Mt1Mt2Cln / MIL-53(al)ht@ZSM-5 hollow microsphere core-shell catalyst and preparation method and application thereof
By using the supported double salt design of the Mt1Mt2Cln/MIL-53(Al)ht@ZSM-5 hollow microsphere core-shell catalyst, the problems of low dimethyldichlorosilane yield and high and low boiling point treatment were solved, achieving efficient catalytic M1/M3 disproportionation and boiling point conversion, and improving the stability and selectivity of the catalyst.
Patent Information
- Application Number
- CN202611330497.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-13
AI Technical Summary
In existing technologies, the yield of dimethyldichlorosilane is low, and the problems of treating high-boiling and low-boiling substances have not been effectively solved, resulting in resource waste and environmental pollution.
The core-shell catalyst of hollow microspheres Mt1Mt2Cln/MIL-53(Al)ht@ZSM-5 is adopted. By loading the double salt Mt1Mt2Cln onto the MIL-53(Al)ht@ZSM-5 support, a core-shell structure is formed. The high catalytic activity of MOFs and the thermal stability of inorganic support are utilized to realize the disproportionation of M1/M3 and the conversion of high and low boiling points.
It significantly improved the yield of dimethyldichlorosilane, enhanced the stability and selectivity of the catalyst, expanded the scope of catalytic applications, and solved the problem of insufficient catalytic efficiency in existing technologies.
Smart Images

Figure CN123079409A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of organosilicon technology, and particularly relates to an Mt1Mt2Cl n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst, its preparation method and application. Background Technology
[0002] Organosilicon materials are a class of polymeric compounds with silicon-oxygen bonds as the main chain and linked to organic groups. They possess the dual characteristics of inorganic and organic materials, exhibiting excellent high and low temperature resistance, electrical insulation, and chemical stability. They have wide applications in aerospace, automotive, construction, and electronic medical fields. As a high-performance new material with superior properties, diverse forms, and wide applications, the importance and strategic position of organosilicon materials are fully reflected in national development plans.
[0003] In the organosilane industry, dimethyldichlorosilane ((CH3)2SiCl2, abbreviated as M2) is the core monomer for the preparation of organosilicon materials and is widely used in products such as silicone resins, elastomers, and silicone oils. Currently, the main method for synthesizing methylchlorosilanes in industrial production is the Rochow-Müller direct process. This method inevitably generates large amounts of monomethyltrichlorosilane (CH3SiCl3, M1), trimethylmonochlorosilane ((CH3)3SiCl, abbreviated as M3), and other chlorosilane byproducts during production. Direct discharge of these byproducts not only causes serious environmental pollution and safety hazards but also corrodes infrastructure, leading to economic losses. Therefore, converting M1 and M3 into the high-value-added M2 through catalytic disproportionation is a key approach to solving the problem of byproduct accumulation and improving resource utilization efficiency.
[0004] However, the yield of M2 in existing technologies is generally low, only around 70%, which is insufficient to meet the demands of efficient industrial production. Furthermore, the organosilicon industry faces the challenge of handling low-boiling-point substances (boiling points approximately 26-58℃) and high-boiling-point substances (boiling points approximately 70.5-160℃). High-boiling-point substances are currently only used in low-value-added products such as waterproofing agents; large-scale accumulation not only wastes valuable resources but also causes severe corrosion to storage tanks, and direct discharge would severely pollute the environment. Therefore, developing high-performance catalysts capable of simultaneously and efficiently catalyzing the disproportionation of M1 / M3 and the conversion of high-boiling-point to low-boiling-point substances is of great significance for promoting the sustainable development of the organosilicon industry.
[0005] Metal-organic frameworks (MOFs) such as MIL-53(Al) possess advantages such as large specific surface area, tunable pore structure, and abundant acidic sites. When combined with the inorganic molecular sieve ZSM-5, they can form a core-shell structure support, combining the catalytic activity of organic ligands with the high stability of inorganic materials. Studies have shown that MIL-53(Al)... htThe ZSM-5 core-shell structure possesses certain functions in the cracking and disproportionation of high-boiling-point substances, but its catalytic activity remains limited when used alone. Building upon this, by loading a complex salt active component to construct a synergistic catalytic system, it is expected to further reduce the activation energy of Lewis acid active sites, increase the M2 yield, and expand the application range of the catalyst for the disproportionation reactions of both high- and low-boiling-point substances. This would address the technical problems of insufficient catalytic efficiency and low product selectivity in existing technologies. Summary of the Invention
[0006] To solve the above-mentioned technical problems, this invention proposes a Mt1Mt2Cl n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst, its preparation method and application.
[0007] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a Mt1Mt2Cl n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst, with MIL-53(Al) ht Hollow microspheres form the core, and ZSM-5 molecular sieve forms the outer shell, constituting a core-shell carrier. The complex salt Mt1Mt2Cl is loaded onto this core-shell carrier. n As an active component; wherein, the complex salt Mt1Mt2Cl n In this context, Mt1 is selected from Li + Na + K + 、Rb + and Cs + Any one of them; Mt2 is selected from Al 3+ Fe 3+ and La 3+ Any one of the following, n=4; or Mt2 is selected from Cu. 2+ Fe 2+ Any one of them, n=3.
[0008] The present invention also provides the above-mentioned Mt1Mt2Cl n / MIL-53(Al) ht The preparation method of the ZSM-5 hollow microsphere core-shell catalyst includes the following steps: (1) Aluminum source and terephthalic acid are mixed in an organic solvent, and after hydrothermal reaction, washing and drying, MIL-53(Al) is obtained; (2) The MIL-53(Al) is calcined to obtain MIL-53(Al). ht carrier; (3) Mix tetrapropylammonium hydroxide with water, add a silicon source, sonicate, then add sodium aluminate, stir at room temperature to obtain ZSM-5 precursor solution, and then add the MIL-53(Al). ht The carrier, after pH adjustment, was subjected to hydrothermal crystallization, washing, drying, and calcination to obtain MIL-53(Al). ht @ZSM-5 hollow microsphere carrier; (4) The MIL-53(Al) ht The ZSM-5 hollow microsphere carrier is first impregnated in a chloride solution containing Mt1, dried, and then impregnated in a chloride solution containing Mt2. After crystallization and drying, it is then used in the MIL-53(Al) carrier. ht @ZSM-5 hollow microsphere carrier for forming complex salts Mt1Mt2Cl n The Mt1Mt2Cl was obtained. n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst.
[0009] Further, in step (1), the aluminum source is aluminum nitrate nonahydrate, and the mass ratio of aluminum nitrate nonahydrate to terephthalic acid is 3.75:1.66; the hydrothermal reaction temperature is 220℃, the reaction time is 72h, and the hydrothermal reaction is carried out in a reactor lined with tetrafluoroethylene; the washing is done by alternating washing with DMF (dimethylformamide) and deionized water, and the number of washings is 3; the drying is done at 80-100℃ for 10-12h.
[0010] Furthermore, in step (2), the roasting temperature is 330°C and the roasting time is 24 hours.
[0011] Further, in step (3), the silicon source is tetraethyl orthosilicate; the pH is adjusted to 10.
[0012] Furthermore, in step (3), the hydrothermal crystallization temperature is 180°C and the reaction time is 48h; the calcination is calcined at 380°C for 6h.
[0013] Further, in step (4), the molar concentrations of the chloride solution containing Mt1 and the chloride solution containing Mt2 are both 0.0415~0.1668 mol / L; the immersion time in the chloride solution containing Mt1 is 1 h, and the immersion time in the chloride solution containing Mt2 is 0.5-3.5 h; the molar ratio of Mt1 to Mt2 in the chloride solution containing Mt1 and the chloride solution containing Mt2 is (1-2):(1-3), for example 2:1, 1:1, 1:2 and 1:3; the double salt Mt1Mt2Cl n In the MIL-53(Al) htThe loading amount on the ZSM-5 hollow microsphere carrier is 10-14 wt%.
[0014] In step (4), the impregnation time of the chloride solution containing Mt1 and the chloride solution containing Mt2 affects the deposition of the double salt on the support surface, indirectly affecting the number and acid strength of the catalyst activation acidic sites. The presence of the double salt can reduce the active component Mt2Cl n-1 Loss; as the loading of active components increases, it helps to increase the number of active sites on the catalyst surface.
[0015] Furthermore, in step (4), the crystallization reaction temperature is 190°C and the reaction time is 17h.
[0016] The present invention also provides the above-mentioned Mt1Mt2Cl n / MIL-53(Al) ht The application of the ZSM-5 hollow microsphere core-shell catalyst in the catalytic disproportionation of monomethyltrichlorosilane and trimethylchlorosilane to prepare dimethyldichlorosilane; further, the volume ratio of monomethyltrichlorosilane to trimethylchlorosilane is 1:(1-2), and the Mt1Mt2Cl n / MIL-53(Al) ht The dosage of the ZSM-5 hollow microsphere core-shell catalyst in the system was 0.7 g / 4 μL.
[0017] The present invention also provides the above-mentioned Mt1Mt2Cl n / MIL-53(Al) ht Application of @ZSM-5 hollow microsphere core-shell catalyst in the disproportionation reaction of organosilicon high-boiling and low-boiling substances; further, the Mt1Mt2Cl n / MIL-53(Al) ht The dosage of the ZSM-5 hollow microsphere core-shell catalyst in the system was 0.7 g / 20 mL.
[0018] Patent CN113457726A discloses a hollow microsphere core-shell catalyst, its preparation method, and its application. It uses γ-Al₂O₃ as a porous outer shell and ZSM-5 as a core, with NaAlCl₄ double salt supported on the outer shell. This invention differs fundamentally from it, as follows: (1) Different active component systems: Existing technologies only use a single NaAlCl4 double salt and have not conducted systematic research; this invention targets Mt1Mt2Cl nA series of complex salts were systematically investigated. In the selection of complex salts, the commonly used AlCl3 was expanded to common L acids such as LaCl3, FeCl3 and CuCl2, and NaCl was expanded to LiCl, KCl, CsCl and RbCl. The active site was expanded from Al-Cl bond to Mt2-Cl bond with better catalytic disproportionation effect, thus improving the catalytic activity. (2) Different core-shell support structures: The existing technology uses pure inorganic ZSM-5 / γ-Al2O3 support, which has limited ability to confine the reaction system. Based on the principle of like dissolves like, the present invention constructs an inorganic@organic metal MOFs core-shell support. Its organic ligands are homologous and polarity matched with the organic substrate skeleton, forming a substrate-pore interface affinity effect. It not only improves the disproportionation activity with the help of MOFs, but also solves the problem of poor stability of MOFs through the inorganic core. (3) Different catalytic application range: The existing technology is only applicable to the disproportionation reaction of monomethyltrichlorosilane and trimethylchlorosilane. On this basis, the present invention further extends to the disproportionation reaction of low-boiling and high-boiling substances.
[0019] This invention uses MIL-53(Al) as the outer shell and inorganic ZSM-5 as the core, fully utilizing the high catalytic activity of MOFs and the high thermal stability of the inorganic support. By leveraging the barrier effect, it breaks down the trade-off barrier between metal-organic and inorganic materials, achieving the Mt1Mt2Cl... n The synergistic catalysis of the double salt confinement effect and the Lewis acidic Mt2-Cl site significantly improves the catalyst stability and dimethyldichlorosilane selectivity. Compared with the prior art, the present invention has the following advantages and technical effects: (1) The present invention uses a hydrothermal synthesis method with aluminum nitrate nonahydrate as aluminum source and terephthalic acid as ligand to synthesize MIL-53(Al), which can maintain the integrity of its pore structure, increase the specific surface area, and facilitate the full contact between reactant molecules and internal acidic sites.
[0020] (2) The catalyst of this invention is a combination of organometallic and inorganic materials. The organometallic material selected is MIL-53(Al), a metal-organic framework material, which has excellent properties such as large specific surface area and numerous internal acidic sites, enabling the catalyst to fully contact the reactants. The inorganic material selected is ZSM-5, which has a high BET (Brunauer-Emmett-Teller) surface area, a special channel structure, abundant acidic sites, and thermal and hydrothermal stability. The loading of Mt1Mt2Cln and the synergistic effect of the Brønsted acid and Lewis acid generated by the interfacial interaction also enrich the active centers for the disproportionation preparation of dimethyldichlorosilane, improving the catalytic activity. n It can decompose into Mt2Cl during the reaction. n-1 As a reactive center, it can reversibly form Mt1Mt2Cl after the reaction. n Solved Mt2Cln-1 This addresses the issue of easy loss of a single active component and improves the thermal stability of the catalyst.
[0021] (3) The catalyst of the present invention has good catalytic effect on the preparation of dimethyldichlorosilane by disproportionation of methyltrichlorosilane and trimethylchlorosilane, and the yield of dimethyldichlorosilane is 86.14% at 220°C. The yield of dimethyldichlorosilane prepared by disproportionation of high-boiling and low-boiling substances at 200°C can reach more than 38%. Attached Figure Description
[0022] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The NaAlCl4 / MIL-53(Al) prepared in Example 1. ht TEM characterization images of the ZSM-5 hollow microsphere core-shell catalyst at different magnifications; Figure 2 The NaAlCl4 / MIL-53(Al) prepared in Example 1. ht @ZSM-5 hollow microsphere core-shell catalyst, MIL-53(Al) support, and MIL-53(Al) ht FT-IR characterization analysis of the @ZSM-5 core-shell vector; Figure 3 MIL-53(A1) in Example 1 ht Carrier, MIL-53(A1) ht @ZSM-5 core-shell vector, 10% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst, 14% NaAlCl4 / MIL-53(Al) from Example 2 ht @ZSM-5 hollow microsphere core-shell catalyst, Comparative Example 1: 6% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst and Comparative Example 2: 18% NaAlCl4 / MIL-53(Al) ht XRD characterization of the ZSM-5 hollow microsphere core-shell catalyst; Figure 4 In Figure (a), MIL-53(Al) is shown in Example 1. ht Carrier, MIL-53(A1) ht @ZSM-5 core-shell vector, 10% NaAlCl4 / MIL-53(Al) ht@ZSM-5 hollow microsphere core-shell catalyst, 14% NaAlCl4 / MIL-53(Al) from Example 2 ht @ZSM-5 hollow microsphere core-shell catalyst, Comparative Example 1: 6% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst and Comparative Example 2: 18% NaAlCl4 / MIL-53(Al) ht Thermogravimetric curve of the ZSM-5 hollow microsphere core-shell catalyst, (b) is for 10% NaAlCl4 / MIL-53(Al). ht Thermogravimetric curve of @ZSM-5. Detailed Implementation
[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0024] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0025] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0026] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0027] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0028] This invention provides a Mt1Mt2Cl n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst, with MIL-53(Al) ht Hollow microspheres form the core, ZSM-5 molecular sieve forms the outer shell, and the double salt Mt1Mt2Cl is loaded onto the core-shell support. n As the active component; among which, the complex salt Mt1Mt2Cl n In this context, Mt1 is selected from Li + Na + K + 、Rb + and Cs + Any one of them; Mt2 is selected from Al 3+ Fe 3+ and La 3+ Any one of the following, n=4; or Mt2 is selected from Cu. 2+ Fe 2+ Any one of the following, where n=3. For example, the catalyst of this invention is NaAlCl4 / MIL-53(Al). ht @ZSM-5 hollow microsphere core-shell catalyst or LiLaCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst.
[0029] The Mt1Mt2Cl of the present invention n / MIL-53(Al) ht The preparation method of the ZSM-5 hollow microsphere core-shell catalyst includes the following steps: (1) Aluminum source and terephthalic acid are mixed in an organic solvent, and after hydrothermal reaction, washing and drying, MIL-53(Al) is obtained; (2) MIL-53(Al) was calcined to obtain MIL-53(Al). ht carrier; (3) Mix tetrapropylammonium hydroxide (TPAOH) with water, add a silicon source, sonicate, then add sodium aluminate (NaAlO2), stir at room temperature to obtain ZSM-5 precursor solution, and then add MIL-53 (Al). ht The carrier, after pH adjustment, was subjected to hydrothermal crystallization, washing, drying, and calcination to obtain MIL-53(Al). ht @ZSM-5 hollow microsphere carrier; (4) MIL-53(Al) ht The ZSM-5 hollow microsphere carrier was first impregnated in a chloride solution containing Mt1 (Mt1Cl), dried, and then impregnated in a chloride solution containing Mt2 (Mt2Cl). n-1 In a solution, after crystallization and drying, it is then processed in MIL-53(Al) ht@ZSM-5 hollow microsphere carrier for forming complex salts Mt1Mt2Cl n Mt1Mt2Cl n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst.
[0030] In step (1) of the preferred embodiment of the present invention, the aluminum source is aluminum nitrate nonahydrate, and the mass ratio of aluminum nitrate nonahydrate to terephthalic acid is 3.75:1.66; the hydrothermal reaction temperature is 220℃, the reaction time is 72h, and the hydrothermal reaction is carried out in a reactor lined with tetrafluoroethylene; the washing is done by alternating washing with DMF (dimethylformamide) and deionized water, and the number of washings is 3; the drying is done at 80-100℃ for 10-12h.
[0031] In step (2) of the preferred embodiment of the present invention, the calcination temperature is 330°C and the calcination time is 24h.
[0032] In step (3) of the preferred embodiment of the present invention, the silicon source is tetraethyl orthosilicate (TEOS); the pH is adjusted to 10.
[0033] In step (3) of the preferred embodiment of the present invention, the hydrothermal crystallization temperature is 180°C and the reaction time is 48h; the calcination is carried out at 380°C for 6h.
[0034] In step (4) of the preferred embodiment of the present invention, the molar concentrations of the chloride solution containing Mt1 and the chloride solution containing Mt2 are both 0.0415~0.1668 mol / L; the immersion time in the chloride solution containing Mt1 is 1 h, and the immersion time in the chloride solution containing Mt2 is 0.5-3.5 h; the molar ratio of Mt1 to Mt2 in the chloride solution containing Mt1 and the chloride solution containing Mt2 is (1-2):(1-3), for example 2:1, 1:1, 1:2 and 1:3; the double salt Mt1Mt2Cl n In MIL-53(A1) ht The loading amount on the ZSM-5 hollow microsphere carrier is 10-14 wt%.
[0035] In step (4) of the preferred embodiment of the present invention, the crystallization reaction temperature is 190°C and the reaction time is 17h.
[0036] Mt1Mt2Cl prepared in the embodiments of the present invention n / MIL-53(Al) ht The ZSM-5 hollow microsphere core-shell catalyst can be used in the catalytic disproportionation of monomethyltrichlorosilane and trimethylchlorosilane to prepare dimethyldichlorosilane; or in the disproportionation reactions of organosilicon high-boiling and low-boiling organosilicon compounds.
[0037] In the application example of this invention, the high-boiling organosilicon compounds used are by-product mixtures with boiling points higher than dimethyldichlorosilane (>70.5°C) at ambient pressure during the direct method (Rojo method) for the preparation of dimethyldichlorosilane, and the low-boiling compounds are all components with boiling points lower than dimethyldichlorosilane at ambient pressure.
[0038] The catalytic disproportionation reaction of methyltrichlorosilane and trimethylchlorosilane (high-boiling and low-boiling components) to prepare dimethyldichlorosilane in this invention is as follows: methyltrichlorosilane and trimethylchlorosilane (high-boiling and low-boiling components) are mixed in a certain proportion and injected into a gas chromatograph using a micro-syringe. After vaporization in the vaporization chamber, the mixture enters the reaction tube of a single-stage high-temperature furnace along with the carrier gas; a certain amount of Mt1Mt2Cl... n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst was added to a single-stage high-temperature furnace reaction tube. The reaction temperature of the high-temperature furnace was adjusted, and the reaction yield of dimethyldichlorosilane was measured. At high temperature, the mixture and catalyst were in full contact, and a disproportionation reaction occurred to generate dimethyldichlorosilane and other byproducts. Subsequently, all products were carried by a carrier gas into a chromatographic column for detection and analysis. The type of substance can be determined based on the retention time of the chromatographic peak, and the relative content of the substance can be determined based on the size of the chromatographic peak. Therefore, Mt1Mt2Cl can be obtained based on the yield of dimethyldichlorosilane. n / MIL-53(Al) ht The catalytic effect of the ZSM-5 core-shell catalyst on the disproportionation of monomethyltrichlorosilane and trimethylchlorosilane (high-boiling and low-boiling components) to prepare dimethyldichlorosilane.
[0039] The reaction reagent ratios are based on volume, with methyltrichlorosilane:trimethylchlorosilane (high-boiling substance: low-boiling substance) ratios of 2:1, 1:1, 1:2, and 1:3.
[0040] In this embodiment of the invention, room temperature / room temperature refers to "25±3℃".
[0041] The technical solution of the present invention will be further illustrated by the following embodiments.
[0042] Example 1 (1) Weigh 3.75g of aluminum nitrate nonahydrate and 1.66g of terephthalic acid, dissolve them in 65mL of DMF, stir on a magnetic stirrer at room temperature for 0.5h, and after stirring evenly, pour the mixture into a 100mL polytetrafluoroethylene-lined reactor and react at 220℃ for 72h. Then, let the reactor cool naturally to room temperature. After centrifuging the obtained mixture, wash it three times with DMF and distilled water respectively, and then put it in an oven and dry it at 80℃ for 12h to obtain the MIL-53(Al) carrier.
[0043] (2) The obtained MIL-53(Al) support was placed in a muffle furnace and calcined at 330°C for 24 hours to obtain MIL-53(Al). ht Carrier.
[0044] (3) Weigh 5.49 g of template agent TPAOH into a beaker, add 25.92 mL of deionized water and mix thoroughly, then add 15.62 g of TEOS liquid, sonicate for 0.5 h, and after mixing evenly, add 0.04 g of NaAlO2, stir at room temperature for 4 h, and after stirring evenly, add 2 g of MIL-53(Al) prepared in step (2). ht The carrier was added, and NaOH solid was added to adjust the pH of the mixture to 10. The mixture was then transferred to a 100 mL polytetrafluoroethylene-lined reactor and reacted at 180 °C for 48 h. After the reaction, the resulting product was washed three times by filtration with ethanol and deionized water, and then dried in an oven at 100 °C for 10 h. After complete drying, it was calcined in a muffle furnace at 380 °C for 6 h to obtain MIL-53(Al). ht @ZSM-5 core-shell vector.
[0045] (4) According to the molar ratio of Na to Al (i.e., Mt1 is Na) + Mt2 is Al 3+ Weigh out 0.072 g of NaCl and 0.328 g of AlCl3 respectively in a 1:2 ratio, and dissolve them in 20 mL of deionized water to obtain NaCl solution and AlCl3 solution respectively; add 4 g of the prepared MIL-53(Al) ht @ZSM-5 hollow microsphere carriers were impregnated in NaCl solution for 1 hour; after impregnation, they were placed in a drying oven at 100℃ for 2 hours, and then NaCl / MIL-53(Al) was obtained. ht @ZSM-5 catalyst, followed by NaCl / MIL-53(Al) ht The ZSM-5 catalyst was impregnated in a prepared AlCl3 solution for 2.5 h, and then poured into a crystallization vessel. It was crystallized at 190 °C for 17 h, and then dried at 80 °C. After drying, NaAlCl4 / MIL-53(Al) with a double salt loading of 10 wt% was obtained. ht @ZSM-5 hollow microsphere core-shell catalyst, denoted as 10% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst.
[0046] Application Example 1 4 μL of a reaction solution was prepared by mixing methyltrichlorosilane (M1) and trimethylchlorosilane (M3) at a volume ratio of 1:2. The prepared reaction solution was injected into the injection chamber (vaporization chamber) of a gas chromatograph, where it was instantly vaporized into a gaseous reactant at high temperature. The gaseous reactant, propelled by a carrier gas, entered the reaction tube of a single-stage high-temperature furnace and reacted with 0.7 g of NaAlCl4 / MIL-53(Al) prepared in Example 1, which was pre-filled in the reaction tube. ht The catalyst, ZSM-5, is fully contacted, and a disproportionation reaction occurs at a constant temperature of 220°C, producing dimethyldichlorosilane (M2) and other byproducts. The product mixture is then carried by a carrier gas into a gas chromatographic column for separation, followed by detection. The product types are qualitatively identified based on the retention time of the chromatographic peaks, and the content of each component is quantitatively determined based on the peak area, thereby calculating the yield of dimethyldichlorosilane at that temperature.
[0047] The results showed that the yield of dimethyldichlorosilane prepared by disproportionation using the core-shell catalyst of Example 1 was 86.14%.
[0048] Example 2 Same as Example 1, except that in step (4), NaCl and AlCl3 with a molar ratio of Na to Al of 1:1 are weighed in weights of 0.171 g and 0.389 g respectively, so that the double salt loading is 14 wt%, to obtain NaAlCl4 / MIL-53(Al). ht @ZSM-5 hollow microsphere core-shell catalyst.
[0049] Application Example 2 4 μL of a reaction solution was prepared by mixing methyltrichlorosilane (M1) and trimethylchlorosilane (M3) at a volume ratio of 1:2. The prepared reaction solution was injected into the injection chamber (vaporization chamber) of a gas chromatograph, where it was instantly vaporized into a gaseous reactant at high temperature. The gaseous reactant, propelled by a carrier gas, entered the reaction tube of a single-stage high-temperature furnace and reacted with 0.7 g of NaAlCl4 / MIL-53(Al) prepared in Example 2, which was pre-filled in the reaction tube. ht The catalyst, ZSM-5, is fully contacted, and a disproportionation reaction occurs at a constant temperature of 220°C, producing dimethyldichlorosilane (M2) and other byproducts. The product mixture is then carried by a carrier gas into a gas chromatographic column for separation, followed by detection. The product types are qualitatively identified based on the retention time of the chromatographic peaks, and the content of each component is quantitatively determined based on the peak area, thereby calculating the yield of dimethyldichlorosilane at that temperature.
[0050] The results showed that the yield of dimethyldichlorosilane prepared by disproportionation using the core-shell catalyst of Example 2 was 79.64%.
[0051] Example 3 Same as Example 1, except that in step (4), NaCl and AlCl3 with a molar ratio of Na to Al of 1:1 are weighed in a ratio of 0.122 g and 0.278 g respectively, so that the double salt loading is 10 wt%, to obtain NaAlCl4 / MIL-53(Al). ht @ZSM-5 hollow microsphere core-shell catalyst.
[0052] Application Example 3 4 μL of a reaction solution was prepared by mixing methyltrichlorosilane (M1) and trimethylchlorosilane (M3) at a volume ratio of 1:2. The prepared reaction solution was injected into the injection chamber (vaporization chamber) of a gas chromatograph, where it was instantly vaporized into a gaseous reactant at high temperature. The gaseous reactant, propelled by a carrier gas, entered the reaction tube of a single-stage high-temperature furnace and reacted with 0.7 g of NaAlCl4 / MIL-53(Al) prepared in Example 3, which was pre-filled in the reaction tube. ht The catalyst, ZSM-5, is fully contacted, and a disproportionation reaction occurs at a constant temperature of 220°C, producing dimethyldichlorosilane (M2) and other byproducts. The product mixture is then carried by a carrier gas into a gas chromatographic column for separation, followed by detection. The product types are qualitatively identified based on the retention time of the chromatographic peaks, and the content of each component is quantitatively determined based on the peak area, thereby calculating the yield of dimethyldichlorosilane at that temperature.
[0053] The results showed that the yield of dimethyldichlorosilane prepared by disproportionation using the core-shell catalyst of Example 3 was 76.98%.
[0054] Example 4 Same as Example 1, except that in step (4), the molar ratio of Na to Al is 1:2; 0.101g of NaCl and 0.459g of AlCl are weighed respectively, and the molar ratio of Na / Al is 1:2, finally obtaining NaAlCl4 / MIL-53(Al) with a complex salt loading ratio of 14wt%. ht @ZSM-5 hollow microsphere core-shell catalyst, designated as 14% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst.
[0055] Application Example 4 4 μL of a reaction solution was prepared by mixing methyltrichlorosilane (M1) and trimethylchlorosilane (M3) at a volume ratio of 1:2. The prepared reaction solution was injected into the injection chamber (vaporization chamber) of a gas chromatograph, where it was instantly vaporized into a gaseous reactant at high temperature. The gaseous reactant, propelled by a carrier gas, entered the reaction tube of a single-stage high-temperature furnace and reacted with 0.7 g of NaAlCl4 / MIL-53(Al) prepared in Example 4, which was pre-filled in the reaction tube. htThe catalyst, ZSM-5, is fully contacted, and a disproportionation reaction occurs at a constant temperature of 220°C, producing dimethyldichlorosilane (M2) and other byproducts. The product mixture is then carried by a carrier gas into a gas chromatographic column for separation, followed by detection. The product types are qualitatively identified based on the retention time of the chromatographic peaks, and the content of each component is quantitatively determined based on the peak area, thereby calculating the yield of dimethyldichlorosilane at that temperature.
[0056] The results showed that the yield of dimethyldichlorosilane prepared by disproportionation using the core-shell catalyst of Example 4 was 81.29%.
[0057] Example 5 Same as Example 1, except that in step (4), according to the molar ratio of Li to La (i.e., Mt1 is Li), + Mt2 is La 3+ LiCl and LaCl3 were weighed in a 1:2 ratio, with masses of 0.032 g and 0.368 g respectively. Each was dissolved in 20 mL of deionized water to obtain LiCl solution and LaCl3 solution, respectively. The remaining steps were the same as in Example 1. The resulting catalyst was LiLaCl4 / MIL-53(Al). ht @ZSM-5 hollow microsphere core-shell catalyst.
[0058] Application Example 5 4 μL of a reaction solution was prepared by mixing methyltrichlorosilane (M1) and trimethylchlorosilane (M3) at a volume ratio of 1:2. The prepared reaction solution was injected into the injection chamber (vaporization chamber) of a gas chromatograph, where it was instantly vaporized into a gaseous reactant at high temperature. The gaseous reactant, propelled by a carrier gas, entered the reaction tube of a single-stage high-temperature furnace and reacted with 0.7 g of LiLaCl4 / MIL-53(Al) prepared in Example 5, which was pre-filled in the reaction tube. ht The catalyst, ZSM-5, is fully contacted, and a disproportionation reaction occurs at a constant temperature of 220°C, producing dimethyldichlorosilane (M2) and other byproducts. The product mixture is then carried by a carrier gas into a gas chromatographic column for separation, followed by detection. The product types are qualitatively identified based on the retention time of the chromatographic peaks, and the content of each component is quantitatively determined based on the peak area, thereby calculating the yield of dimethyldichlorosilane at that temperature.
[0059] The results showed that the yield of the core-shell catalyst of Example 5 for disproportionation preparation of dimethyldichlorosilane was 81.74%.
[0060] Application Example 6 0.7g of the 10% NaAlCl4 / MIL-53(Al) prepared in Example 1 was used. htThe ZSM-5 hollow microsphere core-shell catalyst was loaded into a fixed-bed reactor. The reaction tube was placed in a single-stage high-temperature furnace. 10 mL of high-boiling-point material and 10 mL of low-boiling-point material were weighed as raw materials to prepare a mixed feed solution. The mixed feed solution was injected into the reactor. Under the conditions of 200℃ and normal pressure, the gaseous raw material and the catalyst were in full contact to undergo a disproportionation and cracking reaction. After the reaction temperature stabilized, the reaction was continuously fed for 0.5 h. After the catalyst activity and product distribution reached a steady state, product collection and gas chromatography analysis were started.
[0061] The results showed that the conversion rate of high-boiling-point substances reached 90.68%, the conversion rate of low-boiling-point substances reached 90.14%, and the selectivity of the target product (dimethyldichlorosilane) reached 38.04%, demonstrating good catalytic activity and promising prospects for industrial application.
[0062] Comparative Example 1 Same as Example 1, except that in step (4), the mass of NaCl is 0.043g and the mass of AlCl3 is 0.197g, so that the double salt loading is 6wt%, resulting in 6% NaAlCl4 / MIL-53(Al). ht @ZSM-5 hollow microsphere core-shell catalyst.
[0063] Comparative Application Example 1 The test was conducted according to the method in Application Example 1. The results showed that the yield of the core-shell catalyst of Comparative Example 1 for the disproportionation preparation of dimethyldichlorosilane was 71.29%, which is attributed to the presence of MIL-53(Al) in the catalyst of the comparative example. ht The surface of the @ZSM-5 core-shell carrier has very little NaAlCl4, the main active component. Due to the insufficient density of the shell, the acid strength and density are not strong, which affects the yield of dimethyldichlorosilane.
[0064] Comparative Example 2 Same as Example 1, except that in step (4), the mass of NaCl is 0.129g and the mass of AlCl3 is 0.591g, so that the double salt loading is 18wt%, resulting in 18% NaAlCl4 / MIL-53(Al). ht @ZSM-5 hollow microsphere core-shell catalyst.
[0065] Comparative Application Example 2 The 18% NaAlCl4 / MIL-53(Al) in Comparative Example 2 was processed according to the method described in Application Example 1. ht The ZSM-5 hollow microsphere core-shell catalyst was tested, and the results showed that the yield of dimethyldichlorosilane prepared by disproportionation using the core-shell catalyst of Comparative Example 2 was 73.28%. This was attributed to the higher loading ratio and the higher molar concentration of the AlCl3 solution compared to the loaded solution in the comparative example, resulting in excessive AlCl3 in the loaded solution.3+ Hydrothermal action accelerates the growth of NaAlCl4 crystals, leading to the formation of MIL-53(Al). ht The excessively dense shell layer on the surface of the ZSM-5 core-shell support may affect the total acidity of the catalyst and the adhesion points of acidic factors, thereby reducing the catalytic effect.
[0066] Comparative Application Example 3 Same as Application Example 1, except that the NaAlCl4 / MIL-53(Al) prepared in Example 1... ht The amount of @ZSM-5 catalyst used was 0.3g. The results showed that the yield of dimethyldichlorosilane prepared by disproportionation was 79.97%. The reason for this was that the amount of catalyst used was small. In the catalytic system, the number of catalytic active centers determines the contact area between the reaction liquid and the catalyst. Too little contact area between the reaction liquid and the catalyst leads to a decrease in the yield of dimethyldichlorosilane.
[0067] Comparative Application Example 4 Same as Application Example 1, except that the NaAlCl4 / MIL-53(Al) prepared in Example 1... ht The amount of @ZSM-5 catalyst used was 0.9g. The results showed that the yield of dimethyldichlorosilane prepared by disproportionation was 83.11%. The reason is that the excess of catalyst caused the already generated dimethyldichlorosilane to undergo the reverse reaction of disproportionation, which shifted the reaction equilibrium towards the formation of monomethyltrichlorosilane (M1) and trimethylmonochlorosilane (M3), thus affecting the yield of dimethyldichlorosilane in the product.
[0068] Comparative Application Example 5 Similar to Application Example 1, the only difference is that methyltrichlorosilane (M1) and trimethylchlorosilane (M3) were mixed at a volume ratio of 2:1 to obtain a reaction solution. The results showed that the yield of dimethyldichlorosilane (M2) prepared by disproportionation was 82.11%. This was because the increase in the volume ratio of M1 / M3 reduced the proportion of M3, decreased the concentration of M3, and caused the reaction to proceed in reverse, thus reducing the yield of M2.
[0069] Comparative Application Example 6 Similar to Application Example 1, the only difference is that methyltrichlorosilane (M1) and trimethylchlorosilane (M3) were mixed at a volume ratio of 1:3 to obtain a reaction solution. The results showed that the yield of dimethyldichlorosilane (M2) prepared by disproportionation was 82.67%. This is because the more M3 used, the more side reactions occur, and a large amount of byproducts adhere to the surface of the catalyst, affecting the catalyst's efficiency and leading to a decrease in the reaction rate, thus reducing the yield of M2.
[0070] Performance testing Figure 1The NaAlCl4 / MIL-53(Al) prepared in Example 1. ht TEM characterization images of the ZSM-5 hollow microsphere core-shell catalyst at different magnifications. From figures (a) and (b), we can see that MIL-53(Al) ht The particles tend to concentrate, with ZSM-5 crystals coated on the surface. The increased particle size after epitaxial growth of ZSM-5 zeolite particles on the shell indicates the formation of a core-shell support structure and a relatively dispersed distribution of NaAlCl4 on the support surface. The core-shell catalyst possesses a disordered pore distribution structure, indicating that the small ZSM-5 molecules formed during hydrothermal synthesis gradually accumulate in MIL-53(Al). ht In-situ growth can be performed on the surface of the catalyst, or deposition can be carried out within the porous structure, thereby altering the original pore distribution of the entire catalyst support. The hollow microsphere structure facilitates the diffusion and mass transfer of reactant molecules, shortens the diffusion path, and improves the accessibility of active sites.
[0071] Figure 2 The 10% NaAlCl4 / MIL-53(Al) prepared in Example 1 is shown. ht @ZSM-5 hollow microsphere core-shell catalyst, MIL-53(Al) support, and MIL-53(Al) ht FT-IR characterization analysis of the @ZSM-5 core-shell vector. As shown in the figure, at 3625 cm⁻¹... -1 The absorption peak at 1621 cm⁻¹ is due to the stretching vibration of the -OH group bridging the Al metal center; -1 1542 cm -1 The characteristic peak at 1441 cm⁻¹ is due to the asymmetric stretching vibration of OCO. -1 1432 cm -1 The characteristic peaks at the [location] originate from the symmetric stretching vibration of OCO. These are characteristic absorption peaks of carboxyl functional groups, indicating the presence of aluminum metal centers and carboxyl functional groups in the sample, thus demonstrating the successful preparation of MIL-53(Al). ht At 1098 cm -1 The absorption peak at 814 cm⁻¹ is caused by the asymmetric stretching mode of the TOT (T is Si or Al) bond. -1 1231 cm -1 The absorption peak at 451 cm⁻¹ is due to the antisymmetric stretching of the TO bond and the external asymmetric stretching vibration. -1 550 cm -1 The absorption peaks at the specified locations are caused by the angular vibrations of the TO bonds, and both belong to the vibrational spectra of the inner tetrahedron. These peaks are attributed to the five-membered ring basic structural unit unique to the ZSM-5 zeolite molecular sieve in the sample, indicating that MIL-53(Al) was successfully synthesized via hydrothermal synthesis and in-situ growth methods. ht@ZSM-5 core-shell vector.
[0072] The crystal phase and crystallinity of the powder in the calcined samples were characterized by powder X-ray diffraction (XRD). The rotation angle 2θ ranged from 5° to 80°, and the rotation rate was 5° / min. Figure 3 MIL-53(A1) in Example 1 ht Carrier, MIL-53(A1) ht @ZSM-5 core-shell vector, 10% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst, 14% NaAlCl4 / MIL-53(Al) from Example 2 ht @ZSM-5 hollow microsphere core-shell catalyst, Comparative Example 1: 6% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst and Comparative Example 2: 18% NaAlCl4 / MIL-53(Al) ht XRD characterization of the ZSM-5 hollow microsphere core-shell catalyst. It can be seen that the peaks at diffraction angles of 27.3° and 20.6° in Comparative Examples 1 and 2, and Examples 1 and 2, are typical MFI topologies, corresponding to the ZSM-5 zeolite molecular sieve, indicating the successful synthesis of MIL-53(Al). ht @ZSM-5 support; compared to loading with double salt NaAlCl4, 2 θ New diffraction peaks appeared at 31.7° and 45.15°, which matched well with the main diffraction peaks of ordinary JCPDS card number 20-0847, corresponding to the main diffraction peaks of the NaAlCl4 phase. The core-shell catalyst modified with double salt belongs to MIL-53(Al). ht The phase peaks are present, but the peak heights are reduced, indicating that NaAlCl4 is dispersed in MIL-53(Al). ht On the ZSM-5 carrier, it will not affect MIL-53(Al). ht The original structure of the @ZSM-5 supported composite catalyst was well preserved, indicating the successful synthesis of NaAlCl4 / MIL-53(Al). ht @ZSM-5 core-shell double salt catalyst.
[0073] Figure 4 In Figure (a), MIL-53(Al) is shown in Example 1. ht Carrier, MIL-53(A1) ht @ZSM-5 core-shell vector, 10% NaAlCl4 / MIL-53(Al) ht@ZSM-5 hollow microsphere core-shell catalyst, 14% NaAlCl4 / MIL-53(Al) from Example 2 ht @ZSM-5 hollow microsphere core-shell catalyst, Comparative Example 1: 6% NaAlCl4 / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst and Comparative Example 2: 18% NaAlCl4 / MIL-53(Al) ht Thermogravimetric curve of the ZSM-5 hollow microsphere core-shell catalyst, (b) is for 10% NaAlCl4 / MIL-53(Al). ht The thermogravimetric curves of @ZSM-5 are shown in Figure (a). As can be seen, when the loading ratio exceeds 10%, the weight loss increases with increasing temperature between 120-330 °C. This is consistent with the results of catalyst activity experiments. With increasing loading ratio and rising temperature, the active component NaAlCl4 is more easily decomposed and lost, leading to a decrease in catalyst activity and thus a reduction in the yield of dimethyldichlorosilane. The figure also shows that the MIL-53(Al) modified by ZSM-5... ht The thermal stability of the carrier is enhanced compared to MIL-53(Al). ht The core-shell catalyst with loaded double salt shows that after being coated with ZSM-5 shell, the skeleton collapse temperature of the support increases from about 500℃ to over 550℃, indicating that the core-shell structure significantly enhances the thermal stability of the material. The analysis results in Figure (b) show that the sample mainly experienced three weight loss stages. The first stage occurred around 100 °C, with a weight loss of approximately 1.09%, primarily due to the removal of residual moisture from the pores or outer surface of the sample. The second stage occurred between 100-350 °C, with a weight loss of approximately 6.16%, mainly due to the decomposition of the complex salt active component NaAlCl4 and the removal of residual guest molecule DMF. This aligns with the catalytic activity experiment, where the yield of dimethyldichlorosilane decreased with increasing temperature at 220-330 °C. The third stage occurred between 350-550 °C, with a weight loss of approximately 13.96%, primarily due to the removal of the organic template agent TPAOH. Furthermore, above 500 °C, the yield of MIL-53(Al) decreased. ht The skeleton will gradually collapse.
[0074] The above results indicate that the core-shell catalyst prepared in this embodiment can be used for the disproportionation preparation of dimethyldichlorosilane. The general formula of this invention is Mt1Mt2Cl. n Different types of double salts in the double salt system are all applicable to this hollow core-shell catalyst system, verifying the universality of the general double salt formula. In this invention, Mt1Mt2Cl... n The double salt partially dissociates into Mt2Cl at the reaction temperature. n-1It acts as a Lewis acidic site to activate Si-Cl bonds; simultaneously, MIL-53(Al) ht The organic ligands exhibit an affinity effect with the methylchlorosilane substrate, and the two work together to lower the activation energy of the reaction and promote the redistribution of methyl and chlorine.
[0075] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A type of Mt1Mt2Cl n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst, characterized in that... With MIL-53(A1) ht Hollow microspheres form the core, and ZSM-5 molecular sieve forms the outer shell, constituting a core-shell carrier. The complex salt Mt1Mt2Cl is loaded onto this core-shell carrier. n As an active component; wherein, the complex salt Mt1Mt2Cl n In this context, Mt1 is selected from Li + Na + K + 、Rb + and Cs + Any one of them; Mt2 is selected from Al 3+ Fe 3+ and La 3+ Any one of the following, n=4; or Mt2 is selected from Cu. 2+ Fe 2+ Any one of them, n=3.
2. A Mt1Mt2Cl as described in claim 1 n / MIL-53(Al) ht The preparation method of @ZSM-5 hollow microsphere core-shell catalyst is characterized by, Includes the following steps: (1) Aluminum source and terephthalic acid are mixed in an organic solvent, and after hydrothermal reaction, washing and drying, MIL-53(Al) is obtained; (2) The MIL-53(Al) is calcined to obtain MIL-53(Al). ht carrier; (3) Mix tetrapropylammonium hydroxide with water, add a silicon source, sonicate, then add sodium aluminate, stir at room temperature to obtain ZSM-5 precursor solution, and then add the MIL-53(Al). ht The carrier, after pH adjustment, was subjected to hydrothermal crystallization, washing, drying, and calcination to obtain MIL-53(Al). ht @ZSM-5 hollow microsphere carrier; (4) The MIL-53(Al) ht The ZSM-5 hollow microsphere carrier is first impregnated in a chloride solution containing Mt1, dried, and then impregnated in a chloride solution containing Mt2. After crystallization and drying, it is then used in the MIL-53(Al) carrier. ht Complex salts Mt1 and Mt2Cl are formed on the ZSM-5 hollow microsphere carrier. n The Mt1Mt2Cl was obtained. n / MIL-53(Al) ht @ZSM-5 hollow microsphere core-shell catalyst.
3. The preparation method according to claim 2, characterized in that, In step (1), the aluminum source is aluminum nitrate nonahydrate, and the mass ratio of aluminum nitrate nonahydrate to terephthalic acid is 3.75:1.66; the hydrothermal reaction temperature is 220℃, and the reaction time is 72h.
4. The preparation method according to claim 2, characterized in that, In step (2), the roasting temperature is 330°C and the roasting time is 24 hours.
5. The preparation method according to claim 2, characterized in that, In step (3), the silicon source is tetraethyl orthosilicate; the pH is adjusted to 10.
6. The preparation method according to claim 2, characterized in that, In step (3), the hydrothermal crystallization temperature is 180℃ and the reaction time is 48h; the calcination is calcined at 380℃ for 6h.
7. The preparation method according to claim 2, characterized in that, In step (4), the molar concentrations of the chloride solution containing Mt1 and the chloride solution containing Mt2 are both 0.0415~0.1668 mol / L; the immersion time in the chloride solution containing Mt1 is 1 h, and the immersion time in the chloride solution containing Mt2 is 0.5-3.5 h; the molar ratio of Mt1 to Mt2 in the chloride solution containing Mt1 and the chloride solution containing Mt2 is (1-2):(1-3); the double salt Mt1Mt2Cl n In the MIL-53(Al) ht The loading amount on the ZSM-5 hollow microsphere carrier is 10-14 wt%.
8. The preparation method according to claim 2, characterized in that, In step (4), the crystallization reaction temperature is 190°C and the reaction time is 17h.
9. A Mt1Mt2Cl as described in claim 1 n / MIL-53(Al) ht Application of @ZSM-5 hollow microsphere core-shell catalyst in the catalytic disproportionation of methyltrichlorosilane and trimethylchlorosilane to prepare dimethyldichlorosilane.
10. A Mt1Mt2Cl as described in claim 1 n / MIL-53(Al) ht Application of ZSM-5 hollow microsphere core-shell catalyst in the disproportionation reaction of organosilicon high-boiling and low-boiling substances.
Citation Information
Patent Citations
Hollow microsphere core-shell catalyst as well as preparation method and application thereof