High-transparency Yb-doped yttrium gallium garnet laser ceramic as well as preparation method and application thereof
Highly transparent Yb-doped yttrium gallium garnet laser ceramics were prepared by a co-precipitation method and oxygen pre-calcination combined with hot isostatic pressing sintering, solving the preparation problem of highly transparent ceramics and realizing their application potential in the fields of ultrashort pulse lasers and broadband light sources. They have the characteristics of low cost and high performance.
Patent Information
- Application Number
- CN202511429922.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-30
- Publication Date
- 2025-12-16
AI Technical Summary
Existing technologies make it difficult to prepare highly transparent and low-cost Yb-doped yttrium gallium garnet laser ceramics, and their application potential in ultrashort pulse lasers and broadband light sources has not been fully realized.
Nanoparticle powders were prepared by co-precipitation and then high-transparency Yb-doped yttrium gallium garnet laser ceramics were prepared by oxygen pre-calcination combined with hot isostatic pressing. The volatilization of Ga ions and the distribution of Y ions were controlled to ensure accurate composition.
A Yb-doped yttrium gallium garnet transparent laser ceramic with high hardness, high transmittance, long excited-state energy level lifetime, and wide emission spectrum half-width at half maximum has been achieved. It has the advantages of simple preparation process and low cost, and is suitable for ultrashort pulse lasers and broadband light sources.
Smart Images

Figure CN121135376A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of transparent and optical functional ceramics, in particular to a high-transparency Yb-doped yttrium gallium garnet laser ceramic and its preparation and application. BACKGROUND
[0002] Yttrium gallium garnet (Y3Ga5O 12 As a homologous material of yttrium aluminum garnet (YAG), yttrium gallium garnet (Y3Ga5O12, YGG) continues the excellent physical properties of garnet structure, and has high hardness and high thermal conductivity, making it an ideal rare earth ion-doped matrix. When Yb 3+ ions are doped into the matrix to form Yb:YGG, the material exhibits unique energy level characteristics: the excited state energy level lifetime is 1.1 ms, the main emission peak is at 1025 nm, and the emission spectrum half-width can be expanded to 22 nm, which is four times higher than the spectrum width of traditional Yb:YAG at 1030 nm, significantly enhancing the spectral modulation capability.
[0003] A team from Shandong University successfully prepared high-performance Yb:YGG crystals using the optical floating zone method, and systematically studied the thermal mechanical properties and energy level characteristics (H. H. Yu, et al. IEEE J. Quantum Electron., 46 (2010) 1689-1695.). A team from Xi'an University of Electronic Science and Technology measured the absorption spectrum of the crystal at room temperature, which showed a double-peak characteristic: the main absorption peak was at 970 nm, and the absorption cross-section reached 2.71×10 -20 cm 2 , which matched well with the commercial high-power laser diode (LD) pumping source; a wide absorption band formed by the superposition of two secondary peaks at 930 nm and 944 nm appeared in the 940 nm band, and the corresponding absorption cross-sections were 1.33×10 -20 cm 2 and 1.10×10 -20 cm 2 (Y. Zhang, et al. Opt. Lett., 34 (2009) 3316-3318.). When pumped by 970 nm laser, the quantum loss of the crystal at the 1025 nm emission peak was as low as 5%, and combined with its 22 nm wide spectrum emission characteristics, it showed application potential in the fields of ultra-short pulse lasers and broadband light sources. SUMMARY
[0004] The present application provides a new type of high-transparency Yb-doped yttrium gallium garnet laser ceramic and its preparation method and application.
[0005] In one aspect, the present application provides a high-transparency Yb-doped yttrium gallium garnet laser ceramic, the composition of the ceramic is (Ybx Y 1-x )3Ga5O 12 wherein 0.001≤x≤0.2.
[0006] Preferably, x = 0.01-0.15.
[0007] Preferably, the linear transmittance of the ceramic at 1100 nm is ≥ 74%.
[0008] Preferably, the average grain size of the ceramic is 0.5-10 μm.
[0009] In another aspect, the present application provides a method for preparing the high-transparency Yb-doped yttrium gallium garnet laser ceramic as described above, comprising:
[0010] Step 1, preparing a raw material powder by co-precipitation according to a stoichiometric proportion of a solution;
[0011] Step 2, forming a ceramic green body after the raw material powder is formed;
[0012] Step 3, obtaining a ceramic pre-fired body after the ceramic green body is pre-fired in oxygen;
[0013] Step 4, obtaining a final ceramic after the ceramic pre-fired body is hot isostatic pressed and sintered.
[0014] Preferably, the primary particle size of the raw material powder in Step 1 is 80-780 nm.
[0015] Preferably, Step 1 comprises:
[0016] Step 1.1, taking a solution according to a stoichiometric proportion of the raw material powder, and uniformly mixing to obtain a mixed metal ion solution;
[0017] Step 1.2, mixing the mixed metal ion solution, a dispersing agent, and a precipitating agent to obtain a precipitating solution;
[0018] Step 1.3, obtaining the raw material powder after the precipitating solution is aged, washed, dried, sieved, and calcined.
[0019] Preferably, the raw material powder in Step 2 is dry-pressed at 4-6 MPa, and then cold isostatic pressed at 150-250 MPa to obtain the ceramic green body.
[0020] Preferably, the ceramic green body in Step 3 is pre-fired in oxygen at 1300-1600 °C to obtain the ceramic pre-fired body.
[0021] Preferably, the ceramic pre-fired body in Step 4 is hot isostatic pressed and sintered at 1500-1600 °C to obtain the final ceramic.
[0022] The technical scheme of the present application provides a Yb-doped yttrium gallium garnet transparent laser ceramic with high hardness, high transmittance, long excited state energy level lifetime and wide emission spectrum half-width, and a preparation method thereof. BRIEF DESCRIPTION OF DRAWINGS
[0023] Other features, objects, and advantages of the present application will become more apparent from the following detailed description of non-limiting embodiments thereof, read in conjunction with the accompanying drawings.
[0024] Figure 1 is an X-ray diffraction (XRD) pattern of the nano raw material powder prepared in Example 1 of the present application;
[0025] Figure 2 is a field emission scanning electron microscope (FESEM) morphology photo of the nano raw material powder prepared in Example 1 of the present application;
[0026] Figure 3 is an emission spectrum of the transparent laser ceramic (with a thickness of 1 mm) prepared in Example 1 of the present application;
[0027] Figure 4 is a photo of each transparent laser ceramic (with a thickness of 1 mm) prepared in Example 2 of the present application;
[0028] Figure 5 is the straight-line transmittance of each transparent laser ceramic (with a thickness of 1 mm) prepared in Example 2 of the present application. DETAILED DESCRIPTION
[0029] Example embodiments will now be described more fully with reference to the accompanying drawings. Example embodiments, however, can be implemented in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the concept of example embodiments to those skilled in the art, and the present application should only be defined by the appended claims. Like reference numerals refer to like elements throughout the specification. Repetitive descriptions of like elements will be omitted for sake of brevity.
[0030] Compared with single crystal materials, the (Yb x Y 1-x )3Ga5O 12 The transparent laser ceramic has the advantages of short preparation period, low cost, strong design control, etc., and does not require a high-temperature, high-purity environment for single crystal growth.
[0031] According to the development needs of ultra-short pulse laser gain medium materials, the present application provides a highly transparent Yb-doped yttrium gallium garnet laser ceramic and a preparation method thereof.
[0032] The embodiment of the present application discloses a Yb-doped yttrium gallium garnet transparent laser ceramic, which has a composition of (Yb x Y 1-x )3Ga5O 12 , wherein 0.001≤x≤0.2, preferably 0.01≤x≤0.15, and further preferably x=0.1.
[0033] The present application also provides a preparation method of the Yb:YGG transparent laser ceramic.
[0034] (1) According to the chemical composition, a certain concentration of metal ion salt solution containing metal ions Yb 3+ , Y 3+ and Ga 3+ is prepared, and the concentrations of the metal ions are calibrated by chemical analysis.
[0035] Then, the solution is taken according to the stoichiometric ratio of (Yb x Y 1-x )3Ga5O 12 , and the metal ion mixed solution is obtained after uniform mixing, wherein the concentration of cations in the metal ion mixed solution is preferably 0.01-2 mol / L.
[0036] Further, the solution is taken according to the stoichiometric ratio of (Yb x Y 1-x )3Ga 5(1+y) O 12 , wherein -0.006≤y≤0.006, which is used for further controlling the Ga content.
[0037] The Ga content is controlled mainly because the precipitation pH ranges of Y 3+ and Ga 3+ are different, and there is step-by-step precipitation, and Ga2O3 is easy to volatilize during powder calcination and ceramic sintering, and the reaction equation is Ga2O3→Ga2O+O2↑. Therefore, the stoichiometric ratio can be adjusted during the preparation of the powder, the influence of the Ga 3+ content on the preparation of YGG powder and ceramic is explored, the solution is taken according to the stoichiometric ratio of (Yb x Y 1-x )3Ga 5(1+y) O 12 , and the deviation of the components caused by the solubility product differences of different metal carbonates and metal hydroxides in the precipitation process and the washing process is effectively controlled.
[0038] (2) adding the mixed metal ion solution obtained in step (1) into the precipitant solution containing the dispersant, or adding the precipitant solution into the mixed metal ion solution containing the dispersant, and obtaining a precipitate solution after sufficient stirring. The stoichiometric ratio in step (1) effectively controls the deviation of components due to the difference in solubility product of different metal carbonates and metal hydroxides during the precipitation process and the washing process; and the end point pH value is 6-8;
[0039] The dispersant is preferably at least one of polyethylene glycol, ammonium sulfate, polyethylene imine, ammonium polyacrylate and ammonium citrate, and the content of the dispersant is preferably 0.1wt.%-5wt.%.
[0040] The precipitant is preferably at least one of ammonia, ammonium bicarbonate, oxalic acid and urea, and the concentration of the precipitant solution is preferably 0.01-4.0 mol / L.
[0041] (3) aging, washing, drying and sieving the precipitate solution obtained in step (2), and calcining the sieved powder at 500-1500°C for 1-10 hours to obtain the raw material powder.
[0042] Preferably, the precipitate solution is aged at 25°C for no more than 30 hours after the precipitation is completed.
[0043] Preferably, the precipitate is washed with deionized water and anhydrous ethanol. The washed precipitate is dried at 30-150°C for 10-100 hours, and the drying method is preferably at least one of oven drying, microwave drying and freeze drying. Then, the dried powder is sieved through a 60-300 mesh sieve to obtain the precursor powder. The precursor powder is calcined in air at 500-1500°C for 1-10 hours to obtain the raw material powder.
[0044] (4) dry pressing the nano raw material powder obtained in step (3) at 4-6 MPa, and then cold isostatic pressing at 150-250 MPa to obtain a ceramic green body;
[0045] (5) oxygen pre-sintering the ceramic green body in step (4) at 1300-1600°C to obtain a ceramic pre-sintered body; oxygen protection can inhibit the volatilization of Ga2O3, and the oxygen pre-sintering can obtain a preliminarily densified ceramic sample, and the relative density is preferably >90%.
[0046] Preferably, the holding temperature of the oxygen pre-sintering is 1300-1600°C, and the holding time is 3-20 hours.
[0047] (6) hot isostatic pressing sintering the ceramic pre-sintered body in step (5) at 1500-1600°C, which can remove the residual pores in the ceramic and further improve the relative density to obtain the final Yb:YGG transparent laser ceramic.
[0048] The holding temperature of the hot isostatic sintering is preferably 1500-1600 DEG C, the holding time is 3h, and the Ar gas pressure is 150-200 MPa.
[0049] The embodiment of the application prepares the nanometer raw material powder with good dispersing performance by the coprecipitation method, and then uses oxygen sintering combined with hot isostatic sintering as a sintering process to prepare the final ceramic. The embodiment of the application prepares the Yb:YGG ceramic with high transmittance by inhibiting the volatilization of Ga ions and the distribution and precipitation of Y ions, and has the advantages of simple preparation process and low cost, and can be applied to the fields of ultrashort pulse laser and broadband light source.
[0050] The application will be described below by specific examples and comparative examples:
[0051] Example 1
[0052] According to (Yb 0.1 Y 0.9 )3Ga5O 12 Chemical composition, respectively, 7.29ml concentration of 1.2344mol / L Yb(NO3)3 solution, 36.40ml concentration of 2.2252mol / L Y(NO3)3 solution and 96.16ml concentration of 1.5599mol / L Ga(NO3)4 solution into a beaker, first add a small amount of deionized water, uniform mixing, finally add deionized water to constant volume to 500ml.
[0053] Then prepare 640ml concentration of 1mol / L NH4HCO3 precipitant solution, and add 150ml concentration of 1mol / L (NH4)2SO4 dispersant solution. The metal ion mixed solution is dropped into NH4HCO3 precipitant at a drop rate of 20ml / min and fully stirred, and when the metal solution is dropped, it is aged at 25 DEG C for 30min.
[0054] The slurry after aging is washed with deionized water for 3 times, washed with anhydrous ethanol for 2 times, and the precipitate after washing is dried in an oven at 70 DEG C for 36h, and the dried powder is sieved through a 200 mesh sieve to obtain the precursor powder.
[0055] The precursor powder is calcined at 1100 DEG C in air for 4h to obtain the nanometer raw material powder.
[0056] The nanometer raw material powder is dry pressed and formed, and then cold isostatic pressed, and sintered in an oxygen furnace, with a holding temperature of 1575 DEG C and a holding time of 2h.
[0057] The pre-sintered body in the oxygen atmosphere is further sintered by hot isostatic pressing, with a holding temperature of 1550 DEG C, an Ar gas pressure of 180 MPa, and a holding time of 3h, and finally the sample is polished on both sides to obtain a chemical structural formula of (Yb 0.1Y 0.9 )3Ga5O 12 Transparent laser ceramics.
[0058] like Figure 1 As shown, the XRD diffraction peaks of the raw material powder are basically consistent with the peak positions of the YGG standard card, and no extra peaks were observed.
[0059] like Figure 2 As shown, the raw material powder has a worm-like morphology, and the primary particle size ranges from 80 to 780 nm.
[0060] like Figure 3 The image shows the emission spectrum of the final laser-emitted ceramic (1 mm thick) under 980 nm excitation. Upon testing, the obtained (Yb...) 0.1 Y 0.9 )3Ga5O 12 The transparent laser ceramic has an emission spectrum with a full width at half maximum (FWHM) of approximately 15 nm, a long excited-state lifetime of 0.85 ms, a Vickers hardness of HV 1148.5, and a thermal conductivity of approximately 2 W / (m·K).
[0061] Example 2
[0062] The preparation method is the same as in Example 1, except that in step 1, it is prepared according to (Yb x Y 1-x )3Ga 5(1+y) O 12 (Where x = 0.1, y = -0.06, -0.003, +0.003) Chemical composition, stoichiometric ratio, and measure the solution.
[0063] like Figure 4 and Figure 5 As shown, the optical quality is optimal at y = -0.003 (i.e., X = -0.003 in the figure), with the linear transmittance of the laser ceramic (1 mm thick) ≥ 74% at 1100 nm. To suppress compositional deviations caused by Ga volatilization or Y element precipitation, y = -0.003 effectively makes the final ceramic composition closest to (Yb... 0.1 Y 0.9 )3Ga5O 12 .
[0064] In summary, the embodiments of the present invention provide a Yb-doped yttrium gallium garnet transparent laser ceramic with high hardness, high thermal conductivity, high transmittance, long excited-state energy level lifetime, and wide emission spectrum half-width at half maximum. Its preparation method has the advantages of simple preparation process and low cost, and can be applied to the fields of ultrashort pulse lasers and broadband light sources.
[0065] The above is further detailed description of the present application in combination with specific preferred embodiments, and cannot be deemed as limitation of the specific implementation of the present application to these descriptions. For those skilled in the art to which the present application belongs, without departing from the concept of the present application, a number of simple deductions or substitutions can be made, and all of them shall be deemed as falling within the protection scope of the present application.
Claims
1. A highly transparent Yb-doped yttrium gallium garnet laser ceramic, characterized in that, The ceramic composition is (Yb x Y 1-x )3Ga5O 12 , where 0.001≤x≤0.
2.
2. The highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claim 1, characterized in that: The x = 0.01 to 0.
15.
3. The highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claims 1 and 2, characterized in that: The ceramic has a linear transmittance of ≥74% at 1100 nm.
4. The highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claims 1 and 2, characterized in that: The average grain size of the ceramic is 0.5–10 μm.
5. The method for preparing highly transparent Yb-doped yttrium gallium garnet laser ceramics according to claim 1, characterized in that: Step 1: Prepare a solution according to the stoichiometric ratio, and prepare raw material powder by co-precipitation; Step 2: After shaping the raw material powder, a ceramic blank is obtained; Step 3: After pre-firing the ceramic green body in oxygen, a pre-fired ceramic body is obtained; Step 4: After hot isostatic pressing, the pre-fired ceramic body is sintered to obtain the final ceramic.
6. The method for preparing highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claim 5, characterized in that: The primary particle size of the raw material powder in step 1 is 80-780 nm.
7. The method for preparing highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claim 5, characterized in that: Step 1 includes: Step 1.1: Measure the solution according to the stoichiometric ratio of the raw material powder, mix them evenly to obtain a mixed solution of metal ions; Step 1.2: Mix the metal ion mixed solution, dispersant, and precipitant to obtain a precipitate; Step 1.3: After aging, washing, drying, sieving, and calcining the precipitate, the raw material powder is obtained.
8. The method for preparing highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claim 5, characterized in that: In step 2, the raw material powder is dry-pressed at 4-6 MPa and then cold isostatically pressed at 150-250 MPa to obtain a ceramic blank.
9. The method for preparing highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claim 5, characterized in that: In step 3, the ceramic blank is pre-fired in oxygen at 1300-1600℃ to obtain a pre-fired ceramic body.
10. The method for preparing highly transparent Yb-doped yttrium gallium garnet laser ceramic according to claim 5, characterized in that: In step 4, the pre-fired ceramic body is subjected to hot isostatic pressing sintering at 1500-1600℃ to obtain the final ceramic.