Width gradient tungsten disulfide nanobelt, preparation method of width gradient tungsten disulfide nanobelt and application of width gradient tungsten disulfide nanobelt in self-driven photoelectric detector
By controlling the thickness and growth kinetics of the metal catalyst film, the width gradient of tungsten disulfide nanoribbons was achieved, solving the construction problem of self-driven optoelectronic devices and realizing efficient photoelectric detection, which has significant application potential.
Patent Information
- Application Number
- CN202511789871.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-12-01
- Publication Date
- 2026-02-27
AI Technical Summary
Existing technologies struggle to precisely control the width gradient of tungsten disulfide nanoribbons, making it difficult to construct self-driven optoelectronic devices and hindering the realization of efficient photoelectric detection without external bias.
By controlling the thickness of the metal catalyst film and the growth kinetics during chemical vapor deposition, the continuous gradient change of the nanoribbon width along the axial direction is regulated, and efficient photoelectric detection under zero bias voltage is achieved using the built-in electric field.
We have achieved the fabrication of high-quality tungsten disulfide nanoribbons with wide gradients, and constructed a self-driven photodetector with high responsivity and high detectivity under zero bias conditions, which significantly reduces device power consumption and has important application value.
Smart Images

Figure CN121575368A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application belongs to the field of low-dimensional nanomaterial preparation technology and optoelectronic device application, and particularly relates to a one-dimensional tungsten disulfide nanobelt material with a width gradient characteristic, a controllable chemical vapor deposition preparation method thereof, and application of the width gradient characteristic to a self-driven photodetector without an external power supply. BACKGROUND
[0002] Tungsten disulfide (WS2) as a typical transition metal dichalcogenide has shown great application potential in the field of optoelectronics due to its tunable band gap, excellent photoelectric performance and good environmental stability. Compared with two-dimensional materials, one-dimensional WS2 nanostructures, especially nanobelts, have become ideal materials for improving the performance of optoelectronic devices due to their higher specific surface area, stronger quantum confinement effect and efficient charge transport characteristics along the axial direction.
[0003] At present, the preparation of WS2 nanobelts mainly adopts two types of methods, i.e., a "top-down" method and a "bottom-up" method. The "top-down" method includes electron beam etching, plasma etching and the like, which can realize the patterning of nanobelts, but has problems of many edge defects, low crystal quality and high cost. In the "bottom-up" synthesis method, the hydrothermal method can realize batch preparation, but the obtained product usually has poor crystallinity and wide size distribution, which is difficult to meet the requirements of high-performance devices. The chemical vapor deposition method (CVD) is the mainstream method for preparing high-quality, single-crystal WS2 nanostructures at present, but the existing CVD technology still faces significant bottlenecks in controllable synthesis of one-dimensional nanobelts. For example, when WO3 nanowires are used as precursors for sulfuration, the solid-gas reaction is often insufficient, resulting in unreacted tungsten oxides in the product, which affects the stoichiometric accuracy; although the growth assisted by alkali metal salts can promote the formation of nanostructures, the residual metal ions will become charge scattering centers, which deteriorate the carrier mobility.
[0004] Especially important is that the WS2 nanobelts prepared by the CVD method in the existing reports are mostly uniform or randomly variable in width, and there is still a lack of effective means for continuous and directional gradient control of the width of the nanobelt. The lack of such a width gradient structure limits the in-depth research and application development of the gradient physical effect (such as the gradual change of the energy band and the formation of the built-in electric field) in one-dimensional nanomaterials. In fact, the nanobelt structure with a continuous width gradient can generate a controllable built-in electric field in the axial direction, which provides an ideal platform for realizing a self-driven photodetector without an external bias. Therefore, it is of urgent need and great significance to develop a preparation method of high-quality WS2 nanobelts capable of accurately controlling the width gradient and to construct an efficient self-driven optoelectronic device on this basis, which promotes the application of low-dimensional semiconductor materials in the next generation of energy-saving optoelectronic systems. SUMMARY
[0005] The present application is directed to the prior art in the accurate control of tungsten disulfide nanostructure morphology, unable to achieve the width gradient controllable preparation, and the resulting self-driven optoelectronic device construction difficulties and other problems, the application proposes a width gradient tungsten disulfide nanobelt, its preparation method and its application in self-driven photoelectric detector. The core of the present application is to realize the continuous gradient change of the nanobelt width along the axial direction by adjusting the thickness of the metal catalyst film and the growth kinetics in the chemical vapor deposition process, and to realize high-efficiency photoelectric detection under zero bias by using the built-in electric field induced by the gradient structure.
[0006] In order to achieve the above-mentioned purpose, the present application adopts the following technical scheme: A preparation method of a width gradient tungsten disulfide nanobelt, comprising the following steps: (1) depositing a metal Ni film with a thickness of 2-10 nm on a SiO2 / Si substrate, and then annealing in a reducing atmosphere at 900-1000℃ for 1-3 hours; (2) placing sulfur powder at a position 30-40 cm upstream of the center of the tube furnace; placing tungsten trioxide powder in the center temperature zone of the tube furnace; placing the growth substrate obtained in step (1) at a position 15-20 cm downstream of the center of the tube furnace, and setting the temperature at this position to be 50-100℃ lower than the center temperature zone; (3) when the center temperature zone is raised to 950-1050℃, a mixed gas of hydrogen and argon is introduced, and solid sulfur powder is pushed into the high-temperature zone at a constant rate for growth reaction, forming a width gradient tungsten disulfide nanobelt on the substrate; (4) after the growth is completed, stop pushing the sulfur source and turn off the hydrogen, and cool to room temperature under a protective atmosphere.
[0007] Further, in step (3), the hydrogen flow rate is 5-50 sccm, the argon flow rate is 100-300 sccm, the pushing rate of the solid sulfur powder is 0.5-2 cm / min, and the growth time is 5-20 min.
[0008] Further, in steps (1) and (3), the temperature is raised to the target temperature at a rate of 20-50℃ / min.
[0009] Further, the structure of the nanobelt is that the wide end is connected with Ni, and the narrow end is sharp and suspended, with a continuously changing width gradient along the growth direction.
[0010] Further, the nanobelt has a widest part of 150-500 nm, a narrowest part of 50-120 nm, and a length of 3-12 μm; the edge is armchair type, and the crystal structure is 3R phase stacking.
[0011] Further, the second-order nonlinear optical polarizability tensor component ratio of the nanobelt is |χ (2) xxx / χ (2) xyy |>10, wherein χ (2) xxx corresponds to the second-order nonlinear response along the axial direction of the nanobelt.
[0012] A self-driven photodetector, the photosensitive channel of the detector is composed of the above-mentioned width gradient tungsten disulfide nanobelt.
[0013] Further, the width gradient tungsten disulfide nanobelt is transferred from the growth substrate to the insulating substrate, and metal electrodes are deposited at the end with larger width and the end with smaller width of the nanobelt, respectively, to form an asymmetric electrode contact structure.
[0014] Further, under the irradiation of a laser with a wavelength of 532 nm and a power density of 0.10 mW / cm 2 , the zero-bias responsivity is not less than 1 A / W, and the detectivity is not less than 1.0 × 10 12 Jones.
[0015] Further, the electrode is a titanium / gold electrode, a gold electrode or a chromium / gold electrode, the thickness of the gold electrode is 50-100 nm, and in the titanium / gold electrode or the chromium / gold electrode, the thickness of the titanium layer or the chromium layer is 1-10 nm, and the thickness of the gold layer is 50-100 nm.
[0016] The design idea of the present application is: By controlling the initial thickness of the nickel catalyst film, the size of the nickel nanoparticles formed after annealing is regulated, and then the nucleation behavior and initial width of the tungsten disulfide nanobelt are affected. In the chemical vapor deposition process, by accurately controlling the growth time and the reaction atmosphere, the growth mode of the nanobelt gradually changes from the vapor-liquid-solid (VLS) mechanism to the vapor-solid (VS) mechanism with the reaction process. With the dynamic evolution of the catalyst particles and the gradient change of the reactant concentration, the width of the nanobelt continuously decreases during the growth process, and finally a gradient structure continuously changing along the axial direction is formed. The width gradient leads to differences in the energy band structure of different regions of the nanobelt, forming a built-in electric field pointing from the wide end to the narrow end. Under light conditions, the electric field can drive the directional separation of photo-generated carriers, thereby realizing self-driven photoelectric response without external power supply.
[0017] The characteristics and benefits of the present application are: 1. By regulating the thickness of the nickel film and the growth time and other key parameters, the width gradient of the tungsten disulfide nanobelt is accurately controlled, and the prepared nanobelt has a continuous geometric feature along the axial direction, a clear armchair edge and a 3R phase stacking structure, providing a new method for the morphology regulation of low-dimensional materials.
[0018] 2. By using the built-in electric field unique to the width gradient nanoribbon, a self-driven photodetector is constructed, high responsivity and high detectivity are achieved under zero bias, the power consumption of the device is significantly reduced, the system structure is simplified, and it has important application value in the fields of optical communication and environmental monitoring. BRIEF DESCRIPTION OF DRAWINGS
[0019] Figure 1 Schematic diagram for growing width gradient tungsten disulfide nanoribbons by chemical vapor deposition method. In the figure, 11 is a reaction chamber quartz tube; 12 is a gas inlet; 13 is a gas outlet; 14 is tungsten trioxide powder; 15 is solid sulfur powder; and 16 is a growth substrate.
[0020] Figure 2 Scanning electron microscope (SEM) image of width gradient tungsten disulfide nanoribbons obtained after growing for 15 min on a SiO2 / Si substrate coated with a 2 nm thick nickel film. The experimental conditions are shown in Example 1.
[0021] Figure 3 Atomic force microscope (AFM) image and length and thickness distribution histograms of width gradient tungsten disulfide nanoribbons obtained after growing for 15 min on a SiO2 / Si substrate coated with a 2 nm thick nickel film. The experimental conditions are shown in Example 1.
[0022] Figure 4 Transmission electron microscope (TEM) characterization of width gradient tungsten disulfide nanoribbons obtained after growing for 15 min on a SiO2 / Si substrate coated with a 2 nm thick nickel film: (a) low-magnification ADF-STEM image, which intuitively presents the width gradient; (b) edge region ADF-STEM image, with armchair atomic arrangement marked; (c) central region ADF-STEM image; (d) corresponding bright-field STEM image; (e-f) atomic spacing intensity line scans, extracted from the dashed lines marked in figure (c), measuring 0.31 nm and 0.27 nm lattice spacings; (g) FIB-prepared cross-sectional image; (h) high-resolution cross-sectional HR-STEM image, showing ABC stacking sequence, confirming that the tungsten disulfide is in 3R phase. The experimental conditions are shown in Example 1.
[0023] Figure 5 Gradient analysis of optical properties of width gradient tungsten disulfide nanoribbons obtained after growing for 15 min on a SiO2 / Si substrate coated with a 2 nm thick nickel film: (a) optical photograph of the nanoribbon; (b-d) Raman spectra, photoluminescence spectra and SHG intensity comparison for positions 1-3 (from wide to narrow) are sequentially shown; (e-f) SHG polar coordinate diagrams under horizontal and vertical polarization, which intuitively present strong anisotropy. The experimental conditions are shown in Example 1.
[0024] Figure 6Scanning electron microscope image of width gradient tungsten disulfide nanoribbons obtained after 15 min growth on SiO2 / Si substrate coated with 6 nm thick nickel film. Experimental conditions are given in Example 2.
[0025] Figure 7 Transmission electron microscope image of width gradient tungsten disulfide nanoribbons obtained after 15 min growth on SiO2 / Si substrate coated with 6 nm thick nickel film. Experimental conditions are given in Example 2.
[0026] Figure 8 Scanning electron microscope image of width gradient tungsten disulfide nanoribbons obtained after 5 min growth on SiO2 / Si substrate coated with 2 nm thick nickel film. Experimental conditions are given in Example 3.
[0027] Figure 9 Schematic diagram and scanning electron microscope image of width gradient tungsten disulfide nanoribbons self-driven photodetector device. Experimental conditions are given in Example 4.
[0028] Figure 10 Optoelectronic performance test of width gradient tungsten disulfide nanoribbons self-driven photodetector device: (a) I-V curves in dark state and at different light power densities; (b) I sc , response R vs. light power density curves; (c) external quantum efficiency EQE, detectivity D* vs. light power density curves; (d) I-T curves under 0.1 Hz modulation. Experimental conditions are given in Example 4. DETAILED DESCRIPTION
[0029] In the specific implementation process, the application provides a preparation method and application of width gradient tungsten disulfide nanoribbons. A layer of Ni thin film is deposited on a clean SiO2 / Si substrate, and annealing treatment is performed to form Ni nanoparticles; tungsten trioxide powder and the treated substrate are placed in a chemical vapor deposition system, hydrogen and sulfur source are introduced into an argon atmosphere, and chemical vapor deposition reaction is performed to grow width gradient tungsten disulfide nanoribbons along the axial direction. The chemical vapor deposition system of the application is shown in Figure 1 The two ends of the horizontal type tube furnace reaction chamber quartz tube 11 are respectively provided with a gas inlet 12 and a gas outlet 13. The outer end of the gas inlet 12 is connected with a gas mass flow meter for accurately controlling the flow rate of the reaction gas or carrier gas. The tungsten trioxide powder 14 serving as the tungsten source is located in the center constant temperature heating zone of the reaction chamber quartz tube 11. The solid sulfur powder 15 for providing the sulfur source is located in the upstream region of the center heating zone of the reaction chamber quartz tube 11. The growth substrate 16 is located in the downstream region of the center heating zone of the quartz tube 11 to grow the nanoribbons at the optimal temperature.
[0030] The application will be further described in detail through examples below.
[0031] Example 1 A clean SiO2 / Si substrate (SiO2 layer thickness of about 285 nm) was selected as the growth substrate and placed in the vacuum chamber of a thermal evaporation instrument to deposit a 2 nm thick metal nickel film by thermal evaporation. After evaporation, argon gas was introduced to normal pressure, and the substrate was cooled to room temperature and removed. The substrate with the deposited nickel film was placed in the center heating zone of a tube furnace, and annealed at 950 °C for 2 hours in a mixed atmosphere of hydrogen (10 sccm) and argon (100 sccm) at a rate of 20 °C / min. This process caused the Ni film to agglomerate to form uniformly distributed nickel nanoparticles. The reaction system was a single-temperature-zone quartz tube furnace with an inner diameter of 25 mm and a length of 1000 mm. As shown in FIG. 1, the annealed growth substrate 16 was placed in the downstream temperature zone (about 15 cm from the heating center) which was about 50 °C lower than the center temperature zone. 500 mg of tungsten trioxide powder (purity 99.9%, particle size <200 nm) 14 was placed in the center temperature zone, and 650 mg of sulfur powder (particle size 200 mesh, purity 99.999%) 15 was placed in the upstream normal temperature zone (about 35 cm from the heating center). After sealing the quartz tube, 500 sccm of argon gas was introduced as a carrier gas to remove air. Subsequently, the center temperature zone was heated to 1000 °C at a rate of 25 °C / min. When the temperature was stable, the argon flow was adjusted to 100 sccm, and 15 sccm of hydrogen was introduced at the same time. Subsequently, the quartz boat containing 650 mg of sulfur powder was pushed into the heating zone at a constant speed of 1 cm / min. The growth reaction lasted for 15 min. During this process, by controlling the uniform pushing of the sulfur source, the dynamic change of the S / W atomic ratio in the reaction environment from high to low was achieved, guiding the growth mode to change from the initial VLS mechanism to the later VS mechanism. After the reaction was completed, the introduction of hydrogen was stopped. The furnace was naturally cooled to room temperature under the protection of 200 sccm of argon gas, and the growth of the sample was completed. Figure 1
[0032] The obtained sample was comprehensively characterized to confirm that it was a high-quality width gradient tungsten disulfide nanobelt. The scanning electron microscope photograph is shown in FIG. 2, which shows that the nanobelt presents a continuous change in width along its length direction, with a blunt wide end connected to the Ni catalyst, reflecting the gas-liquid-solid (VLS) growth origin; a sharp narrow end hanging in the air, reflecting the gas-solid (VS) epitaxial growth terminal. After the nanobelt was transferred to a clean silicon wafer, atomic force microscope testing was performed, and a typical result is shown in FIG. 3. Figure 2 Figure 3 The thickness of the nanobelt was measured to be between 5-25 nm, with an average thickness of about 14.5 nm. A statistical analysis of 240 nanobelts showed that the length distribution was between 3-12 μm, with an average length of about 5 μm, and the width continuously changed from about 200 nm at the starting end to about 50 nm at the termination end. The transmission electron microscope analysis result is shown in FIG. 4. Figure 4 : Figure 4 The image in section a shows that the nanoribbons have a significant width gradient, and the diffraction spots along the growth axis are uniform and clear, indicating high crystallinity; the energy-dispersive X-ray spectroscopy (EDS) image shows a uniform distribution of W and S elements. Figure 4 Images b and c in section 4 are annular dark-field scanning transmission electron microscopy (ADF-STEM) images of the edge and center of the nanoribbon, respectively. Figure 4 b clearly shows that the edge has an armchair atomic arrangement feature. Figure 4 In the image, d represents the bright-field STEM image of the corresponding region. Figure 4 In the middle of e and 4, f is Figure 4 Line scan analysis of the interatomic spacing in selected regions of C showed that the interatomic spacings were 0.31 nm and 0.27 nm, respectively, which are consistent with the lattice parameters of tungsten disulfide. Figure 4 Image g shows a cross-sectional view of a nanoribbon sample prepared by focused ion beam (FIB). Figure 4 The middle h clearly shows that the interlayer stacking sequence is of type ABC, confirming that the crystal structure is a 3R phase. Figure 5 Based on the optical characterization results of nanoribbons, the system reveals the continuous regulation of the optical properties of the material by the width gradient. Figure 5 Representative positions were selected along the growth direction of the nanoribbon (from the wide end to the narrow end) for testing. Position 1 corresponds to the starting end with a width of approximately 200 nm, position 2 corresponds to the middle section with a width of approximately 150 nm, and position 3 corresponds to the ending end with a width of approximately 100 nm. Raman spectroscopy analysis showed ( Figure 5 (b) All three positions mentioned above show a value of 350 cm. -1 (E) 1 2g ) and 420 cm -1 (A) 1g The presence of characteristic peaks with a shift of less than 1 cm⁻¹ confirms excellent crystal quality. The peak intensity decreases sequentially from position 1 to position 3, attributed to the reduced light absorption cross-section due to the decreased width and enhanced edge scattering. Photoluminescence spectroscopy indicates that ( Figure 5 In the middle (c), the PL peak position exhibits a significant gradient blue shift, continuously shifting from 648 nm (1.91 eV) at position 1 to 640 nm (1.94 eV) at position 3, with a total blue shift of 8 nm (approximately 30 meV), attributed to the enhanced quantum confinement effect as the width decreases; the PL intensity decays synchronously, consistent with the Raman trend. Second harmonic generation test ( Figure 5 (d) shows that the SHG intensity exhibits a strong width dependence, confirming that the nonlinear response is proportional to the volume change of the nanoribbon; polar plot ( Figure 5 In sections e and f) of 5, the structure is a sharp bilobed structure only along the belt axis. The result obtained through fitting calculations is |χ (2) xxx / χ (2)xyy | ≈ 16.4, significantly higher than the theoretical value of large-area 3R-WS2 (~2.0), proving that the width gradient and armchair edge synergistically disrupt the in-plane C3 symmetry, greatly enhancing the axial nonlinear response. These results demonstrate that this embodiment successfully prepared high-quality tungsten disulfide nanoribbons with a width gradient geometry, armchair edges, and a 3R phase structure, with a width gradient ranging from approximately 150~250 nm (starting end) to 50~120 nm (terminating end), establishing the baseline process parameters for preparing high-quality gradient nanoribbons.
[0033] Example 2 The same SiO2 / Si substrate and evaporation process as in Example 1 were used. The nickel film deposition thickness was increased to 6 nm. Under these conditions, the average size of the nickel nanoparticles formed after annealing increased, the interparticle spacing decreased significantly, and a closely packed quasi-continuous film was formed, with almost no exposed SiO2 surface. Figure 1 As shown, the annealed growth substrate 16 was placed in a downstream temperature zone (approximately 15 cm from the heating center) about 50°C lower than the central temperature zone. 500 mg of tungsten trioxide powder 14 was placed in the central temperature zone, and 650 mg of sulfur powder 15 was placed in the upstream room temperature zone (35 cm from the heating center). After sealing the quartz tube, 500 sccm of argon gas was introduced as a carrier gas to purge air. The central temperature zone was then heated to 1000°C at a rate of 25°C / min. Once the temperature stabilized, the argon gas flow rate was adjusted to 100 sccm, and 15 sccm of hydrogen gas was simultaneously introduced. Subsequently, the quartz boat containing 650 mg of sulfur powder was advanced into the heating zone at a constant rate of 1 cm / min. The growth reaction lasted for 15 min. During this process, by controlling the uniform advancement of the sulfur source, a dynamic change in the S / W atomic ratio in the reaction environment was achieved from high to low, guiding the growth mode from the initial VLS mechanism to the later VS mechanism. After the reaction was completed, the hydrogen gas introduction was stopped. Sample growth was completed by allowing the furnace to cool naturally to room temperature under argon protection at 200 sccm. Figure 6 and Figure 7 As shown, scanning electron microscopy and transmission electron microscopy images of the obtained samples reveal a significant decrease in nanoribbon growth density and sparse distribution, with an average length shortened to approximately 3-5 μm. While the width gradient characteristics are still maintained (approximately 320-380 nm at the starting end and 50-100 nm at the ending end), the gradient slope is significantly increased. This is because the increased nickel film thickness leads to excessively large and tightly packed catalytic particles, reducing the effective nucleation edges and restricting axial growth, resulting in a steeper width change. Simultaneously, enhanced radial growth increases the overall thickness and shortens the length, exhibiting a "short and steep" gradient morphology.
[0034] Example 3 A SiO2 / Si substrate was chosen, and the nickel film deposition thickness was the same as in Example 1 (2 nm), and the annealing conditions were unchanged. The key adjustments were: the amount of sulfur powder was reduced to 200 mg, and the growth time was shortened to 5 min. The rest of the growth parameters (temperature, gas flow, etc.) were the same as in Example 1. The scanning electron microscope image of the obtained sample (Figure Figure 8 ) shows that the nanobelt width is significantly small, but a large number of tungsten oxide crystal particles that are not completely sulfidized are present in the sample. The reason is that the sulfur source supply is insufficient and the reaction time is too short, resulting in the WO3 precursor failing to be fully sulfidized, and part of the tungsten source directly deposits to form WO3 crystals; at the same time, the rapid heating and short growth inhibit the preferred growth of the crystals along the axial direction, forming small but poor-quality nanobelts. This example serves as a comparison and, from the negative side, confirms the importance of the aforementioned technical feature of “controlling the advance of the sulfur source and the growth time to regulate the dynamic change of the S / W atomic ratio in the reaction environment from high to low, and realizing the transition of the growth mode from VLS to VS”, and clearly defines the process boundary for obtaining pure-phase high-quality products.
[0035] Example 4 The width gradient tungsten disulfide nanobelt prepared in Example 1 was transferred from the growth substrate to a clean SiO2 / Si (285 nm thick SiO2) substrate. A maskless ultraviolet lithography technology (ATS-07-UV Litho-ACA) was used to position Ti / Au (5 nm / 50 nm) electrodes at both ends of a single nanobelt to construct a metal-semiconductor-metal (MSM) self-driven photodetector. The device structure schematic diagram and scanning electron microscope image are shown in Figure Figure 9 . A semiconductor analyzer (Keithley 4200A-SC) was used to test the electrical performance of the device. A 532 nm wavelength laser (calibrated by a Thorlabs PM100D power meter) was vertically irradiated on the channel, and the light power density P in was adjustable in the range of 0.10-10.19 mW / cm 2 ; the sample temperature was constant at 300 K by a Lake Shore 336 temperature controller. Under zero bias conditions, the device produced a significant short-circuit current I sc and an open-circuit voltage V oc . When the 532 nm laser power density increased from 0.10 mW / cm 2 to 10.19 mW / cm 2 , I sc monotonically increased from 0.32 nA to 5.07 nA, and V oc asymptotically from 90 mV to 0.20 V (Figure Figure 10 ), confirming that the device has a self-driven photoelectric conversion capability; the built-in electric field induced by the gradient drives the photo-generated carriers to separate directionally, and high-efficiency photovoltaic response can be achieved without an external bias. According to the measured Isc With the incident power P in , the core performance parameters: responsivity R, external quantum efficiency EQE and detectivity D* are calculated, and the results (a-c) show that all gradually decrease with the increase of power, which is consistent with the general law of photovoltaic devices. When the incident power density is 0.10 mW / cm 2 , R = 5.04 A / W, EQE = 1170%, D* = 3.23 × 10 12 Jones. Figure 10 d in the above shows the time-resolved switching curve (I-T) under different powers under 0.1 Hz square wave modulation, and the device shows fast and repeatable optical switching characteristics. Figure 10
[0036] The above results fully prove that the self-driven photodetector based on the width gradient nanobelt of the application has excellent photoelectric performance, and can realize high responsivity and high detectivity of photoelectric conversion under zero bias voltage, and has practical application value in the field of optical signal detection and optical switching.
[0037] Although the basic structure and performance of the self-driven photodetector have been described in detail in the above embodiments, those skilled in the art should understand that the detector can be further extended to various application scenarios. For example, by integrating a signal amplification circuit and a wireless communication module, the photodetector can be used as a receiving end in a wireless optical communication system; by being packaged in a flexible substrate and combined with an environmental monitoring sensor, it can be used for light intensity monitoring in extreme environments; by miniaturization design and integration with wearable electronic devices, it can be used for light signal acquisition in human health monitoring. These applications are all based on the core advantages of the detector described in the application, such as self-driving, fast response and good stability, and belong to the protection scope of the application.
Claims
1. A method for preparing tungsten disulfide nanoribbons with width gradient, characterized in that, The method comprises the following steps: (1) depositing a metal Ni film with a thickness of 2-10 nm on a SiO2 / Si substrate, and then annealing in a reducing atmosphere at 900-1000 ℃ for 1-3 hours; (2) placing sulfur powder at a position 30-40 cm away from the center of a chemical vapor deposition tube furnace, placing tungsten trioxide powder at the center temperature zone of the tube furnace, and placing the growth substrate obtained in step (1) at a position 15-20 cm away from the center of the tube furnace, with the temperature of the position being set to be 50-100 ℃ lower than that of the center temperature zone; (3) when the center temperature zone is raised to 950-1050 ℃, a mixed gas of hydrogen and argon is introduced, and the solid sulfur powder is pushed from the normal temperature zone to the high temperature zone at a constant rate to carry out a growth reaction, thereby forming a width gradient tungsten disulfide nanobelt on the substrate; and (4) after the growth is completed, the pushing of the sulfur source is stopped, the hydrogen is turned off, and the temperature is cooled to room temperature under a protective atmosphere.
2. The method of claim 1, wherein the width-gradient tungsten disulfide nanoribbons are prepared by the method comprising: In step (3), the hydrogen flow rate is 5-50 sccm, the argon flow rate is 100-300 sccm, the pushing rate of the solid sulfur powder is 0.5-2 cm / min, and the growth time is 5-20 min.
3. The method of claim 1 or 2, wherein the folded width-graded tungsten disulfide nanoribbons have a width gradient of 0.1 nm to 10 nm. The nanobelt has a structure in which the wide end is connected to Ni, the narrow end is sharp and suspended, and the width gradient changes continuously along the growth direction.
4. The width-gradient tungsten disulfide nanoribbons of claim 3, wherein, The nanobelt has a widest width of 150-500 nm, a narrowest width of 50-120 nm, and a length of 3-12 μm. The edge of the nanobelt is armchair type, and the crystal structure is 3R phase stacking.
5. The width-graded tungsten disulfide nanoribbons of claim 4, wherein, the second-order nonlinear optical susceptibility tensor component of the nanoribbon is |χ (2) xxx / χ (2) xyy | > 10, wherein χ (2) xxx corresponding to the second-order nonlinear response along the ribbon axis direction.
6. A self-driven photodetector, characterized in that, The photosensitive channel of the detector is composed of the width gradient tungsten disulfide nanobelt as described in claims 3-5.
7. The self-driven photodetector of claim 6, wherein, The width gradient tungsten disulfide nanobelt is transferred from the growth substrate to an insulating substrate, and metal electrodes are deposited at the end with a larger width and the end with a smaller width of the nanobelt, respectively, to form an asymmetric electrode contact structure.
8. The self-driven photodetector of claim 7, wherein, Under the laser irradiation with a wavelength of 532 nm and a power density of 0.10 mW / cm 2 The zero-bias responsivity is not less than 1 A / W, and the detectivity is not less than 1.0 × 10 12 Jones.
9. The self-driven photodetector of claim 7, wherein, The electrodes are titanium / gold electrodes, gold electrodes or chromium / gold electrodes, the thickness of the gold electrodes is 50-100 nm, and in the titanium / gold electrodes or the chromium / gold electrodes, the thickness of the titanium layer or the chromium layer is 1-10 nm, and the thickness of the gold layer is 50-100 nm.