Ultrathin anti-sliding layer material based on industrial solid waste
The composite filler preparation process using multi-component solid waste and SBS-modified emulsified asphalt improves the skid resistance and rutting resistance of asphalt pavement, solves the problems of high cost and poor interfacial adhesion of traditional anti-skid layer materials, and realizes efficient utilization of solid waste resources and environmentally friendly maintenance.
Patent Information
- Application Number
- CN202610180076.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-09
- Publication Date
- 2026-05-19
AI Technical Summary
The anti-skid performance of existing asphalt pavements declines over long-term use. Traditional anti-skid layer materials are costly and unsustainable. Steel slag has poor interfacial adhesion with asphalt, and waste tire rubber powder is not compatible with asphalt, making it difficult to meet the needs of modern road traffic.
Using multi-component solid waste as the core raw material, combined with SBS modified emulsified asphalt, and through the preparation process of composite fillers, including the compounding of polymer-coated rubber powder, recycled LDPE particles and silanized fly ash, chemical bonds are formed to improve the interfacial bonding strength and material stability.
It improves skid resistance and rutting resistance, solves the performance defects of traditional materials, realizes the efficient utilization of solid waste resources, and provides an environmentally friendly and efficient asphalt pavement maintenance solution.
Smart Images

Figure REF-OBJ-1770605469774-000001
Abstract
Description
Technical Field
[0001] This invention relates to the field of road engineering materials technology, specifically to an ultra-thin anti-skid layer material based on industrial solid waste. Background Technology
[0002] Over long-term use, asphalt pavements are prone to surface function degradation due to repeated exposure to environmental factors and traffic loads. Ultraviolet radiation, oxidative aging, and water erosion can lead to the deterioration of asphalt binder properties, manifesting as decreased skid resistance, microcrack expansion, and aggregate spalling, thereby affecting driving safety and pavement durability. Furthermore, traditional anti-skid layer materials often rely on new polymer modifiers, which are costly and unsustainable. At the same time, the skid resistance and durability of traditional materials are insufficient to meet the demands of modern road traffic.
[0003] While waste tire rubber powder can improve elasticity and crack resistance as an asphalt modifier, it has significant drawbacks when used alone. The powder has a highly inert surface, poor compatibility with asphalt, and is prone to agglomeration and segregation, leading to insufficient storage stability. At high temperatures, the powder softens, causing a decrease in the rutting resistance of the anti-skid layer, while at low temperatures, its insufficient rigidity makes it difficult to provide adequate shear resistance. Furthermore, rubber-modified asphalt often lacks sufficient adhesion and abrasion resistance, making it difficult to meet the stringent requirements of high strength and durability for extremely thin anti-skid layers.
[0004] Steel slag, a major solid waste from the steel industry, is produced in my country annually, exceeding 100 million tons. However, its comprehensive utilization rate is less than 10%, and large-scale stockpiling not only occupies land but also poses a potential environmental pollution risk. Nevertheless, steel slag possesses high hardness, high polishing value, and good angularity, making its physical and mechanical properties ideal for road surface anti-skid materials. In recent years, domestic and international scholars have attempted to apply steel slag to asphalt mixtures, finding that it can significantly improve rutting resistance and anti-skid performance. However, the poor interfacial adhesion between steel slag and asphalt, along with the risk of volume expansion, limits its large-scale application.
[0005] Therefore, it is necessary to provide an improved anti-skid layer material to solve the above problems. Summary of the Invention
[0006] To address the shortcomings of existing technologies, the present invention aims to provide an ultra-thin anti-skid layer material based on industrial solid waste. This invention uses multi-component solid waste as the core raw material, combined with SBS modified emulsified asphalt, to develop a novel ultra-thin anti-skid layer material. This material improves the anti-skid performance of the road surface and alleviates rutting, while also achieving efficient utilization of solid waste resources. This provides the road maintenance industry with an environmentally friendly, efficient, and high-performance asphalt pavement maintenance solution.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 60-80 parts steel slag, 10-15 parts composite filler, 2-4 parts waste glass fiber, and 12-18 parts SBS modified emulsified asphalt.
[0008] In the technical solution disclosed in this invention, the steel slag is selected as single-grade steel slag with a particle size of 3-6mm or 4-7mm. The number of parts of steel slag can be 60, 62, 65, 68, 70, 72, 75, 78, or 80 parts, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0009] In the technical solution disclosed in this invention, the preparation method of the composite filler is as follows: S1. Waste tire rubber powder, maleic anhydride and dicumyl peroxide are mixed evenly in a high-speed mixer, then extruded and granulated by a twin-screw extruder, crushed and sieved to obtain polymer-coated rubber powder. S2. Mix waste LDPE film fragments and antioxidants evenly, plasticize them in a two-roll mill, then extrude and granulate them through a twin-screw extruder, crush and sieve them to obtain recycled LDPE granules. S3. Disperse fly ash in an ethanol aqueous solution, then add silane coupling agent KH560, stir, filter, wash and dry to obtain silanized fly ash. S4. Add polymer-coated rubber powder, recycled LDPE granules and PE-g-MAH compatibilizer to a mixer for mixing to obtain a premix; then mix the premix and silanized fly ash evenly on a two-roll mill, and then granulate through a twin-screw extruder to obtain the composite filler.
[0010] In the technical solution disclosed in this invention, in step S1, the mass ratio of the waste tire rubber powder, maleic anhydride and dicumyl peroxide is 100:1.5-3:0.2-0.5.
[0011] In the technical solution disclosed in this invention, in step S1, the mesh size of the waste tire rubber powder is 80 mesh.
[0012] In step S1, dicumyl peroxide (DCP) acts as a free radical initiator, decomposing under high-temperature shear conditions to generate free radicals. These free radicals initiate a graft copolymerization reaction between the active sites on the polymer powder molecular chain and MAH, forming chemical bonds. Carboxyl and anhydride groups are introduced onto the surface of the polymer powder. The polymer-coated polymer powder serves as an elastic reinforcing phase, providing flexibility and fatigue resistance in the composite system. Simultaneously, its surface-active groups can form chemical or physical crosslinks with recycled LDPE and fly ash, optimizing the overall interfacial bonding.
[0013] In the technical solution disclosed in this invention, in step S2, the mass ratio of the waste LDPE film fragments to the antioxidant is 100:0.3-0.8. For example, 100:0.3, 100:0.4, 100:0.5, 100:0.6, 100:0.7, and 100:0.8 can be selected, but it is not limited to the listed values. Other unlisted values within the range are also applicable.
[0014] In the technical solution disclosed in this invention, in step S2, the antioxidant is selected from antioxidant 1010 or antioxidant 168.
[0015] In the technical solution disclosed in this invention, in step S2, the plasticizing temperature is 145-155℃, for example, 145℃, 150℃, or 155℃ can be selected; the plasticizing time is 3-5min, for example, 3min, 4min, or 5min can be selected, but it is not limited to the listed values. Other unlisted values within the range are also applicable.
[0016] In step S2, waste LDPE is plasticized by a two-roll open mill and melt-granulated by twin-screw extrusion to achieve molecular chain rearrangement and partial chain breakage regeneration. The addition of antioxidants inhibits oxidative degradation during high-temperature processing and maintains the mechanical properties of LDPE.
[0017] In the technical solution disclosed in this invention, in step S3, the mass ratio of fly ash to silane coupling agent KH560 is 100:1-3. For example, 100:1, 100:1.5, 100:2, 100:2.5, and 100:3 can be selected, but are not limited to the listed values. Other unlisted values within the range are also applicable.
[0018] In step S3, the fly ash is treated with silane coupling agent KH560. The silanols (-SiOH) on its surface undergo a condensation reaction with the silanols (-Si(OH)3) generated by the hydrolysis of KH560, forming chemical bonds. The long-chain organic groups (such as epoxy groups) of KH560 have enhanced affinity with the polymer matrix, strengthening the interfacial bonding force. At the same time, the hydrophobic treatment reduces the hygroscopicity of the fly ash and reduces the risk of water erosion.
[0019] In the technical solution disclosed in this invention, in step S4, the mass ratio of polymer-coated adhesive powder, recycled LDPE particles, PE-g-MAH compatibilizer and silanized fly ash is 60-80:30-50:4-8:15-30.
[0020] In the technical solution disclosed in this invention, in step S4, the mixing temperature is 145-155℃ and the mixing time is 5-10min.
[0021] In the technical solution disclosed in this invention, in step S4, the initial mixing temperature is 140-150℃ and the initial mixing time is 5-10 min.
[0022] In step S4, the components are uniformly dispersed through segmented mixing using an internal mixer and a two-roll mill.
[0023] The composite filler provided by this invention uses waste plastics, fly ash, and polymer-coated rubber powder for compounding. The continuous network or island structure formed by the waste plastics effectively "locks in" the rubber powder particles, inhibiting their softening and flow at high temperatures, thereby significantly improving the anti-rutting ability of the anti-skid layer material. The elastic particles of the rubber powder also act as stress concentration points and flexible buffer units, preventing the propagation of brittle cracks in the plastic phase at low temperatures and improving low-temperature crack resistance. The silanized fly ash, as rigid particles, is dispersed in the organic matrix. When the material is under stress, these hard particles can bear and disperse stress, improving modulus and compressive strength. After treatment with a silane coupling agent, the fly ash particles form chemical bonds or strong physical adsorption with the organic phase (rubber powder, plastic), effectively transferring stress at the interface and improving the toughness of the material.
[0024] Compared to the physical blending of rubber powder, waste plastics and fly ash, this invention uses a smelting process to composite rubber powder, waste plastics and activated fly ash. The high-temperature shearing action during the smelting process promotes the formation of chemical bonds between the components, significantly improving the interfacial bonding strength and effectively solving the common component segregation problem in physical blending. This results in materials with better stability and storage performance. The final composite filler has excellent comprehensive performance, maintaining the advantages of each component while overcoming the performance defects of single materials through synergistic effects.
[0025] In the technical solution disclosed in this invention, the length of the waste glass fiber is 5-50 mm, more preferably 10-20 mm, and the number of waste glass fibers can be selected as 2 parts, 2.5 parts, 3 parts, 3.5 parts, or 4 parts, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0026] In the technical solution disclosed in this invention, the SBS modified emulsified asphalt has an Englar viscosity of 1-10s at 25°C, a penetration of 40-120 (0.1mm), a softening point ≥50°C, and a ductility ≥20cm at 5°C. The number of parts of the SBS modified emulsified asphalt can be selected as 12, 13, 14, 15, 16, 17, or 18 parts, but is not limited to the listed values. Other unlisted values within the range are also applicable.
[0027] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention uses multi-component solid waste as the core raw material and combines it with SBS modified emulsified asphalt to develop a new type of ultra-thin anti-skid layer material, which improves the anti-skid performance of the road surface and alleviates road rutting. At the same time, it realizes the efficient utilization of solid waste resources and provides the road maintenance industry with an environmentally friendly, efficient and high-performance asphalt pavement maintenance solution.
[0028] (2) The composite filler provided by the present invention is compounded by using waste plastics, fly ash and polymer-coated rubber powder. The continuous network or island structure formed by the waste plastics effectively "locks" the rubber powder particles and inhibits their softening and flow at high temperature, thereby greatly improving the anti-rutting ability of the anti-skid layer material. The elastic particles of the rubber powder also act as stress concentration points and flexible buffer units, preventing the expansion of brittle cracks in the plastic phase at low temperature and improving the low temperature crack resistance. The silanized fly ash, as rigid particles, is dispersed in the organic matrix. When the material is under stress, these hard particles can bear and disperse the stress, improve the modulus and compressive strength. After being treated with silane coupling agent, the fly ash particles form chemical bonds or strong physical adsorption with the organic phase (rubber powder, plastic), effectively transferring stress at the interface and improving the toughness of the material.
[0029] (3) Compared with the physical blending of rubber powder, waste plastic and fly ash directly, the present invention combines rubber powder, waste plastic and activated fly ash through a smelting process. The high temperature shearing action during the smelting process promotes the formation of chemical bonds between the components, greatly improves the interfacial bonding strength, effectively solves the common component segregation problem in physical blending, and makes the material have better stability and storage performance. The final composite filler has excellent comprehensive performance, which not only maintains the characteristic advantages of each component, but also overcomes the performance defects of single materials through synergistic effect. Detailed Implementation
[0030] The present invention will be further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0031] It should be noted that, unless otherwise specified, all chemical reagents involved in this invention were purchased through commercial channels.
[0032] The steel slag used in this embodiment of the invention is single-grade steel slag with a particle size of 4-7 mm; the length of waste glass fiber is 10-20 mm; the grade of fly ash is Grade I; the solid content of SBS modified emulsified asphalt is 70 wt%, the SBS content is 6 wt%, the Engler viscosity at 25℃ is 4 s, the penetration is 65 (0.1 mm), the softening point is 60℃, the ductility at 5℃ is 22 cm; and the mesh size of waste tire rubber powder is 80 mesh.
[0033] Example 1 An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 65 parts steel slag, 12 parts composite filler, 3 parts waste glass fiber, and 15 parts SBS modified emulsified asphalt.
[0034] The preparation method of the composite filler is as follows: S1. Mix 100 parts of waste tire rubber powder, 1.5 parts of maleic anhydride and 0.2 parts of dicumyl peroxide in a high-speed mixer at a speed of 1000 rpm for 10 min, then extrude and granulate the mixture through a twin-screw extruder at 160°C, and pulverize it through an 80-mesh sieve to obtain polymer-coated rubber powder. S2. Mix 100 parts of waste LDPE film fragments and 0.3 parts of antioxidant 1010 evenly, plasticize in a two-roll mill at 150°C for 4 minutes, then extrude and granulate through a twin-screw extruder at 145°C, and crush through an 80-mesh sieve to obtain recycled LDPE granules. S3. Disperse 100 parts of fly ash in 1000 parts of ethanol aqueous solution (volume ratio of ethanol to water is 4:1), then add 2 parts of silane coupling agent KH560, stir at room temperature for 3 hours, filter, wash and dry to obtain silanized fly ash. S4. Add 60 parts of polymer-coated rubber powder, 30 parts of recycled LDPE granules and 4 parts of PE-g-MAH compatibilizer to a mixer and mix at 150°C for 8 minutes to obtain a premix. Then mix the premix with 30 parts of silanized fly ash on a two-roll mill at 145°C for 8 minutes. Finally, extrude and granulate the mixture using a twin-screw extruder at 155°C to obtain the composite filler.
[0035] Example 2 An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 60 parts steel slag, 10 parts composite filler, 2 parts waste glass fiber, and 12 parts SBS modified emulsified asphalt.
[0036] The preparation method of the composite filler is as follows: S1. Mix 100 parts of waste tire rubber powder, 2 parts of maleic anhydride and 0.4 parts of dicumyl peroxide in a high-speed mixer at a speed of 1000 rpm for 10 min, then extrude and granulate the mixture through a twin-screw extruder at 160°C, and pulverize it through an 80-mesh sieve to obtain polymer-coated rubber powder. S2. Mix 100 parts of waste LDPE film fragments and 0.5 parts of antioxidant 1010 evenly, plasticize in a two-roll mill at 150°C for 4 minutes, then extrude and granulate through a twin-screw extruder at 145°C, and crush through an 80-mesh sieve to obtain recycled LDPE granules. S3. Disperse 100 parts of fly ash in 1000 parts of ethanol aqueous solution (volume ratio of ethanol to water is 4:1), then add 1 part of silane coupling agent KH560, stir at room temperature for 3 hours, filter, wash and dry to obtain silanized fly ash. S4. Add 80 parts of polymer-coated rubber powder, 50 parts of recycled LDPE granules and 8 parts of PE-g-MAH compatibilizer to a mixer and mix at 150°C for 8 minutes to obtain a premix. Then mix the premix with 15 parts of silanized fly ash on a two-roll mill at 145°C for 8 minutes. Finally, extrude and granulate the mixture using a twin-screw extruder at 155°C to obtain the composite filler.
[0037] Example 3 An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 80 parts steel slag, 15 parts composite filler, 4 parts waste glass fiber, and 18 parts SBS modified emulsified asphalt.
[0038] The preparation method of the composite filler is as follows: S1. Mix 100 parts of waste tire rubber powder, 3 parts of maleic anhydride and 0.5 parts of dicumyl peroxide in a high-speed mixer at 1000 rpm for 10 min, then extrude and granulate the mixture through a twin-screw extruder at 160°C, and pulverize it through an 80-mesh sieve to obtain polymer-coated rubber powder. S2. Mix 100 parts of waste LDPE film fragments and 0.8 parts of antioxidant 1010 evenly, plasticize in a two-roll mill at 150°C for 4 minutes, then extrude and granulate through a twin-screw extruder at 145°C, and crush through an 80-mesh sieve to obtain recycled LDPE granules. S3. Disperse 100 parts of fly ash in 1000 parts of ethanol aqueous solution (volume ratio of ethanol to water is 4:1), then add 3 parts of silane coupling agent KH560, stir at room temperature for 3 hours, filter, wash and dry to obtain silanized fly ash. S4. Add 70 parts of polymer-coated rubber powder, 40 parts of recycled LDPE granules and 6 parts of PE-g-MAH compatibilizer to a mixer and mix at 150°C for 8 minutes to obtain a premix. Then mix the premix with 20 parts of silanized fly ash on a two-roll mill at 145°C for 8 minutes. Finally, extrude and granulate the mixture using a twin-screw extruder at 155°C to obtain the composite filler.
[0039] Comparative Example 1 An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 65 parts steel slag, 12 parts waste tire rubber powder, 3 parts waste glass fiber, and 15 parts SBS modified emulsified asphalt.
[0040] Compared with Example 1, waste tire rubber powder was used to replace the composite filler in Comparative Example 1.
[0041] Comparative Example 2 An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 65 parts steel slag, 12 parts composite filler, 3 parts waste glass fiber, and 15 parts SBS modified emulsified asphalt.
[0042] The preparation method of the composite filler is as follows: S1. Mix 100 parts of waste tire rubber powder, 1.5 parts of maleic anhydride and 0.2 parts of dicumyl peroxide in a high-speed mixer at a speed of 1000 rpm for 10 min, then extrude and granulate the mixture through a twin-screw extruder at 160°C, and pulverize it through an 80-mesh sieve to obtain polymer-coated rubber powder. S2. Disperse 100 parts of fly ash in 1000 parts of ethanol aqueous solution (volume ratio of ethanol to water is 4:1), then add 2 parts of silane coupling agent KH560, stir at room temperature for 3 hours, filter, wash and dry to obtain silanized fly ash. S3. Add 60 parts of polymer-coated rubber powder and 4 parts of PE-g-MAH compatibilizer to a mixer and mix at 150°C for 8 minutes to obtain a premix. Then mix the premix with 30 parts of silanized fly ash on a two-roll mill at 145°C for 8 minutes. Finally, extrude and granulate the mixture using a twin-screw extruder at 155°C to obtain the composite filler.
[0043] Compared with Example 1, no recycled LDPE particles were added to the composite filler in Comparative Example 2.
[0044] Comparative Example 3 An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 65 parts steel slag, 12 parts composite filler, 3 parts waste glass fiber, and 15 parts SBS modified emulsified asphalt.
[0045] The preparation method of the composite filler is as follows: S1. Mix 100 parts of waste tire rubber powder, 1.5 parts of maleic anhydride and 0.2 parts of dicumyl peroxide in a high-speed mixer at a speed of 1000 rpm for 10 min, then extrude and granulate the mixture through a twin-screw extruder at 160°C, and pulverize it through an 80-mesh sieve to obtain polymer-coated rubber powder. S2. Mix 100 parts of waste LDPE film fragments and 0.3 parts of antioxidant 1010 evenly, plasticize in a two-roll mill at 150°C for 4 minutes, then extrude and granulate through a twin-screw extruder at 145°C, and crush through an 80-mesh sieve to obtain recycled LDPE granules. S3. Add 60 parts of polymer-coated rubber powder, 30 parts of recycled LDPE granules and 4 parts of PE-g-MAH compatibilizer into a mixer and mix at 150°C for 8 minutes to obtain a premix; then granulate the premix by extruding it through a twin-screw extruder at 155°C to obtain the composite filler.
[0046] Compared with Comparative Example 3 and Example 1, no silanized fly ash was added to the composite filler.
[0047] Comparative Example 4 An ultra-thin anti-skid layer material based on industrial solid waste comprises the following raw materials in parts by weight: 65 parts steel slag, 12 parts composite filler, 3 parts waste glass fiber, and 15 parts SBS modified emulsified asphalt.
[0048] The preparation method of the composite filler is as follows: S1. Mix 100 parts of waste tire rubber powder, 1.5 parts of maleic anhydride and 0.2 parts of dicumyl peroxide in a high-speed mixer at a speed of 1000 rpm for 10 min, then extrude and granulate the mixture through a twin-screw extruder at 160°C, and pulverize it through an 80-mesh sieve to obtain polymer-coated rubber powder. S2. Mix 100 parts of waste LDPE film fragments and 0.3 parts of antioxidant 1010 evenly, plasticize in a two-roll mill at 150°C for 4 minutes, then extrude and granulate through a twin-screw extruder at 145°C, and crush through an 80-mesh sieve to obtain recycled LDPE granules. S3. Disperse 100 parts of fly ash in 1000 parts of ethanol aqueous solution (volume ratio of ethanol to water is 4:1), then add 2 parts of silane coupling agent KH560, stir at room temperature for 3 hours, filter, wash and dry to obtain silanized fly ash. S4. Mix 60 parts of polymer-coated adhesive powder, 30 parts of recycled LDPE granules and 30 parts of silanized fly ash evenly in a mixer to obtain the composite filler.
[0049] Compared with Example 1, Comparative Example 4 involved the physical blending of polymer-coated adhesive powder, recycled LDPE particles, and silanized fly ash.
[0050] The anti-skid layer materials prepared in Examples 1-3 and Comparative Examples 1-4 were laid on the surface of SMA-13 rut slabs with a thickness of 6 mm. Performance tests were then conducted, and the experimental results are shown in Table 1.
[0051] Table 1 Performance test results for different groups As can be seen from the table, the ultra-thin anti-skid layer material provided in this embodiment of the invention can improve the lateral force coefficient, exhibit excellent wear resistance, and solve the road traffic safety problem caused by insufficient anti-skid performance of the road surface. question.
[0052] Finally, it should be noted that the above embodiments do not limit the present invention in any way. Those skilled in the art can make modifications and improvements based on the present invention. Therefore, any modifications or improvements made without departing from the spirit of the present invention are within the scope of protection claimed by the present invention.
Claims
1. An ultra-thin anti-slip layer material based on industrial solid waste, characterized in that, The raw materials include the following parts by weight: 60-80 parts steel slag, 10-15 parts composite filler, 2-4 parts waste glass fiber, and 12-18 parts SBS modified emulsified asphalt.
2. The ultra-thin anti-slip layer material according to claim 1, characterized in that, The preparation method of the composite filler is as follows: S1. Waste tire rubber powder, maleic anhydride and dicumyl peroxide are mixed evenly in a high-speed mixer, then extruded and granulated by a twin-screw extruder, crushed and sieved to obtain polymer-coated rubber powder. S2. Mix waste LDPE film fragments and antioxidants evenly, plasticize them in a two-roll mill, then extrude and granulate them through a twin-screw extruder, crush and sieve them to obtain recycled LDPE granules. S3. Disperse fly ash in an ethanol aqueous solution, then add silane coupling agent KH560, stir, filter, wash and dry to obtain silanized fly ash. S4. Add polymer-coated rubber powder, recycled LDPE granules and PE-g-MAH compatibilizer to a mixer for mixing to obtain a premix; then mix the premix and silanized fly ash evenly on a two-roll mill, and then granulate through a twin-screw extruder to obtain the composite filler.
3. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S1, the mass ratio of waste tire rubber powder, maleic anhydride and dicumyl peroxide is 100:1.5-3:0.2-0.
5.
4. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S2, the mass ratio of waste LDPE film fragments to antioxidant is 100:0.3-0.
8.
5. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S2, the antioxidant is selected from antioxidant 1010 or antioxidant 168.
6. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S2, the plasticizing temperature is 145-155℃ and the plasticizing time is 3-5 min.
7. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S3, the mass ratio of fly ash to silane coupling agent KH560 is 100:1-3.
8. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S4, the mass ratio of polymer-coated adhesive powder, recycled LDPE particles, PE-g-MAH compatibilizer, and silanized fly ash is 60-80:30-50:4-8:15-30.
9. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S4, the mixing temperature is 145-155℃ and the mixing time is 5-10 minutes.
10. The ultra-thin anti-slip layer material according to claim 2, characterized in that, In step S4, the initial refining temperature is 140-150℃, and the initial refining time is 5-10 minutes.