Use of a catalyst combination in the preparation of n-alkylcarbazoles
Patent Information
- Application Number
- CN202610921851.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-25
- Publication Date
- 2026-09-11
- Estimated Expiration
- 2046-06-25
AI Technical Summary
同样,在该体系中,反应温度虽低于部分传统工艺,但仍属高温能耗过程,对加热设备和能源消耗要求较高
(1)本发明提供了一种利用特定组合催化剂来合成N-烷基咔唑的方法,通过在合成N-烷基咔唑的原料体系中,先加入钌基催化剂进行反应,然后在分离除去钌基催化剂后再加入钯基催化剂,通过两步催化配合,其实现了合成中对酸碱等添加剂的省略,并在较低的反应温度下实现了高效催化,在大幅提升N-烷基咔唑产率的同时,还实现了催化剂的高回收活性。
Smart Images

Figure CN122482981B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of organic catalysis technology, and particularly relates to the application of a catalyst combination in the preparation of N-alkylcarbazole. Background Technology
[0002] Hydrogen energy is an abundant, green, low-carbon, and widely applicable secondary energy source. Developing hydrogen energy is crucial for building a clean, low-carbon, safe, and efficient energy system. However, the safe and efficient storage and transportation of hydrogen have limited its development. Hydrogen storage is one of the core technologies in the hydrogen energy industry. Among numerous hydrogen storage technologies, organic liquid hydrogen storage technology stands out due to its advantages such as high storage capacity, safe and convenient transportation, and reusability, becoming a current research hotspot in the hydrogen energy field. N-alkylcarbazole, with its advantages of high capacity, suitable operating temperature, low volatility, and low toxicity, has become a widely recognized organic liquid hydrogen storage carrier.
[0003] The synthesis of N-alkylcarbazole, represented by the synthesis of N-ethylcarbazole, involves a typical method where carbazole is reacted with sodium hydroxide or potassium hydroxide in a suitable solvent to generate sodium or potassium carbazole salts. These salts are then reacted with an alkylating agent to obtain the corresponding product. Industrially viable synthetic routes include the haloalkane method, the diethyl sulfate method, and the ethyl p-toluenesulfonate method. The preparation of N-ethylcarbazole from carbazole is influenced by numerous factors, including deprotonating agents (bases), alkylating agents, solvents, and catalysts. Carbazole requires the removal of hydrogen atoms from the nitrogen atom in a strong base system to generate carbazole salts. These salts further react with alkylating agents to produce N-ethylcarbazole, but this generates waste salts. Furthermore, the addition of appropriate organic solvents is usually necessary to accelerate the deprotonation of carbazole. These synthetic routes require large amounts of strong bases and organic solvents, resulting in high costs, complex operations, numerous byproducts, and significant pollution.
[0004] Some new synthesis methods have been developed that eliminate the need for additives such as strong bases, but some shortcomings still exist.
[0005] CN116920855A discloses a method for synthesizing N-alkylcarbazole using a heterogeneous catalyst. The method involves reacting carbazole with an alkyl alcohol in the presence of a catalyst to obtain N-alkylcarbazole. The catalyst comprises an active component Cu and a support, wherein the support is a MOx / ZrO2 solid solution. While this method offers advantages such as environmental friendliness and the absence of byproduct salts, it suffers from several drawbacks. First, the catalytic reaction temperature is high, reaching 220-350℃, and the reaction pressure is 3-9 MPa, requiring high pressure and heat resistance from the equipment, resulting in high energy consumption and hindering industrial-scale application. Second, the catalyst requires multiple steps, including co-current precipitation to prepare the support, followed by impregnation, drying, calcination, and hydrogen reduction, making the process cumbersome. Furthermore, the use of precursors such as nitrates and chlorides may generate waste liquid. Additionally, the optimal conversion rate is only about 78% (4h), with a selectivity of about 88%, and the conversion rate drops to about 74% after 50h of operation, indicating significant catalyst deactivation and insufficient long-term stability.
[0006] CN118546088A discloses a method for the co-production of N-ethylcarbazole and N-ethylaniline. This method involves introducing aniline, ethanol, and 1,2-cyclohexanediol as reactants into a reactor, while simultaneously introducing water vapor and H2. A catalytic reaction is carried out in the reactor under the action of a catalyst to prepare N-ethylcarbazole and N-ethylaniline. The catalyst is a Ni-based composite metal catalyst supported on Al2O3, γ-Al2O3, or SiO2. The catalytic reaction temperature is 280-380℃, and the yield of synthesized N-ethylcarbazole reaches up to 78%. Similarly, although the reaction temperature in this system is lower than some traditional processes, it is still a high-temperature and energy-intensive process, requiring high standards for heating equipment and energy consumption. The yield of N-ethylcarbazole is 68-78%, while the yield of N-ethylaniline is only 20-38%. Some N-ethylaniline is consumed as an intermediate, resulting in low overall atom utilization. Furthermore, the raw material aniline is in large excess (molar ratio of aniline, ethanol, and 1,2-cyclohexanediol is 6:5:1 to 12:9:1), and a large amount of unreacted aniline needs to be recovered, significantly increasing the separation energy consumption.
[0007] Based on the existing technologies mentioned above, how to avoid the addition of strong bases and organic solvents and other additives in the synthesis of N-alkylcarbazole, reduce costs and by-products, simplify the synthesis process, significantly reduce the reaction temperature, and further improve the yield of N-alkylcarbazole while ensuring high catalyst recovery activity has become an urgent technical problem to be solved. Summary of the Invention
[0008] To address the shortcomings of existing technologies, the present invention aims to provide an application of a catalyst combination in the preparation of N-alkylcarbazole. This invention involves first adding a ruthenium-based catalyst to the raw material system for the synthesis of N-alkylcarbazole, and then adding a palladium-based catalyst after separating and removing the ruthenium-based catalyst. This two-step catalytic combination eliminates the need for additives such as acids and bases in the synthesis and achieves highly efficient catalysis at a lower reaction temperature. This not only significantly improves the yield of N-alkylcarbazole but also results in high catalyst recovery activity.
[0009] To achieve this objective, the present invention adopts the following technical solution: This invention provides an application of a catalyst combination in the preparation of N-alkylcarbazole, the application including: Using N-alkylaniline and 1,2-cyclohexanediol as reactants, the reaction was first carried out in the presence of a first catalyst. After the reaction was completed, the first catalyst was separated and removed, and then a second catalyst was added to carry out the reaction to obtain the target product. The first catalyst is a ruthenium-based catalyst; the ruthenium-based catalyst is composed of a support and an active component, wherein the support is a nitrogen-doped amorphous mesoporous carbon material, and the active component is metallic ruthenium; The second catalyst is a palladium-based catalyst.
[0010] In this invention, N-alkylaniline and 1,2-cyclohexanediol are used as reaction raw materials. On the one hand, the synthesis method uses a combination of a ruthenium-based catalyst and a palladium-based catalyst with specific structures and compositions. On the other hand, the two catalysts are added separately and sequentially, with the ruthenium-based catalyst added first and then the palladium-based catalyst. Furthermore, after the catalytic reaction of the ruthenium-based catalyst is completed, the ruthenium-based catalyst needs to be separated and removed. When there is no ruthenium-based catalyst, the palladium-based catalyst is added, and the two catalysts are added separately for catalytic reaction.
[0011] This invention, through the adoption of a corresponding synthesis method, not only eliminates the need for additives such as acids and bases in the synthesis, but also achieves highly efficient catalysis at a lower reaction temperature. This not only significantly improves the yield of N-alkylcarbazole, but also ensures high catalyst recovery activity, maintaining high catalytic activity even after more than 6 repetitions.
[0012] The ruthenium-based catalyst described in this invention contains only metallic ruthenium as its active component. This active component, combined with a nitrogen-doped amorphous mesoporous carbon support, achieves synergistic effects, resulting in excellent catalytic performance and a high yield of N-alkylcarbazole.
[0013] When other active components, such as palladium, nickel, cobalt, or copper, are added to the active component ruthenium, the combination of multiple active components will reduce the catalytic effect and decrease the product yield. That is, when ruthenium is combined with other active components, it will not only fail to produce synergistic effect, but may even have antagonistic effect, and will not be able to better catalyze the synthesis of N-alkylcarbazole.
[0014] In this invention, if the active component ruthenium is replaced with other active components, such as palladium, nickel, cobalt or copper, while keeping the support unchanged, the catalytic effect of the catalyst will also decrease, and the yield of N-alkylcarbazole will decrease to below 65%.
[0015] The ruthenium-based catalyst described in this invention is supported on a nitrogen-doped amorphous mesoporous carbon material. This structure achieves synergistic effects when combined with the active component ruthenium, demonstrating excellent performance in the catalytic synthesis of N-alkylcarbazole.
[0016] In this invention, while keeping the active components unchanged, when the support is replaced with other supports, such as commercially available carbon nitride, aluminum oxide, zirconium oxide, silicon dioxide, titanium dioxide, activated carbon, carbon nanotubes, etc., the catalytic effect of the resulting catalyst is significantly reduced, causing the yield of N-alkylcarbazole to drop below 55%.
[0017] When the active component and support of the catalyst described in this invention are replaced simultaneously, for example, the support is replaced with commercially available carbon nitride, aluminum oxide, silicon dioxide, etc., and the active component is replaced with palladium, nickel, copper, or a mixture of ruthenium and other active components, the resulting catalyst will not be able to achieve the high efficiency of this invention, and the yield of N-alkylcarbazole will drop to below 62%.
[0018] Preferably, the support for the ruthenium-based catalyst of the present invention is prepared by the following method, which includes the following steps: mixing an organic compound containing carbon and nitrogen with a silica template agent in a solvent, pretreating at 30-100°C, centrifuging the pretreated mixture, drying it, calcining the resulting solid at 600-800°C, and removing the silica template from the calcined product with HF solution to obtain the support; wherein the silica template agent is ordered mesoporous silica.
[0019] This invention uses ordered mesoporous silica as a template, pretreats it with organic matter containing carbon and nitrogen at 30-100℃, then calcines it at 600-800℃, and then removes the silica template with HF (e.g., 10% by mass) solution to obtain the corresponding support. By selecting specific raw materials and controlling the two-step heating process and the temperature selection, nitrogen-doped amorphous mesoporous carbon materials can be prepared.
[0020] The carrier described in this invention needs to start with an ordered mesoporous silica template agent, preferably MCM-41 and / or MCM-48. By using it as a silica template agent, and in conjunction with the two-step specific temperature treatment in this invention, the transformation from an "ordered mesoporous" template agent to a nitrogen-doped "amorphous mesoporous" carbon material is achieved, thereby obtaining a better catalytic effect.
[0021] When preparing the support, regarding the selection of silica template agents, when ordered mesoporous silica is replaced with disordered mesoporous silica, such as commonly available commercially available spherical silica, fumed silica, or Ludox HS-40 colloidal silica in monodisperse solid spheres, the catalytic effect decreases significantly after being combined with the active component ruthenium. The yield of N-alkylcarbazole reaches at most about 60%, and may even decrease to 30%. When SBA-15 silica template agent is used, after the carbonization treatment of the present invention, its carbon material retains an ordered tubular structure, but the activity is also poor, and the yield of N-alkylcarbazole is low.
[0022] In the carrier preparation method provided by the present invention, the organic raw material containing carbon and nitrogen is preferably any one or a combination of at least two of amino acids, p-phenylenediamine or melamine, wherein the amino acid may be, for example, glutamic acid, alanine or aspartic acid.
[0023] By using organic raw materials rich in carbon and nitrogen, during the high-temperature carbonization process, nitrogen atoms can not only be directly retained in the carbon framework to achieve in-situ and uniform nitrogen doping, but also create abundant intrinsic defects to form coupled active centers (NC topological defect coupling sites) with carbon defects. This allows for better control of surface charge distribution and anchoring of active metals, further improving the catalytic activity of the catalyst. When the corresponding organic materials are not used, the catalytic effect will decrease significantly.
[0024] The carrier preparation method provided by this invention employs a two-step temperature control. The first step involves pretreatment at 30-100℃. If the pretreatment temperature is outside this range, the carbonized material will have a loose structure, reduced specific surface area, and reduced pore volume. This results in fewer surface defects and a decrease in the density of active sites, significantly reducing the conductivity, catalytic activity, and structural stability of the obtained carrier material.
[0025] In the carrier preparation method provided by this invention, the second step involves calcination at 600-800℃. When the calcination temperature is below 600℃, the ordered mesoporous silica template agent will still maintain its structure, making it impossible to prepare the nitrogen-doped amorphous mesoporous carbon material of this invention. When this carrier is combined with the active component ruthenium, it cannot exhibit excellent catalytic effects. When the calcination temperature is above 800℃, the nitrogen content in the nitrogen-doped amorphous mesoporous carbon material decreases significantly, which also leads to a significant decrease in catalytic effects when combined with the active component ruthenium.
[0026] Under the premise of using at least one of amino acids, p-phenylenediamine or melamine as a source of carbon and nitrogen organic matter, and ordered mesoporous silica as a template agent, and with a pretreatment temperature of 30-100℃ and a calcination temperature of 600-800℃, the carrier prepared by this invention, when combined with ruthenium, can achieve a yield of N-alkylcarbazole of more than 80%.
[0027] The pretreatment described in this invention is carried out at a temperature of 30-100°C. The pretreatment temperature can be, for example, 30°C, 40°C, 45°C, 50°C, 55°C, 60°C, 70°C, 80°C, 90°C, or 100°C, preferably 40-60°C.
[0028] The calcination at 600-800℃ described in this invention can be, for example, 600℃, 650℃, 700℃, 720℃, 750℃, 780℃ or 800℃, preferably 750-800℃.
[0029] In the method for preparing the support provided by the present invention, when the pretreatment temperature is further preferably 40-60℃ and the calcination temperature is 750-800℃, the support prepared has better performance, and the catalyst formed with the active component ruthenium has higher catalytic activity, which can further improve the yield of N-alkylcarbazole.
[0030] As a preferred technical solution, the method for preparing the support for the ruthenium-based catalyst includes the following steps: Organic compounds containing carbon and nitrogen are mixed with a silica template agent in a solvent and pretreated at 40-60°C. The pretreated mixture is then centrifuged, dried, and the resulting solid is calcined at 750-800°C. After calcination, the silica template is removed from the product using an HF solution to obtain the carrier. The organic compounds containing carbon and nitrogen are any one or a combination of at least two of amino acids, p-phenylenediamine, or melamine. The silica template agent is MCM-41 and / or MCM-48.
[0031] Preferably, the ruthenium-based catalyst of the present invention is prepared by the following method, which includes the following steps: (1) Dissolve the ruthenium source in a solvent to obtain a precursor solution of the active component; disperse the support in a solvent to obtain a support suspension; (2) Mix the active component precursor solution and the support suspension, and then carry out a solvothermal reaction of the mixture at 180-240℃ to obtain the ruthenium-based catalyst.
[0032] Preferably, the ruthenium source in step (1) is any one or a combination of at least two of ruthenium chloride, ruthenium nitrite, ruthenium acetate, ruthenium acetylacetone, or trichlorohexamine ruthenium.
[0033] Preferably, the solvent in the active component precursor solution and the carrier suspension in step (1) is any one or a combination of at least two of ethanol, ethylene glycol, methanol or butanol, preferably ethanol.
[0034] Preferably, the mixing in step (2) is a stirring impregnation at room temperature, and the stirring speed is preferably 250-300 rpm, such as 250 rpm, 280 rpm or 300 rpm.
[0035] In this invention, the temperature of the solvothermal reaction in step (2) is 180-240℃, for example, it can be 180℃, 190℃, 200℃, 210℃, 220℃, 230℃ or 240℃, preferably 200-220℃.
[0036] Preferably, the solvothermal reaction time is 2-6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.
[0037] In the ruthenium-based catalyst provided by the present invention, the active component accounts for 1-5% of the mass percentage of the catalyst, for example, 1%, 2%, 3%, 4% or 5%.
[0038] The palladium-based catalyst of the present invention comprises a support and an active component; the support is any one of nitrogen-doped amorphous mesoporous carbon material, carbon nitride, activated carbon or aluminum oxide; the active component contains metallic palladium.
[0039] Preferably, the support in the palladium-based catalyst is a nitrogen-doped amorphous mesoporous carbon material, preferably the same as the support in the ruthenium-based catalyst, and is obtained using the same preparation method as the support in the ruthenium-based catalyst.
[0040] As a preferred embodiment of the present invention, the application of the catalyst combination in the preparation of N-alkylcarbazole includes: (1) N-alkylaniline, 1,2-cyclohexanediol and ruthenium-based catalyst are mixed in a solvent and the first catalytic reaction is carried out at 150-180 °C; (2) After the first catalytic reaction is completed, the ruthenium-based catalyst is separated and removed, and the palladium-based catalyst is directly added to the filtrate. The second catalytic reaction is carried out at 160-200℃ to obtain the target product.
[0041] In this invention, the structures of the N-alkylaniline and 1,2-cyclohexanediol are shown in Formula I and Formula II, respectively: Formula I; Formula II; Wherein, R1 is any one of alkyl (e.g., methyl, ethyl, propyl, isopropyl, etc.), benzyl or cycloalkyl (e.g., cyclopentyl, cyclohexyl, etc.); R2, R3, and R4 are each independently any one of hydrogen, alkyl (e.g., methyl, ethyl, propyl, isopropyl, etc.), cycloalkyl (e.g., cyclopentyl, cyclohexyl, etc.), aryl or heteroaryl; R3 and R4 exist independently or are linked together by chemical bonds to form a ring.
[0042] For example, the structural formula represented by formula I in this invention can be: , , , , The structural formula shown in Equation II can be, for example: , , , , .
[0043] In this invention, the reaction temperature for synthesizing N-alkylcarbazole can be as low as below 200°C. At this lower reaction temperature, N-alkylcarbazole can still achieve a high yield.
[0044] The reaction temperature for adding a ruthenium-based catalyst in this invention may be, for example, 150°C, 160°C, 170°C, or 180°C; the reaction temperature for adding a palladium-based catalyst may be, for example, 160°C, 170°C, 180°C, 190°C, or 200°C.
[0045] Preferably, the solvent is mesitylene.
[0046] The first catalytic reaction takes 22-28 hours, for example, 22 hours, 24 hours, 25 hours, 26 hours, or 28 hours; the second catalytic reaction takes 22-28 hours, for example, 22 hours, 24 hours, 25 hours, 26 hours, or 28 hours.
[0047] In the method of the present invention, the amount of ruthenium-based catalyst and palladium-based catalyst added is 1-5% of the molar ratio of the metal active component to N-alkylaniline.
[0048] In this invention, the molar ratio of N-alkylaniline to 1,2-cyclohexanediol is 1:2.5-1:6, for example, it can be 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5 or 1:6, preferably 1:3-1:5.
[0049] The numerical range described in this invention includes not only the point values listed above, but also any point values within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values included in the range.
[0050] Compared with the prior art, the present invention has the following beneficial effects: (1) This invention provides a method for synthesizing N-alkylcarbazole using a specific combination of catalysts. By first adding a ruthenium-based catalyst to the raw material system for synthesizing N-alkylcarbazole and then adding a palladium-based catalyst after separating and removing the ruthenium-based catalyst, the synthesis process can be simplified by eliminating the need for additives such as acids and bases, and efficient catalysis can be achieved at a lower reaction temperature. This significantly improves the yield of N-alkylcarbazole and also achieves high catalyst recovery activity.
[0051] (2) The yield of N-alkylcarbazole synthesized by catalysis in this invention can reach 89-95%.
[0052] (3) The ruthenium-based catalyst and palladium-based catalyst described in this invention can still maintain high activity and have excellent cycle stability when reused more than 6 times. Attached Figure Description
[0053] Figure 1 This is a schematic diagram of the carrier preparation process in Example 1.
[0054] Figure 2 This is a Ru3p XPS characterization diagram of the catalyst prepared in Preparation Example 1.
[0055] Figure 3 This is a TEM image of the carrier NC1-d800 prepared in Preparation Example 1.
[0056] Figure 4 This is a TEM image of the carrier NC4-d500 prepared in Preparation Example 4.
[0057] Figure 5 This is a TEM image of the carrier NC8-d1000 prepared in Preparation Example 8.
[0058] Figure 6 This is the 1H NMR spectrum of N-methylcarbazole synthesized in Example 1.
[0059] Figure 7 This is the carbon NMR spectrum of N-methylcarbazole synthesized in Example 1.
[0060] Figure 8 This is the 1H NMR spectrum of N-ethylcarbazole synthesized in Example 2.
[0061] Figure 9 This is the carbon NMR spectrum of N-ethylcarbazole synthesized in Example 2.
[0062] Figure 10 This is the 1H NMR spectrum of N-propylcarbazole synthesized in Example 3.
[0063] Figure 11 This is the carbon NMR spectrum of N-propylcarbazole synthesized in Example 3.
[0064] Figure 12 This is a TEM image of a carrier prepared using amorphous silica as a template agent.
[0065] Figure 13 This is a TEM image of a carrier prepared using spherical silica as a template agent.
[0066] Figure 14 This is a TEM image of a carrier prepared using SBA-15 as a template agent.
[0067] Figure 15 This is a TEM image of a carrier prepared using LUDOX-40 as a template agent.
[0068] Figure 16 The graph shows the yield of N-methylcarbazole obtained by repeating the catalyst used in Example 1 six times. Detailed Implementation
[0069] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.
[0070] Preparation Example 1 This preparation example provides a ruthenium-based catalyst, which consists of a nitrogen-doped amorphous mesoporous carbon material support and an active component ruthenium supported on the support, wherein the active component ruthenium accounts for 5% of the catalyst mass.
[0071] The ruthenium-based catalyst is prepared by the following method, specifically including the following steps: Step 1: Preparation of the carrier: (I) L-glutamic acid (5.8 g) and mesoporous silica MCM-41 (2 g) were dispersed in deionized water (100 mL) and stirred in an oil bath at 60 °C for 4 h. After the reaction was completed, the mixture was centrifuged (10000 rpm, 15 min / time), and the resulting white solid was dried overnight at 80 °C in a vacuum drying oven.
[0072] (II) The dried white solid was placed in a tube furnace and heated to 800°C at a rate of 5°C / min under a N2 atmosphere, held at that temperature for 2 h, and then allowed to cool naturally to room temperature. The resulting product was washed with 10 wt% HF solution for 24 h, filtered through a polytetrafluoroethylene funnel, and washed with deionized water until neutral. The resulting black powder was dried overnight at 85°C in a vacuum drying oven to obtain the final support, denoted as NC1-d800.
[0073] Figure 1 The diagram shows the preparation process of the NC1-d800 carrier. As can be seen from the diagram, the template agent used is ordered mesoporous silica with a tubular structure. After pretreatment with L-glutamic acid at 60°C and carbonization at 800°C followed by HF etching, the ordered tubular mesoporous structure of the template disappears, becoming a nitrogen-doped amorphous mesoporous carbon material carrier.
[0074] Step 2: Loading ruthenium metal: (I) 21.6 mg of anhydrous RuCl3 was dispersed in 60 mL of anhydrous ethanol, and the resulting solution was added to 80 mL of anhydrous ethanol suspension containing 200 mg of carrier. The mixture was stirred at room temperature for 24 h.
[0075] (II) The mixture was transferred to a 250 mL hydrothermal reactor and reacted at 220 °C for 4 h, followed by natural cooling to room temperature. The reaction product was separated by centrifugation (10,000 rpm, 15 min / time) and washed three times with anhydrous ethanol. The resulting catalyst was dried overnight at 85 °C in a vacuum drying oven. The final product was designated as Ru / NC1-d800.
[0076] Figure 2 The figure shows the Ru3p XPS characterization of the catalyst prepared in Example 1. As can be seen from the figure, two spin orbital peaks (Ru3p3 / 2 and Ru3p1 / 2) were detected in the Ru3p spectrum. The peaks at 462.03 eV and 485.00 eV are mainly attributed to metallic Ru, which is the core valence state of the active metal ruthenium.
[0077] Preparation Example 2 This preparation example provides a ruthenium-based catalyst, which consists of a nitrogen-doped amorphous mesoporous carbon material support and an active component ruthenium supported on the support, wherein the active component ruthenium accounts for 3% of the catalyst mass.
[0078] The ruthenium-based catalyst is prepared by the following method, specifically including the following steps: Step 1: Preparation of the carrier: (I) L-glutamic acid (1 g) and melamine (5 g) were dispersed with mesoporous silica MCM-48 (2.9 g) in deionized water (100 mL) and stirred in an oil bath at 40 °C for 6 h. After the reaction was completed, the mixture was centrifuged (10000 rpm, 15 min / time), and the resulting white solid was dried overnight at 80 °C in a vacuum drying oven.
[0079] (II) The dried white solid was placed in a tube furnace and heated to 780°C at a rate of 3°C / min under a N2 atmosphere, held at that temperature for 4 h, and then allowed to cool naturally to room temperature. The resulting product was washed with 10 wt% HF solution for 24 h, filtered through a polytetrafluoroethylene funnel, and washed with deionized water until neutral. The resulting black powder was dried overnight at 85°C in a vacuum drying oven to obtain the final support, denoted as NC2.
[0080] Step 2: Loading ruthenium metal: (I) Disperse 20 mg Ru(NO)(NO3)3 in 60 mL of anhydrous ethanol, and add the resulting solution to 80 mL of anhydrous ethanol suspension containing 200 mg of carrier. Stir at room temperature for 20 h.
[0081] (II) The mixture was transferred to a 250 mL hydrothermal reactor and reacted at 200 °C for 6 h, followed by natural cooling to room temperature. The reaction product was separated by centrifugation (10,000 rpm, 15 min / time) and washed three times with anhydrous ethanol. The resulting catalyst was dried overnight at 85 °C in a vacuum drying oven. The final product was denoted as Ru / NC2.
[0082] Preparation Example 3 This preparation example provides a ruthenium-based catalyst, which consists of a nitrogen-doped amorphous mesoporous carbon material support and an active component ruthenium supported on the support, wherein the active component ruthenium accounts for 5% of the catalyst mass.
[0083] The ruthenium-based catalyst is prepared by the following method, specifically including the following steps: Step 1: Preparation of the carrier: (I) After mixing p-phenylenediamine (10.8 g) with mesoporous silica MCM-41 (3.2 g), the mixture was stirred in an oil bath at 50 °C for 5 h. After the reaction was completed, the mixture was centrifuged (10,000 rpm, 15 min / time), and the resulting brown solid was placed in a vacuum drying oven and dried at 80 °C overnight.
[0084] (II) The dried brown solid was placed in a tube furnace and heated to 760°C at a rate of 2°C / min under a N2 atmosphere, and calcined for 6 h, followed by natural cooling to room temperature. The resulting product was washed with 10 wt% HF solution for 24 h, filtered through a polytetrafluoroethylene funnel, and washed with deionized water until neutral. The resulting black powder was dried overnight at 85°C in a vacuum drying oven to obtain the final support, denoted as NC3.
[0085] Step 2: Loading ruthenium metal: (I) 41.3 mg Ru(acac)3 was dispersed in 60 mL of anhydrous ethanol, and the resulting solution was added to 80 mL of anhydrous ethanol suspension containing 200 mg of carrier. The mixture was stirred at room temperature for 24 h.
[0086] (II) The mixture was transferred to a 250 mL hydrothermal reactor and reacted at 180 °C for 6 h, followed by natural cooling to room temperature. The reaction product was separated by centrifugation (10,000 rpm, 15 min / time) and washed three times with anhydrous ethanol. The resulting catalyst was dried overnight at 85 °C in a vacuum drying oven. The final product was designated as Ru / NC3.
[0087] Preparation Examples 4 to 8 Compared with Preparation Example 1, only the calcination temperature of step (II) during the preparation of the carrier was changed, from 800℃ to 500℃ (Preparation Example 4), 600℃ (Preparation Example 5), 750℃ (Preparation Example 6), 850℃ (Preparation Example 7), and 1000℃ (Preparation Example 8), while the others remained unchanged.
[0088] Preparation Examples 4 to 8 are labeled as Ru / NC1-d500, Ru / NC1-d600, Ru / NC1-d750, Ru / NC1-d850, and Ru / NC1-d1000, respectively, where "d" is an abbreviation for "calcination temperature".
[0089] Figure 3 , Figure 4 and Figure 5 TEM images of the carriers prepared in Preparation Example 1, Preparation Example 4 and Preparation Example 8 are shown respectively. It can be seen from the figures that Preparation Example 1 and Preparation Example 8 formed an amorphous structure after calcination at 800℃ and 1000℃ respectively, while Preparation Example 4 maintained a tubular ordered mesoporous structure after calcination at 500℃ and did not achieve the transformation to an amorphous structure.
[0090] Preparation Examples 9 to 12 Compared with Preparation Example 1, only the pretreatment temperature of step (I) during carrier preparation was changed from 60°C to ice-water bath 0°C (Preparation Example 9), 20°C (Preparation Example 10), 80°C (Preparation Example 11), and 100°C (Preparation Example 12), while the other conditions remained unchanged.
[0091] Preparation Examples 9 to 12 are labeled as Ru / NC1-c0, Ru / NC1-c20, Ru / NC1-c80, and Ru / NC1-c100, respectively, where "c" is an abbreviation for "pretreatment temperature".
[0092] Preparation Example 13 Compared to Preparation Example 1, in the preparation of the support, the stirring reaction in a 60°C oil bath for 4 h in step (I) was omitted, and it was changed to a single-stage heating process, specifically: L-glutamic acid (5.8 g) and mesoporous silica MCM-41 (2 g) were dispersed in deionized water (100 mL). After dehydration under reduced pressure, the mixture was dried under vacuum at 85 °C. The resulting white solid was then heated to 800 °C at a heating rate of 5 °C / min and calcined for 2 h, followed by natural cooling to room temperature. The product was washed with 10 wt% HF solution for 24 h, filtered through a polytetrafluoroethylene funnel, and washed with deionized water until neutral. The resulting black powder was dried overnight at 85 °C in a vacuum drying oven to obtain the final carrier.
[0093] Everything else remains the same, and the final product is denoted as Ru / NC13.
[0094] Preparation Examples 14 to 16 Compared with Preparation Example 1, in the preparation of the carrier, only the L-glutamic acid in step (I) was replaced with aniline (Preparation Example 14), a mixture of ethylenediamine and CCl4 in a mass ratio of 10:24 (Preparation Example 15), and a mixture of glucose and 4-nitrobenzene in a mass ratio of 1:1 (Preparation Example 16), while the others remained unchanged.
[0095] Preparation Examples 14 to 16 are labeled as Ru / NC1-y1, Ru / NC1-y2, and Ru / NC1-y3, respectively, where "y" is an abbreviation for "organic compound containing carbon and nitrogen".
[0096] Preparation Examples 17 to 18 Compared with Preparation Example 1, when loading ruthenium metal, the anhydrous ethanol solvent used in step (I) was replaced with ethylene glycol (Preparation Example 17) and methanol (Preparation Example 18), while the others remained unchanged.
[0097] Preparation Examples 17 to 18 are labeled as Ru / NC1-r1 and Ru / NC1-r2, respectively, where "r" is an abbreviation for "solvent".
[0098] Preparation Example 19 This preparation example provides a palladium-based catalyst, which consists of a nitrogen-doped amorphous mesoporous carbon material support (same as in Preparation Example 1) and an active component palladium supported on the support, wherein the active component palladium accounts for 5% of the catalyst mass.
[0099] The palladium-based catalyst is prepared by the following method, specifically including the following steps: Step 1: Preparation of the carrier: The preparation method is the same as that in Example 1.
[0100] Step 2: Loading palladium: (I) 16.3 mg K2PdCl4 was dispersed in 60 mL of anhydrous ethanol, and the resulting solution was added to 100 mg of anhydrous ethanol suspension containing the carrier in 80 mL of anhydrous ethanol. The mixture was stirred at room temperature for 24 h.
[0101] (II) The mixture was transferred to a 250 mL hydrothermal reactor and reacted at 220 °C for 4 h, followed by natural cooling to room temperature. The reaction product was separated by centrifugation (10,000 rpm, 15 min / time) and washed three times with anhydrous ethanol. The resulting catalyst was dried overnight at 85 °C in a vacuum drying oven. The final product was designated as Pd / NC1.
[0102] Preparation Example 20 Compared to Preparation Example 19, the catalyst support was replaced with commercially available carbon nitride (g-C3N4), while everything else remained the same, labeled as Pd / g-C3N4.
[0103] Preparation Example 21 Compared to Preparation Example 19, the catalyst support was replaced with aluminum oxide, while everything else remained the same, labeled as Pd / Al2O3.
[0104] Comparative Preparation Example 1-1 Compared with Preparation Example 1, the active component in this comparative preparation example was replaced with nickel, while everything else remained unchanged. The final product was denoted as Ni / NC1-d800.
[0105] Comparative Preparation Examples 1-2 to 1-6 Compared with Comparative Preparation Example 1-1, only the catalyst support was changed, and it was replaced with aluminum oxide (Comparative Preparation Example 1-2), silicon dioxide (Comparative Preparation Example 1-3), activated carbon (Comparative Preparation Example 1-4), HZSM-5 (Comparative Preparation Example 1-5), and commercially available carbon nitride (Comparative Preparation Example 1-6), while other aspects remained unchanged.
[0106] Comparative Preparation Example 2-1 Compared with Preparation Example 1, the active component in this comparative preparation example was replaced with copper, while everything else remained unchanged. The final product was denoted as Cu / NC1.
[0107] Comparative Preparation Examples 2-2 to 2-4 Compared with Comparative Preparation Example 2-1, only the catalyst support was changed, replacing it with aluminum oxide (Comparative Preparation Example 2-2), zirconium oxide (Comparative Preparation Example 2-3), and commercially available carbon nitride (Comparative Preparation Example 2-4), while other aspects remained unchanged.
[0108] Comparative Preparation Example 3-1 Compared with Preparation Example 1, the active component in this comparative preparation example was replaced by ruthenium with ruthenium and palladium in a molar ratio of 1:1, while other aspects remained unchanged.
[0109] Comparative Preparation Example 3-2 Compared with Preparation Example 1, the active component in this comparative preparation example was replaced by ruthenium with ruthenium and nickel in a molar ratio of 1:1, while the others remained unchanged.
[0110] Comparative Preparation Example 3-3 Compared with Preparation Example 1, the active component in this comparative preparation example was replaced by ruthenium with ruthenium and copper in a molar ratio of 1:1, while the others remained unchanged.
[0111] Comparative preparation examples 3-4 Compared with Preparation Example 1, the active component in this comparative preparation example was replaced by ruthenium with ruthenium and cobalt in a molar ratio of 1:1, while the others remained unchanged.
[0112] Comparative Preparation Example 4-1 Compared with Preparation Example 1, the support in this comparative preparation example is replaced with aluminum oxide instead of the support in Preparation Example 1, while everything else remains unchanged.
[0113] Comparative preparation example 4-2 Compared with Preparation Example 1, the support in this comparative preparation example is replaced with commercially available carbon nitride instead of the support in Preparation Example 1, while everything else remains the same.
[0114] Comparative preparation example 4-3 Compared with Preparation Example 1, the carrier in this comparative preparation example is replaced by MCM-41, while everything else remains unchanged.
[0115] Comparative Preparation Examples 5-1 to 5-5 Compared with Preparation Example 1, in the preparation of the carrier, only the mesoporous silica MCM-41 in step (I) was replaced with amorphous silica (Comparative Preparation Example 5-1), commercially available spherical silica (Comparative Preparation Example 5-2), SBA-15 (Comparative Preparation Example 5-3), LUDOX-40 colloidal silica (Comparative Preparation Example 5-4), and fumed silica (Comparative Preparation Example 5-5), respectively, while the others remained unchanged.
[0116] Example 1 This embodiment provides a method for synthesizing N-methylcarbazole, including: N-methylaniline (41 mg, 0.38 mmol), 1,2-cyclohexanediol (176 mg, 1.52 mmol), and 5 wt% Ru / NC1-d800 catalyst (38 mg) obtained in Preparation Example 1 were added to a reaction tube, with mesitylene (1.5 mL) as the solvent. The reaction system was purged with argon three times and reacted at 150 °C for 26 h. After cooling to room temperature, the reaction solution was removed and placed in a centrifuge tube. After centrifugation for 3 min, the supernatant was returned to the reaction tube, and Pd / NC1 catalyst (41 mg) obtained in Preparation Example 19 was added. The mixture was again purged with argon three times, and the temperature was raised to 190 °C for another 24 h. After the reaction was complete, the catalyst was recovered by simple centrifugation. 1 H NMR analysis showed that the reaction conversion rate was 100% and the yield of the target product was 95%.
[0117] The synthesis process is as follows:
[0118] Figure 6 and Figure 7 The 1H NMR spectrum and 1C NMR spectrum of the N-methylcarbazole synthesized in Example 1 are shown respectively. The characterization of the N-methylcarbazole is as follows: 1 H NMR (500 MHz, CDCl3) δ 8.02 (d, J = 7.8 Hz, 2H), 7.39 (ddd, J =8.3, 7.0, 1.2 Hz, 2H), 7.28 (s, 2H), 7.20 – 7.13 (m, 2H), 3.66 (s, 3H). 13 CNMR (126 MHz, CDCl3) δ 141.10, 125.79, 122.88, 120.42, 118.96, 108.56, 29.07. Example 2 This embodiment provides a method for synthesizing N-ethylcarbazole, including: N-ethylaniline (41 mg, 0.34 mmol), 1,2-cyclohexanediol (128 mg, 1.1 mmol), and 3 wt% Ru / NC2 catalyst (57 mg) obtained in Preparation Example 2 were added to a reaction tube, using mesitylene (1.5 mL) as the solvent. The reaction system was purged three times with argon gas and reacted at 160 °C for 24 h. After cooling to room temperature, the reaction solution was removed and placed in a centrifuge tube. After centrifugation for 3 min, the supernatant was returned to the reaction tube, and Pd / NC1 catalyst (36 mg) obtained in Preparation Example 19 was added. The mixture was again purged three times with argon gas, and the temperature was raised to 180 °C for another 24 h. After the reaction was complete, the catalyst was recovered by simple centrifugation. 1 H NMR analysis showed that the reaction conversion rate was 100% and the yield of the target product was 91%.
[0119] The synthesis process is as follows:
[0120] Figure 8 and Figure 9 The 1H NMR and 1C NMR spectra of the N-ethylcarbazole synthesized in Example 2 are shown respectively. The characterization of the N-ethylcarbazole is as follows: 1 H NMR (500 MHz, CDCl3) δ 8.14 (d, J = 7.8 Hz, 2H), 7.50 (ddd, J =8.2, 7.0, 1.2 Hz, 2H), 7.44 (d, J = 8.1 Hz, 2H), 7.28 – 7.24 (m, 2H), 4.40(q, J = 7.2 Hz, 2H), 1.46 (t, J = 7.3 Hz, 3H). 13 C NMR (126 MHz, CDCl3) δ139.96, 125.62, 122.95, 120.44, 118.76, 108.44, 37.53, 13.83. Example 3 This embodiment provides a method for synthesizing N-propylcarbazole, including: N-propylaniline (41 mg, 0.30 mmol), 1,2-cyclohexanediol (174 mg, 1.5 mmol), and 5 wt% Ru / NC3 catalyst (30 mg) obtained in Preparation Example 3 were added to a reaction tube, using mesitylene (1.5 mL) as the solvent. The reaction system was purged three times with argon gas and then reacted at 150 °C for 24 h. After cooling to room temperature, the reaction solution was transferred to a 2.0 mL centrifuge tube and centrifuged for 3 min. The supernatant was returned to the reaction tube, and Pd / NC1 catalyst (32 mg) obtained in Preparation Example 19 was added. The mixture was again purged three times with argon gas, and the temperature was raised to 180 °C for another 24 h. After the reaction was complete, the catalyst was recovered by simple centrifugation. 1 H NMR analysis showed that the reaction conversion rate was 100% and the yield of the target product was 89%.
[0121] The synthesis process is as follows:
[0122] Figure 10 and Figure 11 The 1H NMR spectrum and 1C NMR spectrum of the N-propylcarbazole synthesized in Example 3 are shown respectively. The characterization of the N-propylcarbazole is as follows: 1 H NMR (500 MHz, CDCl3) δ 8.13 (d, J = 7.8 Hz, 2H), 7.49 (ddq, J =8.2, 7.0, 1.3 Hz, 2H), 7.46 – 7.41 (m, 2H), 7.25 (dddd, J = 8.0, 6.9, 3.0,1.3 Hz, 2H), 4.30 (t, J = 7.2 Hz, 2H), 1.98 – 1.90 (m, 2H), 1.00 (ddd, J =8.1, 7.2, 1.4 Hz, 3H). 13 C NMR (126 MHz, CDCl3) δ 140.54, 125.59, 122.83, 120.36, 118.73, 108.72, 44.65, 22.35, 11.86. Examples 4 to 18 Compared with Example 1, the catalyst Ru / NC1-d800 obtained in Preparation Example 1 was replaced with the catalysts obtained in Preparation Examples 4 to 18, while other aspects remained unchanged.
[0123] Examples 19 to 20 Compared with Example 1, the catalyst Pd / NC1 obtained in Preparation Example 19 was replaced with the catalysts obtained in Preparation Examples 20 to 21, while other aspects remained unchanged.
[0124] Table 1 below shows the yields of N-alkylcarbazole corresponding to Examples 1 to 20.
[0125] Table 1
[0126] As shown in Table 1, when a more optimized method for preparing the ruthenium-based catalyst support is adopted, the two catalysts can exert a more excellent synergistic effect, resulting in a yield of N-alkylcarbazole of at least 80%. However, changing the calcination temperature (not in the range of 600-800℃), pretreatment temperature (not in the range of 30-100℃), number of heating cycles (not using two heating cycles), and the types of organic compounds containing carbon and nitrogen as well as the types of solvents in the preparation method of the ruthenium-based catalyst support will lead to a decrease in the catalytic effect of the two catalysts, thereby reducing the yield of N-alkylcarbazole.
[0127] Comparative Example 1-1 Compared with Example 1, the catalyst Ru / NC1-d800 in Preparation Example 1 was replaced with the catalyst of Comparative Preparation Example 1-1, and everything else was the same as in Example 1.
[0128] Comparative Examples 1-2 to 2-4 Compared with Example 1, the catalyst Ru / NC1-d800 in Preparation Example 1 was replaced with the catalysts of Comparative Preparation Examples 1-2 to 2-4, and everything else was the same as in Example 1.
[0129] Table 2 below shows the yields of N-alkylcarbazole corresponding to Example 1 and Comparative Examples 1-1 to 2-4.
[0130] Table 2
[0131] As can be seen from Table 2, for the ruthenium-based catalyst in this invention, when the active component ruthenium is replaced with other elements, or when both the active component and the support are replaced at the same time, the catalytic effect will decrease and the yield of N-alkylcarbazole will decrease.
[0132] Comparative Examples 3-1 to 4-3 Compared with Example 1, the catalyst Ru / NC1-d800 in Preparation Example 1 was replaced with the catalysts of Comparative Preparation Examples 3-1 to 4-3, and everything else was the same as in Example 1.
[0133] Table 3 below shows the yields of N-alkylcarbazole corresponding to Example 1 and Comparative Examples 3-1 to 4-3.
[0134] Table 3
[0135] As can be seen from Table 3, for the ruthenium-based catalyst of this invention, when ruthenium is kept as the active component and other active components are added at the same time, its catalytic effect will also decrease, resulting in a decrease in the yield of N-alkylcarbazole. When the ruthenium single active component is kept unchanged and the catalyst support is replaced, the catalytic effect will be greatly reduced, and the yield of N-alkylcarbazole will be reduced to below 55%.
[0136] Comparative Examples 5-1 to 5-5 Compared with Example 1, the catalyst Ru / NC1-d800 in Preparation Example 1 was replaced with the catalysts of Comparative Preparation Examples 5-1 to 5-5, and everything else was the same as in Example 1.
[0137] Table 4 below shows the yields of N-alkylcarbazole corresponding to Example 1 and Comparative Examples 5-1 to 5-5.
[0138] Table 4
[0139] Figure 12 , Figure 13 , Figure 14 and Figure 15 These are the corresponding carrier structures when amorphous silica (Comparative Preparation Example 5-1), commercially available spherical silica (Comparative Preparation Example 5-2), SBA-15 (Comparative Preparation Example 5-3), and LUDOX-40 colloidal silica (Comparative Preparation Example 5-4) are used as template agents.
[0140] pass Figures 12 to 15 Combined with the product yields in Table 4, it can be seen that although the carbon material obtained by Comparative Preparation Example 5-1 (using amorphous silica as a template) has an amorphous structure, its catalytic activity is poor; the carbon material obtained by Comparative Preparation Example 5-2 (using commercially available spherical silica as a template) perfectly maintains its spherical morphology and does not form an amorphous structure, but its activity is still not ideal, and the product yield is low; the carbon material obtained by Comparative Preparation Example 5-3 (using ordered tubular mesoporous silica SBA-15 as a template) retains its ordered tubular structure, but its activity is also poor; the carbon material obtained by Comparative Preparation Example 5-4 (using LUDOX-40 colloidal silica as a template) has basically lost its mesoporous structure, and the reaction is poor; when these comparative preparation examples are used for corresponding catalysis, the yield of N-alkylcarbazole is significantly reduced.
[0141] Therefore, only by using ordered mesoporous silica as a template and forming amorphous carbon material after carbonization (calcination) can a suitable degree of carbon defect and nitrogen content be obtained, thereby effectively anchoring the active metal, promoting the catalytic reaction, and resulting in a higher yield of N-alkylcarbazole. In other words, the support of the first catalyst in this invention must simultaneously satisfy the two conditions of "the template being ordered mesoporous silica" and "the carbonization product being amorphous carbon" in order to achieve a higher yield of N-alkylcarbazole.
[0142] Comparative Example 6 Compared to Example 1, the order of adding the two catalysts was adjusted, that is, the Pd / NC1 catalyst obtained in Preparation Example 19 was added first, followed by the Ru / NC1-d800 catalyst obtained in Preparation Example 1, while other steps remained unchanged. Specifically, the steps included are as follows: N-methylaniline (41 mg, 0.38 mmol), 1,2-cyclohexanediol (176 mg, 1.52 mmol), and the Pd / NC1 catalyst (41 mg) obtained in Preparation Example 19 were added to a reaction tube, with mesitylene (1.5 mL) as the solvent. The reaction system was purged with argon three times and reacted at 150 °C for 26 h. After cooling to room temperature, the reaction solution was removed and placed in a centrifuge tube. After centrifugation for 3 min, the supernatant was returned to the reaction tube, and 5 wt% Ru / NC1-d800 catalyst (38 mg) obtained in Preparation Example 1 was added. The system was purged with argon three times again, and the temperature was raised to 190 °C to continue the reaction for 24 h.
[0143] Comparative Example 7 Compared to Example 1, the catalyst obtained in Preparation Example 1 and the catalyst obtained in Preparation Example 19 were added simultaneously, without any sequential addition, while other aspects remained unchanged. Specifically, the steps included were as follows: N-methylaniline (41 mg, 0.38 mmol), 1,2-cyclohexanediol (176 mg, 1.52 mmol), 5 wt% Ru / NC1-d800 catalyst (38 mg) obtained in Preparation Example 1, and Pd / NC1 catalyst (41 mg) obtained in Preparation Example 19 were added to a reaction tube, with mesitylene (1.5 mL) as the solvent. The reaction system was purged with argon three times and then reacted at 190 °C for 50 h.
[0144] Comparative Example 8 Compared to Example 1, instead of adding the catalyst obtained in Preparation Example 1, the catalyst from Preparation Example 19 was added twice, while other steps remained unchanged. Specifically, the steps included: N-methylaniline (41 mg, 0.38 mmol), 1,2-cyclohexanediol (176 mg, 1.52 mmol), and 5 wt% Pd / NC1 catalyst (41 mg) obtained in Preparation Example 19 were added to a reaction tube, with mesitylene (1.5 mL) as the solvent. The reaction system was purged with argon three times and reacted at 150 °C for 26 h. After cooling to room temperature, the Pd / NC1 catalyst (41 mg) obtained in Preparation Example 19 was added directly, and the system was purged with argon three times again. The temperature was then raised to 190 °C and the reaction was continued for 24 h.
[0145] Comparative Example 9 Compared to Example 1, the catalyst obtained in Preparation Example 19 was not added; instead, the catalyst from Preparation Example 1 was added twice, while other steps remained unchanged. Specifically, the steps included: N-methylaniline (41 mg, 0.38 mmol), 1,2-cyclohexanediol (176 mg, 1.52 mmol), and 5 wt% Ru / NC1-d800 catalyst (38 mg) obtained in Preparation Example 1 were added to a reaction tube, with mesitylene (1.5 mL) as the solvent. The reaction system was purged with argon three times and reacted at 150 °C for 26 h. After cooling to room temperature, the Ru / NC1-d800 catalyst (38 mg) obtained in Preparation Example 1 was added directly, and the system was purged with argon three times again. The temperature was then raised to 190 °C and the reaction was continued for 24 h.
[0146] Table 5 below shows the yields of N-alkylcarbazole corresponding to Example 1 and Comparative Examples 6 to 9.
[0147] Table 5
[0148] As can be seen from Table 5, the two catalysts in this invention should be added separately and sequentially, first the ruthenium-based catalyst and then the palladium-based catalyst, to achieve excellent catalytic performance in the N-alkylcarbazole yield. If the order of addition is adjusted, or if they are added simultaneously, the catalytic effect will decrease significantly, and the product yield will drop to below 24%. When only one catalyst is used, it also fails to achieve excellent catalytic performance, and the product yield will be significantly reduced.
[0149] Catalyst cycle performance test Application Example 1 The catalyst used in Example 1 was filtered and dried, and the resulting catalyst was used to continue the synthesis method of Example 1, repeated 6 times. During each repetition, the reaction temperature and time remained constant. The yields of N-methylcarbazole obtained in Example 1 and each repetition are as follows: Figure 16 As shown.
[0150] pass Figure 16 It can be seen that when using the ruthenium-based catalyst and palladium-based catalyst already used in Example 1, the yield of N-methylcarbazole obtained by the catalyst is basically above 95% when repeated up to the 6th time. This also confirms that the corresponding catalyst in this invention can maintain high activity when recycled after only simple filtration and drying treatment, and the corresponding catalyst has excellent cycle stability.
[0151] Comparative Application Example 1 Based on Example 1, in the synthesis of N-methylcarbazole, after the first catalytic reaction using a ruthenium-based catalyst was completed, the ruthenium-based catalyst was not separated and removed, but a palladium-based catalyst was directly added. After all catalysis was completed, the catalyst was recovered by filtration and drying, resulting in a mixture of ruthenium-based and palladium-based catalysts.
[0152] The catalyst mixture was then used in the synthesis method of Example 1, with the reaction temperature and time remaining unchanged. After one repetition, the yield of N-methylcarbazole was only 15%, which could not maintain the high activity of the catalyst and resulted in poor cycle stability.
[0153] The applicant declares that the above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.
Claims
1. The application of a catalyst combination in the preparation of N-alkylcarbazole, characterized in that, The applications include: Using N-alkylaniline and 1,2-cyclohexanediol as reactants, the reaction was first carried out in the presence of a first catalyst. After the reaction was completed, the first catalyst was separated and removed, and then a second catalyst was added to carry out the reaction to obtain the target product. The first catalyst is a ruthenium-based catalyst; the ruthenium-based catalyst is composed of a support and an active component, wherein the support is a nitrogen-doped amorphous mesoporous carbon material, and the active component is metallic ruthenium; The second catalyst is a palladium-based catalyst; the palladium-based catalyst is composed of a support and an active component, wherein the support is a nitrogen-doped amorphous mesoporous carbon material, and the active component is metallic palladium; The supports in both the ruthenium-based and palladium-based catalysts were prepared using the following method, which includes the following steps: Organic matter containing carbon and nitrogen is mixed with silica template agent in a solvent and pretreated at 30-100°C. The pretreated mixture is centrifuged and dried. The resulting solid is calcined at 600-800°C. After calcination, the silica template is removed by HF solution to obtain the carrier. The silica template agent is MCM-41 and / or MCM-48; The organic compound containing carbon and nitrogen is any one or a combination of at least two of amino acids, p-phenylenediamine, or melamine.
2. The application according to claim 1, characterized in that, The temperature of the pretreatment after mixing is 40-60℃; the temperature of the calcination is 750-800℃.
3. The application according to claim 1, characterized in that, The ruthenium-based catalyst was prepared by the following method, which includes the following steps: (1) Dissolve the ruthenium source in a solvent to obtain a precursor solution of the active component; disperse the support in a solvent to obtain a support suspension; (2) Mix the active component precursor solution and the support suspension, and then carry out a solvothermal reaction of the mixture at 180-240℃ to obtain the ruthenium-based catalyst.
4. The application according to claim 3, characterized in that, The ruthenium source in step (1) is any one or a combination of at least two of ruthenium chloride, ruthenium nitrite, ruthenium acetate, ruthenium acetylacetone, or trichlorohexamineruthenium. The solvent in the active component precursor solution and the carrier suspension in step (1) is any one or a combination of at least two of ethanol, ethylene glycol, methanol or butanol; The mixing in step (2) is a stirring and impregnation process at room temperature; The temperature of the solvothermal reaction in step (2) is 200-220℃, and the reaction time is 2-6h.
5. The application according to claim 1, characterized in that, The applications include: (1) N-alkylaniline, 1,2-cyclohexanediol and ruthenium-based catalyst are mixed in a solvent and the first catalytic reaction is carried out at 150-180 °C; (2) After the first catalytic reaction is completed, the ruthenium-based catalyst is separated and removed, and the palladium-based catalyst is directly added to the filtrate. The second catalytic reaction is carried out at 160-200℃ to obtain the target product.
6. The application according to claim 5, characterized in that, The solvent is mesitylene; The first catalytic reaction takes 22-28 hours; The second catalytic reaction takes 22-28 hours.
Citation Information
Patent Citations
Method and system for co-production of N-ethyl carbazole and N-ethyl aniline
CN118546088A
Preparation method of N-alkyl carbazole
CN116425638A
Heterogeneous N-alkylation catalyst as well as preparation method and application thereof