Liquid phase synthesis of high purity lithium sulfide

By using a mixed solvent system of carbon disulfide and alcohol, lithium trisulfide intermediates are generated, solving the problems of purity and solvent usage in lithium sulfide preparation, achieving the preparation of high-purity lithium sulfide, and reducing safety risks and environmental pollution.

CN123082218APending Publication Date: 2026-11-13HUBEI THREE GORGES LAB +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611046125.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-07-09
Filing Date
2026-07-14
Publication Date
2026-11-13

AI Technical Summary

Technical Problem

Existing methods for preparing lithium sulfide suffer from problems such as low product purity, large solvent consumption, high safety risks, and serious environmental pollution.

Method used

A mixed solvent system of carbon disulfide and alcohol is used to generate lithium trisulfide carbonate intermediate through reflux reaction, which is then dissolved in ethanol, concentrated under reduced pressure and sintered. This avoids the use of hydrogen sulfide gas, reduces solvent usage and improves purity.

Benefits of technology

The preparation of high-purity (≥99.9%) lithium sulfide was achieved, reducing solvent usage, avoiding the use of highly toxic gases, reducing safety risks and environmental pollution, and improving yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123082218A_ABST
    Figure CN123082218A_ABST
Patent Text Reader

Abstract

This invention discloses a liquid-phase synthesis method for high-purity lithium sulfide, belonging to the field of battery material synthesis technology, to solve the problems of limited purity, high cost, and high safety risks in existing lithium sulfide products. The method involves dissolving barium sulfide in a mixed solvent of carbon disulfide and ethanol; adding lithium sulfate to the mixed solvent; refluxing the reaction under a protective atmosphere; filtering after the reaction and washing the filter cake with ethanol to obtain a lithium trithiocarbonate solution; concentrating the lithium trithiocarbonate solution under reduced pressure to obtain crude lithium trithiocarbonate; and sintering the crude lithium trithiocarbonate to obtain high-purity lithium sulfide. This invention achieves the preparation of high-purity lithium sulfide under mild conditions through a liquid-phase synthesis method using a mixed solvent system of carbon disulfide and ethanol and a lithium trithiocarbonate intermediate route. The resulting lithium sulfide product has a purity of over 99.9%, and the operation is highly safe and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery material synthesis technology, and in particular relates to a method for synthesizing high-purity lithium sulfide. Background Technology

[0002] Lithium sulfide is an important inorganic compound widely used in solid-state battery electrolytes and cathode materials. Traditional liquid-phase preparation methods for lithium sulfide mainly include the hydrogen sulfide gas neutralization method and the metathesis method. The purity of the product is limited, making it difficult to meet the purity requirements of high-end applications. Although the hydrogen sulfide gas method can be carried out at relatively low temperatures, hydrogen sulfide gas is highly toxic and corrosive, posing significant safety risks and environmental pollution problems during the production process. While the traditional metathesis method avoids the use of hydrogen sulfide, the use of sodium sulfide as a sulfur source makes it difficult to completely separate the trace sodium ions introduced into the product, and lithium sulfide has very low solubility in organic solvents such as ethanol, requiring a large amount of solvent. This invention introduces carbon disulfide to convert sulfide anions in the system into thiocarbonate ions, thereby promoting the reaction equilibrium to shift towards the product. Simultaneously, lithium trithiocarbonate has better solubility in ethanol. These characteristics significantly reduce the amount of reaction solvent used, and more importantly, high-purity lithium sulfide (purity ≥99.9%) can be prepared without additional purification operations. Summary of the Invention

[0003] The purpose of this invention is to provide a liquid-phase synthesis method for high-purity lithium sulfide, in order to solve the problems of low product purity and large solvent consumption in the metathesis method in the prior art, as well as the problems of high safety risks and serious environmental pollution caused by the absence of highly toxic gases such as hydrogen sulfide in the process.

[0004] To achieve the above objectives, the present invention adopts the following technical solution: A liquid-phase synthesis method for high-purity lithium sulfide includes the following steps: (1) Dissolve barium sulfide in a mixed solvent of carbon disulfide and alcohol, wherein the volume ratio of carbon disulfide to alcohol is 1:4 to 1:10; (2) Add a lithium source to the mixed solvent; (3) Reflux reaction under argon protective atmosphere; (4) After the reaction is complete, filter the solution and wash the filter cake with ethanol to obtain a lithium trithiocarbonate solution; (5) The lithium trithiocarbonate solution is concentrated under reduced pressure and then cooled to crystallize to obtain lithium trithiocarbonate crystals; (6) Sinter the lithium trithiocarbonate crystals to obtain high-purity lithium sulfide.

[0005] Preferably, the cation of the sulfur source selected in step (1) needs to be a sulfide carbonate salt that is insoluble in alcohol, such as barium sulfide or calcium sulfide, and the amount used is 1.05 to 1.1 times the lithium salt equivalent.

[0006] Preferably, the volume ratio of carbon disulfide to alcohol in step (1) is 1:4 to 1:10.

[0007] Preferably, the alcohol includes any one or a combination of ethanol, isopropanol, butanol, and pentanol.

[0008] The water content in the carbon disulfide and alcohol is less than 0.005%.

[0009] Preferably, the lithium source in step (2) is lithium sulfate or lithium carbonate.

[0010] Preferably, the argon gas in step (3) has a purity of ≥99.999%, a reflux reaction temperature of 80 °C, and a reaction time of 6-10 h.

[0011] Preferably, the washing operation in step (4) is also performed three times with anhydrous ethanol in a high-purity argon atmosphere. The water content of the anhydrous ethanol is less than 0.005%. The purity of the argon gas is ≥99.999%. Preferably, the vacuum degree of the reduced pressure concentration in step (5) is 0.001~0.01 MPa.

[0012] Preferably, the temperature for vacuum concentration in step (5) is 18~25℃.

[0013] Preferably, the sintering temperature in step (6) is 300-500℃ and the sintering time is 2-6h.

[0014] The beneficial effects of this invention are: (1) By using a mixed solvent system of carbon disulfide and ethanol as the reaction medium, compared with the traditional metathesis reaction method using ethanol as the solvent, the sulfur anion is converted into trithiocarbonate ion during the reaction process, and the reaction is more complete. Therefore, the product purity and yield are higher after sintering. In addition, lithium trithiocarbonate has higher solubility in ethanol than lithium sulfide, so the amount of solvent used is lower.

[0015] (2) Due to the use of liquid phase reaction and intermediate purification process, impurities introduced under high temperature conditions are avoided. Through the preparation and thermal decomposition of lithium trisulfide intermediate, the by-product carbon disulfide gas is discharged with the tail gas and can be recycled. Attached Figure Description

[0016] Figure 1 This is the XRD pattern in Embodiment 2 of this application. Detailed Implementation

[0017] The present invention will be further described in detail below with reference to the embodiments.

[0018] Unless otherwise specified, all raw materials used in the following examples are commercially available. Lithium sulfate, lithium carbonate, barium sulfide, and calcium sulfide were purchased from Beijing Innovent Technology Co., Ltd., with a purity ≥99.0%. Carbon disulfide and anhydrous ethanol were analytical grade and purchased from Beijing Innovent Technology Co., Ltd., with a water content ≤0.005%. High-purity argon gas with a purity ≥99.999% was purchased from Wuhan Newride Specialty Gases Co., Ltd.

[0019] Product purity was determined using an inductively coupled plasma atomic emission spectrometer (ICP-AES, model: Agilent 5110); X-ray diffractometer (XRD, model: Bruker D8 Advance) was used for phase analysis.

[0020] Example 1 51.1 g of barium sulfide was added to a 1000 mL three-necked flask. Under a high-purity argon atmosphere (99.999% purity), 500 mL of a mixed solvent of carbon disulfide and ethanol (volume ratio 1:4) was added. At room temperature (25°C), 33.5 g of lithium sulfate was slowly added and stirred until homogeneous. The mixture was then heated to 80°C. o The reaction was carried out under reflux for 8 hours. After the reaction, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with 50 mL of anhydrous ethanol each time. The filtrates were combined to obtain a lithium trithiocarbonate solution. The lithium trithiocarbonate solution was concentrated under reduced pressure at 20 °C and a vacuum of 0.001 MPa to obtain crude lithium trithiocarbonate. The crude lithium trithiocarbonate was placed in a vacuum tube furnace and sintered at 400 °C for 3 hours under nitrogen protection. After cooling to room temperature, 13.2 g of high-purity lithium sulfide was obtained, with a yield of 94.3%. Product characterization: XRD analysis showed that the product was pure-phase lithium sulfide with no impurity phase detected; ICP-AES analysis showed that the product purity was 99.9%, with sodium content of 1.6 PPM, calcium content of 2.3 PPM, magnesium content of 5.5 PPM, iron content of 0.2 PPM, and total impurity content of less than 0.01%.

[0021] Example 2 The difference between this embodiment and Embodiment 1 is that the volume ratio of carbon disulfide to ethanol is 1:10, while the other conditions are the same as in Embodiment 1.

[0022] 51.2 g of barium sulfide was added to a 1000 mL three-necked flask. Under a high-purity argon atmosphere (99.999% purity), 500 mL of a mixed solvent of carbon disulfide and ethanol (volume ratio 1:10) was added. At room temperature (25°C), 33.3 g of lithium sulfate was slowly added and stirred until homogeneous. The mixture was then heated to 80°C. oThe reaction was carried out under reflux for 8 hours. After the reaction, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with 50 mL of anhydrous ethanol each time. The filtrates were combined to obtain a lithium trithiocarbonate solution. The lithium trithiocarbonate solution was concentrated under reduced pressure at 20 °C and a vacuum of 0.001 MPa to obtain crude lithium trithiocarbonate. The crude lithium trithiocarbonate was placed in a vacuum tube furnace and sintered at 400 °C for 3 hours under nitrogen protection. After cooling to room temperature, 13.4 g of high-purity lithium sulfide was obtained, with a yield of 95.7%. Product characterization: XRD analysis showed that the product was pure-phase lithium sulfide with no impurity phase detected; ICP-AES analysis showed that the product purity was 99.9%, with sodium content of 1.8 PPM, calcium content of 2.7 PPM, magnesium content of 4.3 PPM, iron content of 0.9 PPM, and total impurity content of less than 0.01%.

[0023] Example 3 The difference between this embodiment and Embodiment 1 is that the sintering temperature is 200℃ and the sintering time is 3 hours, while the other conditions are the same as in Embodiment 1.

[0024] 51.2 g of barium sulfide was added to a 1000 mL three-necked flask. Under a high-purity argon atmosphere (99.999% purity), 500 mL of a mixed solvent of carbon disulfide and ethanol (volume ratio 1:10) was added. At room temperature (25°C), 33.1 g of lithium sulfate was slowly added and stirred until homogeneous. The mixture was then heated to 80°C. o The reaction was carried out under reflux for 8 hours. After the reaction, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with 50 mL of anhydrous ethanol each time. The filtrates were combined to obtain a lithium trithiocarbonate solution. The lithium trithiocarbonate solution was concentrated under reduced pressure at 20 °C and a vacuum of 0.001 MPa to obtain crude lithium trithiocarbonate. The crude lithium trithiocarbonate was placed in a vacuum tube furnace, heated to 200 °C under nitrogen protection, and sintered for 3 hours. After cooling to room temperature, 14.0 g of product was obtained. Product characterization: XRD analysis showed that the product was pure-phase lithium sulfide and undecomposed lithium thiocarbonate. Further sintering of the product at 400 °C yielded 13.1 g of high-purity lithium sulfide, with a yield of 92.9%. Product characterization: XRD analysis showed that the product was pure phase lithium sulfide with no impurity phase detected; ICP-AES analysis showed that the product purity was 99.9%, with sodium content of 4.1 PPM, calcium content of 2.3 PPM, magnesium content of 5.5 PPM, iron content of 0.2 PPM, and total impurity content of less than 0.01%.

[0025] Example 4 The difference between this embodiment and Embodiment 1 is that calcium sulfide is used as the sulfur source, while the other conditions are the same as in Embodiment 1.

[0026] 22.2 g of calcium sulfide was added to a 1000 mL three-necked flask. Under a high-purity argon atmosphere (99.999% purity), 500 mL of a mixed solvent of carbon disulfide and ethanol (volume ratio 1:4) was added. At room temperature (25°C), 33.5 g of lithium sulfate was slowly added and stirred until homogeneous. The mixture was then heated to 80°C. o The reaction was carried out under reflux for 8 hours. After the reaction, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with 50 mL of anhydrous ethanol each time. The filtrates were combined to obtain a lithium trithiocarbonate solution. The lithium trithiocarbonate solution was concentrated under reduced pressure at 20 °C and a vacuum of 0.001 MPa to obtain crude lithium trithiocarbonate. The crude lithium trithiocarbonate was placed in a vacuum tube furnace and sintered at 400 °C for 3 hours under nitrogen protection to obtain 13.7 g of high-purity lithium sulfide (97.8%). Product characterization: XRD analysis showed that the product was pure-phase lithium sulfide with no impurity phase detected; ICP-AES analysis showed that the product purity was 99.9%, with sodium content of 2.2 PPM, calcium content of 114.5 PPM, magnesium content of 5.5 PPM, iron content of 0.4 PPM, and total impurity content of less than 0.01%.

[0027] Example 5 The difference between this embodiment and Embodiment 1 is that lithium carbonate is used as the lithium source, while the other conditions are the same as in Embodiment 1.

[0028] 51.2 g of barium sulfide was added to a 1000 mL three-necked flask. Under a high-purity argon atmosphere (99.999% purity), 500 mL of a mixed solvent of carbon disulfide and ethanol (volume ratio 1:4) was added. At room temperature (25°C), 21.9 g of lithium carbonate was slowly added and stirred until homogeneous. The mixture was then heated to 80°C. o The reaction was carried out under reflux for 8 hours. After the reaction, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with 50 mL of anhydrous ethanol each time. The filtrates were combined to obtain a lithium trithiocarbonate solution. The lithium trithiocarbonate solution was concentrated under reduced pressure at 20 °C and a vacuum of 0.001 MPa to obtain crude lithium trithiocarbonate. The crude lithium trithiocarbonate was placed in a vacuum tube furnace and sintered at 400 °C for 3 hours under nitrogen protection to obtain 13.3 g of high-purity lithium sulfide, with a yield of 95.0%. Product characterization: XRD analysis showed that the product was pure-phase lithium sulfide with no impurity phase detected; ICP-AES analysis showed that the product purity was 99.9%, with sodium content of 1.7 PPM, calcium content of 9.8 PPM, magnesium content of 12.6 PPM, iron content of 0.3 PPM, and total impurity content of less than 0.1%.

[0029] Comparative Example 1 Add 51.1 g of barium sulfide to a 1000 mL three-necked flask, and add 500 mL of ethanol under a high-purity argon atmosphere (99.999% purity). At room temperature (25°C), slowly add 33.5 g of lithium sulfate, stirring until homogeneous. Then, heat to 80°C. o The reaction was carried out under reflux for 8 hours. After the reaction, the mixture was cooled to room temperature, filtered, and the filter cake was washed three times with 50 mL of anhydrous ethanol each time. The filtrates were combined to obtain a lithium sulfide solution. The lithium trithiocarbonate solution was concentrated under reduced pressure at 20 °C and a vacuum of 0.001 MPa to obtain 5.5 g of lithium sulfide product, with a yield of 39%. Product characterization: XRD analysis showed that the product was pure phase lithium sulfide with no impurity phase detected; ICP-AES analysis showed that the product purity was ≥98.7%, containing approximately 1.1% lithium sulfate, 1.6 PPM of sodium, 2.3 PPM of calcium, 5.5 PPM of magnesium, and 0.2 PPM of barium, with a total impurity content of less than 1.3%.

[0030] Comparative Example 2 Mix 0.05 mol sodium and 5 ml ethanol together, add the mixture to 50 ml toluene, and stir the mixture for 1 h to allow it to react fully. Add 0.05 mol LiCl to the mixture in (1) and stir thoroughly for 6 h. Centrifuge at 10000 r / min for 5 min, collect the solution, and the precipitate is NaCl. Pass a 10% hydrogen sulfide / argon mixture into the solution, control the gas flow rate at 100 sccm, and control the gas flow time at 30 min to allow it to react fully. Centrifuge at 10000 r / min for 5 min and collect the precipitate. Calcine the collected precipitate at 500 ℃ for 4 h in an argon atmosphere to obtain the product Li2S. Product characterization: ICP-AES analysis showed that the product purity was 98.2%, with sodium content of 872.4 PPM, calcium content of 9.8 PPM, magnesium content of 12.6 PPM, iron content of 0.3 PPM, and total impurity content of 1.5%.

[0031] The lithium sulfide yields obtained in Examples 1-5 of this invention are all greater than 90%, exceeding the 39% of Example 1; the purity is all above 99.9%, significantly higher than the 98.2% of Comparative Example 2; and the total impurity content is all below 0.1%, far lower than the 1.3% of Comparative Example 1 and 1.5% of Comparative Example 2. This indicates that this invention, by employing a carbon disulfide / ethanol mixed solvent system and a lithium trithiocarbonate intermediate route, achieves the preparation of high-purity lithium sulfide under mild conditions, demonstrating significant advantages in efficiency and product purity compared to existing liquid-phase metathesis technologies. Obviously, the washing solvent is not limited to anhydrous ethanol, but can also be isopropanol, acetone, or other organic solvents. It is understood that the nitrogen protective atmosphere can be replaced with argon, helium, or other inert gases. Obviously, the sintering temperature is not limited to 400℃; high-purity lithium sulfide products can be obtained within the range of 350~450℃. It is understood that the lithium thiosulfate can be replaced with other lithium carbonates, lithium chloride, lithium sulfite, and other lithium salts.

Claims

1. A liquid-phase synthesis method for high-purity lithium sulfide, comprising the following steps: (1) Dissolve barium sulfide in a mixed solvent of carbon disulfide and alcohol; (2) Add a lithium source to the mixed solvent; (3) Reflux reaction under argon protective atmosphere; (4) After the reaction is complete, filter the solution and wash the filter cake with ethanol to obtain a lithium trithiocarbonate solution; (5) The lithium trithiocarbonate solution was concentrated under reduced pressure and then cooled to crystallize to obtain lithium trithiocarbonate crystals; (6) The lithium trithiocarbonate crystals are sintered to obtain high-purity lithium sulfide.

2. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, The barium sulfide mentioned in step (1) can also be replaced with calcium sulfide, and the amount of barium sulfide or calcium sulfide is 1.05 to 1.1 times the molar equivalent of lithium salt.

3. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, The volume ratio of carbon disulfide to alcohol in step (1) is 1:4 to 1:10; The alcohols include any one or more combinations of ethanol, isopropanol, butanol, and pentanol.

4. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, The water content in the carbon disulfide and alcohol is less than 0.005%.

5. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, The lithium source in step (2) is selected from lithium sulfate or lithium carbonate.

6. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, The argon gas in step (3) has a purity of ≥99.999%, a reflux temperature of 80℃, and a reaction time of 6-10 h.

7. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, The washing operation described in step (4) is carried out in a high-purity argon atmosphere and is washed three times with anhydrous ethanol.

8. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, The vacuum degree of the vacuum concentration in step (5) is 0.001~0.01 MPa, and the temperature of the vacuum concentration is 18~25 ℃.

9. The method for synthesizing high-purity lithium sulfide according to claim 1, characterized in that, In step (6), the sintering temperature is 300-500℃ and the sintering time is 2-6 h.

10. The method for synthesizing high-purity lithium sulfide according to any one of claims 1-9, characterized in that, The high-purity lithium sulfide has a purity of ≥99.9% and a total content of impurities such as calcium, magnesium, and iron of ≤0.1%, more preferably <0.05%, and even more preferably <0.01%.