A controlled dissolution catalyst for weakly crystallized RP phase-mediated alloys, its preparation method and application
By generating a weakly crystallized RP phase through narrow-window co-doping at B sites and low oxygen partial pressure reduction technology, the problem of nickel particle migration and agglomeration in nickel-based catalysts during tar steam reforming was solved, and the controllable dissolution of nickel-based alloy particles was achieved, thereby improving the stability and activity of the catalyst.
Patent Information
- Application Number
- CN202611590568.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-14
- Publication Date
- 2026-11-10
AI Technical Summary
Existing nickel-based catalysts suffer from problems such as easy migration and agglomeration of nickel particles, decrease in specific surface area, and loss of active sites during tar steam reforming. Furthermore, traditional perovskite-based catalysts exhibit uneven distribution of B-site metals and difficulty in controlling the size of metal particles during reduction.
By co-doping transition metals such as Co, Fe, and Cu at the B-site narrow window and combining the dissolution process with low oxygen partial pressure reduction, weakly crystalline RP-phase layered perovskite is generated, enabling the controllable dissolution of nickel-based alloy nanoparticles and preparing a weakly crystalline RP-phase mediated alloy catalyst.
It achieves precise size constraint of nickel-based alloy particles, improves the stability and activity of catalysts, maintains high conversion rate and product distribution, and is suitable for tar steam reforming, methane dry reforming and water-gas shift reaction.
Smart Images

Figure CN123059656A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalytic material preparation technology, and in particular to a weakly crystallized RP phase-mediated alloy controllable dissolution catalyst, its preparation method, and its application. Background Technology
[0002] Biomass, as a widely distributed, carbon-neutral, and renewable energy carrier, relies on gasification technology as a crucial pathway for its high-value utilization. However, the gasification process inevitably generates a large amount of tar byproducts, accounting for approximately 5-15 wt.% of the gasification products. These byproducts not only significantly reduce the calorific value of the fuel gas but also condense and deposit in downstream pipelines and equipment, causing blockages and corrosion, severely hindering the long-term stable operation of biomass gasification systems.
[0003] Currently, tar removal technologies mainly include physical methods (such as cyclone separation, water washing, and adsorption) and thermochemical conversion methods (such as thermal cracking and catalytic reforming). Among them, catalytic steam reforming technology is considered a tar treatment solution with great engineering application prospects because it can convert large tar molecules into combustible small molecule gases such as H2, CO, and CH4 under relatively mild conditions, and has the dual advantages of high purification efficiency and high energy recovery rate.
[0004] In the tar steam reforming catalyst system, nickel-based catalysts have long been widely studied and used due to their high activity and relatively low cost. However, there are still key bottlenecks in the practical application of this type of catalyst that need to be overcome: at high temperatures, metallic Ni particles are prone to migration and agglomeration, leading to a decrease in specific surface area and loss of active sites; during the dehydrogenation process of tar molecules on the Ni surface, graphitized carbon species are easily formed, which cover the active sites and cause deactivation.
[0005] To overcome the above limitations, perovskite oxides have attracted widespread attention due to their unique structural tunability and excellent thermal stability: by controlling the type and ratio of B-site metals, in-situ confined dissolution of active components can be achieved, and the migration and aggregation of metal particles can be inhibited by utilizing the anchoring effect of the perovskite framework.
[0006] Nevertheless, existing perovskite-based tar steam reforming catalysts still face several challenges: Firstly, in traditional methods, the distribution of metal at the B-site in leached perovskite materials is uneven, and local over-reduction is prone to occur during the reduction process, resulting in larger metal particle size and poor dispersion. Secondly, the dissolution kinetics of single Ni-doped perovskite are difficult to control during the reduction process: insufficient reduction results in low Ni dissolution and low density of active sites, while excessive reduction leads to excessive Ni dissolution and the formation of large-sized particles. There is no universal method to achieve precise constraints on the size and dispersion of Ni particles. Third, existing research focuses on single metal leaching systems, lacks universal screening of B-site doped metals, and has not formed a general strategy for controlling Ni leaching behavior through co-doping. In particular, it lacks a technical solution to control Ni particle growth and suppress high-temperature sintering by doping without significantly changing the intrinsic activity of Ni. Summary of the Invention
[0007] The purpose of this invention is to provide a controllable dissolution catalyst of weakly crystallized RP phase mediated alloy, its preparation method and application. By co-doping at the B site with narrow window and the dissolution process, the size of the nickel-based alloy on the support surface is precisely constrained, solving the problems of excessive growth and uncontrollable size of traditional nickel-based catalyst particles.
[0008] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing a controllable dissolution catalyst of a weakly crystallized RP phase-mediated alloy, comprising the following steps: (1) Preparation of a catalyst precursor co-doped with nickel and soluble transition metal M at the B-site of perovskite: A mixed solution containing lanthanum salt, nickel salt and soluble transition metal M salt was prepared, and a dry gel was prepared by the sol-gel method; the dry gel was subjected to stepwise temperature-programmed calcination to obtain a catalyst precursor co-doped with nickel and soluble transition metal M at the B-site of perovskite; the chemical formula of the catalyst precursor is La 1-a Ni 1-x M x For O3, 0 < a ≤ 0.1, 0 < x ≤ 0.2, the doping amount of soluble transition metal M in the catalyst precursor is 0.01~5 wt.%; (2) Temperature-programmed reduction-induced formation of weakly crystallized RP phase and in-situ co-dissolution of B-site metal: The catalyst precursor is reduced in a low-oxygen partial pressure atmosphere. During the reduction process, a weakly crystallized RP phase layered perovskite mesophase is generated in situ. This weakly crystallized RP phase layered perovskite mesophase is used to induce in-situ co-dissolution of nickel and soluble transition metal M at the B-site, forming dispersed nickel-based alloy nanoparticles with an average particle size of 5~40 nm on the surface of the catalyst precursor, thus obtaining the catalyst. The chemical formula of the weakly crystallized RP phase layered perovskite mesophase is La. n+1 (Ni 1-x M x ) n O 3n+1±δ , 0<x≤0.2, n is an integer from 1 to 3, and δ is the number of oxygen vacancies.
[0009] Preferably, the soluble transition metal M in step (1) is one or more of Co, Fe, and Cu.
[0010] As a preferred embodiment, the sol-gel method in step (1) specifically includes: mixing lanthanum salt, nickel salt, and soluble transition metal M salt with water, then adding citric acid and ethylene glycol, heating and stirring at 80~90 ℃, aging and drying to obtain a dry gel.
[0011] Preferably, the amount of soluble transition metal M doped in the catalyst precursor in step (1) is 0.01~5 wt.% and the amount of nickel doped is 15~25 wt.%.
[0012] Preferably, the conditions for the stepped temperature-programmed calcination in step (1) include: in an oxygen-deficient atmosphere, first heating to 240-260 ℃ at a heating rate of 8-12 ℃ / min and holding for 0.5-1.5 h, then heating to 480-520 ℃ at a heating rate of 8-12 ℃ / min and holding for 0.5-1.5 h, and then heating to 780-820 ℃ at a heating rate of 8-12 ℃ / min and holding for 3-5 h; the oxygen-deficient atmosphere is an atmosphere with an oxygen volume fraction lower than that of air.
[0013] Preferably, the low oxygen partial pressure atmosphere in step (2) has an equilibrium oxygen partial pressure ≤ 1 × 10⁻⁶. -20 The reducing atmosphere of atm; the reducing atmosphere is an H2 / Ar mixture with a volume fraction of 3~10% H2.
[0014] Preferably, the conditions for the programmed temperature reduction in step (2) include: a heating rate of 5~12 ℃ / min, a temperature of 500~700 ℃, and a time of 0.5~4 h.
[0015] The present invention also provides a controllable dissolution catalyst for a weakly crystallized RP phase-mediated alloy prepared by the above preparation method.
[0016] This invention also provides an application of a weakly crystallized RP phase-mediated alloy controllable dissolution catalyst in catalytic tar steam reforming, methane dry reforming, or water-gas shift reaction.
[0017] In this invention, the relevant terms are defined as follows: Controllable dissolution of nickel-based alloys: This refers to the core of the invention, namely, controlling the migration and precipitation process of nickel ions through narrow-window co-doping at B sites, thereby achieving controllable adjustment of the size and dispersion of nickel-based alloy nanoparticles.
[0018] Weakly crystallized RP phase: refers to the Ruddlesden-Popper (RP) type layered phase induced by narrow-window doping, a special state distinct from undoped / overdoped RP phases, specifically characterized by a relative crystallinity of the main peak ≤30% (compared to the reference sample). The reference sample is a catalyst obtained by the same preparation method as this invention, with a crystallinity of 100% obtained from a sample without B-site doping of a soluble transition metal M. The weakly crystallized RP phase has three distinct characteristics: ① Low phase abundance: the integrated intensity of the XRD characteristic diffraction peaks is significantly lower than that of the RP phase of undoped / overdoped samples; ② Numerous structural defects: a large number of oxygen vacancies and dislocations exist in the lattice, resulting in higher ionic conductivity than the fully crystallized RP phase; ③ Dispersed spatial distribution: discrete distribution, without forming a continuous dense layer. In this invention, the weakly crystallized RP phase is mainly composed of La2NiO4, and its loose interlayer bonding is the structural basis for the controlled dissolution of nickel-based alloys.
[0019] Narrow window: refers to the doping range of 0.01~5 wt.% of transition metals that can be dissolved. It is the core parameter threshold for achieving controllable dissolution of nickel-based alloys. The weakly crystallized RP phase generated within this window can effectively balance the amount of nickel dissolved and the particle size.
[0020] As can be seen from the above technical solution, compared with the prior art, the present invention has the following beneficial effects: (1) The linkage mechanism of "doping amount - RP phase weak crystallization degree - nickel dissolution behavior" is revealed for the first time: This invention selects specific transition metals such as Co, Fe, and Cu as structure regulators. When the doping amount is in a narrow window of 0.01~5 wt.%, the RP phase is mainly La2NiO4. The RP phase has large lattice distortion and limited growth, and cannot form a continuous dense structure. It presents a weak crystallization state with low abundance, high defects, and discrete distribution. While facilitating the in-situ co-dissolution of B-site metals during the reduction process, it effectively constrains the size of alloy particles. When the doping amount exceeds 5 wt.%, the RP phase gradually evolves towards higher bond energy, improved RP phase lattice integrity, and growth into a continuous dense structure, thus hindering metal migration. Although the undoped sample generates the La2NiO4 phase, it is a continuous thick layer formed by the spontaneous decomposition of perovskite, without weak crystallization characteristics, and cannot restrict nickel ion migration. This change in the weak crystallization degree of the RP phase regulated by the doping amount is the fundamental reason for the controllable dissolution of nickel-based alloys in this invention.
[0021] (2) The narrow window effect of B-site doping was established: by controlling the doping amount of soluble transition metal within a narrow window of 0.01~5wt.%, the catalyst structure can be adjusted while maintaining the high activity of Ni, so as to achieve controllable dissolution of active metal, suppress nickel agglomeration, improve stability, and have long-term industrial application value.
[0022] (3) The method has universality and adjustability: the Co, Fe, and Cu doped metals of this invention have ionic radii similar to Ni.2+ The similar characteristics (difference ≤15%) and ease of alloying with Ni constitute a scalable technological branch. By changing the type and ratio of doped metals, the size of Ni-based alloy particles can be precisely adjusted to the nanometer level, adapting to the structural requirements of active sites in different reaction systems.
[0023] (4) Simple process, easy to scale up industrially: This invention adopts a mature sol-gel combined low oxygen partial pressure reduction process, which can achieve fine control of dissolution kinetics without complicated equipment, and the resulting catalyst has a BET specific surface area of up to 30m². 2 / g, with good process repeatability and low difficulty in scale-up.
[0024] (5) Excellent performance stability: This invention refines the Ni particle size control through narrow window co-doping, and provides a better structural basis for long-term operation while maintaining the toluene conversion rate (100% at 450 °C) and product distribution (combustible components such as hydrogen and methane account for more than 65%) comparable to single Ni-based catalysts. Attached Figure Description
[0025] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below.
[0026] Figure 1 X-ray diffraction patterns of the catalysts prepared in Example 1 and Comparative Examples 1-5; Figure 2 Atomic force microscopy images of the catalysts prepared in Example 1 and Comparative Examples 1-5; Figure 3 The images show the Ni 2p and Co 2p X-ray photoelectron spectra of the catalysts prepared in Example 1 and Comparative Examples 1-3; where a is the Ni 2p X-ray photoelectron spectrum and b is the Co 2p X-ray photoelectron spectrum. Figure 4 Transmission electron microscopy (TEM) images of the catalysts prepared in Example 1 and Comparative Example 3; Figure 5 Aberration-corrected high-angle annular dark-field scanning transmission electron microscope image of the catalyst prepared in Example 1; Figure 6 These are performance test graphs of the catalysts prepared in Example 1 and Comparative Examples 1-5; Figure 7 The graph shows the stability test results of the catalyst prepared in Example 1 after 80 h. Detailed Implementation
[0027] This invention provides a method for preparing a controllable dissolution catalyst of a weakly crystallized RP phase-mediated alloy, comprising the following steps: (1) Preparation of a catalyst precursor co-doped with nickel and soluble transition metal M at the B-site of perovskite: A mixed solution containing lanthanum salt, nickel salt and soluble transition metal M salt was prepared, and a dry gel was prepared by the sol-gel method; the dry gel was subjected to stepwise temperature-programmed calcination to obtain a catalyst precursor co-doped with nickel and soluble transition metal M at the B-site of perovskite; the chemical formula of the catalyst precursor is La 1-a Ni 1-x M x For O3, 0 < a ≤ 0.1, 0 < x ≤ 0.2, the doping amount of soluble transition metal M in the catalyst precursor is 0.01~5 wt.%; (2) Temperature-programmed reduction-induced formation of weakly crystallized RP phase and in-situ co-dissolution of B-site metal: The catalyst precursor is reduced in a low-oxygen partial pressure atmosphere. During the reduction process, a weakly crystallized RP phase layered perovskite mesophase is generated in situ. This weakly crystallized RP phase layered perovskite mesophase is used to induce in-situ co-dissolution of nickel and soluble transition metal M at the B-site, forming dispersed nickel-based alloy nanoparticles with an average particle size of 5~40 nm on the surface of the catalyst precursor, thus obtaining the catalyst. The chemical formula of the weakly crystallized RP phase layered perovskite mesophase is La. n+1 (Ni 1-x M x ) n O 3n+1±δ , 0<x≤0.2, n is an integer from 1 to 3, and δ is the number of oxygen vacancies.
[0028] In this invention, the catalyst precursor in step (1) is a composite oxide with a perovskite structure, where La occupies the A site (the cavity site surrounded by oxygen octahedra) of the perovskite structure, and nickel and the soluble transition metal M jointly occupy the B site (the central site of oxygen octahedra) of the perovskite structure; the perovskite structure includes ABO3 type, non-stoichiometric perovskite type, double perovskite type or layered perovskite type.
[0029] In this invention, the soluble transition metal M mentioned in step (1) is preferably one or more of Co, Fe, and Cu, and more preferably Co. The divalent ionic radius of the soluble transition metal is related to that of Ni. 2+ The difference is no more than 15%, which can stably occupy the B-site lattice of perovskite, and can alloy with Ni under reducing conditions, thus helping to achieve the controllable dissolution of nickel-based alloys.
[0030] In this invention, the sol-gel method in step (1) specifically includes: mixing lanthanum salt, nickel salt, and soluble transition metal M salt with water, then adding citric acid and ethylene glycol, heating and stirring at 80~90 ℃, aging, and drying to obtain a dry gel; the ratio of the total molar amount of lanthanum salt, nickel salt, soluble transition metal M salt, molar amount of citric acid, and molar amount of ethylene glycol is preferably 1:1:2; the aging time is preferably 3 h; the drying conditions include: the temperature is preferably 120 ℃, and the time is preferably 12 h.
[0031] In this invention, the preferred conditions for the stepped temperature-programmed calcination in step (1) include: in an oxygen-deficient atmosphere, first heating to 240-260°C at a heating rate of 8-12°C / min and holding for 0.5-1.5 h, then heating to 480-520°C at a heating rate of 8-12°C / min and holding for 0.5-1.5 h, then heating to 780-820°C at a heating rate of 8-12°C / min and holding for 3-5 h; more preferably, in an oxygen-deficient atmosphere, first heating to 250°C at a heating rate of 10°C / min and holding for 1 h for dehydration and decomposition, then heating to 500°C at a heating rate of 10°C / min and holding for 1 h for denitrification, then heating to 800°C at a heating rate of 10°C / min and holding for 4 h. h crystallizes the perovskite; the oxygen-deficient atmosphere is an atmosphere with an oxygen volume fraction lower than that of air, and more preferably an inert gas atmosphere or a vacuum / sealed self-generated atmosphere with an oxygen volume fraction ≤ 5%.
[0032] In this invention, the doping amount of the soluble transition metal M in the catalyst precursor described in step (1) is preferably 0.01~5 wt.%, more preferably 5 wt.%, and the doping amount of nickel is preferably 15~25 wt.%, more preferably 25 wt.%. The doping range of the soluble transition metal is defined as a "narrow window" to achieve a balance between high activity and high dispersion. When the doping amount is less than 0.01 wt.%, the control effect is insufficient, resulting in excessive dissolution of Ni, larger particle size, weak metal-support interaction, and easy agglomeration. When the doping amount is greater than 5 wt.%, the metal-support interaction is too strong, which in turn inhibits the dissolution behavior of Ni, resulting in a significant decrease in the density of surface active Ni sites, which is not conducive to catalysis.
[0033] In this invention, the low oxygen partial pressure atmosphere in step (2) is preferably an equilibrium oxygen partial pressure ≤ 1 × 10⁻⁶. -20 The reducing atmosphere is atm (600 °C, residual H2O ≤ 1000 ppm according to H2 / H2O balance); the reducing atmosphere is preferably an H2 / Ar mixture with H2 volume fraction of 3~10%, and more preferably an H2 / Ar mixture with H2 volume fraction of 5%.
[0034] In this invention, the conditions for the programmed temperature rise reduction in step (2) include: the heating rate is preferably 5~12 ℃ / min, more preferably 10 ℃ / min, the temperature is preferably 500~700 ℃, more preferably 600 ℃, and the time is preferably 0.5~4 h, more preferably 2 h.
[0035] In this invention, the average particle size of the nickel-based alloy nanoparticles in step (2) is ≤40 nm. The in-situ co-dissolution process is controlled by low oxygen partial pressure, so that the average particle size of the dissolved nickel-based alloy nanoparticles is controlled below 40 nm, thereby achieving precise constraint on the size and morphology of nickel particles.
[0036] In this invention, the nickel atomic ratio in the nickel-based alloy nanoparticles described in step (2) is not less than 50%, and the soluble transition metals mainly exist as structural control units.
[0037] The present invention also provides a controllable dissolution catalyst for a weakly crystallized RP phase-mediated alloy prepared by the above preparation method.
[0038] This invention also provides an application of a weakly crystallized RP phase-mediated alloy controllable dissolution catalyst in catalytic tar steam reforming, methane dry reforming, or water-gas shift reaction.
[0039] The present invention relates to a method for the controlled dissolution of nickel-based alloy nanoparticles from perovskite surfaces based on narrow-window co-doping at B-sites. The core of this method is the narrow-window co-doping of perovskite at B-sites with transition metals of specific ionic radii, combined with a low-oxygen partial pressure reduction process, to achieve the controlled dissolution of Ni particles. The following detailed description uses Co, a typical example among the soluble transition metals, as an example. Those skilled in the art should understand that other transition metals such as Fe and Cu, which meet the requirements for ionic radius and alloying, can be used to replace Co to achieve the controllable dissolution effect described in this invention.
[0040] The common characteristics of soluble transition metals defined in this invention are: the radius of divalent ions and Ni 2+ The difference (0.69 Å) is no greater than 15%, which allows for stable embedding in the perovskite B-site lattice. Under reducing conditions, it can partially dissolve and form alloys with Ni, specifically including Co. 2+ (0.745Å), Fe 2+ (0.78Å), Cu 2+ (0.73Å) This type of metal mainly plays a role in structural regulation in the system, rather than as the main active component.
[0041] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0042] Example 1
[0043] The preparation of a controlled dissolution catalyst for nickel-based alloys mediated by weakly crystallized RP phase based on B-site narrow-window co-doping includes the following steps: Perovskite precursors were synthesized using the sol-gel method: Based on the prepared perovskite La 0.95 Co 0.2 Ni 0.8 To determine the theoretical stoichiometry of O3, weigh out the required amounts of metal nitrates: 5.586 g of lanthanum nitrate hexahydrate, 3.159 g of nickel nitrate hexahydrate, and 0.79 g of cobalt nitrate hexahydrate. Dissolve these in 30 mL of deionized water and heat in a water bath at 80 °C for 10 min until fully mixed and uniformly dispersed. Add 5.087 g of citric acid to chelate and stabilize the metal ions. Continue heating and stirring for 10 min, then add 2.953 mL of ethylene glycol solution dropwise to construct a three-dimensional polyester organic network. The molar ratio of the total metal ions, citric acid, and ethylene glycol is 1:1:2.
[0044] When heated and stirred until it becomes a viscous gel, the resulting viscous gel, along with the reaction vessel, is left to stand at room temperature for 3 hours to release the internal stress of the gel and form a uniform and transparent wet gel.
[0045] The aged wet gel was placed in a forced-air drying oven and dried at 120 ℃ for 12 h to dehydrate and expand, forming a low-density, fluffy, sponge-like dry gel. The gel was then scraped off and ground into a fine powder.
[0046] The obtained dry gel powder was placed in a covered crucible and calcined in a muffle furnace under a closed autogenous atmosphere with an oxygen volume fraction ≤5%. The temperature was increased to 250 °C at a rate of 10 °C / min and held for 1 h to remove residual moisture and decompose citric acid. The temperature was then increased to 500 °C at a rate of 10 °C / min and held for 1 h to completely remove nitrates and prevent deflagration. The temperature was then increased to 800 °C at a rate of 10 °C / min and held for 4 h to complete the crystallization of the perovskite structure. After the reaction, the furnace was allowed to cool naturally to room temperature to obtain a black powdery perovskite-based catalyst precursor with abundant defects.
[0047] Controlled dissolution of nickel-based alloy nanoparticles: The obtained perovskite-based catalyst precursor powder was transferred to a quartz boat and placed in a tube furnace. The furnace was then reduced to 600 °C for 2 h at a heating rate of 10 °C / min under a 5% hydrogen-argon atmosphere. At this point, the equilibrium oxygen partial pressure of the system was 6 × 10⁻⁶. -28 atm (calculated based on H2 / H2O equilibrium at 600 ℃, with residual H2O ≤ 1000 ppm). After the reaction is complete, the furnace is naturally cooled to room temperature to obtain the perovskite-based catalyst with dissolved nano-sized nickel-based alloy.
[0048] Comparative Examples 1-5
[0049] Same as Example 1, except for the content of nickel and cobalt in the catalyst, as shown in Table 1 below: Table 1. Composition of the catalysts in Example 1 and Comparative Examples 1-5
[0050] The structural properties of the catalysts prepared in Example 1 and the comparative example were characterized, and the results are as follows: Figure 1 X-ray diffraction patterns of the catalysts prepared in Example 1 and Comparative Examples 1-5: The RP phase in the undoped sample is strongly crystallized and difficult to confine nickel migration; the RP phase in the overdoped comparative examples gradually evolves towards increased crystallinity as the doping amount increases; the RP phase in Example 1 is mainly La2NiO4, exhibiting weak crystallization characteristics.
[0051] Figure 2 The images show atomic force microscopy (AFM) images of the catalysts prepared in Example 1 and Comparative Examples 1-5, showing that compared to all comparative examples, the metal particles dissolved from the surface of Example 1 are smaller in size, denser in density, and better dispersed.
[0052] Figure 3 The X-ray photoelectron spectra of Co 2p and Ni 2p of the catalysts prepared in Example 1 and Comparative Examples 1-3 are shown, confirming that nickel and cobalt are dissolved on the surface in elemental form.
[0053] Figure 4 The images show transmission electron microscopy (TEM) images of the catalysts prepared in Example 1 and Comparative Example 3. The enrichment of precursor sites is visible, confirming the structural transformation and metal dissolution of the perovskite precursor. In Example 1, a smaller cobalt-nickel alloy is produced on the surface.
[0054] Figure 5 The image shows an aberration-corrected high-angle annular dark-field scanning transmission electron microscope image of the catalyst prepared in Example 1, which shows the nanoscale cobalt-nickel alloy particles on the surface of the catalyst in Example 1 and the tight interface between the particles and the RP phase.
[0055] Using toluene as a model compound for biomass gasification tar, the performance of the catalysts prepared in Example 1 and the comparative example was tested in an apparatus consisting of a feed gas-liquid conveying system, a catalytic steam reforming system, and a product composition analysis system. The specific operation included: placing 0.25 g of catalyst as a bed material in the center of a quartz reaction tube with an outer diameter of 10 mm, an inner diameter of 6 mm, and a tube length of 32 cm, supported by quartz wool. This quartz reaction tube was placed in the center of an electrically heated furnace. Gaseous toluene with a concentration of 1000 ppm was introduced into the system at a flow rate of 50 mL / min, at which point the gas hourly space velocity was 12000 mL·h. -1 ·g - 1 To simulate the moisture content (approximately 5.6%) in biomass gasification gas, deionized water was pumped into the mixing and preheating chamber at a rate of 2.2519 μL / min using a syringe pump. The mixture was then mixed with toluene gas, vaporized, and passed through a heating element into a quartz tube. An electric heater heated the material inside the quartz tube at different temperatures, causing a reaction. The gaseous products after the reaction were subjected to gas chromatography for component analysis, and the tail gas was treated by an absorption device. All parameters were set and controlled by the equipment control system.
[0056] The conversion rate X of toluene is calculated using the following formula:
[0057] in, n T,in This represents the concentration of toluene in the intake air (mol / min). n T,out This represents the concentration of toluene in the exhaust gas (mol / min).
[0058] Figure 6The figures show the performance test results of the catalysts prepared in Example 1 and Comparative Examples 1-5. The following conclusions can be drawn: The catalyst prepared in Example 1 can efficiently convert toluene, a model compound of tar in biomass gasification gas, at low temperatures. The toluene conversion rate reaches 87.0% at 400 °C and 100% at 450 °C. Furthermore, the combustible gas content (i.e., hydrogen, methane, and carbon monoxide) in the product gas can reach over 60%, which is essentially equivalent to the conversion rate of undoped nickel-based catalysts (Comparative Examples 4 and 5). This demonstrates that the intrinsic activity of nickel is not significantly altered. Simultaneously, the moderate mediating effect of the weakly crystallized RP phase effectively constrains the size of the nickel-based alloy particles, enhancing the metal-support interaction and inhibiting sintering. As the doping concentration exceeds the upper limit of the narrow window (Comparative Examples 1-3), the toluene conversion rate shows a significant decreasing trend, indicating hindered dissolution of the active metal and a decrease in the total number of active sites on the surface capable of participating in the reaction. Although the initial activity of the undoped nickel-based catalysts (Comparative Examples 4 and 5) was similar to that of Example 1, the larger nickel particle size and weaker metal-support interaction made them more prone to activity decay due to sintering during long-term operation. In contrast, the dissolved alloy of Example 1 had a smaller particle size and stronger MSI, exhibiting higher stability in long-term experiments. Figure 7 Therefore, the narrow-window co-doping proposed in this invention is necessary.
[0059] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a controlled dissolution catalyst of a weakly crystallized RP phase-mediated alloy, characterized in that, Includes the following steps: (1) Preparation of a catalyst precursor co-doped with nickel and soluble transition metal M at the B-site of perovskite: A mixed solution containing lanthanum salt, nickel salt and soluble transition metal M salt was prepared, and a dry gel was prepared by the sol-gel method; the dry gel was subjected to stepwise temperature-programmed calcination to obtain a catalyst precursor co-doped with nickel and soluble transition metal M at the B-site of perovskite; the chemical formula of the catalyst precursor is La 1-a Ni 1-x M x For O3, 0 < a ≤ 0.1, 0 < x ≤ 0.2, the doping amount of soluble transition metal M in the catalyst precursor is 0.01~5 wt.%; (2) Temperature-programmed reduction-induced formation of weakly crystalline RP phase and in-situ co-dissolution of B-site metal: The catalyst precursor is placed in a low-oxygen partial pressure atmosphere for reduction. During the reduction process, a weakly crystalline RP phase layered perovskite mesophase is generated in situ. This weakly crystalline RP phase layered perovskite mesophase is used to induce in-situ co-dissolution of nickel in the B-site with soluble transition metal M, forming dispersed nickel-based alloy nanoparticles with an average particle size of 5~40 nm on the surface of the catalyst precursor, thus obtaining the catalyst; the low-oxygen partial pressure atmosphere is an equilibrium oxygen partial pressure ≤1×10 -20 The reducing atmosphere of atm; the reducing atmosphere is an H2 / Ar mixture with a volume fraction of 3-10% H2; the chemical formula of the weakly crystallized RP phase layered perovskite mesophase is La. n+1 (Ni 1-x M x ) n O 3n+1±δ , 0<x≤0.2, n is an integer from 1 to 3, and δ is the number of oxygen vacancies.
2. The preparation method according to claim 1, characterized in that, The soluble transition metal M mentioned in step (1) is one or more of Co, Fe, and Cu.
3. The preparation method according to claim 1, characterized in that, The sol-gel method described in step (1) specifically includes: mixing lanthanum salt, nickel salt, and soluble transition metal M salt with water, then adding citric acid and ethylene glycol, heating and stirring at 80~90 ℃, aging and drying to obtain a dry gel.
4. The preparation method according to claim 1, characterized in that, The amount of nickel doped in the catalyst precursor described in step (1) is 15~25 wt.%.
5. The preparation method according to claim 1, characterized in that, The conditions for the stepped temperature-programmed calcination in step (1) include: in an oxygen-deficient atmosphere, first heating to 240-260 ℃ at a heating rate of 8-12 ℃ / min and holding for 0.5-1.5 h, then heating to 480-520 ℃ at a heating rate of 8-12 ℃ / min and holding for 0.5-1.5 h, and then heating to 780-820 ℃ at a heating rate of 8-12 ℃ / min and holding for 3-5 h; the oxygen-deficient atmosphere is an atmosphere with an oxygen volume fraction lower than that of air.
6. The preparation method according to claim 1, characterized in that, The conditions for the programmed temperature reduction in step (2) include: a heating rate of 5~12 ℃ / min, a temperature of 500~700 ℃, and a time of 0.5~4 h.
7. A controlled dissolution catalyst for a weakly crystallized RP phase-mediated alloy prepared by the preparation method according to any one of claims 1 to 6.
8. The application of the weakly crystallized RP phase-mediated alloy controllable dissolution catalyst as described in claim 7 in catalytic tar steam reforming, methane dry reforming or water-gas shift reaction.