Lithium manganese iron phosphate carbon interface doped modified nano coating material as well as preparation method and application thereof

By constructing a polymaleic anhydride/polypyrrole copolymer composite carbon coating layer on the surface of lithium manganese iron phosphate, the problem of insufficient conductivity of lithium manganese iron phosphate is solved, the charge and discharge rate and power output capability of the battery are improved, and the structural stability and resistance to manganese leaching of the material are enhanced.

CN121885599APending Publication Date: 2026-04-17WUHAN BOLI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610074824.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-01-20
Publication Date
2026-04-17

AI Technical Summary

Technical Problem

Lithium manganese iron phosphate, as a positive electrode material for batteries, has insufficient conductivity, resulting in slow battery charging and discharging rates and limited power output capabilities. In particular, its performance degrades rapidly under high-rate charging and discharging conditions, which limits its use in fast charging and discharging and high-power output applications.

Method used

A composite carbon coating layer with high adhesion, high conductivity and chemical barrier function is constructed by the synergistic effect of polymaleic anhydride and polypyrrole. The copolymer with block or graft structure is formed on the surface of lithium manganese iron phosphate through in-situ polymerization, which improves the conductivity and structural stability of the material.

Benefits of technology

It significantly improves the conductivity of lithium manganese iron phosphate, reduces manganese leaching rate by about 30%, decreases charge transfer resistance by about 25%, and enhances the material's cycle stability and anti-peeling ability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a lithium manganese iron phosphate carbon interface doped modified nanometer coating material and a preparation method and application thereof, and relates to the technical field of lithium ion batteries, and the preparation method comprises the following steps: adding a maleic anhydride monomer into deionized water to prepare an aqueous solution, and dropwise adding hydrogen peroxide into the aqueous solution to initiate polymerization to obtain a polymaleic anhydride pre-polymerization solution; adding a pyrrole monomer into the pre-polymerized solution, supplementing hydrogen peroxide as an oxidizing agent, and generating a polymaleic anhydride / polypyrrole copolymer through in-situ polymerization; mixing the lithium manganese iron phosphate nano-particles with the copolymer, adding a dispersing agent and a solvent, and then performing ball milling; and drying the ball-milled mixed slurry to obtain spherical precursor particles, introducing inert gas into the spherical precursor particles for protection, carrying out constant-temperature calcination, and carrying out in-situ carbonization on the copolymer to form a composite carbon coating layer with conductive network and chemical barrier functions, thereby obtaining the coating material. According to the coating material prepared by the preparation method, the conductivity of the lithium manganese iron phosphate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, specifically to a lithium manganese iron phosphate carbon interface doped modified nano-coating material, its preparation method, and its application. Background Technology

[0002] Lithium manganese phosphate has significant advantages over lithium iron phosphate in several aspects, mainly in energy density, discharge voltage platform, cost, low temperature performance, and application prospects.

[0003] Lithium manganese iron phosphate (LMP) has a higher energy density than lithium iron phosphate (LFP). Specifically, LMP has a voltage platform of 4.1V, significantly higher than LFP's 3.4V. This advantage allows LMP to theoretically achieve a 15% to 20% higher energy density than LFP under the same conditions, essentially reaching the level of ternary lithium batteries (NCM523). This means that using LMP as the cathode material can provide a longer driving range, which is of great significance for applications requiring large amounts of power, such as electric vehicles and mobile devices.

[0004] Lithium manganese iron phosphate (LMFP) also has a high discharge voltage platform, which helps to improve the voltage and power output of the battery system. In battery systems, voltage and power output are one of the important indicators for measuring battery performance. Therefore, this advantage of lithium manganese iron phosphate makes it more competitive in application scenarios that require high voltage and high power output.

[0005] Although manganese has poor electrical conductivity, global manganese ore resources are abundant, which makes the manufacturing cost of lithium manganese iron phosphate relatively low. Compared with lithium iron phosphate, the cost of lithium manganese iron phosphate is only about 5% to 10% higher. However, considering the improvement in energy density, the cost per watt-hour of lithium manganese iron phosphate in battery installation is slightly lower than that of lithium iron phosphate and significantly lower than that of ternary batteries. This makes lithium manganese iron phosphate highly competitive in terms of cost, which helps to promote its use in a wider range of application areas.

[0006] At extremely low temperatures (-20°C), lithium manganese iron phosphate can retain approximately 75% of its capacity, while lithium iron phosphate retains only 60% to 70%. This advantage makes lithium manganese iron phosphate more competitive in cold regions, meeting the specific battery performance requirements of these areas.

[0007] Given the aforementioned advantages of lithium manganese iron phosphate (LMP), it has broad application prospects in fields such as electric vehicles, energy storage devices, and consumer electronics. In the electric vehicle sector, LMP's high energy density and long lifespan can significantly improve the driving range of electric vehicles and reduce maintenance costs. In the energy storage sector, LMP's safety and stability make it an ideal choice for large-scale energy storage devices. In consumer electronics, LMP's low cost and long lifespan can reduce the overall cost of products and extend their service life.

[0008] However, lithium manganese iron phosphate, as a battery cathode material, still has shortcomings in conductivity. This shortcoming mainly stems from the characteristics of its crystal structure and the influence of manganese on the conductivity. Lithium manganese iron phosphate also has the following shortcomings in conductivity:

[0009] 1. The crystal structure of lithium manganese iron phosphate is similar to that of lithium iron phosphate, both being olivine-type structures. This structure has a relatively narrow and complex lithium-ion transport path, resulting in a slower lithium-ion diffusion rate and thus affecting the ionic conductivity of the material. Furthermore, the electron transport capability in the olivine-type structure is also relatively weak, leading to a lower electronic conductivity in lithium manganese iron phosphate.

[0010] 2. While the addition of manganese improves the voltage platform and energy density of lithium manganese iron phosphate, it also negatively impacts the material's conductivity. Manganese is prone to valence state transitions during charging and discharging, leading to structural instability and consequently affecting electron and ion transport efficiency. Furthermore, manganese leaching is a significant cause of decreased conductivity in lithium manganese iron phosphate. Manganese leaching not only reduces structural stability but also forms a resistive layer on the material surface, hindering electron and ion transport.

[0011] 3. The low conductivity of lithium manganese iron phosphate manifests in practical applications as a slow charge and discharge rate, limited power output capability, and rapid performance degradation under high charge and discharge conditions. These shortcomings limit the use of lithium manganese iron phosphate in application scenarios that require fast charge and discharge and high power output.

[0012] To improve the conductivity of lithium manganese iron phosphate (LFP), researchers have employed various modification methods, including carbon coating, ion doping, and nano-sizing. Carbon coating, by coating the material surface with a layer of highly conductive carbon, can significantly improve the electronic conductivity. Ion doping, by incorporating other metal ions into the material, creates defects or alters interatomic bond lengths, thereby increasing the ion diffusion coefficient and conductivity. Nano-sizing reduces the crystal grain size, shortens the lithium-ion diffusion path, and enhances lithium-ion migration efficiency. These modification methods have alleviated the insufficient conductivity of LFP to some extent, but current carbon coating modification methods still leave the conductivity performance somewhat lacking. Summary of the Invention

[0013] Given the existing problem of insufficient conductivity in lithium manganese iron phosphate, the present invention aims to provide a carbon interface doped modified nano-coating material for lithium manganese iron phosphate, its preparation method, and its application. The coating material prepared by this method constructs a composite carbon coating layer with high adhesion, high conductivity, and chemical barrier function through the synergistic effect of polymaleic anhydride and polypyrrole, thereby improving the conductivity of lithium manganese iron phosphate.

[0014] This invention is achieved through the following technical solution:

[0015] In a first aspect, this application provides a method for preparing a lithium manganese iron phosphate carbon interface doped modified nano-coating material, comprising the following steps:

[0016] Maleic anhydride monomer was added to deionized water to prepare an aqueous solution. Hydrogen peroxide was then added dropwise to the aqueous solution to initiate polymerization, resulting in a polymaleic anhydride prepolymer solution.

[0017] Pyrrole monomer was added to the polymaleic anhydride prepolymer solution, and hydrogen peroxide was added as an oxidant to generate polymaleic anhydride / polypyrrole copolymer through in-situ polymerization.

[0018] Lithium manganese iron phosphate nanoparticles were mixed with polymaleic anhydride / polypyrrole copolymer, and then ball-milled after adding dispersant and solvent.

[0019] The ball-milled slurry was dried to obtain spherical precursor particles. An inert gas was introduced into the spherical precursor particles for protection, and the mixture was calcined at a constant temperature to carbonize the copolymer in situ, forming a composite carbon coating layer that has both conductive network and chemical barrier functions, thus obtaining a lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0020] This invention employs hydrogen peroxide-initiated polymerization to synthesize polymaleic anhydride, followed by in-situ polymerization of pyrrole to form polypyrrole. Utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomers, the pyrrole monomers are guided to grow directionally on the long polymaleic anhydride chains, forming a stable copolymer system with block or graft structures. This constructs a polymaleic anhydride / polypyrrole block copolymer. The polymaleic anhydride segments provide a high density of carboxyl anchoring sites, forming strong chelation with metal ions on the surface of lithium manganese iron phosphate; the polypyrrole segments provide an excellent conductive network. Together, they construct a composite carbon coating layer with high adhesion, high conductivity, and chemical barrier functions, thereby improving the conductivity of lithium manganese iron phosphate.

[0021] Furthermore, the polymaleic anhydride segments, with their high-density carboxyl structure, not only achieve more uniform coating but also form stronger chemical bonds with the surface of lithium manganese iron phosphate through strong chelation, enhancing the structural stability and peel resistance of the coating layer. The polymaleic anhydride segments also provide excellent electrical conductivity. Due to the high SP2 carbon content of polypyrrole, excellent conductivity can be achieved during low-temperature firing (600℃~800℃). Compared to other carbon sources, polypyrrole forms a higher carbon density, which is beneficial for improving the compaction of lithium manganese iron phosphate, thereby further increasing its density.

[0022] In addition, due to its high-density carboxyl structure, polymaleic anhydride not only has excellent dispersibility, but also significantly enhances the interfacial bonding force with the surface of lithium manganese iron phosphate, inhibits manganese dissolution, and improves cycle stability. Meanwhile, experiments show that, compared with the polyacrylic acid system, the polymaleic anhydride / polypyrrole composite coating layer reduces the Mn dissolution rate by about 30% and the charge transfer resistance by about 25% under the same process conditions.

[0023] In one specific embodiment, the concentration of hydrogen peroxide added during the preparation of the polymaleic anhydride prepolymer is 25% to 30%.

[0024] In one specific embodiment, the concentration of hydrogen peroxide added during the preparation of the polymaleic anhydride / polypyrrole copolymer is 20% to 30%.

[0025] In one specific embodiment, the molar ratio of the maleic anhydride monomer to the pyrrole monomer is 1:(1.5~4.5).

[0026] In one specific embodiment, the molar ratio of the pyrrole monomer to the total hydrogen peroxide is controlled at 1:(0.8~3.5).

[0027] In one specific embodiment, the solid content mass ratio of the lithium manganese iron phosphate nanoparticles to the polymaleic anhydride / polypyrrole copolymer is 100:(2~10).

[0028] In one specific embodiment, the inlet air temperature of the mixed slurry during drying is 150℃~200℃, and the outlet air temperature is 80℃~110℃.

[0029] In one specific embodiment, the isothermal calcination temperature is 600℃~800℃, the heating rate is 2℃ / min~10℃ / min, and the isothermal calcination time is 4~10 hours.

[0030] Secondly, this application provides a lithium manganese iron phosphate carbon interface doped modified nano-coating material, which is prepared by the above-mentioned preparation method.

[0031] Thirdly, this application provides an application of lithium manganese iron phosphate carbon interface doped modified nano-coating material, including its use in preparing battery cathode materials.

[0032] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0033] (1) In this invention, after the synthesis of polymaleic anhydride by hydrogen peroxide-initiated polymerization, pyrrole is further polymerized in situ to form polypyrrole. The hydrogen bond and charge interaction between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomers are used to guide the directional growth of the pyrrole monomers on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structure, and constructing a polymaleic anhydride / polypyrrole block copolymer. The polymaleic anhydride segments provide high-density carboxyl anchoring sites, which form a strong chelating effect with the metal ions on the surface of lithium manganese iron phosphate; the polypyrrole segments provide an excellent conductive network. The two work together to construct a composite carbon coating layer with high adhesion, high conductivity and chemical barrier function, thereby improving the conductivity of lithium manganese iron phosphate.

[0034] (2) The polymaleic anhydride segments in this invention, with their high-density carboxyl structure, can not only achieve more uniform coating, but also form stronger chemical bonds with the surface of lithium manganese iron phosphate through strong chelation, thereby improving the structural stability and anti-peeling ability of the coating layer. The polymaleic anhydride segments can provide good electrical conductivity. Due to the high SP2 carbon content of polypyrrole, it can achieve good electrical conductivity when fired at low temperature (600℃~800℃). Compared with other carbon sources, polypyrrole forms a higher carbon density, which is beneficial to improve the compaction of lithium manganese iron phosphate, thereby further increasing the density.

[0035] (3) Due to its high-density carboxyl structure, the polymaleic anhydride in this invention not only has excellent dispersibility, but also significantly enhances the interfacial bonding force with the surface of lithium manganese iron phosphate, inhibits manganese dissolution, and improves cycle stability. At the same time, experiments show that, compared with the polyacrylic acid system, the polymaleic anhydride / polypyrrole composite coating layer reduces the Mn dissolution rate by about 30% and the charge transfer resistance by about 25% under the same process conditions. Detailed Implementation

[0036] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. The illustrative embodiments and descriptions of this invention are only used to explain this invention and are not intended to limit this invention.

[0037] In the following description, numerous specific details are set forth in order to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that these specific details are not necessary to practice the invention. In other embodiments, well-known materials or methods have not been specifically described in order to avoid obscuring the invention.

[0038] Throughout this specification, references to "an embodiment," "an example," or "an example" mean that a particular feature, structure, or characteristic described in connection with that embodiment or example is included in at least one embodiment of the invention. Therefore, the phrases "an embodiment," "an example," "an example," or "an example" appearing in various places throughout the specification do not necessarily refer to the same embodiment or example. Furthermore, specific features, structures, or characteristics can be combined in one or more embodiments or examples in any suitable combination and / or sub-combination. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described herein, as well as the features of those different embodiments or examples.

[0039] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is understood that ranges of 60–110 and 80–120 are also expected. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0040] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0041] Example 1

[0042] This embodiment provides a method for preparing a lithium manganese iron phosphate carbon interface doped modified nano-coating material, the specific preparation steps of which are as follows:

[0043] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0044] S2. A 25% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0045] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:3, and supplement with 25% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:2. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0046] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 20:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0047] Example 2

[0048] This embodiment provides a method for preparing a carbon interface-doped modified nano-coated material of lithium manganese iron phosphate. The difference from Example 1 is that the molar ratio of maleic anhydride to pyrrole in this embodiment is 1:1.5; otherwise, it is the same as Example 1. The specific preparation steps are as follows:

[0049] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0050] S2. A 25% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0051] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:1.5, and supplement with 25% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:2. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0052] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 20:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0053] Example 3

[0054] This embodiment provides a method for preparing a carbon interface-doped modified nano-coated material of lithium manganese iron phosphate. The difference from Example 1 is that the molar ratio of maleic anhydride to pyrrole in this embodiment is 1:4.5; otherwise, it is the same as Example 1. The specific preparation steps are as follows:

[0055] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0056] S2. A 25% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0057] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:4.5, and supplement with 25% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:2. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0058] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 20:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0059] Example 4

[0060] This embodiment provides a method for preparing lithium manganese iron phosphate carbon interface doped modified nano-coating material. The difference from Embodiment 1 is that the concentration of hydrogen peroxide in step S2 of this embodiment is 30%, while the rest is the same as in Embodiment 1. The specific preparation steps are as follows:

[0061] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0062] S2. A 30% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0063] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:3, and supplement with 25% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:2. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0064] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 20:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0065] Example 5

[0066] This embodiment provides a method for preparing a carbon interface-doped modified nano-coated material of lithium manganese iron phosphate. Unlike Example 1, the concentration of hydrogen peroxide in step S3 of this embodiment is 20%, and the molar ratio of pyrrole to total hydrogen peroxide is 1:0.8. Other steps are the same as in Example 1. The specific preparation steps are as follows:

[0067] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0068] S2. A 25% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0069] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:3, and supplement with 20% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:0.8. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0070] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 20:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0071] Example 6

[0072] This embodiment provides a method for preparing a carbon interface-doped modified nano-coated material of lithium manganese iron phosphate. Unlike Example 1, the concentration of hydrogen peroxide in step S3 of this embodiment is 30%, and the molar ratio of pyrrole to total hydrogen peroxide is 1:3.5. Other steps are the same as in Example 1. The specific preparation steps are as follows:

[0073] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0074] S2. A 25% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0075] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:3, and supplement with 30% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:3.5. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0076] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 20:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0077] Example 7

[0078] This embodiment provides a method for preparing lithium manganese iron phosphate carbon interface doped modified nano-coating material. Compared with Example 1, in step S4 of this embodiment, lithium manganese iron phosphate nanoparticles are mixed with self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 50:1. The specific preparation steps are as follows:

[0079] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0080] S2. A 25% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0081] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:3, and supplement with 25% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:2. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0082] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 50:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0083] Example 8

[0084] This embodiment provides a method for preparing lithium manganese iron phosphate carbon interface doped modified nano-coating material. Compared with Example 1, in step S4 of this embodiment, lithium manganese iron phosphate nanoparticles are mixed with self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 10:1. The specific preparation steps are as follows:

[0085] S1. Add maleic anhydride monomer to deionized water to prepare a 25% aqueous solution. Under nitrogen protection, heat the solution to 70°C and start high-speed stirring.

[0086] S2. A 25% hydrogen peroxide solution was added dropwise using a micro-pump as an initiator. The drop rate was controlled at 1 ml / min to ensure that the system reaction was mild and did not cause violent exothermic reactions. After the addition was completed, the reaction was kept at this temperature for 4 hours to obtain a polymaleic anhydride prepolymer solution with a uniform molecular weight distribution.

[0087] S3. Adjust the temperature of the polymaleic anhydride prepolymer solution to 70℃. Slowly add pyrrole monomer to the system at a molar ratio of maleic anhydride to pyrrole monomer of 1:3, and supplement with 25% hydrogen peroxide as an oxidant. At this point, the molar ratio of pyrrole to total hydrogen peroxide is controlled at 1:2. Through in-situ polymerization, utilizing the hydrogen bonds and charge interactions between the carboxyl groups on the polymaleic anhydride segments and the pyrrole monomer, the pyrrole monomer is guided to grow directionally on the long chain of polymaleic anhydride, forming a stable copolymer system with block or graft structures. Continue stirring the reaction for 6 hours until the system turns dark black and has no obvious monomer odor. After the reaction solution cools naturally to room temperature, obtain the copolymer solid powder by vacuum concentration or spray drying, which will be used for subsequent coating modification with lithium manganese iron phosphate.

[0088] S4. Lithium manganese iron phosphate nanoparticles were mixed with a self-made polymaleic anhydride / polypyrrole copolymer at a solid content mass ratio of 10:1. Polyethylene glycol and deionized water were added, and the mixture was ball-milled for 4 hours. This allowed the copolymer to be uniformly anchored on the surface of lithium manganese iron phosphate through high-density carboxyl chelation. The ball-milled mixture was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃, to obtain spherical precursor particles with uniform coating and controllable particle size. Inert gas was introduced into the precursor powder for protection, and the temperature was increased to 700℃ at a heating rate of 7℃ / min. The mixture was then calcined at this temperature for 7 hours to allow the copolymer to carbonize in situ, forming a composite carbon coating layer that combines conductive network and chemical barrier functions, thus obtaining the lithium manganese iron phosphate carbon interface doped modified nano-coated material.

[0089] Comparative Example 1

[0090] This comparative example uses polyacrylic acid as a single carbon source, and the specific preparation method is as follows:

[0091] Lithium manganese iron phosphate nanoparticles were mixed with polyacrylic acid at a solid content mass ratio of 20:1. A dispersant and solvent were added, and the mixture was ball-milled for 4 hours. The ball-milled slurry was then spray-dried, with the inlet air temperature controlled at 180℃ and the outlet air temperature at 100℃ to obtain spherical precursor particles. An inert gas was introduced into the precursor powder for protection, and the temperature was raised to 700℃ at a rate of 7℃ / min, followed by constant-temperature calcination for 7 hours to obtain the coated material.

[0092] Comparative Example 2

[0093] This comparative example uses ferric chloride as an oxidant to prepare a polypyrrole single-coating system.

[0094] The specific method is as follows: Lithium manganese iron phosphate nanoparticles are dispersed in deionized water, pyrrole monomer is added, and after stirring and mixing evenly, ferric chloride aqueous solution is slowly added dropwise as an oxidant. The reaction is carried out at room temperature with stirring for 6-12 hours, allowing pyrrole to polymerize in situ on the surface of lithium manganese iron phosphate to form a polypyrrole coating layer. After the reaction is completed, the mixture is centrifuged and washed several times with deionized water and ethanol to obtain a polypyrrole-coated lithium manganese iron phosphate precursor. The precursor is then heated to 600℃ at a heating rate of 5℃ / min under inert gas protection and calcined at this temperature for 6 hours to obtain a polypyrrole-coated lithium manganese iron phosphate material.

[0095] The Mn dissolution rate, discharge specific capacity at 1C rate, charge transfer resistance, compaction density, and retention rate after 500 cycles of the coating materials prepared by the methods of Examples 1-8 and Comparative Examples 1-2 were tested, and the test results are shown in Table 1.

[0096] All tests were conducted at ambient temperature (25±2℃) unless otherwise specified. The specific test procedures are as follows:

[0097] For the determination of manganese (Mn) leaching rate, a high-temperature immersion combined with elemental analysis method was used. 0.500 g of sample was accurately weighed and placed in a sealed glass bottle, and 10.0 mL of commercial lithium-ion battery electrolyte (1 mol / L LiPF6 in EC / DMC, volume ratio 1:1) was added. The sample bottle was placed in a constant temperature water bath at 60°C for 7 days to simulate the harsh environment of long-term battery operation. After leaching, the supernatant was centrifuged at 8000 rpm for 10 minutes to completely separate the solid particles. Subsequently, 2.0 mL of the clarified liquid was transferred and diluted to 10 mL with 2% dilute nitric acid (analytical grade). The concentration of manganese in the solution was determined using inductively coupled plasma optical emission spectrometry (ICP-OES). The Mn leaching rate was calculated using the following formula: Leaching rate (%) = (Total mass of Mn measured in the leaching solution / Theoretical total mass of Mn in the sample) × 100%, which quantitatively evaluated the inhibitory effect of the coating layer on the leaching of manganese ions from the active material.

[0098] The specific capacity and rate performance of the materials were tested by assembling coin cells. First, the coating material to be tested was used as the positive electrode active material and mixed uniformly with conductive carbon black (Super P) and binder polyvinylidene fluoride (PVDF) in an N-methylpyrrolidone (NMP) solvent at a mass ratio of 90:5:5 to form a slurry, which was then coated onto an aluminum foil current collector. After vacuum drying at 120°C for 12 hours, a circular positive electrode sheet with a diameter of 12 mm was punched out. In an argon-filled glove box, a CR2032 type coin cell was assembled using a lithium metal sheet as the counter electrode, a Celgard 2325 membrane as the separator, and 1 mol / L LiPF6 in EC / DMC / EMC (1:1:1) as the electrolyte. After a 12-hour static activation period, the battery underwent charge-discharge testing on a battery testing system. First, activation was completed by three charge-discharge cycles at a low current of 0.1C (1C is calculated as 170 mA / g). Then, constant current-constant voltage charging (to 4.5V, cutoff current 0.05C) and constant current discharging (to 2.0V) were performed at a rate of 1C. The discharge capacity was recorded, and the discharge specific capacity per unit mass of active material (unit: mAh / g) was calculated.

[0099] Electrochemical impedance spectroscopy (EIS) was used to characterize the charge transfer resistance inside the battery. The assembled half-cell was charged to 50% state of charge (SOC, approximately 3.8V) and then tested on an electrochemical workstation. The test frequency range was 100 kHz to 10 mHz, and the AC perturbation signal amplitude was 5 mV. The obtained Nyquist plots were analyzed using specialized equivalent circuit fitting software (such as ZView). An equivalent circuit model incorporating solution resistance, constant phase angle elements, and charge transfer resistance was used for fitting. The charge transfer resistance (Rct) value was directly read from the fitting results, which directly reflects the ease or difficulty of reaction kinetics at the electrode / electrolyte interface.

[0100] Compacted density was determined using the powder compression method. 0.500 g of dry coating material powder was weighed and placed into a cylindrical mold with a diameter of 10 mm. A dense disc was prepared by pressing the disc under 10 MPa pressure for 30 seconds using a powder press. The mass of the compressed disc was accurately weighed using an electronic balance (accuracy 0.1 mg), and its thickness and diameter were measured using a digital caliper (accuracy 0.01 mm). The compacted density was calculated using the cylinder volume formula: Compacted density (g / cm³) = Mass of compressed disc / (π × (diameter / 2)² × thickness). Each sample was tested in parallel five times, and the average value was taken. This indicator is crucial for evaluating the volumetric energy density of the positive electrode.

[0101] Long-term cycle stability was evaluated using standard charge-discharge cycle testing. Assembled coin cells were placed in a constant-temperature test environment and subjected to continuous charge-discharge cycles at a constant rate of 1C, with a charge-discharge voltage range of 2.0–4.5 V. After every 50 cycles, a calibration cycle at a 0.1C rate was interspersed to monitor capacity decay trends. The discharge capacity of the battery was recorded at the 1st and 500th cycles. The capacity retention rate after 500 cycles was calculated using the following formula: Retention Rate (%) = (Discharge Capacity at 500th Cycle / Discharge Capacity at 1st Cycle) × 100%. This data directly reflects the structural stability and capacity decay of the material during long-term use.

[0102] Table 1

[0103] sample Mn dissolution rate Discharge specific capacity at 1C rate Charge transfer resistance compaction density Retention rate after 500 cycles Example 1 1.1 162 38 2.48 93.5 Example 2 1.5 152 50 2.41 90.8 Example 3 1.8 155 48 2.43 91.2 Example 4 1.3 157 44 2.44 92.0 Example 5 1.4 154 46 2.42 91.5 Example 6 1.6 156 45 2.44 91.8 Example 7 2.1 148 55 2.38 89.0 Example 8 1.0 158 42 2.45 94.0 Comparative Example 1 3.5 142 80 2.30 85.0 Comparative Example 2 4.2 138 95 2.25 82.5

[0104] Comparative Example 1, using polyacrylic acid as a single carbon source for coating, exhibited significantly inferior performance data compared to the embodiments of this invention. This directly reflects the limitations of the single polyacrylic acid carbon coating system in addressing key issues of lithium manganese iron phosphate. Firstly, regarding manganese leaching inhibition, Comparative Example 1 showed a Mn leaching rate as high as 3.5%, far exceeding that of the embodiments (generally between 1.0% and 2.1%). This is primarily because the carboxyl group density and chelating ability of polyacrylic acid are weaker than those of polymaleic anhydride, resulting in insufficient bonding with metal ions on the lithium manganese iron phosphate surface. This inability to effectively anchor manganese ions leads to easier leaching during long-term immersion or cycling in the electrolyte, thereby damaging the material structure and forming an insulating layer on the surface. Secondly, in terms of electrochemical performance, Comparative Example 1 exhibited a 1C discharge specific capacity of only 142 mAh / g and a charge transfer resistance as high as 80 Ω, significantly inferior to the embodiments. This stems from the low degree of graphitization of the carbon layer formed after polyacrylic acid carbonization, resulting in insufficient conductivity and failure to construct an efficient electronic conductive network. Furthermore, the poor interfacial bonding also increases the resistance to charge transport at the interface. Furthermore, the compaction density (2.30 g / cm³) and capacity retention rate after 500 cycles (85.0%) of Comparative Example 1 were also relatively low, indicating that its carbon coating layer had limited effect in improving the material's tap density and maintaining long-term structural stability. In summary, the data from Comparative Example 1, from the opposite perspective, confirms the necessity of using polymaleic anhydride / polypyrrole copolymer in this invention: the synergistic effect of the two achieves a combination of strong interfacial anchoring, a highly conductive network, and an effective chemical barrier, thereby comprehensively improving the material's performance.

[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be covered within the scope of the claims and specification of the present invention.

Claims

1. A method for preparing a lithium manganese iron phosphate carbon interface doped modified nano-coating material, characterized in that, Includes the following steps: Maleic anhydride monomer was added to deionized water to prepare an aqueous solution. Hydrogen peroxide was then added dropwise to the aqueous solution to initiate polymerization, resulting in a polymaleic anhydride prepolymer solution. Pyrrole monomer was added to the polymaleic anhydride prepolymer solution, and hydrogen peroxide was added as an oxidant to generate polymaleic anhydride / polypyrrole copolymer through in-situ polymerization. Lithium manganese iron phosphate nanoparticles were mixed with polymaleic anhydride / polypyrrole copolymer, and then ball-milled after adding dispersant and solvent. The ball-milled slurry was dried to obtain spherical precursor particles. An inert gas was introduced into the spherical precursor particles for protection, and the mixture was calcined at a constant temperature to carbonize the copolymer in situ, forming a composite carbon coating layer that has both conductive network and chemical barrier functions, thus obtaining a lithium manganese iron phosphate carbon interface doped modified nano-coated material.

2. The preparation method of the lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 1, characterized in that, The concentration of hydrogen peroxide added during the preparation of the polymaleic anhydride prepolymer solution is 25%~30%.

3. The preparation method of the lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 1, characterized in that, The concentration of hydrogen peroxide added during the preparation of the polymaleic anhydride / polypyrrole copolymer is 20%~30%.

4. The preparation method of a lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 1, characterized in that, The molar ratio of the maleic anhydride monomer to the pyrrole monomer is 1:(1.5~4.5).

5. The preparation method of a lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 1, characterized in that, The molar ratio of the pyrrole monomer to the total hydrogen peroxide is controlled at 1:(0.8~3.5).

6. The preparation method of a lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 1, characterized in that, The solid content mass ratio of the lithium manganese iron phosphate nanoparticles to the polymaleic anhydride / polypyrrole copolymer is 100:(2~10).

7. The preparation method of a lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 1, characterized in that, The inlet air temperature during the drying of the mixed slurry is 150℃~200℃, and the outlet air temperature is 80℃~110℃.

8. The preparation method of a lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 1, characterized in that, The constant temperature calcination temperature is 600℃~800℃, the heating rate is 2℃ / min~10℃ / min, and the constant temperature calcination time is 4~10 hours.

9. A lithium manganese iron phosphate carbon interface doped modified nano-coating material, characterized in that, The coating material is prepared by the preparation method described in any one of claims 1 to 8.

10. The application of the lithium manganese iron phosphate carbon interface doped modified nano-coating material according to claim 9, characterized in that, This includes materials used to prepare battery cathodes.