Continuous casting method for high-purity rare earth modified high-precision cold-working die flat steel

By utilizing the in-situ reduction of the inner layer and the radial oxygen pumping mechanism of the functionally graded self-breathing electrochemical reaction immersion tube, atomic-level precise injection of rare earth elements and effective gas discharge are achieved, solving the problems of low rare earth yield and nozzle blockage, and improving the purity and impact toughness of the cast billet.

CN121467646APending Publication Date: 2026-02-06XINYU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511769879.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-28
Publication Date
2026-02-06

AI Technical Summary

Technical Problem

The existing rare earth mold steel continuous casting process suffers from low and fluctuating rare earth yield, easy generation of large-particle oxide inclusions leading to nozzle blockage, and structural cracking failure of large-size solid electrolyte reactors due to gas accumulation on the anode side.

Method used

A functionally graded self-breathing electrochemical reaction immersion tube is adopted. Rare earth atoms are generated in situ by reducing the inner rare earth precursor under the action of a DC electric field. A radial oxygen pumping mechanism is constructed by using the middle layer of dense solid electrolyte and the outer layer of porous anode to achieve atomic-level precise injection of rare earth and effective gas discharge. Combined with PLC linkage control, the rare earth injection rate and the steel flow rate are dynamically matched.

Benefits of technology

It improves rare earth recovery and compositional uniformity, reduces total oxygen content, solves the problems of nozzle nodule formation and blockage, ensures the continuity of continuous casting operations and the high purity of the billet, and enhances the transverse impact toughness of cold work die steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of metallurgical manufacturing, and discloses a continuous casting method of high-purity rare earth modified high-precision cold-working die flat steel, which comprises the following steps: S1, smelting to obtain clean die steel liquid, and injecting the clean die steel liquid into a tundish; s2, a functional gradient self-breathing electrochemical reaction immersion tube is installed at the bottom of the tundish; s3, an anode lead on the outer wall of the immersion pipe is connected to the positive electrode of a direct-current power source, and a conductive stopper rod in the tundish or an electrode inserted into molten steel is connected to the negative electrode of the direct-current power source; and S4, in the continuous casting process, the negative-pressure air extractor is started, direct-current voltage is applied, and the inner-layer rare earth precursor is driven to be subjected to a reduction reaction on the inner-layer interface of the molten steel to release rare earth atoms to enter the molten steel. The gradient electrochemical immersion pipe is coupled with negative pressure, rare earth in-situ injection and deep deoxidation are achieved, the rare earth yield and the molten steel purity are improved, nozzle nodulation is eliminated, and continuity and stability of continuous casting operation are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of metallurgical manufacturing, in particular to a continuous casting method of high-purity rare earth modified high-precision cold work die flat steel. BACKGROUND

[0002] High-precision cold work die flat steel is widely used in the manufacture of cold punch die, wire drawing die and other precision tooling, and it has very high requirements for the carbide distribution pattern, isotropy and transverse impact toughness of the material. Rare earth treatment is an effective means to improve the morphology of non-metallic inclusions in die steel, refine the solidification structure and thus improve the comprehensive performance of the material. At present, the method of feeding rare earth alloy cored wire at the end of ladle refining or at the tundish stage is usually used for rare earth treatment in industrial production.

[0003] However, due to the extremely active chemical properties of rare earth elements, in the traditional physical addition process, rare earth is prone to uncontrollable oxidation reaction with dissolved oxygen in the molten steel, top slag on the liquid surface or environmental atmosphere. This violent chemical reaction mechanism leads to generally low and large fluctuation range of rare earth element yield, making it difficult to achieve precise composition control in industrial continuous production. A large amount of high-melting-point rare earth oxides or oxysulfides generated by oxidation reaction are easily adsorbed and grown on the inner wall of the continuous casting submerged entry nozzle, causing serious nozzle clogging and blocking phenomenon, which not only limits the length of continuous casting casting, causes production interruption, but also causes flow field disorder in the crystallizer, inducing slag entrapment defects. In addition, part of the large particle rare earth inclusions that fail to timely float and remove remain in the billet, which will significantly destroy the continuity of the steel matrix, reduce the mirror polishing performance and fatigue life of the die steel.

[0004] Although the electrochemical metallurgy technology based on solid oxide film provides a new idea to solve the above problems, i.e. trying to control the migration of oxygen and alloying elements in situ by electrochemical method, in practical application, the gas transmission limitation in the thick-walled ceramic electrolyte structure becomes the key bottleneck restricting its industrialization. Specifically, in the high-temperature electrochemical reaction process, the oxygen generated at the anode side interface has a large physical diffusion resistance in the dense or thick-walled ceramic matrix. If an efficient gas release path cannot be established, the accumulated high-pressure gas will generate a huge stress in the ceramic matrix, causing structure delamination, cracking and even peeling, thus making the reaction device invalid, which is difficult to meet the stability requirements of long-period continuous casting. SUMMARY

[0005] In view of the deficiencies of the prior art, the present application provides a continuous casting method of high-purity rare earth modified high-precision cold work die flat steel, which solves the problems of low and large fluctuation range of rare earth yield in the existing rare earth die steel continuous casting process, easy production of large particle oxide inclusions leading to nozzle clogging and blocking, and structure cracking failure of large-size solid electrolyte reaction device due to gas accumulation at the anode side.

[0006] To achieve the above object, the present application is implemented by the following technical solutions:

[0007] In a first aspect, the present application provides a continuous casting method of high-purity rare earth modified high-precision cold work die flat steel, comprising the following steps:

[0008] S1, smelting to obtain clean die steel liquid, and injecting it into a tundish;

[0009] S2, installing a functional gradient self-breathing type electrochemical reaction immersion tube at the bottom of the tundish, the immersion tube having a three-layer gradient structure of an inner layer, an intermediate layer and an outer layer, the inner layer containing a rare earth precursor and a conductive phase, the intermediate layer being a dense solid electrolyte, and the outer layer being a porous anode;

[0010] S3, connecting the anode lead of the outer wall of the immersion tube to the positive electrode of a direct current power supply, and connecting the conductive stopper in the tundish or the electrode inserted into the steel liquid to the negative electrode of the direct current power supply; at the same time, connecting the exhaust passage of the flange end of the immersion tube to a negative pressure air extraction device;

[0011] S4, during the continuous casting process, starting the negative pressure air extraction device and applying a direct current voltage to drive the rare earth precursor in the inner layer to occur a reduction reaction at the inner layer interface of the steel liquid to release rare earth atoms into the steel liquid, and the oxygen ions generated at the same time migrate through the intermediate layer to the outer layer to lose electrons to combine into oxygen and be discharged.

[0012] By adopting the above technical solutions, the present application utilizes the coupling of the functional gradient material structure and the applied electric field to construct a dynamic reaction system integrating "in-situ reduction injection" and "radial oxygen pumping". The specific physical and chemical action mechanism is as follows:

[0013] Cathode in-situ reduction mechanism: under the action of the direct current electric field, electrons flow to the steel liquid through the conductive stopper, so that the interface where the steel liquid contacts the inner layer of the immersion tube maintains a cathode potential. The rare earth precursor (such as cerium zirconate or lanthanum aluminate) in the inner layer obtains electrons to occur a reduction reaction at the interface, and the rare earth ions are converted into atomic rare earth which directly dissolves into the steel liquid flowing through the immersion tube. This in-situ injection at the atomic level avoids the problem of excessively high local concentration during traditional alloy core wire addition, and reduces the risk of secondary oxidation of rare earth and air or slag layer contact.

[0014] Solid electrolyte oxygen pumping mechanism: the oxygen ions generated by the decomposition of the rare earth precursor and the original oxygen ions in the steel liquid migrate to the outer wall under the driving of the radial electric field gradient, passing through the intermediate layer composed of dense yttria stabilized zirconia. The intermediate layer as an excellent oxygen ion conductor only allows oxygen ions to pass through, thereby physically blocking the penetration of the steel liquid to the outside, and also preventing the diffusion of the external atmosphere to the steel liquid.

[0015] Anode gas diffusion and exhaust mechanism: oxygen ions migrated to the outer layer lose electrons to form oxygen molecules at the porous anode interface. Because the outer layer has a porous structure and is connected to a negative pressure exhaust device, the generated oxygen is quickly removed, preventing gas accumulation at the electrode interface, which can cause an increase in polarization overpotential or gas resistance circuit, thereby ensuring the continuous and stable progress of the electrochemical reaction.

[0016] Preferably, in step S4, the control range of the direct current voltage is 2.5V-3.8V, the exhaust pressure of the negative pressure exhaust device is controlled between -5kPa and -10kPa, and the casting speed is controlled between 0.8m / min and 1.2m / min.

[0017] By controlling the voltage in the range of 2.5V-3.8V, the electrolyte resistance and interface reaction overpotential can be overcome to drive the reaction, while avoiding excessive voltage that can cause electrolyte structure breakdown or side reactions. Controlling the negative pressure between -5kPa and -10kPa can establish an effective pressure gradient, accelerating the desorption and discharge of oxygen on the anode side and reducing concentration polarization. The limitation of the casting speed ensures that the molten steel flows through the reaction zone for an appropriate time, ensuring sufficient rare earth injection and reaction efficiency.

[0018] Preferably, in step S4, the application of direct current voltage and the continuous casting process adopts a PLC linkage control mode: a linear correspondence model of preset casting speed and voltage is established, and the actual casting speed signal of the continuous casting machine is collected in real time; when the casting speed increases, the PLC control system controls the direct current power supply to linearly increase the output voltage; when the casting speed decreases, the PLC control system controls the direct current power supply to linearly decrease the output voltage, so as to maintain the constant rare earth injection amount per unit volume of molten steel.

[0019] By adopting the above technical solution, the problem of uneven rare earth content caused by casting speed fluctuation in the non-steady state casting stage (such as starting, changing the package, and ending) is solved. According to Faraday's law, the electrolysis reaction rate is proportional to the current (driven by voltage), and by coupling the voltage and casting speed (i.e. molten steel flow) through PLC, the dynamic synchronization matching of rare earth injection rate and molten steel flow is realized, thereby obtaining uniform rare earth content distribution and stable modification effect in the entire length direction of the casting blank.

[0020] Preferably, in step S2, the functional gradient self-breathing type electrochemical reaction immersion tube is made of the following raw materials:

[0021] The inner layer is made of raw materials containing the following weight parts:

[0022] Yttria-stabilized zirconia powder: 550-650 parts;

[0023] Rare earth precursor: 250-350 parts;

[0024] Zirconium carbide powder: 50-100 parts;

[0025] The intermediate layer is made of raw materials including the following parts by weight:

[0026] Yttria stabilized zirconia powder: 1000 parts;

[0027] The outer layer is made of raw materials including the following parts by weight:

[0028] Yttria stabilized zirconia powder: 400-500 parts;

[0029] Lanthanum strontium manganite powder: 400-500 parts;

[0030] Pore-forming agent: 0-200 parts.

[0031] By adopting the above technical solution, zirconium carbide is introduced into the inner layer formula as a conductive reinforcing phase, which cooperates with the zirconia matrix to not only ensure the electronic conductivity at high temperature to maintain the cathode reaction, but also reduce thermal stress cracking by being similar to the thermal expansion coefficient of the intermediate layer material. The intermediate layer uses pure yttria stabilized zirconia to ensure the density and pure oxygen ion conductivity, preventing electronic short circuit. The outer layer introduces lanthanum strontium manganite as an electronic conductive phase and a catalyst to promote the oxygen ion precipitation reaction, and the porous structure formed by the pore-forming agent optimizes the gas transmission path.

[0032] Preferably, the rare earth precursor is one of cerium zirconate powder or lanthanum aluminate powder; the cerium zirconate powder is synthesized by mixing cerium oxide and zirconium oxide at a molar ratio of 1:1 and calcining at 1450°C; and the lanthanum aluminate powder is synthesized by mixing lanthanum oxide and aluminum oxide at a molar ratio of 1:1 and calcining at 1500°C.

[0033] By adopting the above technical solution, zirconium cerate or lanthanum aluminate synthesized at high temperature is selected as the rare earth source, which has better chemical stability in a high-temperature steel liquid environment than directly using simple oxides, has less tendency to decompose under thermal shock, and only selectively dissociates under the drive of an electric field. This characteristic significantly improves the controllability of the process, i.e., "power on to react, power off to stop", achieving precise control of the timing of adding rare earths.

[0034] Preferably, in step S2, during the preparation of the immersion tube, when filling the outer layer raw material, a plurality of polymethyl methacrylate microrods with a diameter of 0.5mm-1.0mm are vertically inserted along the axial direction, the microrods are uniformly distributed in the circumference and the top ends extend to the flange end face, and after sintering, a through exhaust passage is formed.

[0035] By adopting the technical scheme, the macro-scale directional exhaust passage is prefabricated outside the dense ceramic matrix by using the residue-free high-temperature decomposition characteristics of polymethyl methacrylate (PMMA), and the passage serves as a 'highway' for gas convergence, efficiently collects the oxygen generated in the porous structure and guides the oxygen to the flange exhaust port, thereby fundamentally solving the problem that the internal gas diffusion resistance of the thick-wall ceramic material is large and the structure is prone to peeling failure.

[0036] Preferably, in the step S2, the sintering process of the immersion tube is as follows: heating to 600 DEG C at a rate of 1 DEG C / min and keeping the temperature to remove organic matter; passing argon protection, heating to 1500 DEG C-1600 DEG C at a rate of 2 DEG C / min-3 DEG C / min and keeping the temperature for 6-8 hours, and cooling with the furnace; the forming mode of the immersion tube is cold isostatic pressing, the forming pressure is 200 MPa-250 MPa, and the pressure maintaining time is 5-10 minutes.

[0037] By adopting the technical scheme, the staged temperature rising and glue removal process ensures the stable volatilization of the pore forming agent and the binder, and avoids the cracking of the blank. The high-temperature argon sintering ensures the complete grain development of the zirconia and the precursor material, forms the high-strength ceramic bond, and prevents the oxidation of zirconium carbide and other non-oxide components. The cold isostatic pressing forming provides isotropic densification pressure, so that the multilayer gradient structure is tightly combined, the interface has no delamination defects, and can withstand the flushing and thermal shock of molten steel.

[0038] Preferably, in the step S1, the smelting process for obtaining the clean mold steel liquid includes arc furnace preliminary smelting, ladle refining furnace refining and vacuum degassing treatment in sequence, and the liquid overheat degree is controlled in the range of 20 DEG C-40 DEG C; in the step S4, the continuous casting process is carried out in the crystallizer by applying electromagnetic stirring, the electromagnetic stirring current is controlled to be 250 A-350 A, and the frequency is controlled to be 2 Hz-4 Hz; and the specific water amount of the secondary cooling zone is controlled to be 0.4 L / kg-0.6 L / kg.

[0039] By adopting the technical scheme, the preceding refining and vacuum treatment reduce the basic total oxygen content of the liquid steel to a very low level, reduce the load of electrochemical deoxidization, and enable the electrochemical system to focus more on the accurate alloying of rare earth. The subsequent electromagnetic stirring and secondary cooling control, in cooperation with the grain refining effect of rare earth, further break the dendrites and eliminate the center segregation, so that the continuous casting blank obtains a dense, uniform equiaxed crystal structure.

[0040] The application provides a continuous casting method of a high-purity rare earth modified high-precision cold work die flat steel.

[0041] The application has the following beneficial effects:

[0042] 1. The present application realizes the atomic-level precise injection of rare earth by electrochemical in-situ reduction technology, improves the rare earth yield and composition uniformity. Compared with the traditional feeding alloy cored wire process, the present method uses the inner layer interface of the immersion tube as the reaction site, directly reduces the rare earth precursor to atomic state rare earth dissolved in the flowing steel liquid, avoiding the oxidation loss caused by the contact of rare earth with air or slag during the adding process. The polarization voltage is adjusted in real time according to the withdrawal speed by the PLC control system, realizing the dynamic matching of the rare earth injection rate and the steel liquid flow, so that the rare earth yield in the whole continuous casting process is stably above 92%, and the rare earth distribution deviation along the length direction of the billet is extremely small.

[0043] 2. The present application realizes the simultaneous performance of rare earth alloying and deep deoxidation of steel liquid by constructing radial oxygen ion transport channels, and improves the steel liquid purity. Under the driving of direct current electric field, the intermediate dense solid electrolyte layer forces the oxygen ions generated by the rare earth reduction reaction and the original free oxygen ions in the steel liquid to migrate to the outside of the immersion tube and discharge from the system. This mechanism blocks the generation of a large amount of rare earth oxide inclusions from the source, so that the total oxygen content of the final billet can be controlled at about 5ppm, and the residual trace inclusions show the characteristics of fine and dispersed distribution, thereby significantly improving the transverse impact toughness of cold work die steel.

[0044] 3. The present application solves the common nozzle clogging and blocking problem in the rare earth continuous casting process, ensuring the continuity of continuous casting operation. Since the rare earth is in-situ reduced and enters at the last stage of the steel liquid flowing through the immersion tube, the steel liquid does not contain high active rare earth elements before entering the nozzle, so there is no prerequisite for a large amount of high melting point rare earth oxides to accumulate on the inner wall of the nozzle. At the same time, the inner wall of the immersion tube maintains a cathodic polarization state, and the interface electrochemical environment inhibits the adsorption of non-metallic inclusions. In addition, the special micropore exhaust channel of the outer layer of the immersion tube effectively releases the gas generated by the anodic reaction, prevents the ceramic matrix from cracking and peeling due to high internal gas pressure, and prolongs the service life of the key refractory materials. DETAILED DESCRIPTION

[0045] The main raw materials and reagents used in the following examples and comparative examples are as follows, and the reagents not specifically explained are commercially available analytical pure or higher grade products.

[0046] Yttria-stabilized zirconia powder (8YSZ), CAS No. 114168-16-0, yttria doping amount is 8mol%, crystal phase structure is cubic phase, purity is greater than 99.9%, average particle size D50 is 0.5μm to 1.0μm.

[0047] Zirconium carbide powder, chemical formula ZrC, CAS No. 12070-14-3, purity is greater than 99.5%, average particle size D50 is 1.0μm to 3.0μm.

[0048] Cerium oxide powder, CAS No. 1306-38-3, purity greater than 99.95%, average particle size D50 of 1.0 to 3.0 pm.

[0049] Zirconium oxide powder, CAS No. 1314-23-4, purity greater than 99.9%, monoclinic phase, average particle size D50 of 0.5 to 2.0 pm.

[0050] Lanthanum oxide powder, CAS No. 1312-81-8, purity greater than 99.99%, average particle size D50 of 1.0 to 3.0 pm.

[0051] Aluminum oxide powder, CAS No. 1344-28-1, purity greater than 99.99%, alpha phase, average particle size D50 of 0.3 to 0.5 pm.

[0052] Preparation Example 1-3:

[0053] Preparation Example 1:

[0054] The present preparation example provides a functional gradient self-breathing electrochemical reaction immersion tube, the preparation of which comprises the following steps:

[0055] Synthesis of rare earth precursor powder:

[0056] The cerium oxide powder and the zirconium oxide powder are mixed in a molar ratio of 2:2, ball-milled in a planetary ball mill for 24 hours with anhydrous ethanol as the medium, dried, placed in a high-temperature furnace, calcined at 1450°C for 12 hours in an air atmosphere, ground after natural cooling, and sieved to obtain cerium zirconate powder with an average particle size D50 of 2.5 pm as the active B component.

[0057] Preparation of layered powder:

[0058] Inner layer powder: 600 g of yttria-stabilized zirconium oxide powder, 300 g of cerium zirconate powder prepared in step (1), and 50 g of zirconium carbide powder are weighed, 50 g of polyvinyl alcohol aqueous solution (concentration 5 wt%) is added, uniformly mixed and sieved and granulated;

[0059] Middle layer powder: 1000 g of yttria-stabilized zirconium oxide powder is weighed, 50 g of polyvinyl alcohol aqueous solution (concentration 5 wt%) is added, uniformly mixed and sieved and granulated;

[0060] Outer layer powder: 450 g of yttria-stabilized zirconium oxide powder, 450 g of lanthanum strontium manganite powder, and 100 g of spherical graphite powder are weighed, 50 g of polyvinyl alcohol aqueous solution (concentration 5 wt%) is added, uniformly mixed and sieved and granulated.

[0061] Molding and structure building:

[0062] A special steel mold was used, and inner layer powder, middle layer powder and outer layer powder were sequentially filled between the mold center mandrel and the outer wall. During the filling of the outer layer powder, 12 polymethyl methacrylate microrods with a diameter of 0.8 mm were vertically inserted along the axial direction, the microrods were uniformly distributed in the circumference and the top ends extended to the flange end face of the mold. After the loading was completed, cold isostatic pressing was performed, the pressure was 220 MPa, the pressure holding time was 8 minutes, and the green body was obtained after demolding.

[0063] Glue removal and sintering:

[0064] The green body was placed in a sintering furnace, heated to 600℃ at a rate of 1℃ / min and kept for 4 hours to completely remove organic matter and pore forming agent; then argon gas was introduced for protection, heated to 1550℃ at a rate of 3℃ / min and kept for 6 hours, and cooled to room temperature with the furnace.

[0065] Electrode lead-out:

[0066] The flange non-immersion area outer wall of the immersion tube after sintering was coated with high-temperature platinum slurry, sintered and solidified at 850℃, and connected with nickel-chromium wire as anode lead, and then obtained.

[0067] Preparation Example 2:

[0068] The preparation of the functional gradient self-breathing type electrochemical reaction immersion tube provided by the present preparation example includes the following steps:

[0069] Synthesis of rare earth precursor powder:

[0070] The lanthanum oxide powder and the aluminum oxide powder were mixed in a molar ratio of 1:1, ball milled for 24 hours with anhydrous ethanol as the medium, dried, calcined at 1500℃ in air atmosphere for 10 hours, and cooled and ground to obtain lanthanum aluminate powder with an average particle size D50 of 3.0μm as the active B component.

[0071] Preparation of layered powder:

[0072] Inner layer powder: 550g of yttrium-stabilized zirconium oxide powder, 350g of lanthanum aluminate powder prepared in step (1), and 100g of zirconium carbide powder were weighed, 50g of polyvinyl alcohol aqueous solution (concentration 5wt%) was added, mixed uniformly and sieved and granulated;

[0073] Middle layer powder: 1000g of yttrium-stabilized zirconium oxide powder was weighed, 50g of polyvinyl alcohol aqueous solution (concentration 5wt%) was added, mixed uniformly and sieved and granulated;

[0074] Outer layer powder: 400g of yttrium-stabilized zirconium oxide powder, 400g of lanthanum strontium manganite powder and 200g of spherical graphite powder were weighed, 50g of polyvinyl alcohol aqueous solution (concentration 5wt%) was added, mixed uniformly and sieved and granulated.

[0075] Molding and structure building: the operation is the same as that of Preparation Example 1, except that 16 poly(methyl methacrylate) microrods with a diameter of 1.0 mm are vertically inserted along the axial direction when filling the outer layer powder; the cold isostatic pressing pressure is 250 MPa, and the pressure holding time is 10 minutes.

[0076] Glue removal and sintering: the glue removal process is the same as that of Preparation Example 1; the high-temperature sintering stage is under argon protection, heated to 1600℃ at a rate of 3℃ / min and held for 8 hours, and cooled with the furnace.

[0077] Electrode extraction: the operation is the same as that of Preparation Example 1.

[0078] Preparation Example 3:

[0079] This preparation example provides a functional gradient self-breathing electrochemical reaction immersion tube, the preparation of which comprises the following steps:

[0080] Synthesis of rare earth precursor powder: cerium zirconate powder is prepared by the method in Preparation Example 1, and the ball milling time is controlled to be 30 hours, and the final average particle size D50 is 2.0 μm.

[0081] Preparation of layered powder:

[0082] Inner layer powder: 650 g of yttria-stabilized zirconia powder, 250 g of cerium zirconate powder, and 50 g of zirconium carbide powder are weighed, 50 g of polyvinyl alcohol aqueous solution (concentration 5 wt%) is added, mixed uniformly and sieved and granulated;

[0083] Middle layer powder: 1000 g of yttria-stabilized zirconia powder is weighed, 50 g of polyvinyl alcohol aqueous solution (concentration 5 wt%) is added, mixed uniformly and sieved and granulated;

[0084] Outer layer powder: 500 g of yttria-stabilized zirconia powder and 500 g of lanthanum strontium manganite powder are weighed, spherical graphite powder is not added (only relying on the stacking porosity and microrod channels), 50 g of polyvinyl alcohol aqueous solution (concentration 5 wt%) is added, mixed uniformly and sieved and granulated.

[0085] Molding and structure building: the operation is the same as that of Preparation Example 1, except that 8 poly(methyl methacrylate) microrods with a diameter of 0.5 mm are vertically inserted along the axial direction when filling the outer layer powder; the cold isostatic pressing pressure is 200 MPa, and the pressure holding time is 5 minutes.

[0086] Glue removal and sintering: the glue removal process is the same as that of Preparation Example 1; the high-temperature sintering stage is under argon protection, heated to 1500℃ at a rate of 2℃ / min and held for 8 hours, and cooled with the furnace.

[0087] Electrode extraction: the operation is the same as that of Preparation Example 1.

[0088] Example 1-4:

[0089] Example 1:

[0090] The embodiment provides a high-precision cold work die flat steel continuous casting method based on a radial oxygen pumping mechanism and in-situ electrochemical rare earth modification, and comprises the following steps.

[0091] Smelting of ultra-pure molten steel: Cr12Mo1V1 type die steel is smelted, and after EAF initial smelting, LF furnace refining and VD vacuum treatment, the chemical composition (mass percentage) of the molten steel is as follows: C: 1.52%, Cr: 11.8%, Mo: 0.95%, V: 0.80%, S≤0.003%, P≤0.015%, T.O≤8ppm, [O]≤3ppm.

[0092] Construction of an electrochemical continuous casting system: the functional gradient self-breathing type electrochemical reaction immersion tube prepared in Preparation Example 1 is installed at the bottom of the tundish. The anode lead on the outer wall of the immersion tube is connected to the positive electrode of the direct current stabilized power supply, and the upper end of the tundish stopper (made of conductive aluminum carbon) is connected to the negative electrode of the power supply. The exhaust port at the flange of the immersion tube is connected to a micro negative pressure air pump, and the air pumping pressure is set to -8kPa.

[0093] Continuous casting and in-situ modification: the temperature of the molten steel in the tundish is controlled at 1525℃ (about 30℃ of superheat), and the continuous casting is carried out at a pulling speed of 1.0m / min. The direct current power supply is turned on, and a constant voltage of 3.0V is applied, and the system current density is stabilized at 0.3A / cm 2 . The crystallizer is subjected to electromagnetic stirring, the current is 300A, and the frequency is 3Hz. The specific water quantity of the secondary cooling zone is controlled at 0.5L / kg.

[0094] Example 2:

[0095] The embodiment provides a high-precision cold work die flat steel continuous casting method based on a radial oxygen pumping mechanism and in-situ electrochemical rare earth modification, and comprises the following steps.

[0096] Smelting of ultra-pure molten steel: the chemical composition and purity of the molten steel are controlled in the same manner as in Example 1.

[0097] Construction of an electrochemical continuous casting system: the functional gradient self-breathing type electrochemical reaction immersion tube prepared in Preparation Example 2 is used, and the system connection mode is the same as in Example 1, and the air pumping pressure is set to -10kPa.

[0098] Continuous casting and in-situ modification: the temperature of the molten steel in the tundish is controlled at 1535℃ (about 40℃ of superheat), and the continuous casting is carried out at a higher pulling speed of 1.2m / min. The direct current power supply is turned on, and a constant voltage of 3.8V is applied, and the system current density is stabilized at 0.5A / cm 2 . The electromagnetic stirring parameters of the crystallizer are as follows: the current is 350A, and the frequency is 4Hz. The specific water quantity of the secondary cooling zone is controlled at 0.6L / kg.

[0099] Example 3:

[0100] The embodiment provides a high-precision cold work die flat steel continuous casting method based on a radial oxygen pumping mechanism and in-situ electrochemical rare earth modification, and comprises the following steps.

[0101] Smelting of ultra-pure molten steel: the chemical composition and purity of the molten steel are controlled according to Embodiment 1.

[0102] Construction of an electrochemical continuous casting system: the functional gradient self-breathing type electrochemical reaction immersion tube (containing lanthanum aluminate) prepared in Preparation Example 2 is used, the system connection mode is the same as that in Embodiment 1, and the pumping pressure is set to -5 kPa.

[0103] Continuous casting and in-situ modification: the temperature of the molten steel in the tundish is controlled at 1515 ℃ (about 20 ℃ of superheat), and the casting speed is 0.8 m / min. A direct current power supply is turned on, a constant voltage of 2.5 V is applied, and the system current density is stabilized at 0.2 A / cm 2 The electromagnetic stirring parameters of the crystallizer are 250 A of current and 2 Hz of frequency. The specific water quantity of the secondary cooling zone is controlled at 0.4 L / kg.

[0104] Embodiment 4

[0105] The embodiment provides a high-precision cold work die flat steel continuous casting method based on a radial oxygen pumping mechanism and in-situ electrochemical rare earth modification, and comprises the following steps.

[0106] Smelting of ultra-pure molten steel: the chemical composition and purity of the molten steel are controlled according to Embodiment 1.

[0107] Construction of an electrochemical continuous casting system: the functional gradient self-breathing type electrochemical reaction immersion tube prepared in Preparation Example 1 is used, the system connection mode is the same as that in Embodiment 1, and the power supply is linked with the PLC control system of the continuous casting machine.

[0108] Continuous casting and in-situ modification: the initial casting speed is 0.8 m / min, and the PLC system controls the applied voltage to be 2.5 V. During the casting process, the casting speed is linearly increased from 0.8 m / min to 1.2 m / min according to the production plan, and the PLC control system linearly increases the applied voltage from 2.5 V to 3.8 V according to the preset model. Then, when the casting speed is stepwisely decreased from 1.2 m / min to 1.0 m / min, the PLC system stepwisely adjusts the voltage to 3.0 V, so as to maintain the stability of the rare earth content in the molten steel. Other process parameters are adjusted accordingly with the casting speed.

[0109] Comparative Examples 1-4

[0110] Comparative Example 1

[0111] Compared with Example 1, the difference lies in that the functional gradient self-breathing electrochemical reaction immersion tube and in-situ electrochemical modification method of the application are not used, but a conventional Al2O3-C material inert immersion nozzle is used, and a rare earth cerium-iron alloy cored wire is fed into the tundish at a speed of 0.5 m / min by a wire feeder for rare earth modification, and the rest of the process parameters are the same.

[0112] Comparative Example 2:

[0113] Compared with Example 1, the difference lies in that although the functional gradient self-breathing electrochemical reaction immersion tube prepared in Preparation Example 1 is used, no direct current power supply is connected during the whole continuous casting process, that is, no any polarization voltage is applied, and the rest of the process parameters are the same.

[0114] Comparative Example 3:

[0115] Compared with Example 1, the difference lies in that the immersion tube used is a specially prepared non-gradient two-layer structure immersion tube, the inner layer composition is the same as that of the inner layer of Preparation Example 1, and the outer layer is a dense pure YSZ material without porous structure and exhaust passage; the anode of the electrochemical system is connected through an inert graphite electrode arranged in the molten steel in the tundish, instead of being connected to the outer wall of the immersion tube, and the rest of the process parameters are the same.

[0116] Comparative Example 4:

[0117] Compared with Example 1, the difference lies in that the immersion tube used is a homogeneous single-layer structure, which is directly formed and sintered from the inner layer powder (60wt% YSZ, 30wt% cerium zirconate, 10wt% ZrC), without intermediate dense electrolyte layer and outer porous anode layer structure, and the rest of the process parameters are the same.

[0118] Test Examples 1-2:

[0119] Test Example 1: Verification of electrochemical reaction system running stability and exhaust mechanism.

[0120] The test aims to verify the electrochemical response characteristics and gas transmission mechanism effectiveness of the functional gradient self-breathing electrochemical reaction immersion tube in the high-temperature metallurgical environment, especially to verify the necessity of the embedded porous anode layer and exhaust passage for maintaining the continuous electrolysis reaction.

[0121] The experimental steps are as follows:

[0122] The device and process conditions of Example 1, Example 2, Example 3 and Comparative Example 3 were compared. Each group of experiments was started after the intermediate ladle steel liquid temperature was stabilized, and the current intensity and voltage fluctuation in the loop were recorded in real time by a multi-channel electrochemical workstation. The sampling frequency was set to ten times per second. At the same time, a high-precision small flow mass flow meter was connected in series at the exhaust port of the immersion tube flange end for monitoring the real-time outflow rate of the generated gas on the anode side. The test duration was set to 240 minutes, and if the current density decayed to less than 10% of the initial value during this period, the reaction was considered to have terminated, and the actual running time was recorded. During the experiment, the pulling speed was kept constant to exclude the interference of flow field fluctuations on the electrochemical signal.

[0123] The experimental data are shown in Table 1:

[0124] Table 1

[0125]

[0126] Conclusion:

[0127] According to the test results in Table 1, Examples 1-3 all achieved long-period stable operation, and the anode exhaust flow and current density showed a positive correlation. This phenomenon conforms to Faraday's law of electrolysis, that is, the amount of charge passing through the circuit directly determines the amount of material conversion at the electrode interface. In Example 1, the current density was stabilized at about 0.312 A / cm 2 , accompanied by a continuous gas discharge of 14.23 mL / min, indicating that oxygen ions successfully passed through the dense electrolyte layer, lost electrons at the porous anode layer and three-phase interface, combined into oxygen molecules, and then discharged from the system through the pre-set micro channel. The smoothness of this material transport channel ensures that the chemical potential gradient on both sides of the electrochemical reaction interface maintains a balance, and there is no obvious concentration polarization phenomenon, thereby realizing the continuous and uniform injection of rare earth elements into the steel liquid.

[0128] In contrast, although Comparative Example 3 applied the same driving voltage, the average current density was extremely low and rapidly decayed to near zero level within a short time after starting, and no gas discharge was monitored during this period. The failure mechanism is that Comparative Example 3 lacks a porous gas diffusion layer and an exhaust passage, resulting in the inability of oxygen gas generated after oxygen ions migrate to the outer anode interface to be physically released. The high-pressure oxygen gas accumulated at the ceramic layer interface forms a very high gas partial pressure, sharply raising the overpotential of the anode reaction and generating a large reverse electromotive force. This gas barrier effect cuts off the ion transport circuit, forcing the electrolysis reaction to terminate. This comparison result strongly confirms the construction of the embedded porous gas diffusion anode layer and the radial oxygen ion pumping structure in the present scheme, which is a key technical feature for the feasibility of the in-situ electrochemical modification process, and solves the physical blockage problem of traditional dense structures in the gas evolution reaction.

[0129] Test Example 2: Metallurgical quality and mechanical property evaluation of the cast slab.

[0130] This test sampled and analyzed the cold work die steel slabs produced in the steady-state continuous casting stage of each example and comparative example, focusing on the stability of the rare earth yield in the process, the control level of the total oxygen content in the steel, the morphological distribution characteristics of non-metallic inclusions, and the transverse impact toughness of the final material.

[0131] The experimental steps are as follows:

[0132] In the steady-state casting stage of the continuous casting machine (after 40 minutes of casting), metallographic samples and chemical analysis samples were taken at the 1 / 4 width of the cross section of the slab every 15 minutes, a total of 10 groups of samples. The total oxygen content (T.O) in the steel was determined by inert gas melting-infrared absorption method; the rare earth (Ce or La) and sulfur content in the steel was determined by inductively coupled plasma mass spectrometer (ICP-MS), and the rare earth yield and its standard deviation were calculated; the inclusions in the area with a field area greater than 100 square millimeters were counted by automatic scanning electron microscope combined with energy dispersive spectrometer, and the inclusion density and average size with an equivalent diameter greater than 10 microns were recorded. The mechanical property test was based on the metal Charpy impact test standard, and the unnotched sample was prepared to test the transverse impact energy at room temperature.

[0133] For Comparative Example 3, since it was confirmed in Test Example 1 that it could not maintain the electrochemical reaction and the reaction quickly terminated, no effective rare earth modified slab was obtained, so it was not included in the performance data comparison of this section.

[0134] The experimental data is shown in Table 2:

[0135] Table 2

[0136]

[0137]

[0138] Conclusion:

[0139] The data in Table 2 reveals the influence of different process paths on the quality of the final product. The average rare earth yield of Examples 1-4 is stable at more than 92%, and the standard deviation of the rare earth content is extremely small, confirming that the electrochemical dissolution mechanism has the ability to accurately control the atomic level. In contrast, Comparative Example 1, which uses the traditional wire feeding process, has a rare earth yield of only 52.4% and a large fluctuation, and the total oxygen content is as high as 18.7 ppm. This shows that the traditional physical addition method inevitably introduces secondary oxidation, resulting in a large amount of rare earth consumed in the formation of large particle oxide inclusions, thereby deteriorating the purity of the steel, which directly leads to a significant reduction in the transverse impact energy to 42.3 J.

[0140] Comparative Example 2 did not apply voltage, and the detection results showed that no effective content of rare earth was detected, and the total oxygen content of the casting blank was equivalent to that of the unmodified base steel liquid, and the inclusions were mainly unmodified aluminum oxide or spinel, the size was larger than that of the example group, and the impact performance was at the benchmark level. This result indirectly verifies that the entry of rare earth in the example group completely depends on electrochemical reduction driving, rather than physical erosion or thermal decomposition of ceramic materials.

[0141] Comparative Example 4 used a homogenously single-layer structure of the immersion tube, although a certain rare earth alloying (yield 76.3%) was achieved, but its total oxygen content of the casting blank (13.2 ppm) was higher than that of the example group, and the density of large particle inclusions was higher. The reason is that the lack of the selective isolation effect of the intermediate dense electrolyte layer leads to the oxygen generated on the anode side partially entering the steel liquid through physical diffusion in the opposite direction, or the iron elements in the steel liquid penetrate into the tube wall, causing electronic short circuit, reducing the current efficiency and causing re-oxidation of the steel liquid.

[0142] The low total oxygen content (about 5 ppm) and fine inclusion size (average less than 1 micron) exhibited by the example group (especially Examples 1 and 4) are attributed to the unique bidirectional mass transfer mechanism of the present scheme: that is, while the rare earth is "pressed into" the steel liquid in atomic state at the cathode interface, the oxygen ions generated by the reaction are "pumped out" to the outside of the tube by using the ionic conductivity of the YSZ solid-state electrolyte. This mechanism eliminates the chemical potential basis for the in-situ aggregation and growth of rare earth oxides in the steel liquid, so that the small amount of rare earth inclusions formed finally presents the characteristics of nanometerization and dispersion distribution, thereby improving the isotropic mechanical properties and impact resistance of high-precision cold work die steel. Example 4 further reduces the fluctuation of rare earth composition through PLC linkage control, indicating that the system has excellent dynamic response capability and is suitable for the working conditions of changing pulling speed in industrial continuous production.

Claims

1. A continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel, characterized in that, Includes the following steps: S1. Smelting to obtain clean mold steel molten steel and injecting it into the tundish; S2. Install a functional gradient self-breathing electrochemical reaction immersion tube at the bottom of the intermediate tank. The immersion tube has a three-layer gradient structure of inner layer, middle layer and outer layer. The inner layer contains rare earth precursor and conductive phase, the middle layer is dense solid electrolyte, and the outer layer is porous anode. S3. Connect the anode lead on the outer wall of the immersion tube to the positive terminal of the DC power supply, and connect the conductive plug rod in the intermediate ladle or the electrode inserted into the molten steel to the negative terminal of the DC power supply; at the same time, connect the exhaust channel at the flange end of the immersion tube to the negative pressure pumping device. S4. During continuous casting, the negative pressure pumping device is turned on and a DC voltage is applied to drive the inner rare earth precursor to undergo a reduction reaction at the inner interface of the molten steel, releasing rare earth atoms into the molten steel. At the same time, the generated oxygen ions migrate through the intermediate layer to the outer layer, lose electrons, and combine to form oxygen and be discharged.

2. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 1, characterized in that, In step S4, the DC voltage is controlled within the range of 2.5V-3.8V, the suction pressure of the negative pressure suction device is controlled between -5kPa and -10kPa, and the casting speed of the continuous casting is controlled between 0.8m / min and 1.2m / min.

3. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 1, characterized in that, In step S4, the application of DC voltage and the continuous casting process are controlled by a PLC linkage mode. A linear correlation model between casting speed and voltage is preset, and the actual casting speed signal of the continuous casting machine is collected in real time; As the pulling speed increases, the PLC control system controls the DC power supply to linearly increase the output voltage; When the pulling speed decreases, the PLC control system controls the DC power supply to linearly reduce the output voltage in order to maintain a constant amount of rare earth injected per unit volume of molten steel.

4. The continuous casting method for high-purity rare-earth modified high-precision cold-work die flat steel according to claim 1, characterized in that, In step S2, the material composition of each layer of the functionally graded self-breathing electrochemical reaction immersion tube is as follows: The inner layer is made of raw materials comprising the following parts by weight: Yttrium-stabilized zirconia powder: 550-650 parts; Rare earth precursor: 250-350 parts; Zirconium carbide powder: 50-100 parts; The intermediate layer is made from raw materials comprising the following parts by weight: Yttrium oxide stabilized zirconia powder: 1000 parts; The outer layer is made of raw materials comprising the following parts by weight: Yttrium oxide stabilized zirconia powder: 400-500 parts; Lanthanum strontium manganite powder: 400-500 parts; 0-200 parts of pore-forming agent.

5. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 4, characterized in that, The rare earth precursor is either cerium zirconate powder or lanthanum aluminate powder. The cerium zirconate powder is synthesized by mixing cerium oxide and zirconium oxide in a molar ratio of 1:1 and calcining at 1450°C. The lanthanum aluminate powder is synthesized by mixing lanthanum oxide and aluminum oxide in a molar ratio of 1:1 and calcining at 1500°C.

6. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 1, characterized in that, In step S2, during the preparation of the immersion tube, when filling the outer layer material, several polymethyl methacrylate microrods with a diameter of 0.5mm-1.0mm are inserted vertically along the axial direction. The microrods are evenly distributed around the circumference and their tops extend to the flange end face, forming a through exhaust channel after sintering.

7. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 1, characterized in that, In step S2, the sintering process of the immersion tube is as follows: The temperature was increased to 600℃ at a rate of 1℃ / min and held at that temperature to remove organic matter; Argon gas is introduced for protection, and the temperature is increased to 1500℃-1600℃ at a rate of 2℃ / min-3℃ / min and held for 6-8 hours, then cooled with the furnace.

8. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 1, characterized in that, In step S2, the immersion tube is formed by cold isostatic pressing, with a forming pressure of 200MPa-250MPa and a holding time of 5-10 minutes.

9. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 1, characterized in that, In step S1, the smelting process for obtaining clean mold steel molten steel includes, in sequence, electric arc furnace primary smelting, ladle refining furnace refining and vacuum degassing treatment, and the superheat of the molten steel is controlled within the range of 20℃-40℃.

10. The continuous casting method for high-purity rare-earth modified high-precision cold work die flat steel according to claim 1, characterized in that, In step S4, electromagnetic stirring is applied in the crystallizer during the continuous casting process, and the electromagnetic stirring current is controlled to be 250A-350A and the frequency is 2Hz-4Hz; at the same time, the specific water volume in the secondary cooling zone is controlled to be 0.4L / kg-0.6L / kg.