solution is removed, and red mud filter residue is obtained;

[0012] Step 2, second-stage acid immersion: the red mud filter residue is subjected to acid immersion by using oxalic acid; after the acid immersion reaction is completed, the filter residue is removed by filtration, and a filtrate in which iron oxalate complexes are dissolved is obtained;

[0013] Step 3, photocatalytic reaction: the filtrate is subjected to a photocatalytic reaction under light, and FeC2O4 precipitate is obtained;

[0014] Step 4, thermal decomposition: the FeC2O4 precipitate is subjected to heating or calcination in a drying box, and Fe2O3 is obtained;

[0015] Step 5, electrolyte preparation: Fe2O3 is reacted with sulfuric acid to prepare an electrolyte with a pH value of 2-3 and a Fe 3+ concentration of not less than 50 g / L;

[0016] Step 6, electrolytic iron preparation: the electrolyte is subjected to electrolysis by using a graphite plate anode and a graphite plate cathode, so that Fe 3+ is deposited on the cathode graphite plate to form electrolytic iron, and thus pure iron is obtained.

[0017] In step 1, the concentration of the hydrochloric acid is 1 mol / L, the acid immersion reaction temperature is 25-60 DEG C, the proportion is not less than 3 ml of hydrochloric acid:1 g of red mud and not more than 6 ml of hydrochloric acid:1 g of red mud, and vacuum suction filtration is performed by using a filter membrane with a pore size of not more than 45 mu m.

[0018] In step 2, the acid immersion reaction temperature is 40-90 DEG C, and the concentration of the oxalic acid is not less than 2 mol / L; vacuum suction filtration is performed by using a filter membrane with a pore size of not more than 45 mu m.

[0019] In step 4, the heating temperature or the calcination temperature is 200 DEG C-800 DEG C.

[0020] In step 6, the electrolyte temperature is 40-95 DEG C, and the current density is controlled to be 50-2000 A / m 2 .

[0021] The technical effect of the present application is as follows: the process for preparing pure iron from red mud provided by the present application adjusts the red mud to be weakly acidic by first neutralizing the alkali in the red mud with hydrochloric acid, and then performs two-stage acid leaching with oxalic acid; the acid leaching solution is obtained after filtration, the acid leaching solution is irradiated with light to obtain ferrous oxalate, and the ferrous oxalate is separated from the acid leaching solution by filtration; the separated ferrous oxalate powder is calcined to obtain iron oxide, the obtained iron oxide is dissolved in sulfuric acid to form a ferric sulfate solution, and finally pure iron is prepared by electrolysis, so that pure iron is effectively separated and extracted from red mud, red mud is comprehensively utilized, environmental pollution is reduced, and resource utilization rate is improved. BRIEF DESCRIPTION OF DRAWINGS

[0022] Figure 1 The macroscopic morphology of ferrous oxalate in the first embodiment of the present application is shown.

[0023] Figure 2 The macroscopic morphology of ferrous oxalate after thermal decomposition in the first embodiment of the present application is shown.

[0024] Figure 3 The macroscopic morphology of electrolytic iron in the first embodiment of the present application is shown.

[0025] Figure 4 The microstructure of electrolytic pure iron in the first embodiment of the present application is shown. DETAILED DESCRIPTION

[0026] The present application will be described below in conjunction with the accompanying drawings Figures 1-4 and examples.

[0027] Figure 1 The macroscopic morphology of ferrous oxalate in the first embodiment of the present application is shown. Figure 2 The macroscopic morphology of ferrous oxalate after thermal decomposition in the first embodiment of the present application is shown. Figure 3 The macroscopic morphology of electrolytic iron in the first embodiment of the present application is shown. Figure 4 The microstructure of electrolytic pure iron in the first embodiment of the present application is shown. Figures 1 to 4 As shown in the reference, a process for preparing pure iron from red mud includes using Bayer process red mud as raw material, obtaining ferrous oxalate precipitate by acid leaching and photocatalysis of the Bayer process red mud, calcining the ferrous oxalate to obtain iron oxide, dissolving the iron oxide in a sulfuric acid solution to obtain a ferric sulfate solution, using the ferric sulfate solution as an electrolyte in an electrolysis device, and obtaining electrolytic pure iron by the electrolysis device, thereby realizing the preparation of pure iron from red mud.

[0028] It comprises the following steps: step 1, first-stage acid leaching: the bayer process red mud is pretreated by acid leaching with hydrochloric acid, and after the acid leaching reaction is completed, the acid leaching liquid is removed to obtain red mud filter residue; step 2, second-stage acid leaching: the red mud filter residue is subjected to acid leaching with oxalic acid, and after the acid leaching reaction is completed, the filter residue is filtered out to obtain a filtrate in which iron oxalate complex is dissolved; step 3, photocatalytic reaction: the filtrate is subjected to photocatalytic reaction under sunlight to obtain FeC2O4 precipitate; step 4, thermal decomposition: the FeC2O4 precipitate is placed in a drying box for heating or calcination to obtain Fe2O3; step 5, electrolyte preparation: Fe2O3 is reacted with sulfuric acid to prepare an electrolyte with a pH of 2-3 and a Fe 3+ Concentration of no less than 50 g / L; and step 6, electrolytic iron preparation: the electrolyte is subjected to electrolysis with a graphite plate anode and a graphite plate cathode, so that Fe 3+ Is deposited on the cathode graphite plate to form electrolytic iron.

[0029] In step 1, the concentration of hydrochloric acid is 1 mol / L, the acid leaching reaction temperature is 25-60 DEG C, the ratio is no less than 3 ml of hydrochloric acid: 1 g of bayer process red mud, and no more than 6 ml of hydrochloric acid: 1 g of bayer process red mud, and vacuum suction filtration is performed with a filter membrane with a pore size of no more than 45 mu m. In step 2, the acid leaching reaction temperature is 40-90 DEG C, the concentration of oxalic acid is no less than 2 mol / L, and vacuum suction filtration is performed with a filter membrane with a pore size of no more than 45 mu m. In step 4, the heating temperature or calcination temperature is 200 DEG C-800 DEG C. In step 6, the electrolyte temperature is 40-95 DEG C, and the current density is controlled to be 50-2000 A / m 2 .

[0030] The application provides a process and method for preparing high-purity iron from red mud, and belongs to the field of comprehensive utilization of resources. The red mud is a by-product of the electrolytic aluminum industry, and the total iron content in the red mud can reach 40%. However, the treatment of the red mud is difficult due to the high content of alkali and aluminum metal elements. The application first neutralizes the alkali in the red mud with hydrochloric acid, adjusts the red mud to be weakly acidic, and then performs two-stage acid leaching with oxalic acid. After filtration, the acid leaching liquid is subjected to ultraviolet irradiation to obtain ferrous oxalate, which is separated from the acid leaching liquid by filtration. The separated ferrous oxalate powder is calcined to obtain iron oxide, the obtained iron oxide is dissolved in sulfuric acid to form a ferric sulfate solution, and finally iron is prepared by electrolysis. The application can effectively separate and extract iron from the red mud, comprehensively utilize the red mud, reduce environmental pollution, and improve the resource utilization rate.

[0031] 1. The technical problem to be solved by the application

[0032] Complexity of red mud properties: The iron in red mud mainly exists in the form of hematite (Fe2O3), goethite (α-FeO(OH)), and magnetite (Fe3O4) minerals, which have fine particle sizes and are cemented with aluminum, silicon, and other elements, making iron extraction complex. Extraction efficiency: Although direct magnetic separation is simple, the recovery rate and grade of iron are often not high due to the particle size and dissociation degree of iron minerals in red mud. Energy consumption and cost: Although pyrometallurgical methods are effective, they usually have high energy consumption and may produce waste gas and other environmental problems during processing. Environmental impact: Traditional pyrometallurgical methods can produce a large amount of waste gas and waste residue, causing secondary pollution to the environment. Therefore, developing more environmentally friendly extraction methods, such as hydrometallurgy, is the future research direction.

[0033] In view of the problems of complexity of red mud extraction, low extraction efficiency, high energy consumption and cost, and large environmental pollution, the present application provides a process and method for preparing pure iron from red mud, which is simple, efficient, low in energy consumption and cost, and small in environmental pollution. The iron element is selectively extracted by oxalic acid, and reduced to iron single element by electrolysis, reducing the energy consumption of red mud treatment and improving the efficiency of red mud treatment.

[0034] 2. Technical solution

[0035] In order to achieve the above-mentioned purpose, the technical solution provided by the present application is as follows:

[0036] The process and method for preparing pure iron from red mud of the present application selects the industrial solid waste discharged during the extraction of alumina by the Bayer process, first uses 1 mol / L hydrochloric acid to perform one-stage acid leaching on the red mud, then retains the filter residue by filtration to reduce the interfering elements such as K and Na; performs two-stage leaching on the obtained filter residue with oxalic acid, and filters to obtain a filtrate; places the filtrate under light irradiation to make the photocatalysis produce FeC2O4 precipitate; places the FeC2O4 precipitate obtained by filtration into a drying box, dries to decompose FeC2O4 into Fe2O3; reacts the generated Fe2O3 with sulfuric acid to generate a ferric sulfate solution, and the solution can be electrolyzed to obtain electrolytic pure iron.

[0037] Preferably, the specific steps include:

[0038] Step one, one-stage acid leaching

[0039] The red mud produced by the Bayer process is pretreated with 1 mol / L hydrochloric acid, and the acid leaching liquid is removed;

[0040] Step two, two-stage acid leaching

[0041] The filter residue obtained in step one is subjected to two-stage acid leaching with oxalic acid, the reaction temperature is 40-90℃, the reaction time is until the reaction is completed, and the filtrate obtained by the reaction is collected.

[0042] Step three, photocatalytic reaction

[0043] The collected filtrate is placed under light for photocatalytic reaction, and a large amount of FeC2O4 precipitate is generated in the solution after light irradiation;

[0044] Step four, thermal decomposition

[0045] The precipitate is placed in a drying oven for drying to generate Fe2O3.

[0046] Step five, electrolyte configuration

[0047] The generated Fe2O3 is reacted with sulfuric acid to make the configured solution have a pH of 2-3, and the Fe 3+ Concentration of the solution is not less than 50g / L.

[0048] Step 6, preparation of electrolytic iron

[0049] The electrolyte is electrolyzed by using graphite plates as both anode and cathode to obtain pure iron.

[0050] 3. Beneficial effects

[0051] The technical scheme provided by the present application has the following remarkable effects:

[0052] The process and method for preparing pure iron from red mud provided by the present application have a complete set of technology and scheme. First, the red mud produced by the Bayer process is pretreated with 1mol / L hydrochloric acid to reduce the concentration of Na, K, Ca and other ions in the red mud, which is beneficial to the subsequent selective leaching of iron by oxalic acid. The light involved in the present application can accelerate the precipitation rate of FeC2O4, so that iron elements can be separated from the red mud, shortening the entire production process. The Fe2O3 generated by thermal decomposition can be used for the next step of electrolytic iron preparation, and the electrolytic iron prepared has a purity of more than 99wt%.

[0053] A method for preparing pure iron from red mud, comprising: first neutralizing the red mud with sufficient hydrochloric acid to remove excess alkali in the red mud, and then leaching Fe2O3 in the red mud with oxalic acid; filtering and separating the leached solution; placing the separated filtrate under sunlight to obtain ferrous oxalate; calcining the ferrous oxalate to obtain Fe2O3, adding the prepared Fe2O3 to dilute sulfuric acid to dissolve and enrich, generating Fe2(SO4)3 solution, and electrolyzing the solution to obtain pure iron.

[0054] The Fe2O3 content in the selected red mud should be not less than 20wt%, and the impurity elements in the red mud raw material do not need to be considered.

[0055] A sufficient amount of hydrochloric acid is used to neutralize the alkali in the red mud and adjust the pH value of the red mud to 5-7.

[0056] Fe2O3 and Al2O3 in the red mud are selectively leached by oxalic acid to obtain a leaching solution.

[0057] FeC2O4 precipitate is produced by light catalysis of the acid leaching solution by ultraviolet light, so that iron is selectively separated.

[0058] Fe2O3 is prepared by calcining FeC2O4 at a temperature not lower than 200℃ until water is completely evaporated.

[0059] Fe2O3 after calcination is prepared into a ferric sulfate solution with a pH of 2-3 and a Fe2O3 concentration not lower than 50g / L. 3+

[0060] Both the cathode and the anode in the electrolysis process are inert electrodes.

[0061] The electrolyte temperature in the electrolysis process is 40-95℃, and the current density is controlled to be 50-2000A / m 2 .

[0062] Example 1

[0063] In this example, a process for preparing iron from red mud produced by the Bayer process is mainly introduced, and the specific process parameters are set as follows:

[0064] The red mud prepared by the Bayer process is stirred and reacted with 1mol / L hydrochloric acid at 60℃ for 2h, the liquid-solid ratio is 4:1, then the filter membrane with a pore size of 45μm is used for suction filtration, the vacuum degree is 0.07Mpa, and the impurity ions are removed by repeatedly washing with deionized water during the filtration process. The red mud filter residue obtained by filtration is subjected to secondary acid leaching with 2mol / L oxalic acid, the liquid-solid ratio is 4:1, and the stirring and reaction are carried out at 60℃ for 2h. Then the filter membrane with a pore size of 45μm is used for suction filtration, the vacuum degree is 0.07Mpa, and the filtrate is irradiated under sunlight for 4h at this time, a large amount of ferrous oxalate is precipitated from the solution. Then the filter membrane with a pore size of 45μm is used for suction filtration, the vacuum degree is 0.07Mpa, and the impurity ions are removed by repeatedly washing with deionized water during the filtration process. The filtrate is added to the red mud filter residue and heated and stirred to react again, and the above steps are repeated twice to ensure that as much Fe2O3 as possible is dissolved out of the red mud filter residue. The ferrous oxalate obtained by washing and cleaning is dried at 200℃ for 2h, at this time the ferrous oxalate is thermally decomposed into Fe2O3. The obtained Fe2O3 is reacted with sulfuric acid, NaOH is added to adjust the pH to 3, and graphite electrodes are used for electrolysis, so that iron is deposited on the cathode, and the content of iron is more than 99wt%.

[0065] ​The content not described in detail in the specification of the present application belongs to the prior art known to the person skilled in the art. It is indicated here that the above description helps the person skilled in the art to understand the present application, but does not limit the protection scope of the present application. Any implementation of equivalent replacement, modification, improvement and / or deletion of the above description without departing from the essential content of the present application falls within the protection scope of the present application.

Claims

1. A process for preparing pure iron using red mud, characterized in that, The method involves using Bayer red mud as raw material, obtaining ferrous oxalate precipitate by acid leaching and photocatalytic reaction of the Bayer red mud, calcining the ferrous oxalate to obtain ferric oxide, dissolving the ferric oxide in sulfuric acid solution to obtain ferric sulfate solution, using the ferric sulfate solution as electrolyte in an electrolysis device, and obtaining electrolytic iron through the electrolysis device, thereby realizing the preparation of pure iron from red mud.

2. The process for preparing pure iron using red mud according to claim 1, characterized in that, Includes the following steps: Step 1, First stage of acid leaching: Bayer process red mud is pretreated with hydrochloric acid for acid leaching. After the acid leaching reaction is completed, the acid leaching solution is removed to obtain red mud filter residue. Step 2, second stage of acid leaching: The red mud filter residue is leached with oxalic acid. After the acid leaching reaction is completed, the filter residue is filtered out to obtain a filtrate containing dissolved oxalate iron complex. Step 3, photocatalytic reaction: The filtrate is placed under light to carry out a photocatalytic reaction, and FeC2O4 precipitate is obtained; Step 4, thermal decomposition: Place the FeC2O4 precipitate in a drying oven for heating or calcination to obtain Fe2O3; Step 5, Electrolyte preparation: React Fe₂O₃ with sulfuric acid to prepare an electrolyte solution with pH = 2-3 and Fe₂O₃ content of 40-50%. 3+ Electrolyte with a concentration of not less than 50 g / L; Step 6, Electrolytic Iron Preparation: Electrolyze the electrolyte using graphite plate anode and graphite plate cathode to produce Fe... 3+ Electrolytic iron is formed by depositing it on a cathode graphite plate, thereby producing pure iron.

3. The process for preparing pure iron using red mud according to claim 2, characterized in that, In step 1, the concentration of hydrochloric acid is 1 mol / L, the acid leaching reaction temperature is 25-60℃, and the ratio is no less than 3 ml hydrochloric acid: 1 g Bayer red mud and no more than 6 ml hydrochloric acid: 1 g Bayer red mud. Vacuum filtration is performed using a filter membrane with a pore size of no more than 45 μm.

4. The process for preparing pure iron using red mud according to claim 2, characterized in that, Step 2 involves acid leaching at a temperature of 40–90°C, with an oxalic acid concentration of at least 2 mol / L, and vacuum filtration using a filter membrane with a pore size no larger than 45 μm.

5. The process for preparing pure iron using red mud according to claim 2, characterized in that, The heating or calcination temperature in step 4 is 200–800℃.

6. The process for preparing pure iron using red mud according to claim 2, characterized in that, In step 6, the electrolyte temperature is 40–95℃, and the current density is controlled at 50–2000 A / m. 2 .

Citation Information

Cited By

  • Method for separating and enriching iron concentrate from red mud and co-producing polyaluminum ferric silicate flocculant

    CN122480078A