Ceramic tile with dendritic directional crystallization and method for its production
By using a specific ratio of glaze layers and firing process, the problems of uncontrollable dendritic crystal growth and glaze surface defects in crystalline glaze technology have been solved, achieving directional growth of dendritic crystals and a safe and environmentally friendly decorative effect.
Patent Information
- Application Number
- CN202611287971.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-13
AI Technical Summary
Existing crystallization glaze technology cannot achieve the directional growth of dendritic crystals, has poor crystal form controllability, and poses risks of glaze surface defects and lead and cadmium leaching.
By employing a combination of base glaze, top glaze, and dot glaze layers in a specific ratio, and utilizing the zinc ion concentration difference to drive crystal growth, the glaze is processed by ball milling and the firing parameters are controlled to form dendritic fractal crystals, thus avoiding the addition of precious metals.
It enables the controlled growth of dendritic crystals, reduces glaze defects, lowers the risk of metal leaching, improves production efficiency, and reduces costs.
Smart Images

Figure CN123082684A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic technology, and in particular to a ceramic brick with branched directional crystallization and its preparation method. Background Technology
[0002] Crystalline glaze ceramic tiles, as a high-end decorative category, have become a core demand in the high-end architectural decoration market due to their unique crystalline texture and jade-like feel. However, traditional crystalline glaze technology generally suffers from technical defects. First, the controllability of crystal form is extremely poor. Traditional zinc siliceous mineral crystalline glazes adopt a single glaze layer uniform crystallization mode, with random crystal growth direction and uncontrollable morphology. Existing technologies can mostly achieve random precipitation of clustered or snowflake-like crystals, but cannot achieve directional growth of dendritic crystals. Second, existing crystalline glazes are prone to defects in the glaze layer / glaze surface. High-zinc and high-zirconium crystalline glaze formulations are prone to high-temperature viscosity imbalance, resulting in defects such as pinholes, orange peel, water ripples, and prickly heat blisters in the glaze layer / glaze surface. Furthermore, in order to achieve the metallic effect of the crystalline glaze layer, existing technologies rely on the addition of precious metal cosmetics or heavy metal powders, which carries a high risk of lead and cadmium leaching, failing to meet the requirements of national green manufacturing and dual-carbon strategies. Summary of the Invention
[0003] In view of the shortcomings of the prior art, the purpose of this invention is to provide a ceramic tile with dendritic directional crystallization and its preparation method, which aims to solve the problem that the existing crystallization glaze technology has insufficient crystal form control ability, and can only achieve random precipitation of clustered and snowflake-like crystals, but cannot achieve directional growth of dendritic crystals.
[0004] To achieve the above objectives, the present invention adopts the following technical solution: The first aspect of this invention provides a ceramic tile with branched directional crystallization, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dotted glaze layer randomly distributed on the top glaze layer; the raw materials for preparing the base glaze layer, by weight, include: Potassium feldspar 30-34 parts, calcite 18-22 parts, zinc oxide 10-12 parts, iron oxide 8-12 parts, calcined talc 5-7 parts, titanium dioxide 12-14 parts, black clay powder 3-5 parts, high-silicon and high-calcium frit 3-5 parts; The raw materials for preparing the glaze layer, by weight, include: Potassium feldspar 30-34 parts, calcite 18-22 parts, zinc oxide 10-12 parts, iron oxide 8-12 parts, calcined talc 5-7 parts, titanium dioxide 12-14 parts, black clay powder 3-5 parts, high-silicon and high-calcium frit 3-5 parts.
[0005] In the ceramic brick with dendritic directional crystallization, the chemical composition of the high-silicon and high-calcium frit, by mass percentage, includes: SiO2: 61-63%, Al2O3: 7-8%, CaO: 15-17%, B2O3: 5-7%, MgO: 4-5%, K2O: 1.8-2.0%, Na2O: 1.1-1.4%, with the remainder being loss on ignition and impurities.
[0006] In the ceramic tile with dendritic directional crystallization, the raw materials for preparing the surface glaze layer include raw material glaze and ceramic pigments; by weight, the raw materials for preparing the raw material glaze include: 38-42 parts of zinc-based crystallizing agent, 13-17 parts of zirconium silicate, 12-16 parts of calcite, 6-10 parts of potassium feldspar, 5-7 parts of black clay powder, 3-5 parts of calcined zinc oxide, 3-5 parts of titanium dioxide, 2-4 parts of quartz, 2-4 parts of calcined talc, and 2-4 parts of barium carbonate; the zinc-based crystallizing agent is ZnO with a particle size D50 = 1.5-3.5 μm.
[0007] In the ceramic brick with branched directional crystallization, the ceramic colorant is at least one of the following: a bright red colorant, a pure yellow colorant, or an orange colorant.
[0008] A second aspect of the present invention provides a method for preparing ceramic bricks with dendritic directional crystallization, comprising the following steps: S10. The raw materials for preparing the base glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the base glaze slurry. S20. The raw materials for preparing the glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the glaze slurry. S30. Based on the requirements of glazing, the specific gravity of the base glaze slurry is adjusted to obtain the glaze slurry for spot glazing. S40. Apply the base glaze slurry to the surface of the body layer to form the base glaze layer; S50. Apply the top glaze slurry to the surface of the base glaze layer to form the top glaze layer; S60. Use a glazing sprayer to apply the glazing paste onto the surface glaze layer to form a glazing layer. S70, firing, to obtain the ceramic brick with branched directional crystallization.
[0009] In the method for preparing ceramic tiles with dendritic directional crystallization, the specific gravity of the base glaze slurry in step S40 is 1.68–1.72 g / cm³. 3 The application rate of the base glaze slurry is 9.55–11.28 g / dm³. 2 .
[0010] In the method for preparing ceramic tiles with dendritic directional crystallization, the specific gravity of the glaze slurry in step S50 is 1.74–1.78 g / cm³. 3The application rate of the surface glaze slurry is 11.72–13.45 g / dm³. 2 .
[0011] In the method for preparing ceramic tiles with dendritic directional crystallization, the specific gravity of the glaze slurry in step S60 is 1.74–1.78 g / cm³. 3 The glaze application rate is 1.74–2.6 g / dm³. 2 .
[0012] In the method for preparing ceramic bricks with branched directional crystallization, the glazing frequency in step S60 is 15-20Hz.
[0013] The method for preparing ceramic bricks with dendritic directional crystallization includes a firing process in step S70, comprising a heating stage, a rapid heating stage, and a holding stage. The heating stage involves raising the temperature from room temperature to 1000℃ at a heating rate of 15℃ / min; the rapid heating stage involves raising the temperature from 1000℃ to 1225-1235℃ at a heating rate of 20℃ / min; and the holding stage involves holding the temperature at 1225-1235℃ for 7-9 minutes.
[0014] Beneficial effects: The first aspect of this invention provides a ceramic tile with dendritic directional crystallization, the glaze structure of which includes a base glaze layer, a top glaze layer, and a dotted glaze layer. By distributing the dotted glaze layer in a discrete dotted pattern on the surface of the top glaze layer, zinc is enriched within the dotted glaze layer. This creates a stable zinc ion concentration difference between the dotted glaze layer and the top glaze layer during high-temperature firing, driving the high-concentration zinc ions within the dotted glaze layer to diffuse radially into the surrounding top glaze melt. A continuous, gradient-decreasing zinc ion concentration field is constructed around each dotted crystal nucleus. This directional concentration gradient alters the isotropic natural growth pattern of the crystalline phase, inducing the crystalline phase precipitated in the glaze melt to preferentially grow along the radial direction where the zinc ion concentration decreases. Ultimately, this results in the controllable generation of dendritic fractal crystals with regular texture and uniform branching, achieving control over the crystal morphology and growth direction.
[0015] The second aspect of the present invention provides a method for preparing ceramic tiles with branched directional crystallization. The preparation method can meet the requirements of base glaze and spot glaze by ball milling the base glaze slurry, which can save the need for multiple sets of glazes to be separately prepared and ball milled, saving raw material storage and batching control costs, while also improving production efficiency. Attached Figure Description
[0016] Figure 1 This is a flowchart illustrating the preparation process of the ceramic brick with branched directional crystallization according to the present invention.
[0017] Figure 2 This is a glaze image of the ceramic tile from Example 1.
[0018] Figure 3 This is a glaze image of the ceramic tile from Example 2.
[0019] Figure 4 This is a glaze image of the ceramic tile in Example 3.
[0020] Figure 5 This is a glaze image of the ceramic tile in Comparative Example 1.
[0021] Figure 6 This is a glaze image of the ceramic tile in Comparative Example 2.
[0022] Figure 7 This is a glaze image of the ceramic tile in Comparative Example 4.
[0023] Figure 8 This is a glaze image of the ceramic tile in Comparative Example 5.
[0024] Figure 9 This is a glaze image of the ceramic tile in Comparative Example 6.
[0025] Figure 10 This is a glaze image of the ceramic tile in Comparative Example 7.
[0026] Figure 11 This is a glaze image of ceramic tile in Comparative Example 8.
[0027] Figure 12 This is a glaze image of ceramic tile in Comparative Example 9. Detailed Implementation
[0028] This invention provides a ceramic brick with branched directional crystallization and its preparation method. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only for explaining the invention and are not intended to limit the invention.
[0029] The first aspect of the present invention provides a ceramic tile with branched directional crystallization, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer.
[0030] The raw materials for preparing the base glaze layer, by weight, include: Potassium feldspar 30-34 parts, calcite 18-22 parts, zinc oxide 10-12 parts, iron oxide 8-12 parts, calcined talc 5-7 parts, titanium dioxide 12-14 parts, black clay powder 3-5 parts, high-silicon and high-calcium frit 3-5 parts; The raw materials for preparing the glaze layer, by weight, include: Potassium feldspar 30-34 parts, calcite 18-22 parts, zinc oxide 10-12 parts, iron oxide 8-12 parts, calcined talc 5-7 parts, titanium dioxide 12-14 parts, black clay powder 3-5 parts, high-silicon and high-calcium frit 3-5 parts.
[0031] In the ceramic tile with dendritic directional crystallization provided by this invention, the dot glaze layer is distributed on the surface of the surface glaze layer in a discrete dot shape, and zinc element is enriched inside it. During the high-temperature firing process, a stable zinc ion concentration difference is formed between the dot glaze layer and the surface glaze layer, which drives the high concentration of zinc ions in the dot glaze layer to diffuse radially to the surrounding surface glaze melt. A continuous zinc ion concentration field with a decreasing gradient is constructed around each dot crystal nucleus. This directional concentration gradient will change the isotropic natural growth law of the crystalline phase, and induce the crystalline phase (such as the zinc siliceous mineral crystalline phase) precipitated in the glaze melt to grow preferentially in the radial direction of decreasing zinc ion concentration. Finally, it can controllably generate dendritic fractal crystals with regular texture and uniform branching, thereby realizing the control of crystal morphology and growth direction.
[0032] To further reduce raw material and ingredient costs and decrease the types of glazes used in crystalline glaze ceramic tile products, the raw materials for preparing the dot glaze layer are the same as those for the base glaze layer. Furthermore, the raw materials for preparing the base glaze layer of this invention include 3-5 parts of high-silicon, high-calcium frit. This high-silicon, high-calcium frit can adjust the high-temperature viscosity of the base glaze, making its high-temperature viscosity higher than that of the top glaze layer. This allows the base glaze to build a stable, porous support framework between the body and the top glaze, preventing the molten glaze layer from quickly blocking the body's exhaust channels and ensuring that the gases generated by the body's decomposition completely dissipate, thus eliminating pinholes and blister defects in the glaze layer at their source.
[0033] In a preferred embodiment, the chemical composition of the high-silicon, high-calcium frit, by mass percentage, includes: SiO2: 61-63%, Al2O3: 7-8%, CaO: 15-17%, B2O3: 5-7%, MgO: 4-5%, K2O: 1.8-2.0%, Na2O: 1.1-1.4%, with the remainder being loss on ignition and impurities. The high-silicon, high-calcium frit of this embodiment utilizes a high SiO2 content to construct a continuous, dense three-dimensional silicon-oxygen network, while simultaneously combining 7-8% Al2O3 to form an aluminum-silicon composite cross-linked framework, thereby enhancing the degree of polymerization of the melt. Furthermore, in the high-silicon frit, Ca... 2+ It can play a role in charge compensation, stabilize the [AlO4] tetrahedron, and avoid excessive depolymerization of the network; and during the high-temperature firing process, B2O3 forms a BO-Si composite network with [SiO4] in the form of [BO4] tetrahedron, increasing the crosslinking density. Therefore, the introduction of the high-silicon and high-calcium frit into the base glaze layer can make the high-temperature viscosity of the base glaze layer higher than that of the top glaze layer.
[0034] In a preferred embodiment, the raw materials for preparing the glaze layer include raw glaze and ceramic pigments. Adding ceramic pigments to the glaze layer can achieve a colored glaze surface, and combined with the crystallization effect in the glaze layer, can further enrich the style of the ceramic tiles, enabling them to meet diverse decorative needs.
[0035] For example, the ceramic colorant is at least one of the following: a coating of bright red, a coating of pure yellow, and a coating of orange. All are zirconium silicate-coated cadmium sulfide selenide (CdS) x Se1 x Pigments, based on the different ratios of S and Se in the pigment, can present different hues.
[0036] Furthermore, by weight, the raw materials for preparing the raw glaze include: 38-42 parts of zinc-based crystallizing agent, 13-17 parts of zirconium silicate, 12-16 parts of calcite, 6-10 parts of potassium feldspar, 5-7 parts of black clay powder, 3-5 parts of calcined zinc oxide, 3-5 parts of titanium dioxide, 2-4 parts of quartz, 2-4 parts of calcined talc, and 2-4 parts of barium carbonate.
[0037] In the raw materials for preparing the aforementioned raw glaze, barium carbonate can reduce the surface tension of the glaze melt, promoting uniform glaze spreading and thus reducing defects such as water ripples and orange peel on the glaze surface. Zirconium silicate, with its high melting point and high refractive index, does not completely melt under high-temperature firing conditions when introduced into the glaze layer. Instead, it becomes heterogeneous nucleation sites, forming fine composite crystal nuclei. These composite crystal nuclei scatter light, giving the glaze a jade-like translucency. Simultaneously, an appropriate amount of zirconium silicate can increase the high-temperature viscosity of the glaze layer, preventing excessive flow of the glaze melt and thus reducing glaze flow defects. Furthermore, zirconium silicate can also improve the wear resistance and chemical stability of the glaze surface.
[0038] In the raw materials for preparing the above-mentioned raw glaze, the zinc-based crystallizing agent is ZnO with a particle size D50 of 1.5–3.5 μm. Compared with calcined zinc oxide, the zinc-based crystallizing agent has higher reactivity and can dissolve rapidly within the melting range of the glaze, providing free Zn. 2+ This allows for the rapid establishment of a local zinc ion concentration gradient, promoting the directional and complete precipitation of zirconium dendritic crystals. Simultaneously, sufficient free zinc can segregate and accumulate at the gas-fusible interface at the outer edge of the glaze layer, enabling a solid-phase reaction with iron ions in the base glaze layer to generate continuous and uniform zinc-iron spinel microcrystalline bands. This results in a macroscopically uniform and natural metallic luster border effect on the glaze surface, further enriching the decorative style of crystalline ceramic tiles. Compared to existing technologies, this invention achieves a metallic decorative effect without the addition of any metal powder, precious metal slip, or metallic colorant, thus avoiding the risk of lead, cadmium, and other metal leaching.
[0039] like Figure 1 As shown, a second aspect of the present invention provides a method for preparing ceramic bricks with dendritic directional crystallization, comprising the following steps: S10. The raw materials for preparing the base glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the base glaze slurry. S20. The raw materials for preparing the glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the glaze slurry. S30. Based on the requirements of glazing, the specific gravity of the base glaze slurry is adjusted to obtain the glaze slurry for spot glazing. S40. Apply the base glaze slurry to the surface of the body layer to form the base glaze layer; S50. Apply the top glaze slurry to the surface of the base glaze layer to form the top glaze layer; S60. Use a glazing sprayer to apply the glazing paste onto the surface glaze layer to form a glazing layer. S70, firing, to obtain the ceramic brick with branched directional crystallization.
[0040] The preparation method can meet the needs of both base glaze and dotting glaze by preparing a base glaze slurry, which can save the need for multiple sets of glazes to be separately prepared and ball-milled, saving raw material storage and batching control costs, while also improving production efficiency.
[0041] In step S40, the specific gravity of the base glaze slurry is 1.68–1.72 g / cm³. 3 The application rate of the base glaze slurry is 9.55–11.28 g / dm³. 2 When the specific gravity and amount of glaze applied are within the above range, the thickness of the glaze layer is moderate, which can completely cover the base color of the body and the risk of glaze cracking is low.
[0042] In step S50, the specific gravity of the glaze slurry is 1.74–1.78 g / cm³. 3 The application rate of the surface glaze slurry is 11.72–13.45 g / dm³. 2 When the specific gravity and amount of glaze slurry are within the above range, the thickness of the glaze layer is moderate, which can provide sufficient space for crystal growth and ensure the formation of complete dendritic crystals; at the same time, the thickness of the glaze layer is uniform and the glaze surface is smooth, which can reduce appearance defects such as pinholes, prickly heat blisters, and glaze runs.
[0043] In step S60, the specific gravity of the glaze slurry is 1.74–1.78 g / cm³. 3 The glaze application rate is 1.74–2.6 g / dm³. 2 .
[0044] In step S60, the glazing frequency is 15–20 Hz. When the glazing frequency is within the above range, the glaze distribution density is moderate, the crystal nucleus spacing is uniform, and a stable zinc ion concentration gradient can be formed, thereby promoting the directional growth of crystals and forming a uniform and dense dendritic texture.
[0045] In step S70, the firing process of the ceramic tile includes a heating section, a rapid heating section, and a holding section. The heating section involves raising the temperature from room temperature to 1000°C at a rate of 15°C / min to allow the moisture in the body layer and each glaze layer to evaporate and the organic matter and carbonates to decompose. The rapid heating section involves raising the temperature from 1000°C to 1225-1235°C at a rate of 20°C / min. During this stage, the glaze begins to melt, and crystal nuclei begin to form in the glaze melt. The holding section involves holding the temperature at 1225-1235°C for 7-9 minutes to ensure that the crystals in the glaze melt grow sufficiently.
[0046] The present invention will be further illustrated by the following examples and comparative examples.
[0047] Example 1 This embodiment provides a ceramic tile with branched directional crystallization, including a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer.
[0048] Specifically, in this embodiment, the raw materials for preparing the base glaze layer, by weight, include: 32 parts potassium feldspar, 20 parts calcite, 11 parts zinc oxide, 10 parts iron oxide, 6 parts calcined talc, 10 parts titanium dioxide, 4 parts black clay powder, and 4 parts high-silicon and high-calcium frit. The raw materials for preparing the glaze layer, by weight, include: 32 parts potassium feldspar, 20 parts calcite, 11 parts zinc oxide, 10 parts iron oxide, 6 parts calcined talc, 10 parts titanium dioxide, 4 parts black clay powder, and 4 parts high-silicon and high-calcium frit.
[0049] The chemical composition of the high-silicon and high-calcium ingot, by mass percentage, includes: SiO2: 62%, Al2O3: 7.5%, CaO: 16%, B2O3: 6%, MgO: 4.5%, K2O: 1.9%, Na2O: 1.2%, and loss on ignition and impurities of 0.9%.
[0050] In this embodiment, the raw materials for preparing the surface glaze layer include raw glaze and ceramic pigment. The ratio of raw glaze to ceramic pigment by weight is 8:2; the ceramic pigment is a bright red pigment.
[0051] The raw materials for preparing the raw glaze, by weight, include: 40 parts of zinc-based crystallizing agent, 15 parts of zirconium silicate, 14 parts of calcite, 8 parts of potassium feldspar, 6 parts of black clay powder, 4 parts of calcined zinc oxide, 4 parts of titanium dioxide, 3 parts of quartz, 3 parts of calcined talc, and 3 parts of barium carbonate; the zinc-based crystallizing agent is ZnO with a particle size D50 of 1.5 to 3.5 μm.
[0052] This embodiment also provides a method for preparing the ceramic brick of this embodiment, including the following steps: S10. The raw materials for preparing the base glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the base glaze slurry. S20. The raw materials for preparing the glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the glaze slurry. S30. Based on the requirements of glazing, the specific gravity of the base glaze slurry is adjusted to obtain the glaze slurry for spot glazing. S40. Apply the base glaze slurry to the surface of the body layer to form the base glaze layer; S50. Apply the top glaze slurry to the surface of the base glaze layer to form the top glaze layer; S60. Use a glazing sprayer to apply the glazing paste onto the surface glaze layer to form a glazing layer. S70, firing, to obtain the ceramic brick with branched directional crystallization.
[0053] In step S40, the specific gravity of the base glaze slurry is 1.7 g / cm³. 3 The application rate of the base glaze slurry is 10g / dm². 2 In step S50, the specific gravity of the glaze slurry is 1.75 g / cm³. 3 The application rate of the glaze slurry is 12g / dm². 2 In step S60, the specific gravity of the glaze slurry is 1.75 g / cm³. 3 The glaze application rate is 2.0 g / dm. 2 The glazing frequency is 20Hz.
[0054] In step S70, the firing process of the ceramic brick includes a heating section, a rapid heating section, and a holding section; wherein, the heating section is to raise the temperature from room temperature to 1000℃ at a heating rate of 15℃ / min; the rapid heating section is to raise the temperature from 1000℃ to 1230℃ at a heating rate of 20℃ / min; and the holding stage is to hold the temperature at 1230℃ for 8 minutes.
[0055] Example 2 This embodiment provides a ceramic tile with branched directional crystallization, including a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer.
[0056] Specifically, in this embodiment, the raw materials for preparing the base glaze layer, by weight, include: 30 parts potassium feldspar, 18 parts calcite, 10 parts zinc oxide, 8 parts iron oxide, 5 parts calcined talc, 12 parts titanium dioxide, 3 parts black clay powder, and 3 parts high-silicon and high-calcium frit. The raw materials for preparing the glaze layer, by weight, include: 30 parts potassium feldspar, 18 parts calcite, 10 parts zinc oxide, 8 parts iron oxide, 5 parts calcined talc, 12 parts titanium dioxide, 3 parts black clay powder, and 3 parts high-silicon and high-calcium frit.
[0057] The chemical composition of the high-silicon and high-calcium ingot, by mass percentage, includes: SiO2: 62%, Al2O3: 7.5%, CaO: 16%, B2O3: 6%, MgO: 4.5%, K2O: 1.9%, Na2O: 1.2%, and loss on ignition and impurities of 0.9%.
[0058] In this embodiment, the raw materials for preparing the surface glaze layer include raw glaze and ceramic pigments. The ceramic pigments include a pure yellow pigment and an orange-yellow pigment. The raw glaze, the pure yellow pigment, and the orange-yellow pigment are mixed in a weight ratio of 8.4:0.6:0.6.
[0059] The raw materials for preparing the raw glaze, by weight, include: 38 parts of zinc-based crystallizing agent, 13 parts of zirconium silicate, 12 parts of calcite, 6 parts of potassium feldspar, 5 parts of black clay powder, 3 parts of calcined zinc oxide, 3 parts of titanium dioxide, 2 parts of quartz, 2 parts of calcined talc, and 2 parts of barium carbonate; the zinc-based crystallizing agent is ZnO with a particle size D50 of 1.5 to 3.5 μm.
[0060] This embodiment also provides a method for preparing the ceramic brick of this embodiment, including the following steps: S10. The raw materials for preparing the base glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the base glaze slurry. S20. The raw materials for preparing the glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the glaze slurry. S30. Based on the requirements of glazing, the specific gravity of the base glaze slurry is adjusted to obtain the glaze slurry for spot glazing. S40. Apply the base glaze slurry to the surface of the body layer to form the base glaze layer; S50. Apply the top glaze slurry to the surface of the base glaze layer to form the top glaze layer; S60. Use a glazing sprayer to apply the glazing paste onto the surface glaze layer to form a glazing layer. S70, firing, to obtain the ceramic brick with branched directional crystallization.
[0061] In step S40, the specific gravity of the base glaze slurry is 1.68 g / cm³. 3 The application rate of the base glaze slurry is 9.55 g / dm². 2 In step S50, the specific gravity of the glaze slurry is 1.74 g / cm³. 3 The application rate of the glaze slurry is 11.72 g / dm². 2 In step S60, the specific gravity of the glaze slurry is 1.74 g / cm³. 3The glaze application rate is 1.74 g / dm³. 2 The glazing frequency is 15Hz.
[0062] In step S70, the firing process of the ceramic brick includes a heating section, a rapid heating section, and a holding section; wherein, the heating section is to raise the temperature from room temperature to 1000℃ at a heating rate of 15℃ / min, the rapid heating section is to raise the temperature from 1000℃ to 1225℃ at a heating rate of 20℃ / min, and the holding stage is to hold the temperature at 1225℃ for 8 minutes.
[0063] Example 3 This embodiment provides a ceramic tile with branched directional crystallization, including a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer.
[0064] Specifically, in this embodiment, the raw materials for preparing the base glaze layer, by weight, include: Potassium feldspar 34 parts, calcite 22 parts, zinc oxide 12 parts, iron oxide 12 parts, calcined talc 5 parts, titanium dioxide 12 parts, black clay powder 3 parts, high-silicon and high-calcium frit 3 parts; The raw materials for preparing the glaze layer, by weight, include: Potassium feldspar 34 parts, calcite 22 parts, zinc oxide 12 parts, iron oxide 12 parts, calcined talc 5 parts, titanium dioxide 12 parts, black clay powder 3 parts, high-silicon and high-calcium frit 3 parts.
[0065] The chemical composition of the high-silicon and high-calcium ingot, by mass percentage, includes: SiO2: 62%, Al2O3: 7.5%, CaO: 16%, B2O3: 6%, MgO: 4.5%, K2O: 1.9%, Na2O: 1.2%, and loss on ignition and impurities of 0.9%.
[0066] In this embodiment, the raw materials for preparing the surface glaze layer include raw glaze and ceramic pigments. The ceramic pigments include a pure yellow pigment and an orange-yellow pigment. The raw glaze, the pure yellow pigment, and the orange-yellow pigment are mixed in a weight ratio of 8.4:0.6:0.6.
[0067] The raw materials for preparing the raw glaze, by weight, include: 42 parts of zinc-based crystallizing agent, 17 parts of zirconium silicate, 16 parts of calcite, 10 parts of potassium feldspar, 7 parts of black clay powder, 5 parts of calcined zinc oxide, 5 parts of titanium dioxide, 4 parts of quartz, 4 parts of calcined talc, and 4 parts of barium carbonate; the zinc-based crystallizing agent is ZnO with a particle size D50 of 1.5 to 3.5 μm.
[0068] This embodiment also provides a method for preparing the ceramic brick of this embodiment, including the following steps: S10. The raw materials for preparing the base glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the base glaze slurry. S20. The raw materials for preparing the glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the glaze slurry. S30. Based on the requirements of glazing, the specific gravity of the base glaze slurry is adjusted to obtain the glaze slurry for spot glazing. S40. Apply the base glaze slurry to the surface of the body layer to form the base glaze layer; S50. Apply the top glaze slurry to the surface of the base glaze layer to form the top glaze layer; S60. Use a glazing sprayer to apply the glazing paste onto the surface glaze layer to form a glazing layer. S70, firing, to obtain the ceramic brick with branched directional crystallization.
[0069] In step S40, the specific gravity of the base glaze slurry is 1.72 g / cm³. 3 The application rate of the base glaze slurry is 11.28 g / dm³. 2 In step S50, the specific gravity of the glaze slurry is 1.78 g / cm³. 3 The application rate of the glaze slurry is 13.45 g / dm². 2 In step S60, the specific gravity of the glaze slurry is 1.78 g / cm³. 3 The glaze application rate is 2.6 g / dm³. 2 The glazing frequency is 20Hz.
[0070] In step S70, the firing process of the ceramic brick includes a heating section, a rapid heating section, and a holding section; wherein, the heating section is to raise the temperature from room temperature to 1000℃ at a heating rate of 15℃ / min; the rapid heating section is to raise the temperature from 1000℃ to 1235℃ at a heating rate of 20℃ / min; and the holding stage is to hold the temperature at 1235℃ for 8 minutes.
[0071] Comparative Example 1 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer. The only difference between this ceramic tile and the ceramic tile of Example 1 is that the amount of iron oxide in the raw materials for preparing the base glaze layer is reduced from 10 parts to 7 parts.
[0072] This comparative example also provides a method for preparing the ceramic bricks of this comparative example, which is the same as the preparation method provided in Example 1.
[0073] Comparative Example 2 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer. The only difference between this ceramic tile and the ceramic tile of Example 1 is that the amount of iron oxide in the raw materials for preparing the base glaze layer is increased from 10 parts to 13 parts.
[0074] This comparative example also provides a method for preparing the ceramic bricks of this comparative example, which is the same as the preparation method provided in Example 1.
[0075] Comparative Example 3 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer. The only difference between this ceramic tile and the ceramic tile of Example 1 is that high-silicon, high-calcium frit is not used in the raw materials for preparing the base glaze layer.
[0076] This comparative example also provides a method for preparing the ceramic bricks of this comparative example, which is the same as the preparation method provided in Example 1.
[0077] Comparative Example 4 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer. This ceramic tile differs from the ceramic tile of Example 1 in the following ways: (1) The ceramic colorant includes a pure yellow coating and an orange-yellow coating. The raw material glaze, the pure yellow coating, and the orange-yellow coating are mixed in a weight ratio of 8.4:0.6:0.6.
[0078] (2) In the raw materials for preparing raw glaze, the zinc-based crystallizing agent was reduced from 40 parts to 36 parts.
[0079] This comparative example also provides a method for preparing the ceramic bricks of this comparative example, which is the same as the preparation method provided in Example 1.
[0080] Comparative Example 5 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer. This ceramic tile differs from the ceramic tile of Example 1 in the following ways: (1) The ceramic colorant includes a pure yellow coating and an orange-yellow coating. The raw material glaze, the pure yellow coating, and the orange-yellow coating are mixed in a weight ratio of 8.4:0.6:0.6.
[0081] (2) In the raw materials for preparing raw glaze, the zinc-based crystallizing agent was increased from 40 parts to 44 parts.
[0082] This comparative example also provides a method for preparing the ceramic bricks of this comparative example, which is the same as the preparation method provided in Example 1.
[0083] Comparative Example 6 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dotted glaze layer randomly distributed on the top glaze layer. This ceramic tile differs from the ceramic tile of Example 1 in the following way: the ceramic colorant includes a pure yellow coating and an orange-yellow coating. The raw glaze, the pure yellow coating, and the orange-yellow coating are mixed in a weight ratio of 8.4:0.6:0.6.
[0084] This comparative example also provides a method for preparing the ceramic bricks of this comparative example. The difference between this method and the method provided in Example 1 is that, in step S70, the rapid heating stage is to heat from 1000°C to 1210°C at a heating rate of 20°C / min, and the holding stage is to hold at 1210°C for 8 minutes.
[0085] Comparative Example 7 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dotted glaze layer randomly distributed on the top glaze layer. This ceramic tile differs from the ceramic tile of Example 1 in the following way: the ceramic colorant includes a pure yellow coating and an orange-yellow coating. The raw glaze, the pure yellow coating, and the orange-yellow coating are mixed in a weight ratio of 8.4:0.6:0.6.
[0086] This comparative example also provides a method for preparing the ceramic bricks of this comparative example. The difference between this method and the method provided in Example 1 is that, in step S70, the rapid heating stage is to heat from 1000°C to 1250°C at a heating rate of 20°C / min, and the holding stage is to hold at 1250°C for 8 minutes.
[0087] Comparative Example 8 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dotted glaze layer randomly distributed on the top glaze layer. This ceramic tile differs from the ceramic tile of Example 1 in the following way: the ceramic colorant includes a pure yellow coating and an orange-yellow coating. The raw glaze, the pure yellow coating, and the orange-yellow coating are mixed in a weight ratio of 8.4:0.6:0.6.
[0088] This comparative example also provides a method for preparing the ceramic tile of this comparative example. The difference between this method and the method provided in Example 1 is that, in step S60, the glazing frequency is reduced from 20Hz to 15Hz.
[0089] Comparative Example 9 This comparative example provides a ceramic tile, comprising a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dotted glaze layer randomly distributed on the top glaze layer. This ceramic tile differs from the ceramic tile of Example 1 in the following way: the ceramic colorant includes a pure yellow coating and an orange-yellow coating. The raw glaze, the pure yellow coating, and the orange-yellow coating are mixed in a weight ratio of 8.4:0.6:0.6.
[0090] This comparative example also provides a method for preparing the ceramic tile of this comparative example. The difference between this method and the method provided in Example 1 is that, in step S60, the glazing frequency is increased from 20Hz to 25Hz.
[0091] The ceramic tile glaze layers provided in the above embodiments and comparative examples were observed to observe the crystal morphology in the glaze layer, the metallic border effect at the edge of the glaze layer, and whether there were any defects in the glaze layer and glaze surface. The observation results are shown in Table 1 below.
[0092] Table 1:
[0093] As can be seen from the observation results in Table 1 above, the ceramic tile glaze layers provided in Examples 1 to 3 have clear dendritic crystal forms, and the edges of the glaze layers can form a continuous metallic luster border effect. This indicates that the present invention constructs a radial concentration gradient of zinc ions through the discrete distribution of the glaze, which can regulate the directional precipitation of zinc siliceous mineral crystals along the gradient direction, resulting in dendritic crystals with uniform branches and regular texture. At the same time, the zinc-iron spinel microcrystalline band is generated by the solid-phase reaction of zinc and iron components in the top glaze layer and the bottom glaze layer, so that a natural metallic texture can be achieved without adding precious metal or heavy metal powders, taking into account both decorative effect and green environmental protection requirements.
[0094] Observing the glaze layer of the ceramic tile provided in Comparative Example 1, it was found that the dendritic crystal morphology in the glaze layer was basically normal, but the metallic luster border at the edge of the glaze layer showed signs of breakage (see...). Figure 5 (The area within the blue box) This is because the amount of iron oxide in the base glaze material used in Comparative Example 1 was relatively small, resulting in a reduction in the amount of zinc-iron spinel generated by the solid-phase reaction.
[0095] Observation of the ceramic tile glaze layer provided in Comparative Example 2 revealed that the crystal orientation of the glaze layer was basically maintained, but local crystal melting occurred (see...). Figure 6 (Blue box area) At the same time, a small number of black spots appeared in the glaze layer. This is because the amount of iron oxide in the base glaze material used in Comparative Example 2 was too high, which would increase the high temperature viscosity of the glaze and affect the growth of crystals, thus leading to local crystal melting.
[0096] Observation of the ceramic tile glaze layer provided in Comparative Example 3 revealed pinholes and prickly heat bubbles on the glaze surface. This may be because the raw materials used in the preparation of the base glaze layer in Comparative Example 3 do not include high-silicon and high-calcium frit, which leads to a decrease in the high-temperature viscosity of the base glaze layer. The base glaze melt can quickly block the exhaust channels of the body layer, causing the gas generated by the decomposition of the body to be unable to escape in time and remain in the glaze layer, resulting in defects such as pinholes and prickly heat bubbles in the glaze layer.
[0097] Observing the ceramic tile glaze layer provided in Comparative Example 4, it was found that the dendritic structure in the glaze layer was not obvious, but rather clustered. Furthermore, the metal border at the edge of the glaze layer was discontinuous and uneven in width. This is because the amount of zinc-based crystallizing agent in the raw materials used to prepare the surface glaze layer in Comparative Example 4 was too small, resulting in a low supersaturation of zinc ions in the glaze melt, which could not form a stable concentration gradient, thus inhibiting crystal nucleation and growth. In addition, the supply of zinc ions to react with iron ions in the base glaze layer was insufficient, which would affect the formation of zinc-iron spinel microcrystals.
[0098] Observing the ceramic tile glaze layer provided in Comparative Example 5, it was found that the crystals in the glaze layer grew excessively, the dendritic structure was blurred, and large areas of melting and adhesion occurred. At the same time, the metal frame at the edge of the glaze layer was too wide and merged with each other. This is because the zinc-based crystallizing agent used in the glaze layer preparation material of Comparative Example 5 was too much, the high temperature viscosity of the glaze melt was too low, the crystal growth was out of control and melting occurred, and the glaze fluidity was too high, the bubbles could not escape completely, which would lead to pinhole defects in the glaze layer.
[0099] Observing the ceramic tile glaze layer provided in Comparative Example 6, it was found that the amount of crystal precipitation in the ceramic tile glaze layer was small and fine, and there was no dendritic structure. At the same time, there was no continuous metal border at the edge of the glaze layer. This is because in Comparative Example 6, the heat preservation temperature was too low, the glaze did not reach a completely molten state, and the ion diffusion and solid-phase reaction at the edge of the glaze layer could not proceed fully, which hindered the nucleation and growth of crystals in the glaze layer.
[0100] Observing the ceramic tile glaze layer provided in Comparative Example 7, it was found that the crystals in the ceramic tile glaze layer were severely eroded, the dendritic structure was completely destroyed, and no obvious metal border effect was generated at the edge of the glaze layer. This is because in Comparative Example 7, the heat preservation temperature was too high, the high temperature viscosity of the glaze was too low, and the precipitated crystals were remelted; in addition, the glaze fluidity was too high and the spread was uneven, which would cause water ripples and orange peel defects to appear on the glaze surface.
[0101] Observing the ceramic tile glaze layer provided by Comparative Example 8, it was found that the individual crystal forms in the ceramic tile glaze layer grew well and had normal orientation, but the crystal nucleus density was too low, resulting in unclear dendritic texture. This is because in the glazing process of Comparative Example 8, the glazing frequency was too low and the glaze distribution density was insufficient, resulting in too few crystal nucleus sites and too large crystal growth space, which made it impossible to form clear dendritic texture.
[0102] Observation of the ceramic tile glaze layer provided in Comparative Example 9 revealed that the crystal nucleus density in the glaze layer was too high, with crystals overlapping and being compressed, thus disrupting their orientation. Furthermore, the metallic borders at the edges of the glaze layer merged together, forming irregular, sheet-like metallic luster and losing their independent texture. This was because the glazing frequency in Comparative Example 9 was too high, and the glaze dots were too densely distributed, resulting in insufficient spacing between crystal nuclei. This caused mutual interference during crystal growth, preventing the formation of independent, oriented dendritic crystal structures.
[0103] The ceramic tiles provided in Examples 1 to 3 were subjected to performance tests, including breaking strength, modulus of rupture, and stain resistance. The modulus of rupture and breaking strength tests were conducted according to standard GB / T 3810.4 "Ceramic Tiles - Test Methods Part 4: Determination of Modulus of Rupture and Breaking Strength". The stain resistance test was conducted according to standard GB / T 4100-2015 "Ceramic Tiles".
[0104] Table 2:
[0105] As can be seen from the test data in Table 2, the destructive strength of the directional crystallized ceramic tiles prepared by this invention all reached over 1550N, and the modulus of rupture was stably maintained at 41MPa and above, demonstrating excellent mechanical properties and meeting the strength standards for building ceramic tiles. Furthermore, the ceramic tiles in all three embodiments achieved the highest stain resistance rating of 5, indicating a dense and smooth glaze that makes it difficult for stains to penetrate and adhere, facilitating daily cleaning and maintenance. The overall product combines a unique directional crystallization decorative effect with excellent physical and chemical properties, making it suitable for high-end interior wall and floor decoration scenarios.
[0106] It is understood that those skilled in the art can make equivalent substitutions or modifications to the technical solution and inventive concept of the present invention, and all such substitutions or modifications should fall within the protection scope of the appended claims.
Claims
1. A ceramic brick with branched directional crystallization, characterized in that, It includes a body layer, a base glaze layer disposed on the body layer, a top glaze layer disposed on the base glaze layer, and a dot glaze layer randomly distributed on the top glaze layer; The raw materials for preparing the base glaze layer, by weight, include: Potassium feldspar 30-34 parts, calcite 18-22 parts, zinc oxide 10-12 parts, iron oxide 8-12 parts, calcined talc 5-7 parts, titanium dioxide 12-14 parts, black clay powder 3-5 parts, high-silicon and high-calcium frit 3-5 parts; The raw materials for preparing the glaze layer, by weight, include: Potassium feldspar 30-34 parts, calcite 18-22 parts, zinc oxide 10-12 parts, iron oxide 8-12 parts, calcined talc 5-7 parts, titanium dioxide 12-14 parts, black clay powder 3-5 parts, high-silicon and high-calcium frit 3-5 parts.
2. The ceramic brick with branched directional crystallization according to claim 1, characterized in that, The chemical composition of the high-silicon and high-calcium ingot, by mass percentage, includes: SiO2: 61-63%, Al2O3: 7-8%, CaO: 15-17%, B2O3: 5-7%, MgO: 4-5%, K2O: 1.8-2.0%, Na2O: 1.1-1.4%, with the remainder being loss on ignition and impurities.
3. The ceramic brick with branched directional crystallization according to claim 1, characterized in that, The raw materials for preparing the surface glaze layer include raw material glaze and ceramic pigments; by weight, the raw material glaze includes: 38-42 parts of zinc-based crystallizing agent, 13-17 parts of zirconium silicate, 12-16 parts of calcite, 6-10 parts of potassium feldspar, 5-7 parts of black clay powder, 3-5 parts of calcined zinc oxide, 3-5 parts of titanium dioxide, 2-4 parts of quartz, 2-4 parts of calcined talc, and 2-4 parts of barium carbonate; the zinc-based crystallizing agent is ZnO with a particle size D50 of 1.5-3.5 μm.
4. The ceramic brick with branched directional crystallization according to claim 3, characterized in that, The ceramic colorant is at least one of the following: a bright red colorant, a pure yellow colorant, or an orange-yellow colorant.
5. A method for preparing a ceramic brick with dendritic directional crystallization as described in any one of claims 1-4, comprising the following steps: S10. The raw materials for preparing the base glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the base glaze slurry. S20. The raw materials for preparing the glaze layer are put into a ball mill according to the proportion, mixed with water and ball milled to obtain the glaze slurry. S30. Based on the requirements of glazing, the specific gravity of the base glaze slurry is adjusted to obtain the glaze application slurry; S40. Apply the base glaze slurry to the surface of the body layer to form the base glaze layer; S50. Apply the top glaze slurry to the surface of the base glaze layer to form the top glaze layer; S60. Use a glazing sprayer to apply the glazing paste onto the surface glaze layer to form a glazing layer. S70, firing, to obtain the ceramic brick with branched directional crystallization.
6. In the method for preparing ceramic tiles with dendritic directional crystallization according to claim 5, in step S40, the specific gravity of the base glaze slurry is 1.68–1.72 g / cm³. 3 The application rate of the base glaze slurry is 9.55–11.28 g / dm³. 2 .
7. In the method for preparing ceramic tiles with dendritic directional crystallization according to claim 5, in step S50, the specific gravity of the glaze slurry is 1.74–1.78 g / cm³. 3 The application rate of the surface glaze slurry is 11.72–13.45 g / dm³. 2 .
8. In the method for preparing ceramic tiles with dendritic directional crystallization according to claim 5, in step S60, the specific gravity of the glaze slurry is 1.74–1.78 g / cm³. 3 The glaze application rate is 1.74–2.6 g / dm³. 2 .
9. In the method for preparing ceramic bricks with branched directional crystallization according to claim 8, in step S60, the glazing frequency is 15-20Hz.
10. The method for preparing ceramic bricks with dendritic directional crystallization according to claim 5, wherein, in step S70, the firing process of the ceramic bricks includes a heating section, a rapid heating section, and a holding section; wherein, The heating stage involves raising the temperature from room temperature to 1000℃ at a rate of 15℃ / min; the rapid heating stage involves raising the temperature from 1000℃ to 1225-1235℃ at a rate of 20℃ / min; and the holding stage involves holding the temperature at 1225-1235℃ for 7-9 minutes.