Flexible electron-oriented high-wettability reactive nano-silver ink as well as preparation method and application of flexible electron-oriented high-wettability reactive nano-silver ink

By using a combination of silver citrate, ammonia, and surfactants, a highly wettable nano-silver ink was prepared, solving the problem of poor wettability of particle-free inks on flexible substrates. This enabled low-temperature rapid sintering and excellent conductivity, promoting the industrial application of flexible electronics.

CN121574596APending Publication Date: 2026-02-27HARBIN ENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511745104.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-25
Publication Date
2026-02-27

AI Technical Summary

Technical Problem

Existing particle-free nano-silver inks have poor wettability on hydrophobic flexible substrates, resulting in uneven printed metal lines, high resistivity, and poor reliability, which limits their application in high-end flexible electronics.

Method used

Using silver citrate as the silver source, ammonia as the complexing agent, citric acid and ascorbic acid as dual reducing agents, and ethylene glycol as the solvent, combined with polyoxyethylene esters, polyether-modified siloxanes and phenyl ether surfactants, the stability and wettability of the ink are synergistically controlled, forming a spatial protective layer and reducing surface tension.

Benefits of technology

The prepared ink exhibits good stability at room temperature, with no precipitation after standing for 60 days. After rapid sintering at low temperature, the resistivity is as low as 3×10-4Ω·cm, and the contact angle on the silicon substrate can be as low as 18°, demonstrating excellent wettability and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121574596A_ABST
    Figure CN121574596A_ABST
Patent Text Reader

Abstract

The invention discloses high-wettability reactive nano-silver ink for flexible electronics and a preparation method and application thereof.The preparation method comprises the following steps that S1, silver citrate is weighed and placed in a container, ammonia water is added, and a mixture A is obtained; s2, adding a citric acid solution and organic alcohol into the mixture A to obtain a mixture B; s3, adding ascorbic acid into the mixture B, performing ultrasonic treatment, and filtering to obtain filtrate which is a mixture C; and S4, a surfactant is added into the mixture C, the surfactant is one or more than two of a polyoxyethylene acid ester surfactant, a polyether modified siloxane surfactant and a phenyl ether surfactant, and the ink is obtained after ultrasonic filtration. The prepared ink has excellent stability, can realize low-level rapid sintering, and shows excellent wettability on a silicon substrate.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of conductive ink, in particular to a high-wettability reactive nano-silver ink for flexible electronics and a preparation method and application thereof. BACKGROUND

[0002] With the rapid development of flexible electronics, wearable devices and Internet of Things technology, there is an urgent need for related green and low-cost manufacturing technologies. Traditional microelectronic manufacturing relies on photolithography, etching and other "subtractive manufacturing" processes, which need to be carried out in a high-temperature, high-vacuum environment, and the process is complex and costly. In contrast, printed electronics technology adopts an additive manufacturing concept, which realizes the patterning of functional materials through direct writing and inkjet printing, and is particularly suitable for large-area and batch production on flexible substrates. This change in technology paradigm has significantly reduced manufacturing costs, making it possible for electronic products to be popularized and ubiquitous.

[0003] Nano-silver ink, due to its excellent conductivity and oxidation resistance, has become a core functional material in the field of flexible electronics. Silver ink is divided into nanoparticle type and non-particle type according to the form of the conductive phase. The particle type conductive ink has the problems of easy clogging of the print head and high sintering temperature, which causes thermal damage to the substrate. In contrast, non-particle silver ink exists in the form of metal organic compounds or silver salt complexes, which fundamentally solves the problems of clogging and particle aggregation at the molecular level, and the thermal decomposition temperature is usually lower than 200℃, and some can be photochemically sintered, which has better process compatibility with flexible polymer substrates.

[0004] Although non-particle ink avoids the risk of clogging from the source and is expected to achieve lower temperature sintering, its precursor is mostly a silver-amine complex, and the prepared ink has poor wettability on hydrophobic flexible substrates, resulting in problems such as too large contact angle, pattern shrinkage, and significant coffee ring effect, which leads to uneven printed metal lines, high resistivity, and poor reliability, seriously restricting its application in high-end flexible electronics. Therefore, developing a high-performance non-particle nano-silver ink with excellent long-term stability, strong substrate wettability, and truly low-temperature sintering characteristics has become a core technical bottleneck that must be overcome to promote the industrial application of printed flexible electronics from the laboratory. The present application is developed in this background, aiming to provide a feasible solution to solve this multi-performance balance problem through innovative material design and ink engineering. SUMMARY

[0005] Therefore, in order to solve the above technical problems, the purpose of the present application is to provide a high-wettability reactive nano-silver ink for flexible electronics and a preparation method and application thereof. The prepared ink has excellent stability, can realize low-position rapid sintering, and exhibits excellent wettability on a silicon substrate.

[0006] The technical scheme adopted is:

[0007] The preparation method of the high-wettability reactive nano-silver ink for flexible electronics comprises the following steps:

[0008] S1. Citric acid silver is weighed in a container, ammonia is added to obtain mixture A;

[0009] S2. Citric acid solution and organic alcohol are added to mixture A to obtain mixture B;

[0010] S3. Ascorbic acid is added to mixture B, and after ultrasonic treatment, the filtrate obtained is mixture C;

[0011] S4. A surfactant is added to mixture C, the surfactant is one or more of polyoxyethylene acid ester surfactant, polyether modified siloxane surfactant, and phenyl ether surfactant, and the ink is obtained after ultrasonic filtration.

[0012] Further, the mass ratio of citric acid, ammonia, citric acid solution, organic alcohol, ascorbic acid, and surfactant is (0.4-0.6):(0.8-1.2):(0.2-0.4):(0.7-1.4):(0.04-0.06):(0.04-0.06), respectively.

[0013] Further, the mass ratio of citric acid, ammonia, citric acid solution, organic alcohol, ascorbic acid, and surfactant is 0.5:1:0.3:1:0.05:0.05, respectively.

[0014] Further, the organic alcohol is ethylene glycol.

[0015] Further, in step S1, the concentration of the ammonia is 25wt%.

[0016] Further, in step S2, the citric acid solution is a citric acid aqueous solution with a concentration of 5%.

[0017] Further, in step S1, mixture A is obtained after ultrasonic treatment for 15 minutes; and / or, in step S2, mixture B is obtained after ultrasonic treatment for 15 minutes; and / or, in step S3, the filtrate obtained after ultrasonic treatment for 15 minutes is mixture C.

[0018] The high-wettability reactive nano-silver ink for flexible electronics is prepared by the preparation method described above.

[0019] The high-wettability reactive nano-silver ink for flexible electronics is applied to a flexible substrate.

[0020] The application of the flexible electronic-oriented high-wettability reactive nano-silver ink in the preparation of conductive cotton yarn.

[0021] In the above technical solution,

[0022] The present application uses silver citrate as a silver source, ammonia as a complexing agent, citric acid and ascorbic acid as double reducing agents, and an organic alcohol such as ethylene glycol as a solvent, while adding a non-ionic surfactant to achieve the dual needs of high stability and high wettability of the ink. The selected surfactant is one or more of polyoxyethylene ester surfactants, polyether modified siloxane surfactants, and phenyl ether surfactants. Among them, the polyoxyethylene ester surfactant can form a space protection layer around the silver precursor due to its large volume of polyoxyethylene (PEO) hydrophilic end, which not only enhances the long-term dispersion stability of the ink, but also helps to reduce the surface tension; the polyether modified siloxane surfactant has a flexible polysiloxane chain as the main structure, which significantly reduces the surface tension and gives the solution good spreading and hydrophilicity; the phenyl ether surfactant effectively controls the interfacial tension by virtue of the strong hydrophobicity of the benzene ring and branched alkane, further optimizing the wetting behavior of the ink on the substrate. Among them, the polyoxyethylene ester surfactant is, for example, polyoxyethylene oleate or polyoxyethylene stearate; the polyether modified siloxane surfactant is, for example, polyether modified siloxane phosphate; and the phenyl ether surfactant is, for example, polyethylene glycol octylphenyl ether.

[0023] In summary, the present application has the following advantages:

[0024] The prepared ink, based on the hydrogen bond network constructed by organic acid and alcohol solvent, exhibits excellent stability after 60 days of standing at room temperature without precipitation. At the same time, thanks to the effect of the reducing agent, the ink can realize low-temperature rapid sintering, and the resistivity can be as low as 3×10 -4 Ω·cm after heat treatment at 160℃ for 5 minutes. In addition, the ink exhibits excellent wettability on the silicon substrate, with a contact angle as low as 18°. BRIEF DESCRIPTION OF DRAWINGS

[0025] Figure 1 The experimental graphs of three kinds of ink freshly prepared and placed for 60 days; (a) macroscopic morphology and (b) visible ultraviolet spectrum; (c) is the nanoparticle size distribution graph of the three kinds of ink.

[0026] Figure 2 XRD spectrum of the three kinds of ink.

[0027] Figure 3 SEM morphology of four kinds of ink after sintering at 160℃ for 5min; (a)-(d) respectively show the SEM morphology of four kinds of ink after sintering at 160℃ for 5min.

[0028] Figure 4 The figure is the resistance-temperature curve of ink, wherein (a) is the resistance-temperature curve of ink added with surfactant; (b) is the resistance-temperature curve of silver-ammonia solution.

[0029] Figure 5 The figure is the contact angle experiment of four kinds of ink on silicon substrate (SiO2) and polyimide substrate (PI).

[0030] Figure 6 The figure is the resistance-bending frequency curve and the resistance-soaking frequency curve of cotton yarn, wherein (a) is the resistance-bending frequency curve of cotton yarn soaked in silver-ammonia solution; (b) is the resistance-soaking frequency curve; (c) is the resistance-bending frequency curve of cotton yarn soaked in ink Ag-S; (d) is the resistance-soaking frequency curve. DETAILED DESCRIPTION

[0031] The application will be described in detail below through specific examples, but the purpose and object of these example embodiments are only used to exemplify the application, and do not constitute any form of any limitation on the actual protection scope of the application, and do not limit the protection scope of the application thereto.

[0032] Example 1

[0033] The preparation method of the high-wettability reactive nano-silver ink for flexible electronics in this embodiment comprises the following steps:

[0034] (1) Take 0.5 g of silver citrate in a glass container, add 1 g of ammonia water, and obtain mixture A after ultrasonic treatment for 15 min.

[0035] (2) Add 0.3 g of citric acid solution and 1 g of ethylene glycol to mixture A, and obtain mixture B after ultrasonic treatment for 15 min.

[0036] (3) Add 0.05 g of ascorbic acid to mixture B, and obtain mixture C after ultrasonic treatment for 15 min and filtration.

[0037] (4) Add 0.05 g of polyoxyethylene acid ester surfactant to mixture C, and obtain ink D after ultrasonic treatment and filtration.

[0038] Example 2

[0039] The preparation method of the high-wettability reactive nano-silver ink for flexible electronics in this embodiment comprises the following steps:

[0040] (1) Take 0.5 g of silver citrate in a glass container, add 1 g of ammonia water, and obtain mixture A after ultrasonic treatment for 15 min.

[0041] (2) To the mixture A, 0.3 g of citric acid solution, 1 g of ethylene glycol were added, and after ultrasonic treatment for 15 min, mixture B was obtained.

[0042] (3) To the mixture B, 0.05 g of ascorbic acid was added, and after ultrasonic treatment for 15 min, the filtrate obtained by filtration was mixture C.

[0043] (4) To the mixture C, 0.05 g of polyether-modified siloxane surfactant was added, and after ultrasonic treatment and filtration, ink E and were obtained.

[0044] Example 3

[0045] The preparation method of the flexible electronic-oriented high-wettability reactive nano-silver ink of the present embodiment comprises the following steps:

[0046] (1) 0.5 g of silver citrate was weighed into a glass container, 1 g of ammonia water was added, and after ultrasonic treatment for 15 min, mixture A was obtained.

[0047] (2) To the mixture A, 0.3 g of citric acid solution, 1 g of ethylene glycol were added, and after ultrasonic treatment for 15 min, mixture B was obtained.

[0048] (3) To the mixture B, 0.05 g of ascorbic acid was added, and after ultrasonic treatment for 15 min, the filtrate obtained by filtration was mixture C.

[0049] (4) To the mixture C, 0.05 g of phenyl ether surfactant was added, and after ultrasonic treatment and filtration, ink F was obtained.

[0050] Comparative Example 1

[0051] The preparation method of the ink of the present comparative example comprises the following steps:

[0052] (1) 0.5 g of silver citrate was weighed into a glass container, 1 g of ammonia water was added, and after ultrasonic treatment for 15 min, mixture A was obtained.

[0053] (2) To the mixture A, 1.4 g of deionized water was added, and after ultrasonic treatment for 15 min, silver ammonia solution G was obtained.

[0054] The inks D, E, F, G obtained from Examples 1-3 and Comparative Example 1 were respectively named Ag-T, Ag-S, Ag-X, and Ag-P. The following experimental tests were performed.

[0055] Experimental tests:

[0056] Experiment 1

[0057] The macroscopic morphology of the ink is as follows Figure 1As shown in Figure 8a, no obvious precipitation was observed after 60 days of standing, indicating that it has good physical stability. From the UV-visible absorption spectrum (Figure 8b), it can be seen that the three inks have no obvious surface plasmon resonance absorption peaks in the initial state 0 days and after 60 days of standing, indicating that the silver precursor remains molecular or ionic dispersion in the solution, without the aggregation or sedimentation of nanoparticles. Figure 1 As shown in Figure 8a, no obvious precipitation was observed after 60 days of standing, indicating that it has good physical stability. From the UV-visible absorption spectrum (Figure 8b), it can be seen that the three inks have no obvious surface plasmon resonance absorption peaks in the initial state 0 days and after 60 days of standing, indicating that the silver precursor remains molecular or ionic dispersion in the solution, without the aggregation or sedimentation of nanoparticles. Figure 1 c is the dynamic light scattering (DLS) particle size distribution result, after adding the surfactant, the polydispersity index (PDI) of the three inks is about 0.2, indicating that the size distribution of the particles in the system is relatively uniform. The above results from macro-morphology to micro-angle consistently prove that the prepared ink has excellent stability.

[0058] Experiment 2

[0059] The prepared ink was sintered at 180°C for 2min and then subjected to XRD test, and the results are shown in Figure 9. Figure 2 As shown in Figure 9, the three inks all have good crystallinity, and strong diffraction peaks appear at 38.1°, 44.3°, 64.4°, 77.5°, 82.2°, corresponding to the crystal faces (111), (200), (220), (311), (222) of silver, which are consistent with PDF #87 – 0597 (FCC type).

[0060] Experiment 3

[0061] The prepared ink was sintered at 160°C for 5min and then subjected to SEM test, and the results are shown in Figure 10. Figure 3 As shown in Figure 10, Figure 3 a is the micro-morphology of silver ammonia sintered film, the particles are only physically connected to form a conductive network, the network structure is loose and the porosity is high, Figure 3 b-d are the micro-morphologies of the ink added with surfactant, all have formed sintering necks, and the film layer added with polyether modified siloxane surfactant is the most dense, which effectively reduces the contact resistance and improves the conductivity of the entire film layer. The above results show that the reduction temperature of the entire system is effectively reduced under the synergistic action of the reducing agent and the active agent, and the density and conductive continuity of the sintered film are significantly optimized.

[0062] Experiment 4

[0063] The four inks were subjected to resistance test at different sintering temperatures, and the results are shown in Figure 11. Figure 4 As can be seen from Figure 11, the resistance of the ink added with active agent is significantly reduced after sintering, among which the resistivity of the ink Ag-X can reach 8×10-5Ω·cm after sintering at 200°C for 15min, which is due to the fact that the linear polyethylene oxide (PEO) chain of the active agent is completely oxidized to form CO2 after sintering, leaving the least insulating residue and the best conductive effect.

[0064] Experiment 5

[0065] Contact angle tests were conducted on four inks on high surface energy silicon (SiO2) and low surface energy polyimide (PI) substrates, and the results are as follows: Figure 5 As shown, under the action of the three surfactants, the ink system exhibits low surface tension and excellent wetting properties. Ag-X has a contact angle of 30° on PI film, and Ag-S has a contact angle of 18° on silicon-based substrates, demonstrating that this type of ink has excellent spreading ability and wide applicability on substrates with different properties.

[0066] Experiment 6

[0067] An 8cm length of cotton yarn was immersed in Ag-P and Ag-S inks. The effect of the number of immersions on its resistance was investigated. The bendability of the conductive cotton yarn obtained after sintering was also tested. The results are as follows: Figure 6 As shown, where Figure 6 a) When immersed in a silver ammonia solution without surfactant, its resistance increases with the number of bends, rising by 95% after 100 bends. Figure 6 c shows the resistance change curve after immersion in Ag-S ink with the number of bends. After 100 bends, the resistance only increased by 20%, indicating that the ink has good flexibility and stability. The difference between the two indicates that the addition of polyether-modified siloxane surfactants effectively reduced the porosity defects in the conductive layer after sintering, making the conductive network more stable. Figure 6 b and Figure 6 Figure d illustrates the relationship between resistance and the number of soaking cycles. With increasing soaking cycles, the resistance of both systems decreased. After two soaking cycles, the resistance of the ordinary silver ammonia solution decreased more significantly. This is because the unprotected silver ammonia ions are not dispersed and quickly adsorb onto the surface and pores of the cotton fibers, forming a continuous conductive path. In contrast, the surfactant disperses silver ions through steric hindrance, resulting in a more dispersed distribution of silver particles in the first few soaking cycles, making it difficult to quickly form a complete pathway and leading to a relatively higher resistance. As the number of soaking cycles increases, the concentration of silver ions adsorbed by the cotton yarn increases, and the dispersed silver particles gradually aggregate and become denser. After five soaking cycles, the silver particles can construct a conductive network that meets the low-resistance requirements. Subsequent increases in soaking cycles have a weaker effect on improving the conductive network, hence the resistance of both systems no longer changes significantly. The bending test of the conductive cotton yarn demonstrates excellent mechanical flexibility and conductive stability, making it widely applicable in flexible electronics, wearable devices, and other scenarios.

[0068] The detailed descriptions listed above are merely specific illustrations of feasible embodiments of the present invention and are not intended to limit the scope of protection of the present invention. All equivalent embodiments or modifications made without departing from the spirit of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing a highly wettable reactive nano-silver ink for flexible electronics, characterized in that, Includes the following steps: S1. Weigh silver citrate into a container, add ammonia water, and obtain mixture A; S2. Add citric acid solution and organic alcohol to mixture A to obtain mixture B; S3. Add ascorbic acid to mixture B, sonicate, and filter to obtain mixture C; S4. Add a surfactant to mixture C, wherein the surfactant is one or more of polyoxyethylene ester surfactants, polyether-modified siloxane surfactants, and phenyl ether surfactants, and obtain ink after ultrasonic filtration.

2. The method for preparing highly wettable reactive nano-silver ink for flexible electronics according to claim 1, characterized in that, The mass ratio of citric acid, ammonia, citric acid solution, organic alcohol, ascorbic acid, and surfactant is (0.4-0.6):(0.8-1.2):(0.2-0.4):(0.7-1.4):(0.04-0.06):(0.04-0.06).

3. The method for preparing highly wettable reactive nano-silver ink for flexible electronics according to claim 2, characterized in that, The mass ratio of citric acid, ammonia, citric acid solution, organic alcohol, ascorbic acid, and surfactant is 0.5:1:0.3:1:0.05:0.

05.

4. The method for preparing highly wettable reactive nano-silver ink for flexible electronics according to claim 1, characterized in that, The organic alcohol is ethylene glycol.

5. The method for preparing highly wettable reactive nano-silver ink for flexible electronics according to claim 1, characterized in that, In step S1, the concentration of the ammonia water is 25 wt%.

6. The method for preparing highly wettable reactive nano-silver ink for flexible electronics according to claim 1, characterized in that, In step S2, the citric acid solution is an aqueous solution of citric acid with a concentration of 5%.

7. The method for preparing highly wettable reactive nano-silver ink for flexible electronics according to claim 1, characterized in that, In step S1, mixture A is obtained after sonication for 15 minutes; and / or, in step S2, mixture B is obtained after sonication for 15 minutes; and / or, in step S3, mixture C is obtained by filtration after sonication for 15 minutes.

8. A highly wettable reactive nano-silver ink for flexible electronics, characterized in that, It is prepared by the preparation method described in any one of claims 1-7.

9. The application of the highly wettable reactive nano-silver ink for flexible electronics as described in claim 8 on a flexible substrate.

10. The application of the highly wettable reactive nano-silver ink for flexible electronics as described in claim 8 in the preparation of conductive cotton yarn.