Europium-doped silicate green fluorescent powder as well as preparation method and application thereof

By preparing europium-doped silicate green phosphors, the problem of high cost of green lasers in laser displays has been solved, achieving efficient narrow-spectrum green light emission and high thermal stability, thus improving the color gamut and luminous performance of laser displays.

CN121379576APending Publication Date: 2026-01-23LANZHOU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202511431163.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-10-09
Publication Date
2026-01-23

AI Technical Summary

Technical Problem

Current laser display technology faces challenges such as the high cost of green lasers and a lack of efficient semiconductor materials, making it difficult to achieve high color gamut displays.

Method used

A europium-doped silicate green phosphor with the chemical composition RbaKbNacLi12Si4O16:xEu2+ was developed and prepared by a two-stage high-temperature solid-state sintering method. It has a monoclinic crystal structure and narrow-spectrum green light emission characteristics, and is suitable for blue laser excitation.

Benefits of technology

It achieves high light conversion efficiency, narrow spectrum emission and high thermal stability, improves the color gamut and luminous lumen of laser displays, and is suitable for laser displays and white LED devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121379576A_ABST
    Figure CN121379576A_ABST
Patent Text Reader

Abstract

The invention provides europium-doped silicate green fluorescent powder as well as a preparation method and application thereof, and belongs to the technical field of luminescent materials. The green fluorescent powder can generate narrow-spectrum green light with the peak value located at 532 nm under excitation of 450 nm blue light, the full width at half maximum is 46 nm, a white light LED device prepared based on the fluorescent powder has a 110% NTSC color gamut, and it is indicated that the green fluorescent powder has excellent application value in backlight display. The saturation threshold value of the fluorescent powder reaches 21.6 W / mm < 2 > under the excitation of 450nm blue laser, and the lumen at the moment reaches 1157.9 lm. The green fluorescent powder disclosed by the invention has the advantages of high luminous efficiency, narrow full width at half maximum, high light saturation threshold under blue laser excitation, high lumen efficiency and the like, and has application feasibility in the aspect of laser display.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of luminescent materials, in particular to a europium-doped silicate green fluorescent powder and a preparation method and application thereof. BACKGROUND

[0002] Laser display is a new display technology with red, green and blue lasers as light sources. Color image display can be realized by controlling the intensity ratio and spatial distribution of the three primary colors. Due to the good directionality, good monochromaticity and high brightness of laser, laser display has unique advantages of high definition, large color gamut and high comfort. However, the current technology faces an important challenge: the high cost of green laser and the lack of a common semiconductor material to efficiently generate green laser, which hinders the development of full laser display technology.

[0003] In order to break through the technical bottleneck of green laser light source, researchers propose a technical scheme of using blue laser to excite fluorescent material. This technology has been applied in mainstream projection equipment, and its significant advantage is to reduce the number of lasers through fluorescence conversion mechanism, effectively avoiding the cost and preparation difficulty of high-performance green laser. Under the technical framework of "laser fluorescent powder", the performance of fluorescent powder is the core element to determine the final effect of laser display. The technology requires green fluorescent powder to have high light conversion efficiency, narrow spectrum emission spectrum and high laser stability. In view of the high cost of green laser, it is particularly important to develop suitable narrow-spectrum green fluorescent powder. Perovskite quantum dots (PQDs) have attracted attention due to their narrow-spectrum emission characteristics. For example, CsPbBr3 has an ultra-narrow emission spectrum, but its poor environmental stability and lead toxicity limit its practical application. Although β-SiAlON: Eu 2+ With suitable excitation and emission wavelengths, it has become a research hotspot, but its strict synthesis process and relatively wide emission half-width still cannot meet the demand of narrow-spectrum light spectrum for high color gamut laser display. Therefore, the development of new green fluorescent materials with narrow-spectrum emission, high thermal stability and easy preparation has become a key research direction in this field. SUMMARY

[0004] The purpose of the present application is to provide a europium-doped silicate green fluorescent powder and a preparation method and application thereof. The europium-doped silicate green fluorescent powder has a high saturation threshold and luminous flux under blue laser excitation, emits narrow-spectrum green light, has high thermal stability, and can meet the demand of high-performance laser display.

[0005] In order to achieve the above-mentioned purpose of the application, the present application provides the following technical solutions: The present application provides a europium-doped silicate green fluorescent powder, the chemical composition of which is: Rb a K b Na c Li 12Si4O 16 :xEu 2+ , wherein: 0.5≤a≤1, 1.5≤b≤2.5, 1≤c≤1.5, 0.01≤x≤0.15.

[0006] Preferably, a=0.6~0.9, b=1.6~2.4, c=1.1~1.4, x=0.03~0.12.

[0007] Preferably, the crystal structure of the europium-doped silicate green fluorescent powder is monoclinic system, and the space group is C 1 2 / m 1; the emission peak is located at 530~535nm, and the half-height width is 45~47nm.

[0008] The application provides a preparation method of the europium-doped silicate green fluorescent powder, and the preparation method comprises the following steps: According to the required stoichiometric ratio, the Rb compound, the K compound, the Na compound, the Li compound, the Si compound and the Eu compound are ground and mixed to obtain a mixture; The mixture is sequentially subjected to first sintering and second sintering in a reducing atmosphere to obtain the europium-doped silicate green fluorescent powder.

[0009] Preferably, the Rb compound, the K compound, the Na compound and the Li compound are independently the corresponding carbonates or nitrates of the elements; the Si compound comprises SiO2, and the Eu compound comprises Eu2O3.

[0010] Preferably, the reducing atmosphere is composed of 5~10% H2 and 90~95% N2 in terms of volume percentage.

[0011] Preferably, the temperature of the first sintering is 500~550℃, and the holding time is 1~3h; The temperature of the second sintering is 750~770℃, and the holding time is 4~8h.

[0012] Preferably, the heating rate for heating to the first sintering and the second sintering is independently 3~10℃ / min.

[0013] The application provides an application of the europium-doped silicate green fluorescent powder or the europium-doped silicate green fluorescent powder prepared by the preparation method in the field of laser display.

[0014] The application provides an application of the europium-doped silicate green fluorescent powder or the europium-doped silicate green fluorescent powder prepared by the preparation method in a white light LED device.

[0015] This invention provides a europium-doped silicate green phosphor, belonging to the monoclinic crystal system. The structure is mainly composed of LiO4 and SiO4 tetrahedra and Rb / K1O8 and Na / K2O8 cubes. The LiO4 and SiO4 tetrahedra are connected by sharing vertices or edges, forming a high-density lattice framework. Within this framework, Rb / K1 and Na / K2 ions are located in annular interstitial channels formed by the LiO4 and SiO4 tetrahedra. This rigid structural layout effectively reduces non-radiative transitions, thus theoretically providing excellent luminescence performance after activator doping. Eu... 2+ Na occupies a position in the material + The cell position. The reason is: due to Eu 2+ Ionic radius and Na + Ions with similar radii are more likely to exist stably in the structure, resulting in an overall energy level that tends to be the lowest. The cubic structures of Rb / K1O8 and Na / K2O8 are Eu... 2+ The doping provides a highly symmetrical environment, which gives it narrowband emission characteristics.

[0016] This phosphor emits a narrow-spectrum green light with a peak value around 532nm when excited by 450nm blue light, and has a full width at half maximum (FWHM) of 46nm. This green phosphor possesses advantages such as high luminous efficiency, narrow FWHM, high light saturation threshold under blue laser excitation, and high luminous efficiency, making it feasible for application in laser displays.

[0017] When this phosphor is used in backlight displays, the white LED device made based on this phosphor achieves a color gamut of 110% NTSC, indicating that it has excellent application value in backlight displays.

[0018] When this phosphor is used in laser displays, it is combined with a 450 nm blue laser to obtain a device. The optical saturation threshold and luminous flux are tested under 450 nm blue laser excitation. The phosphor achieves a saturation threshold of 21.6 W / mm² under 450 nm blue laser excitation. 2 At this point, the luminous flux reached 1157.9 lm. This indicates that the phosphor has excellent luminous flux and laser saturation threshold. Furthermore, based on the narrow-spectrum green emission characteristics of the phosphor, the color gamut of the laser display can be improved.

[0019] The present invention obtains the green phosphor by secondary high-temperature solid-state sintering, which is a simple method. Attached Figure Description

[0020] Figure 1 This is a schematic diagram of the crystal structure of the europium-doped silicate green phosphor of the present invention; Figure 2 XRD patterns of the green phosphors prepared in Examples 1-5 and comparison diagrams of the calculated XRD patterns are shown. Figure 3 Comparison chart of excitation spectrum of green phosphor prepared for example 1~5; Figure 4 Comparison chart of normalized emission spectrum of green phosphor prepared for example 3 and example 6; Figure 5 Comparison chart of emission spectrum of green phosphor prepared for example 1~5; Figure 6 Emission spectrum of green phosphor prepared for example 3; Figure 7 Chart of emission intensity of green phosphor prepared for example 3 changing with temperature; Figure 8 Emission spectrum of green phosphor prepared for example 3 under laser excitation; Figure 9 Variation of luminous flux of green phosphor prepared for example 3 with incident laser power density; Figure 10 Comparison chart of color gamut of white LED device prepared by using green phosphor (RKNLSO:Eu 2+ ) prepared for example 3, 450nm blue LED chip and commercial red phosphor K2SiF6: Mn 4+ (KSF:Mn 4+ ) in combination and standard color gamut. DETAILED DESCRIPTION

[0021] In the present application, if no special description, the required preparation raw materials or reagents are all the commercially available goods well known by the skilled in the art.

[0022] The present application provides a kind of europium doped silicate green phosphor, chemical composition is: Rb a K b Na c Li 12 Si4O 16 :xEu 2+ , wherein: 0.5≤a≤1, 1.5≤b≤2.5, 1≤c≤1.5, 0.01≤x≤0.15.

[0023] In the present application, a=0.6~0.9, more preferably a=0.7~0.8;B=1.6~2.3, more preferably b=1.8~2.0;C=1.1~1.4, more preferably c=1.2~1.3;X=0.03~0.12, more preferably x=0.04~0.09, further preferably x=0.06~0.08.

[0024] In the present application, the crystal structure of the europium doped silicate green phosphor is monoclinic system, and the space group isC 12 / m 1; emission peak is located at 530~535nm, and half-height width is 45~47nm.

[0025] The application provides a preparation method of the europium-doped silicate green fluorescent powder. According to a required stoichiometric ratio, Rb compound, K compound, Na compound, Li compound, Si compound and Eu compound are ground and mixed to obtain a mixture; The mixture is sequentially subjected to first sintering and second sintering in a reducing atmosphere to obtain the europium-doped silicate green fluorescent powder.

[0026] In the application, the Rb compound, K compound, Na compound and Li compound are independently preferably carbonates or nitrates corresponding to the respective elements; the Rb compound is more preferably Rb2CO3, the K compound is more preferably K2CO3, the Na compound is more preferably Na2CO3, and the Li compound is more preferably Li2CO3.

[0027] In the application, the Si compound preferably comprises SiO2, and the Eu compound preferably comprises Eu2O3.

[0028] In the application, the reducing atmosphere preferably consists of 5~10% H2 and 90~95% N2 in terms of volume percentage, and more preferably 5% H2 and 95% N2.

[0029] In the application, the mixture is preferably placed in an alumina crucible, put into a tube furnace, and subjected to first sintering in the tube furnace by introducing a reducing atmosphere, then cooled to room temperature, ground, and then subjected to second sintering in the tube furnace, then cooled to room temperature, and ground to obtain the europium-doped silicate green fluorescent powder.

[0030] In the application, the temperature of the first sintering is preferably 500~550℃, and more preferably 520~550℃, and the holding time is preferably 1~3h, and more preferably 2~3h.

[0031] In the application, the temperature of the second sintering is preferably 750~770℃, and more preferably 750~760℃, and the holding time is preferably 4~8h, and more preferably 5~6h.

[0032] In the application, the heating rate for heating to the first sintering and the second sintering is independently preferably 3~10℃ / min, and more preferably 5℃ / min.

[0033] The application does not have special limitations on grinding at different stages, and the material is ground uniformly according to a process well known in the art.

[0034] The application provides application of the europium-doped silicate green fluorescent powder in laser display.

[0035] The application provides application of the europium-doped silicate green fluorescent powder in backlight display.

[0036] The specific embodiments of the application are described in detail below, but it should be understood that the scope of protection of the application is not limited by the specific embodiments. Based on the examples in the application, all other examples obtained by those of ordinary skill in the art without creative labor are within the scope of protection of the application.

[0037] The experimental methods in the embodiments of the application are all conventional methods unless otherwise specified; the reagents and raw materials described below are all commercially available unless otherwise specified.

[0038] Example 1

[0039] According to the chemical formula Rb 0.5 K 2.5 NaLi 12 Si4O 16 : 0.03Eu 2+ The stoichiometric ratios of the elements in the chemical formula are as follows: 0.0577 g of Rb2CO3, 0.1727 g of K2CO3, 0.0514 g of Na2CO3, 0.4433 g of Li2CO3, 0.2403 g of SiO2 and 0.0053 g of Eu2O3 are weighed as raw materials; the raw materials are fully ground and uniformly mixed to obtain a mixture; the mixture is placed in an alumina crucible and then put into a tube furnace, a reducing atmosphere (N2:H2=95:5, volume ratio) is introduced, and the temperature is raised to 550 ℃ at a rate of 5 ℃ / min for calcination for 3 h, the furnace is cooled to room temperature, and the ground product is put into a tube furnace and then heated to 750 ℃ at a rate of 5 ℃ / min for calcination for 6 h in a reducing atmosphere (N2:H2=95:5, volume ratio), the furnace is cooled to room temperature, and the ground product is obtained as the final product.

[0040] Example 2

[0041] According to the chemical formula Rb 0.5 K 2.5 NaLi 12 Si4O 16 : 0.06Eu 2+To determine the stoichiometric ratio of each element, 0.0577g Rb₂CO₃, 0.1727g K₂CO₃, 0.0498g Na₂CO₃, 0.4433g Li₂CO₃, 0.2403g SiO₂, and 0.0105g Eu₂O₃ were weighed as raw materials. These raw materials were thoroughly ground and mixed evenly to obtain a mixture. The mixture was placed in an alumina crucible and then placed in a tube furnace. A reducing atmosphere (N₂:H₂ = 95:5, volume ratio) was introduced, and the temperature was raised to 550℃ at a rate of 5℃ / min for 3 hours. After cooling to room temperature with the furnace, the mixture was ground. The ground product was then placed in a tube furnace and calcined again in a reducing atmosphere (N₂:H₂ = 95:5, volume ratio) at a rate of 5℃ / min to 750℃ for 6 hours. After cooling to room temperature with the furnace, the mixture was ground to obtain the final product.

[0042] Example 3

[0043] According to the chemical formula Rb 0.5 K 2.5 NaLi 12 Si4O 16 0.09Eu 2+ The stoichiometric ratios of each element were determined by weighing 0.0577g Rb₂CO₃, 0.1727g K₂CO₃, 0.0482g Na₂CO₃, 0.4433g Li₂CO₃, 0.2403g SiO₂, and 0.0158g Eu₂O₃ as raw materials. The raw materials were thoroughly ground and mixed to obtain a homogeneous mixture. This mixture was placed in an alumina crucible and then placed in a tube furnace. A reducing atmosphere (N₂:H₂ = 95:5, volume ratio) was introduced, and the temperature was raised to 550℃ at a rate of 5℃ / min for 3 hours. The furnace was then cooled to room temperature, ground, and the ground product was placed back into the tube furnace and calcined again in a reducing atmosphere (N₂:H₂ = 95:5, volume ratio) at a rate of 5℃ / min to 750℃ for 6 hours. The furnace was then cooled to room temperature, ground, and the final product was obtained.

[0044] Example 4

[0045] According to the chemical formula Rb 0.5 K 2.5 NaLi 12 Si4O 16 0.12Eu 2+The stoichiometric ratios of each element were determined by weighing 0.0577g Rb₂CO₃, 0.1727g K₂CO₃, 0.0466g Na₂CO₃, 0.4433g Li₂CO₃, 0.2403g SiO₂, and 0.0211g Eu₂O₃ as raw materials. The raw materials were thoroughly ground and mixed to obtain a homogeneous mixture. This mixture was placed in an alumina crucible and then placed in a tube furnace. A reducing atmosphere (N₂:H₂ = 95:5, volume ratio) was introduced, and the temperature was raised to 550℃ at a rate of 5℃ / min for 3 hours. The furnace was then cooled to room temperature, ground, and the ground product was placed back into the tube furnace and calcined again in a reducing atmosphere (N₂:H₂ = 95:5, volume ratio) at a rate of 5℃ / min to 750℃ for 6 hours. The furnace was then cooled to room temperature, ground, and the final product was obtained.

[0046] Example 5

[0047] According to the chemical formula Rb 0.5 K 2.5 NaLi 12 Si4O 16 0.15Eu 2+ The stoichiometric ratios of each element were determined by weighing 0.0577g Rb₂CO₃, 0.1727g K₂CO₃, 0.0450g Na₂CO₃, 0.4433g Li₂CO₃, 0.2403g SiO₂, and 0.0264g Eu₂O₃ as raw materials. The raw materials were thoroughly ground and mixed to obtain a homogeneous mixture. This mixture was placed in an alumina crucible and then placed in a tube furnace. A reducing atmosphere (N₂:H₂ = 95:5, volume ratio) was introduced, and the temperature was raised to 550℃ at a rate of 5℃ / min for 3 hours. The furnace was then cooled to room temperature, ground, and the ground product was placed back into the tube furnace and calcined again in a reducing atmosphere (N₂:H₂ = 95:5, volume ratio) at a rate of 5℃ / min to 750℃ for 6 hours. The furnace was then cooled to room temperature, ground, and the final product was obtained.

[0048] Example 6

[0049] According to the chemical formula RbK2NaLi 12 Si4O 16 0.09Eu 2+The stoichiometric ratios of each element were determined by weighing 0.1154g Rb₂CO₃, 0.1382g K₂CO₃, 0.5299g Na₂CO₃, 0.4433g Li₂CO₃, 0.2403g SiO₂, and 0.0264g Eu₂O₃ as raw materials. The raw materials were thoroughly ground and mixed to obtain a homogeneous mixture. This mixture was placed in an alumina crucible and then placed in a tube furnace. A reducing atmosphere (N₂:H₂ = 95:5, volume ratio) was introduced, and the temperature was raised to 550℃ at a rate of 5℃ / min for 3 hours. The furnace was then cooled to room temperature, ground, and the ground product was placed back into the tube furnace and calcined again in a reducing atmosphere (N₂:H₂ = 95:5, volume ratio) at a rate of 5℃ / min to 750℃ for 6 hours. The furnace was then cooled to room temperature, ground, and the final product was obtained.

[0050] Characterization and performance testing

[0051] Figure 1 This is a schematic diagram of the crystal structure of the green phosphor matrix of the present invention. The phosphor matrix belongs to the monoclinic crystal system, and its structure is mainly composed of LiO4 and SiO4 tetrahedra and Rb / K1O8 and Na / K2O8 cubes. The LiO4 and SiO4 tetrahedra are connected by sharing vertices or edges, forming a high-density lattice framework. In this framework, Rb / K1 and Na / K2 ions are located in the annular interstitial channels formed by the LiO4 and SiO4 tetrahedra.

[0052] Figure 2 The images show the XRD patterns of the green phosphors prepared in Examples 1-5. Figure 2 The results show that the diffraction peaks of all the prepared green phosphors correspond one-to-one with the calculated diffraction peaks, and no other impurity peaks were observed. The results indicate that pure phases were successfully prepared from different components using the corresponding preparation methods.

[0053] Figure 3 The images show the excitation spectra of the green phosphors prepared in Examples 1-5. Figure 3 As can be seen, the excitation spectrum of this phosphor covers the ultraviolet to blue light region. It exhibits strong absorption in the blue light region, indicating that the phosphor can be effectively excited by blue laser light, meeting the application requirements of laser displays.

[0054] Figure 4 This is a comparison of the normalized emission spectra of the green phosphors prepared in Examples 3 and 6. From... Figure 4 As can be seen from Rb + Ions are gradually absorbed by K + With ion substitution, the cyan emission peak at 480 nm in the phosphor's emission spectrum gradually disappears, causing the phosphor to gradually transform into a narrow-band green emission, which is more conducive to its application in displays.

[0055] Figure 5 The emission spectrum of the green phosphor prepared in Example 3 is shown in Figure 3. It can be seen from Figure 3 that the emission spectrum of the phosphor is in the range of 450-600 nm under the excitation of 450 nm, and the emission peak is at 532 nm, indicating that the phosphor prepared in Example 3 emits green color. The half-peak width of the emission spectrum is 46 nm, indicating that the phosphor exhibits narrow-spectrum green emission. Figure 5

[0056] Figure 6 The emission spectrum of the green phosphor prepared in Example 3 is shown in Figure 3. It can be seen from Figure 3 that the emission spectrum of the phosphor is in the range of 450-600 nm under the excitation of 450 nm, and the emission peak is at 532 nm, indicating that the phosphor prepared in Example 3 emits green color. The half-peak width of the emission spectrum is 46 nm, indicating that the phosphor exhibits narrow-spectrum green emission. Figure 6

[0057] Figure 7 The emission spectrum of the green phosphor prepared in Example 3 is shown in Figure 3. It can be seen from Figure 3 that the emission spectrum of the phosphor is in the range of 450-600 nm under the excitation of 450 nm, and the emission peak is at 532 nm, indicating that the phosphor prepared in Example 3 emits green color. The half-peak width of the emission spectrum is 46 nm, indicating that the phosphor exhibits narrow-spectrum green emission. Figure 7

[0058] Figure 8 The emission spectrum of the green phosphor prepared in Example 3 is shown in Figure 3. It can be seen from Figure 3 that the emission spectrum of the phosphor is in the range of 450-600 nm under the excitation of 450 nm, and the emission peak is at 532 nm, indicating that the phosphor prepared in Example 3 emits green color. The half-peak width of the emission spectrum is 46 nm, indicating that the phosphor exhibits narrow-spectrum green emission. Figure 8

[0059] Figure 9 The emission spectrum of the green phosphor prepared in Example 3 is shown in Figure 3. It can be seen from Figure 3 that the emission spectrum of the phosphor is in the range of 450-600 nm under the excitation of 450 nm, and the emission peak is at 532 nm, indicating that the phosphor prepared in Example 3 emits green color. The half-peak width of the emission spectrum is 46 nm, indicating that the phosphor exhibits narrow-spectrum green emission.

[0060] Figure 10 The emission spectrum of the green phosphor prepared in Example 3 is shown in Figure 3. It can be seen from Figure 3 that the emission spectrum of the phosphor is in the range of 450-600 nm under the excitation of 450 nm, and the emission peak is at 532 nm, indicating that the phosphor prepared in Example 3 emits green color. The half-peak width of the emission spectrum is 46 nm, indicating that the phosphor exhibits narrow-spectrum green emission. 2 2+ 4+ 4+ ​​​​​​​A comparison image of the color gamut of a white LED device fabricated using a combination of [RKNLSO:Eu] and the standard color gamut, showing the green phosphor (RKNLSO:Eu). 2+ ) and commercial red phosphor K2SiF6:Mn 4+ (KSF:Mn) 4+ The mixing mass ratio of the phosphors was 1:1, indicating that the device achieved a color gamut of 110% NTSC. These results demonstrate the excellent performance of this phosphor in backlight displays.

[0061] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A europium-doped silicate green phosphor, characterized by, Chemical composition: Rb a K b Na c Li 12 Si4O 16 :xEu 2+ wherein: 0.5 < a < 1, 1.5 < b < 2.5, 1 < c < 1.5, 0.01 < x < 0.

15.

2. The europium-doped silicate green phosphor according to claim 1, characterized in that, a=0.6~0.9, b=1.6~2.4, c=1.1~1.4, x=0.03~0.

12.

3. The europium-doped silicate green phosphor according to claim 1, characterized in that, The crystal structure of the europium-doped silicate green fluorescent powder is monoclinic, and the space group is C 1 2 / m 1;the emission peak is located at 530-535 nm, and the half-height width is 45-47 nm.

4. The method for preparing the europium-doped silicate green phosphor according to any one of claims 1 to 3, characterized in that, comprising the following steps: Grinding and mixing Rb compound, K compound, Na compound, Li compound, Si compound and Eu compound in a desired stoichiometric ratio to obtain a mixture; The mixture is sequentially subjected to first sintering and second sintering in a reducing atmosphere to obtain the europium-doped silicate green fluorescent powder.

5. The preparation method according to claim 4, characterized in that, The Rb compound, K compound, Na compound, Li compound are independently carbonates or nitrates of the corresponding elements; the Si compound comprises SiO2, and the Eu compound comprises Eu2O3.

6. The preparation method according to claim 4, characterized in that, The reducing atmosphere consists of 5~10% H2 and 90~95% N2 by volume percentage.

7. The preparation method according to claim 6, characterized in that, The temperature of the first sintering is 500~550℃, and the holding time is 1~3h; The temperature of the second sintering is 750~770℃, and the holding time is 4~8h.

8. The preparation method according to claim 7, characterized in that, The heating rate for the first sintering and the second sintering is independently 3~10℃ / min.

9. Use of the europium-doped silicate green fluorescent powder of any one of claims 1~3 or prepared by the method of any one of claims 4~8 in the field of laser display.

10. Use of the europium-doped silicate green fluorescent powder of any one of claims 1~3 or prepared by the method of any one of claims 4~8 in white light LED devices.

Citation Information

Cited By

  • Flexible laser backlight panel integrated with laser fluorescence layer and preparation method thereof