A composite photoluminescent and reflective fluorescent heat-adhesive film and its preparation method
By employing a composite structural design and selective vacuum evaporation process, the problem of functional layer interference caused by the mixed coating of phosphor and photoluminescent powder has been solved, achieving high-brightness afterglow and multi-color warning, while improving washability and flame retardancy. It is suitable for fields such as fire rescue, road traffic signs, safety protective clothing, and special operation vehicles.
Patent Information
- Application Number
- CN202611550913.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing photoluminescent reflective warning tapes suffer from interference between functional layers due to the direct mixing and coating of fluorescent powder and photoluminescent powder. This results in insufficient afterglow brightness at night, limited daytime warning colors, poor washability, and difficulty in achieving both high temperature resistance and washability.
The composite structure design includes a reflective structural layer, a transparent adhesive layer, a functional layer, and a white cover layer. The fluorescent layer and the light-gathering layer are adjacent to each other without overlapping. The metal reflective layer is only distributed in the corresponding area of the silver-gray composite adhesive layer. Independent fluorescent and light-gathering functional layers are formed through selective vacuum evaporation and hot-pressing transfer processes. Each layer is made of washable resin to improve washability.
It achieves physical isolation between fluorescence and light storage functions, enhances the brightness of nighttime afterglow, enriches daytime warning colors, and has excellent washability and flame retardant properties, ensuring high visibility and structural integrity in all weather conditions.
Smart Images

Figure CN123104205A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of reflective materials technology, and in particular relates to a composite photoluminescent reflective heat-adhesive film and its preparation method. Background Technology
[0002] Photoluminescent reflective warning tape is widely used in fire rescue, road traffic signs, safety protective clothing, outdoor sports equipment, and special-operation vehicles. This type of material combines "retroreflection" and "long-afterglow self-luminescence" technologies, enabling it to provide strong reflective warnings during the day using glass microspheres, and to continuously release faint light at night or in environments without external light sources, such as during sudden power outages, relying on the light energy absorbed and stored by the photoluminescent material.
[0003] Existing photoluminescent reflective warning tapes are typically made from aluminized film (semi-aluminized film). The conventional manufacturing process involves directly coating the back of the aluminized film with an adhesive mixture of fluorescent pigments and photoluminescent powder. After drying and curing, a substrate or hot-melt adhesive layer is then laminated onto the film, resulting in a heat-applied film that combines color display, reflectivity, and photoluminescence. The fluorescent pigments impart vibrant daytime colors to enhance visual alertness during the day, while the photoluminescent powders provide long-lasting night vision guidance. The metallic areas of the aluminized film provide high-intensity reflectivity.
[0004] However, the above-mentioned process of directly mixing and coating phosphors and photoluminescent powders has significant technical drawbacks in practical use:
[0005] Firstly, the fluorescent pigments and photoluminescent powders mix and interfere with each other in the adhesive layer, which reduces the material's efficiency in absorbing and releasing external light energy. During the day, it only presents a single mixed fluorescent color and reflective effect, resulting in a single warning color that can easily cause visual fatigue. At night, due to the photoluminescent powder being blocked by the fluorescent pigments and interfering with each other, the long afterglow performance is insufficient, the night vision effect is not obvious, and it is difficult to meet the safety warning needs in complex environments.
[0006] Secondly, the direct mixing of fluorescent powder and photoluminescent powder disrupts the uniformity and cohesive strength of the adhesive system, resulting in poor overall washability and severely shortening the service life of the warning tape.
[0007] Third, existing processes cannot simultaneously achieve high temperature resistance and high washability. During subsequent hot-pressing and bonding processes, the mixed adhesive layer is prone to deformation or performance degradation, further affecting the overall performance of the final product.
[0008] Therefore, there is a need to provide an improved technical solution that addresses the shortcomings of the existing technology. Summary of the Invention
[0009] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a composite photoluminescent reflective thermal adhesive film and its preparation method, which solves the problems of mutual interference of functional layers, insufficient afterglow brightness at night, single warning color during the day and poor washability caused by the direct mixing and coating of fluorescent powder and photoluminescent powder in the prior art photoluminescent reflective warning tape.
[0010] To achieve the above and other related objectives, the present invention provides a composite photoluminescent and reflective fluorescent heat-adhesive film, comprising a reflective structural layer, a transparent adhesive layer, a functional layer and a white cover layer stacked sequentially, wherein a flame-retardant adhesive film layer is disposed on the side of the white cover layer away from the functional layer.
[0011] The reflective structure layer comprises a base film layer, a beaded adhesive layer, a glass microsphere layer, a focusing layer, and a metal reflective layer stacked sequentially. The beaded adhesive layer is formed on one side of the base film layer. The glass microsphere layer comprises a plurality of glass microspheres, some of which are embedded in the beaded adhesive layer and fixed by the beaded adhesive layer. The focusing layer is disposed on the side of the glass microsphere layer away from the base film layer. The metal reflective layer is disposed on the side of the focusing layer away from the glass microsphere layer and is spaced apart along the width direction of the heat-bonded film.
[0012] The transparent adhesive layer is disposed on the side of the reflective structural layer away from the base film layer and is used to connect the reflective structural layer and the functional layer;
[0013] The functional layer includes a silver-gray composite adhesive layer, a fluorescent layer, and a light-gathering layer arranged periodically along the width direction of the heat-adhesive film. The fluorescent layer and the light-gathering layer are embedded in the silver-gray composite adhesive layer, and the fluorescent layer and the light-gathering layer are adjacent to each other without overlapping. The projection area of the metal reflective layer in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer is located, and does not coincide with the areas where the fluorescent layer and the light-gathering layer are located.
[0014] The white cover layer is disposed on the side of the functional layer away from the transparent adhesive layer.
[0015] Preferably, the silver-gray composite adhesive layer is provided with a first strip-shaped groove arranged at intervals along the width direction of the film surface, and the fluorescent layer is disposed in the first strip-shaped groove; and the fluorescent layer is provided with a second strip-shaped groove arranged at intervals along the width direction of the film surface, and the light-gathering layer is disposed in the second strip-shaped groove.
[0016] Preferably, the material of the beaded adhesive layer includes one of PP, PE, EVA, EBA, EAA, and a mixture with an opening agent.
[0017] Preferably, the thickness of the bead adhesive layer is 25% to 35% of the diameter of the glass microspheres.
[0018] Preferably, the glass microspheres have a diameter of 45μm to 95μm and a refractive index of 1.9 to 1.95.
[0019] Preferably, the material of the focusing layer includes one or a combination of polyurethane, polyester, and epoxy-modified acrylic resin, and the thickness of the focusing layer is 5μm to 20μm.
[0020] Preferably, the material of the metal reflective layer includes at least one of aluminum, silver, and chromium.
[0021] Preferably, the thickness of the transparent adhesive layer is 10μm to 20μm.
[0022] Preferably, the thickness of the silver-gray composite adhesive layer is 30μm~70μm.
[0023] Preferably, the material of the silver-gray composite adhesive layer includes one or a combination of epoxy resin, polyurethane, and modified acrylic resin, as well as a mixture with silver-gray pigment, flame retardant, and crosslinking agent.
[0024] Preferably, the thickness of the fluorescent layer is 30 μm to 80 μm.
[0025] And / or, the material of the fluorescent layer includes one or a combination of EVA, polyolefin, and polyurethane, and a mixture with fluorescent pigment, flame retardant, and crosslinking agent, wherein the fluorescent pigment includes one or a combination of yellow, orange, and red pigments.
[0026] Preferably, the thickness of the photoluminescence layer is 30μm to 80μm.
[0027] Preferably, the material of the photoluminescent layer includes one or a combination of EVA, polyolefin, and polyurethane, as well as a mixture with photoluminescent powder, flame retardant, and crosslinking agent.
[0028] Preferably, the thickness of the white covering layer is 30μm to 70μm.
[0029] Preferably, the white covering layer comprises one or a combination of epoxy resin, polyurethane, and modified acrylic resin, as well as a mixture with white pigment, flame retardant, and crosslinking agent.
[0030] Preferably, the base layer of the flame-retardant adhesive film is selected from one of TPU, PU, PES, and PVC, and the thickness of the base layer is 30-150 μm.
[0031] The present invention also provides a method for preparing the composite photoluminescent and reflective fluorescent heat-adhesive film as described above, the method comprising the following steps:
[0032] S1. A beaded adhesive layer is formed on the surface of the base film layer. Glass microspheres are partially embedded in the beaded adhesive layer to form a glass microsphere layer. A focusing layer is formed on the side of the glass microsphere layer away from the beaded adhesive layer. Selective vacuum evaporation is performed on the side of the focusing layer away from the glass microsphere layer to form a metal reflective layer that is spaced apart along the width direction of the film surface, thus obtaining a reflective structure layer. Subsequently, a transparent adhesive layer is formed on the side of the reflective structure layer away from the base film layer, and a first release substrate is bonded to it to form a reflective substrate.
[0033] S2. Pre-fabricate the fluorescent layer, the phosphorescent layer, and the white opaque layer respectively:
[0034] A fluorescent layer is formed on the surface of the first release film, and after drying, it is bonded to the second release substrate to obtain a fluorescent layer preform.
[0035] A light-gathering layer is formed on the surface of the second release film, and after drying, it is bonded to the third release substrate to obtain a light-gathering layer preform.
[0036] A white masking layer is formed on the surface of the third release film. After drying, a flame-retardant adhesive film layer is bonded to obtain a white masking layer preform.
[0037] S3. Provide a fourth release film and form a silver-gray composite adhesive layer on the surface of the fourth release film. Perform a first selective removal on the area where the silver-gray composite adhesive layer is located on the side of the silver-gray composite adhesive layer to form a first strip groove that is spaced apart along the width direction of the heat-bonding film. The first strip groove penetrates the silver-gray composite adhesive layer and extends to the fourth release film to form a receiving area for filling the fluorescent layer.
[0038] S4. After peeling off the first release film, the fluorescent layer preform is bonded together, and the fluorescent layer is filled into the first strip groove by hot pressing. After cooling, the second release substrate on the fluorescent layer preform is peeled off, and the excess fluorescent layer in the area outside the first strip groove is removed. Then, the fourth release substrate is bonded together.
[0039] S5. After curing, on the side of the fourth release substrate away from the fluorescent layer, a second selective removal is performed on the area where the fluorescent layer is located to form a second strip groove that is spaced apart along the width direction of the heat-bonding film. The second strip groove penetrates the fluorescent layer and extends to the fourth release film to form a receiving area for filling the light-gathering layer.
[0040] S6. After peeling off the second release film, the photoluminescent layer preform is bonded together, and the photoluminescent layer is filled into the second strip groove by hot pressing. After cooling, the third release substrate on the photoluminescent layer preform is peeled off, the excess photoluminescent layer in the area outside the second strip groove is removed, and the fourth release substrate is peeled off. After curing treatment, a functional layer in which the silver-gray composite adhesive layer, fluorescent layer and photoluminescent layer are periodically arranged along the width direction of the heat-bonded film is obtained.
[0041] S7. The white cover layer preform after peeling off the third release film is attached to the side of the functional layer away from the fourth release film to form a photoluminescent thermal adhesive film.
[0042] S8. Peel off the fourth release film on the phosphorescent fluorescent heat-adhesive film described in step S7, and bond it with the reflective substrate from which the first release substrate was peeled off in step S1 to obtain a composite phosphorescent reflective fluorescent heat-adhesive film.
[0043] Preferably, in step S1, the beaded adhesive layer is formed by extrusion casting.
[0044] Preferably, before embedding the glass microspheres into the bead adhesive layer in step S1, the bead adhesive layer needs to be baked to a molten state.
[0045] Preferably, in step S1, the focusing layer is formed by extrusion coating or scraping coating.
[0046] Preferably, the hot pressing in steps S4 and S6 is hot roller pressing, and the pressing temperature is 110℃~120℃.
[0047] Preferably, in the composite photoluminescent and reflective fluorescent heat-adhesive film obtained in step S8, the projected area of the metal reflective layer in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer is located, and does not overlap with the areas where the fluorescent layer and photoluminescent layer are located.
[0048] As described above, the composite photoluminescent and reflective fluorescent heat-adhesive film and its preparation method of the present invention have the following beneficial effects:
[0049] The heat-bonding film of this invention achieves physical isolation between fluorescence and light-gathering functions, effectively enhancing nighttime afterglow brightness and enriching daytime warning colors, while also possessing excellent washability and flame retardant properties. The fluorescent layer and the light-gathering layer are adjacent and parallel on the film surface without overlapping, avoiding the problems of reduced fluorescence brightness and shortened afterglow time caused by mutual interference in traditional mixed coating processes. Through selective vacuum evaporation, the metal reflective layer is distributed only in the area corresponding to the silver-gray composite adhesive layer. Although the areas containing the fluorescent and light-gathering layers retain the glass microsphere layer and focusing layer, the absence of a metal reflective layer prevents retroreflection of light, instead allowing it to be transmitted to the underlying fluorescent and light-gathering layers for laser emission. This achieves... The physical separation of the retroreflective luminescent area from the corresponding areas of the fluorescent and phosphorescent layers along the width of the film allows the heat-bonded film to simultaneously possess three optical functions: retroreflection, fluorescence color rendering, and phosphorescent afterglow. Each function operates independently, achieving high visibility in all weather conditions. The silver-gray composite adhesive layer, fluorescent layer, phosphorescent layer, and white cover layer all use washable resin as the matrix material, giving each functional layer excellent resistance to hydrolysis and detergent corrosion. At the same time, the fluorescent layer and phosphorescent layer are embedded in the strip-shaped grooves formed by the silver-gray composite adhesive layer, improving the interlayer bonding strength and effectively preventing detachment during long-term washing. This ensures that the heat-bonded film maintains stable optical performance and structural integrity even after multiple washes.
[0050] This invention employs a two-step selective removal and hot-pressing transfer filling process for the fluorescent layer preform and the phosphorescent layer preform. First, a first strip-shaped groove is formed to fill the fluorescent layer. Then, a second selective removal is performed within the fluorescent layer area to form a second strip-shaped groove to fill the phosphorescent layer. This achieves precise positioning of the fluorescent layer and the phosphorescent layer in the width direction, and the two are adjacent to each other without overlapping. Furthermore, this process can be completed using die-cutting or laser equipment, making it suitable for continuous industrial production. It has low manufacturing costs, simple processes, and high yield. Attached Figure Description
[0051] Figure 1 The diagram shown is a structural schematic corresponding to step S1 in Embodiment 1 of the present invention.
[0052] Figure 2a The diagram shows the structure of the fluorescent layer preform prepared in step S2 of Embodiment 1 of the present invention.
[0053] Figure 2b The diagram shows the structure of the photoluminescence layer preform prepared in step S2 of Embodiment 1 of the present invention.
[0054] Figure 2c The diagram shows the structure of the white cover layer preform prepared in step S2 of Embodiment 1 of the present invention.
[0055] Figure 3 The diagram shown is a structural schematic corresponding to step S3 in Embodiment 1 of the present invention.
[0056] Figure 4 The diagram shown is a structural schematic corresponding to step S4 in Embodiment 1 of the present invention.
[0057] Figure 5 The diagram shown is a structural schematic corresponding to step S5 in Embodiment 1 of the present invention.
[0058] Figure 6 The diagram shown is a structural schematic corresponding to step S6 in Embodiment 1 of the present invention.
[0059] Figure 7 The diagram shown is a structural schematic corresponding to step S7 in Embodiment 1 of the present invention.
[0060] Figure 8 The diagram shown is a structural schematic corresponding to step S8 in Embodiment 1 of the present invention.
[0061] Component designation explanation
[0062] 10 Reflective structural layer 101 Base film layer 102 beaded adhesive layer 103 Glass microspheres 104 Focusing layer 105 Metal reflective layer 20 Transparent adhesive layer 30 Silver-gray composite adhesive layer 40 First groove 401 Fluorescent layer 50 Second groove 501 Photoluminescence layer 60 White cover layer 70 Flame-retardant adhesive film layer 801 First release film 802 Second release film 803 Third release film 804 Fourth release film 901 First release substrate 902 Second release substrate 903 Third release substrate 904 Fourth release substrate Detailed Implementation
[0063] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0064] Before further describing specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terminology used in the embodiments of the present invention is for describing specific embodiments and not for limiting the scope of protection of the present invention. Test methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions or as recommended by the respective manufacturers.
[0065] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art. In addition to the specific methods, apparatus, and materials used in the embodiments, based on the knowledge of the prior art possessed by one of ordinary skill in the art and the description of this invention, any prior art methods, apparatus, and materials similar to or equivalent to those described, apparatus, and materials in the embodiments of this invention may be used to implement the present invention.
[0066] Please see Figure 1~,8. It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0067] Example 1
[0068] This embodiment provides a composite photoluminescent reflective heat-adhesive film, including a reflective structural layer 10, a transparent adhesive layer 20, a functional layer and a white cover layer 60 stacked in sequence, wherein a flame-retardant adhesive film layer 70 is disposed on the side of the white cover layer 60 away from the functional layer.
[0069] The reflective structural layer 10 includes a base film layer 101, a beaded adhesive layer 102, a glass microsphere layer 103, a focusing layer 104, and a metal reflective layer 105, which are stacked sequentially. The beaded adhesive layer 102 is formed on one side of the base film layer 101. The glass microsphere layer 103 includes a plurality of glass microspheres, which are partially embedded in and fixed by the beaded adhesive layer 102. The focusing layer 104 is disposed on the side of the glass microsphere layer 103 away from the base film layer 101. The metal reflective layer 105 is disposed on the side of the focusing layer 104 away from the glass microsphere layer 103 and is spaced apart along the width direction of the heat-bonded film.
[0070] The transparent adhesive layer 20 is disposed on the side of the reflective structural layer 10 away from the base film layer 101, and is used to connect the reflective structural layer 10 and the functional layer;
[0071] The functional layer includes a silver-gray composite adhesive layer 30, a fluorescent layer 401, and a light-gathering layer 501 arranged periodically along the width direction of the heat-adhesive film. The fluorescent layer 401 and the light-gathering layer 501 are embedded in the silver-gray composite adhesive layer 30, and the fluorescent layer 401 and the light-gathering layer 501 are adjacent to each other without overlapping. The projection area of the metal reflective layer 105 in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer 30 is located, and does not coincide with the area where the fluorescent layer 401 and the light-gathering layer 501 are located.
[0072] The white cover layer 60 is disposed on the side of the functional layer away from the transparent adhesive layer 20.
[0073] For details, please refer to Figure 8This is a schematic diagram of the composite heat-bonding film. The fluorescent layer 401 and the light-gathering layer 501 are adjacent to each other in the film plane and do not overlap, avoiding the problems of reduced fluorescence brightness and shortened afterglow time caused by mutual interference between the two in the traditional mixed coating process. Through selective vacuum evaporation, the metal reflective layer 105 is distributed only in the area corresponding to the silver-gray composite adhesive layer 30. Although the glass microsphere layer 103 and the focusing layer 104 are retained in the area where the fluorescent layer 401 and the light-gathering layer 501 are located, the light will not be retroreflected because there is no metal reflective layer 105. Instead, the light will be transmitted to the fluorescent layer 401 and the light-gathering layer below. 501 laser emission; this achieves physical separation of the retroreflective luminescent area from the corresponding areas of the fluorescent layer 401 and the phosphorescent layer 501 in the width direction of the film surface, enabling the heat-bonded film to simultaneously possess three optical functions: retroreflection (high-brightness reflection under nighttime vehicle headlight illumination), fluorescent color rendering (vibrant colors under sunlight or ultraviolet light), and phosphorescent afterglow (afterglow indication in dark environments), with each function operating independently to achieve high visibility in all weather conditions. Viewed from the front, the heat-bonded film displays a variety of warning colors during the day, with silver-gray, fluorescent, and phosphorescent colors alternating periodically in the width direction of the film surface. Furthermore, the fluorescent layer 401 and the phosphorescent layer 501 are embedded within the strip-shaped groove formed by the silver-gray composite adhesive layer 30, with their upper surfaces flush. This eliminates the need for additional layer thickness, resulting in a thinner overall thickness, improved interlayer bonding strength, and effective prevention of detachment during long-term washing. This ensures that the heat-bonded film maintains stable optical performance and structural integrity even after multiple washes.
[0074] As an example, the silver-gray composite adhesive layer 30 is provided with first strip-shaped grooves 40 spaced apart along the width direction of the film surface, and the fluorescent layer 401 is disposed in the first strip-shaped grooves 40; and the fluorescent layer 401 is provided with second strip-shaped grooves 50 spaced apart along the width direction of the film surface, and the phosphorescent layer 501 is disposed in the second strip-shaped grooves 50.
[0075] Specifically, the fluorescent layer 401 is embedded in the first strip-shaped groove 40 penetrating the silver-gray composite adhesive layer 30, and the light-gathering layer 501 is embedded in the second strip-shaped groove 50 penetrating the fluorescent layer 401. The fluorescent layer 401 and the light-gathering layer 501 are adjacent to each other but do not overlap, avoiding the problem of reduced fluorescence brightness and shortened afterglow time caused by mutual interference. The projection area of the metal reflective layer 105 in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer 30 is located, so that the silver-gray composite adhesive layer 30 forms a reflective functional area with its corresponding light-emitting structure layer in the width direction of the film surface. The reflective structure layer 10 corresponding to the fluorescent layer 401 in the width direction of the film surface does not include... The metal reflective layer 105 retains the glass microsphere layer 103 and the focusing layer 104. Because there is no metal reflective layer 105, the light will not be retroreflected, but will be transmitted to the lower fluorescent layer 401 to excite light emission and form a fluorescent light emission area. Similarly, the reflective structure layer 10 corresponding to the light-gathering layer 501 also does not have a metal reflective layer 105. The light-gathering layer 501 forms a light-gathering area on the width of the film surface. The reflective functional area, the fluorescent light emission area, and the light-gathering area are physically separated in the width direction of the film surface. The three functions work independently and do not interfere with each other. That is, the silver-gray composite adhesive layer 30, the fluorescent layer 401, and the light-gathering layer 501 respectively form strip-shaped functional areas extending along the length direction of the heat-bonded film.
[0076] In a specific embodiment of the present invention, after the ambient light is refracted by the glass microspheres and focused by the focusing layer 104, the energy density is increased, which can more efficiently excite the fluorescent layer 401 and the light-gathering layer 501. From the direction of the heat-bonded film surface, the heat-bonded film presents a color of silver-gray, fluorescent color and light-gathering color arranged periodically. Of course, in other embodiments, the arrangement of the three colors can be switched arbitrarily, and no restrictions are imposed here.
[0077] As an example, the material of the beaded adhesive layer 102 includes one of PP (polypropylene), PE (polyethylene), EVA (ethylene-vinyl acetate copolymer), EBA (ethylene-butyl acrylate copolymer), and EAA (ethylene-acrylic acid copolymer), as well as a mixture with an opening agent. Specifically, the base film layer 101, as the outermost basic support structure of the heat-bonding film, has the core function of providing a stable adhesion substrate for subsequent beaded adhesive layers 102, glass microsphere layers 103, etc., ensuring the morphological integrity of each layer during processing and use. Simultaneously, the base film layer 101 can resist minor friction and dust contamination from the external environment, preventing premature damage to the inner functional layers and improving the overall structural stability of the heat-bonding film. In a specific embodiment of the present invention, the material of the base film layer 101 is selected from at least one of PET, PB, BOPP, nylon, and super-pressure paper.
[0078] The bead adhesive layer 102 is made of thermoplastic resin, possessing good thermal flowability and extrusion molding properties. It can be efficiently formed into a uniform bead adhesive layer 102 through extrusion casting processes. The bead adhesive layer 102 can firmly encapsulate the glass microspheres in the molten state, ensuring the adhesion between the glass microspheres and the base film layer 101. In a specific embodiment of the invention, some glass microspheres are embedded in the bead adhesive layer, while others are exposed, ensuring unobstructed light reflection paths and preventing light obstruction due to excessive thickness of the bead adhesive layer 102. The addition of an opening agent to the bead adhesive layer 102 prevents interlayer adhesion during processing or storage, while not affecting the adhesion between the bead adhesive layer and the base film layer 101 and the glass microspheres. This ensures that the bead adhesive layer can completely encapsulate the glass microspheres during subsequent molten bead implantation, reducing the processing scrap rate.
[0079] The bead adhesive layer 102 has a melting point below 150℃, allowing it to reach a molten state under gentle heating conditions. At this point, the adhesive layer has moderate fluidity, which allows it to fully coat the surface of the glass microspheres to form a strong bond, without causing the adhesive layer to overflow or cover too many glass microspheres due to excessive fluidity. Simultaneously, it avoids thermal aging, deformation, or damage to the base film layer 101 caused by high temperatures, ensuring the structural integrity of the base film layer 101.
[0080] As an example, the thickness of the bead adhesive layer 102 is 25% to 35% of the diameter of the glass microspheres.
[0081] Specifically, the thickness of the bead adhesive layer 102 is any value within a range such as 25%, 28%, 30%, 32%, or 35% of the diameter of the glass microspheres. This ensures that external light can directly enter the glass microspheres, be refracted internally, and then transmitted to the metal reflective layer 105. This avoids a decrease in reflectivity due to excessive thickness of the bead adhesive layer 102 blocking light. This thickness is sufficient to form a stable adhesive support at the bottom of the glass microspheres, preventing the glass microspheres from loosening or falling off due to water flow impact and rubbing during washing.
[0082] As an example, the glass microspheres have a diameter of 45 μm to 95 μm and a refractive index of 1.9 to 1.95.
[0083] Specifically, the diameter of the glass microspheres can be any value within the range of 45μm, 50μm, 60μm, 70μm, 80μm, 90μm, 95μm, etc. If the diameter of the glass microspheres is too small, it can easily lead to uneven dispersion and difficulty in precise positioning during implantation; if it is too large, it can easily cause large differences in interlayer thickness and uneven coating of the subsequent focusing layer 104. In this specific embodiment of the invention, the range of 45μm to 95μm ensures that the glass microspheres are uniformly implanted into the implantation adhesive layer 102 and form a suitable interlayer structure with the subsequent focusing layer 104, avoiding interlayer gaps or protrusions. The refractive index of the glass microspheres can be any value within the range of 1.9, 1.91, 1.92, 1.93, 1.94, 1.95, etc., and can be adjusted according to actual conditions. The refractive index of the glass microspheres is in the high refractive index range, which allows the incident light to undergo total internal reflection inside the glass microspheres and be precisely guided to the metal reflective layer 105 before being reflected back to the light source.
[0084] As an example, the material of the focusing layer 104 includes one or a combination of polyurethane, polyester, and epoxy-modified acrylic resin, and the thickness of the focusing layer 104 is 5μm to 20μm.
[0085] Specifically, the focusing layer 104 can focus external incident light onto the glass microsphere layer, concentrate the incident light onto the metal reflective layer 105 behind it, and then reflect it back to the light source direction by the metal reflective layer 105, forming a high-brightness retroreflection; the material of the focusing layer 104 is a resin that is resistant to organic solvents and has good light transmittance, including one or more of polyurethane, polyester, and epoxy modified acrylic resin, and its thickness can be any value in the range of 5μm, 10μm, 15μm, 20μm, etc.
[0086] As an example, the material of the metal reflective layer 105 includes at least one of aluminum, silver, and chromium.
[0087] Specifically, the metal reflective layer 105 is distributed at intervals along the width of the heat-adhesive film and is only set in the area where the silver-gray composite adhesive layer 30 is located. It forms a reflective functional area with the corresponding glass microsphere layer 103 and focusing layer 104 to enhance light reflection and further improve the nighttime reflective warning intensity.
[0088] As an example, the thickness of the transparent adhesive layer is 10μm~20μm.
[0089] Specifically, the transparent adhesive layer is transparent and its material is similar to that of the silver-gray composite adhesive layer 30, but it does not contain any pigments; its thickness can be any value in the range of 10μm, 12μm, 14μm, 16μm, 18μm, 20μm, etc.
[0090] As an example, the thickness of the silver-gray composite adhesive layer 30 is 30μm~70μm.
[0091] As an example, the material of the silver-gray composite adhesive layer 30 includes one or a combination of epoxy resin, polyurethane, and modified acrylic resin, as well as a mixture with silver-gray pigment, flame retardant, and crosslinking agent.
[0092] Specifically, the thickness of the silver-gray composite adhesive layer 30 can be any value within a range such as 30μm, 40μm, 50μm, 60μm, and 70μm, and can be selected according to actual needs. The material of the silver-gray composite adhesive layer 30 is a mixture of washable resin, silver-gray pigment, flame retardant, and crosslinking agent in a certain proportion, achieving a combination of high water resistance, flame retardancy, and high temperature resistance, capable of withstanding high temperatures of 200~300℃ without deformation; wherein, the washable resin is selected from at least one of epoxy resin, polyurethane, and modified acrylic resin.
[0093] As an example, the thickness of the fluorescent layer 401 is 30 μm to 80 μm.
[0094] Specifically, the thickness of the fluorescent layer 401 can be any value within the range of 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, etc.; taking into account both high daytime warning color rendering and structural stability, ensuring the color saturation and uniformity of the fluorescent pigment through sufficient thickness to form a strong visual warning effect, while avoiding problems such as reduced flexibility and interlayer cracking caused by excessive thickness.
[0095] As an example, the material of the fluorescent layer 401 includes one or a combination of EVA (ethylene-vinyl acetate copolymer), polyolefin, and polyurethane, as well as a mixture with fluorescent pigment, flame retardant, and crosslinking agent, wherein the fluorescent pigment includes one or a combination of yellow, orange, and red.
[0096] Specifically, EVA (ethylene-vinyl acetate copolymer), polyolefins, and polyurethane are all wash-resistant resins that can resist the chemical erosion of detergents during washing, preventing the resin from dissolving or cracking due to chemical action. The crosslinking agent enables the resin molecules to form a three-dimensional network structure, significantly enhancing the adhesion of the fluorescent layer 401 in the first groove 40 and preventing the fluorescent pigment from falling off due to water flow impact and rubbing. The fluorescent layer 401 is made of wash-resistant resin, fluorescent pigment, flame retardant, and crosslinking agent mixed in a certain proportion, achieving both high wash resistance and flame retardancy, and can be processed at 110~120℃. However, there are no excessive restrictions on the proportions of the ingredients or the types of flame retardants and crosslinking agents used. The fluorescent pigment is at least one of yellow, orange, or red. Yellow, orange, and red are all internationally recognized high-warning colors with strong visual impact, allowing them to be quickly identified by observers in complex outdoor environments.
[0097] As an example, the thickness of the photoluminescence layer 501 is 30μm to 80μm.
[0098] As an example, the material of the photoluminescent layer 501 includes one or a combination of EVA, polyolefin, and polyurethane, as well as a mixture with photoluminescent powder, flame retardant, and crosslinking agent.
[0099] Specifically, the photoluminescent powder in the photoluminescent layer 501 absorbs light during the day and releases light in the dark. The thickness of the photoluminescent layer 501 can be any value within the range of 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, etc. The material of the photoluminescent layer 501 is a mixture of washable hot melt resin, photoluminescent powder, flame retardant and crosslinking agent in a certain proportion to achieve high water resistance, flame retardancy and processing at 110~120℃. However, the ratio between the ingredients is not overly restricted here, as long as the photoluminescent powder is stably dispersed. In addition, the flame retardant provides flame retardant properties, and the crosslinking agent strengthens the crosslinking structure of the resin, improving mechanical strength and washability. The specific types of the two are not overly restricted here.
[0100] As an example, the thickness of the white covering layer 60 is 30μm~70μm.
[0101] Specifically, the white cover layer 60 mainly covers the color of the underlying adhesive layer, ensures the purity of the color in the light-emitting area, improves the display effect of the phosphor layer 401 and the light-gathering layer 501, improves optical contrast, and provides protection for the functional layer. The thickness of the white cover layer 60 can be any value in any range, such as 30μm, 40μm, 50μm, 60μm, or 70μm.
[0102] As an example, the white covering layer 60 includes one or a combination of epoxy resin, polyurethane, and modified acrylic resin, as well as a mixture with white pigment, flame retardant, and crosslinking agent.
[0103] Specifically, the gray composite adhesive layer, fluorescent layer 401, phosphorescent layer 501, and white opacifying layer 60 all use washable resin as the matrix material, giving each functional layer excellent resistance to hydrolysis and detergent corrosion. Flame retardants and crosslinking agents are also added to the materials of each functional layer. The specific types of flame retardants and crosslinking agents are not specifically limited here, as long as they can give each functional layer strong adhesion, washability, and flame retardant properties.
[0104] As an example, the base layer of the flame-retardant adhesive film layer 70 is selected from one of TPU (thermoplastic polyurethane), PU (polyurethane), PES (polyester), and PVC (polyvinyl chloride), and the thickness of the base layer is 30-150 μm.
[0105] Specifically, the base material of the flame-retardant adhesive film layer 70 has excellent flexibility and adhesion, strong weather resistance and washability. The base thickness balances the support strength and flexibility. The thickness of the base can be any value in any range, such as 30μm, 50μm, 80μm, 100μm, 120μm, 150μm.
[0106] Furthermore, each functional layer and the flame-retardant adhesive film layer 70 have flame-retardant properties, meeting the requirements of the safety protection field. At the same time, the use of a hot melt system reduces the use of solvents, making it more environmentally friendly. This heat-bonded film can be widely used for safety markings and decorations on the surfaces of work clothes, fire suits, traffic warning clothing, outdoor equipment, and other textile, plastic, and metal substrates.
[0107] This embodiment also provides a method for preparing the above-mentioned composite photoluminescent and reflective fluorescent heat-adhesive film. The above-mentioned composite photoluminescent and reflective fluorescent heat-adhesive film can be prepared using this method, which includes the following steps:
[0108] S1. A beaded adhesive layer 102 is formed on the surface of the base film layer 101. Glass microspheres are partially embedded in the beaded adhesive layer 102 to form a glass microsphere layer 103. A focusing layer 104 is formed on the side of the glass microsphere layer 103 away from the beaded adhesive layer 102. Selective vacuum evaporation is performed on the side of the focusing layer 104 away from the glass microsphere layer 103 to form a metal reflective layer 105 spaced apart along the width direction of the film surface, resulting in a reflective structure layer 10. Subsequently, a transparent adhesive layer 20 is formed on the side of the reflective structure layer 10 away from the base film layer 101, and a first release substrate 901 is bonded to form a reflective substrate.
[0109] S2. Pre-fabricate the fluorescent layer 401, the phosphorescent layer 501, and the white opaque layer 60 respectively:
[0110] A fluorescent layer 401 is formed on the surface of the first release film 801, and after drying, it is bonded to the second release substrate 902 to obtain a fluorescent layer preform.
[0111] A light-gathering layer 501 is formed on the surface of the second release film 802, and after drying, it is bonded to the third release substrate 903 to obtain a light-gathering layer preform.
[0112] A white masking layer 60 is formed on the surface of the third release film 803, and after drying, a flame-retardant adhesive film layer 70 is bonded to obtain a white masking layer preform.
[0113] S3. Provide a fourth release film 804 and form a silver-gray composite adhesive layer 30 on the surface of the fourth release film 804. Perform a first selective removal on the area where the silver-gray composite adhesive layer 30 is located on the side of the silver-gray composite adhesive layer 30 to form a first strip groove 40 spaced apart along the width direction of the heat-adhesive film. The first strip groove 40 penetrates the silver-gray composite adhesive layer 30 and extends to the fourth release film 804 to form a receiving area for filling the fluorescent layer 401.
[0114] S4. After peeling off the first release film 801, the fluorescent layer preform is bonded together, and the fluorescent layer 401 is filled into the first strip groove 40 by hot pressing. After cooling, the second release substrate 902 on the fluorescent layer preform is peeled off, and the excess fluorescent layer 401 located outside the first strip groove 40 is removed. Then, the fourth release substrate 904 is bonded together.
[0115] S5. After curing, on the side of the fourth release substrate 904 away from the fluorescent layer 401, a second selective removal is performed on the area where the fluorescent layer 401 is located to form a second strip groove 50 spaced apart along the width direction of the heat-bonded film. The second strip groove 50 penetrates the fluorescent layer 401 and extends to the fourth release film 804 to form a receiving area for filling the light-gathering layer 501.
[0116] S6. After peeling off the second release film 802, the photoluminescent layer preform is bonded together, and the photoluminescent layer 501 is filled into the second strip groove 50 by hot pressing. After cooling, the third release substrate 903 on the photoluminescent layer preform is peeled off, the excess photoluminescent layer 501 in the area outside the second strip groove 50 is removed, and the fourth release substrate 904 is peeled off. After curing treatment, a functional layer in which the silver-gray composite adhesive layer 30, the fluorescent layer 401 and the photoluminescent layer 501 are periodically arranged along the width direction of the heat-bonded film is obtained.
[0117] S7. The white cover layer preform after peeling off the third release film 803 is attached to the side of the functional layer away from the fourth release film 804 to form a photoluminescent thermal adhesive film.
[0118] S8. Peel off the fourth release film 804 from the phosphorescent fluorescent heat-adhesive film in step S7, and bond it with the reflective substrate from which the first release substrate 901 was peeled off in step S1 to obtain a composite phosphorescent reflective fluorescent heat-adhesive film.
[0119] The preparation method of the composite photoluminescent reflective fluorescent heat-adhesive film of this embodiment will be described in detail below with reference to the specific accompanying drawings.
[0120] First, refer to Figure 1In step S1, a beaded adhesive layer 102 is formed on the surface of the base film layer 101. Glass microspheres are partially embedded in the beaded adhesive layer 102 to form a glass microsphere layer 103. A focusing layer 104 is formed on the side of the glass microsphere layer 103 away from the beaded adhesive layer 102. Selective vacuum evaporation is performed on the side of the focusing layer 104 away from the glass microsphere layer 103 to form a metal reflective layer 105 spaced apart along the width direction of the film surface, resulting in a reflective structure layer 10. Subsequently, a transparent adhesive layer 20 is formed on the side of the reflective structure layer 10 away from the base film layer 101, and a first release substrate 901 is bonded to form a reflective substrate.
[0121] As an example, in step S1, the beaded adhesive layer 102 is formed by extrusion casting.
[0122] Specifically, the base film layer 101 provides support, enabling the entire film to maintain strength and dimensional stability. The beaded adhesive layer 102 is made of thermoplastic resin, which has good thermal flowability and extrusion molding properties, and can be efficiently formed into a uniform beaded adhesive layer 102 through extrusion casting process.
[0123] As an example, before embedding the glass microspheres into the bead adhesive layer 102 in step S1, the bead adhesive layer 102 needs to be baked until it is in a molten state.
[0124] As an example, in step S1, the focusing layer 104 is formed by extrusion coating or scraping coating.
[0125] Specifically, a bead-coating layer 102 is first fabricated on the base film layer 101. The bead-coating layer 102 is baked until it is molten, and then beads are implanted. Glass microspheres are embedded in the bead-coating layer 102. A focusing layer 104 is then formed by extrusion or scraping. After curing to stabilize the structure, a metal reflective layer 105 is formed by selective evaporation through vacuum evaporation, resulting in a reflective structural layer 10. Next, a transparent adhesive layer 20 is formed on the reflective structural layer 10, and a first release substrate 901 is attached to it. The first release substrate 901 mainly serves a protective function; during subsequent construction, the first release substrate 901 can be removed, and the material can be directly adhered through the transparent adhesive layer 20.
[0126] Specifically, the film forming the beaded adhesive layer 102 is placed in a heating device to soften it and give it a certain degree of fluidity. Then, glass microspheres are placed on the surface of the beaded adhesive layer 102, and the glass microspheres will partially sink into the adhesive layer. After cooling, the glass microspheres are fixed to form a glass microsphere layer 103. After the glass microspheres are fixed, a focusing layer 104 is coated on one side of the glass microspheres to adjust the light propagation particle size, so that the light entering the glass microspheres can more effectively return to the light source direction and improve the reflective brightness. The focusing layer 103 is now complete. 4. After coating, the film is dried and cooled in an oven to remove surface dust and then rolled up. The rolled-up product is then cured, which means that the film after the beading and focusing layer 104 processing is cured for a certain period of time to fully solidify the adhesive layer and each layer, release internal stress, and improve the reliability of subsequent coating and bonding. After curing, the next step of processing the metal reflective layer 105 is carried out. A layer of reflective metal is selectively deposited on the focusing layer 104 side using vacuum evaporation to form an intermittently distributed metal reflective layer 105 to enhance light reflection.
[0127] Next, refer to Figure 2a , Figure 2b , Figure 2c In step S2, a fluorescent layer 401, a phosphorescent layer 501, and a white masking layer 60 are prefabricated respectively.
[0128] See Figure 2a A fluorescent layer 401 is formed on the surface of the first release film 801. After the fluorescent layer 401 dries and cures, a second release substrate 902 is attached to the side of the fluorescent layer 401 away from the first release film 801 to obtain a fluorescent layer preform.
[0129] See Figure 2b A light-gathering layer 501 is formed on the surface of the second release film 802. After the light-gathering layer 501 dries and cures, a third release substrate 903 is attached to the side of the light-gathering layer 501 away from the second release film 802 to obtain a light-gathering layer preform.
[0130] See Figure 2c A white masking layer 60 is formed on the surface of the third release film 803. After the white masking layer 60 dries and cures, a flame-retardant adhesive film layer 70 is attached to the side of the white masking layer 60 away from the third release film 803 to obtain a white masking layer preform.
[0131] Specifically, fluorescent layer preforms, phosphorescent layer preforms, and white opacifying layer preforms with independent structures are prepared using the above methods, so that each functional layer can be filled into the corresponding area by hot pressing transfer.
[0132] Next, refer to Figure 3In step S3, a fourth release film 804 is provided, and a silver-gray composite adhesive layer 30 is formed on the surface of the fourth release film 804. A first selective removal is performed on the area where the silver-gray composite adhesive layer 30 is located on the side of the silver-gray composite adhesive layer 30 to form a first strip groove 40 spaced apart along the width direction of the heat-bonded film. The first strip groove 40 penetrates the silver-gray composite adhesive layer 30 and extends to the fourth release film 804 to form a receiving area for filling the fluorescent layer 401.
[0133] Specifically, the film to be processed is placed in the processing equipment and processed from the side of the silver-gray composite adhesive layer 30. The silver-gray composite adhesive layer 30 is processed using a die-cutting device or a laser device to remove the silver-gray composite adhesive layer 30, thereby forming the first strip-shaped grooves 40 spaced apart along the width direction of the heat-bonded film. The depth of the first strip-shaped grooves 40 extends to the fourth release film 804, forming the filling space of the subsequent fluorescent layer 401.
[0134] Next, refer to Figure 4 In step S4, the fluorescent layer preform after peeling off the first release film 801 is bonded together, and the fluorescent layer 401 is filled into the first strip groove 40 by hot pressing. After cooling, the second release substrate 902 on the fluorescent layer preform is peeled off, and the excess fluorescent layer 401 located outside the first strip groove 40 is removed. Then, the fourth release substrate 904 is bonded together.
[0135] Specifically, this step involves precisely transferring and filling the pre-fabricated fluorescent layer 401 into the first strip groove 40, while removing excess fluorescent material from non-target areas to form an independently embedded fluorescent layer 401.
[0136] The fluorescent layer preform consists of a first release film 801, a fluorescent layer 401, and a second release substrate 902. First, the first release film 801 is peeled off to expose the fluorescent layer 401. The exposed fluorescent layer 401 is then bonded to a heat-bonding film with a first strip-shaped groove 40. Heat and pressure are applied via hot pressing, causing the resin in the fluorescent layer 401 to soften and flow under pressure into the first strip-shaped groove 40. After cooling, the resin solidifies, fixing the fluorescent layer 401 inside the first strip-shaped groove 40. Next, the second release substrate 902 is peeled off, removing excess fluorescent layer 401 located outside the first strip-shaped groove 40. Finally, a protective treatment is performed, and a fourth release substrate 904 is bonded to form an intermediate product with an embedded fluorescent layer 401. (See [reference]). Figure 4 .
[0137] As an example, the hot pressing in step S4 is hot roller pressing, and the pressing temperature is 110℃~120℃.
[0138] Specifically, hot rollers are used for high-temperature pressing, and the pressing temperature can be any value within the range of 110℃, 112℃, 114℃, 116℃, 118℃, 120℃, etc.
[0139] Next, refer to Figure 5 In step S5, after curing, a second selective removal is performed on the side of the fourth release substrate 904 away from the fluorescent layer 401, to form a second strip groove 50 spaced apart along the width direction of the heat-bonded film. The second strip groove 50 penetrates the fluorescent layer 401 and extends to the fourth release film 804 to form a receiving area for filling the light-gathering layer 501.
[0140] Specifically, this step involves placing the cured film with an independent fluorescent region in a processing device and processing it from one side of the fourth release substrate 904. A second selective removal of the fluorescent layer 401 is performed using a die-cutting device or a laser device to form a second strip-shaped groove 50 for filling the phosphorescent layer 501, thereby achieving the parallel arrangement of the fluorescent layer 401 and the phosphorescent layer 501.
[0141] Curing refers to the process by which freshly processed materials gradually become stable. This involves placing the material for a certain period of time or storing it at a specific temperature to allow its properties to gradually stabilize. In step S4, the fluorescent layer 401 after hot-pressing transfer needs to undergo curing treatment to further solidify the resin system in the fluorescent layer 401, allowing the fluorescent layer 401 to achieve a stable bond with the surrounding structure.
[0142] The second selective removal mainly targets the already formed fluorescent layer 401 region. A second strip-shaped groove 50 is formed inside the fluorescent layer 401. The second strip-shaped groove 50 is arranged at intervals along the width direction of the heat-bonded film. The second strip-shaped groove 50 penetrates the fluorescent layer 401 and extends to the fourth release film 804. The second strip-shaped groove 50 is used for subsequent filling of the light-gathering layer 501, so that the fluorescent layer 401 and the light-gathering layer 501 form an adjacent but non-overlapping structure in the film surface, avoiding mutual interference between the fluorescent material and the light-gathering material, and realizing the independent performance of fluorescence and light-gathering functions.
[0143] Next, refer to Figure 6 In step S6, the photoluminescent layer preform after peeling off the second release film 802 is bonded together, and the photoluminescent layer 501 is filled into the second strip groove 50 by hot pressing. After cooling, the third release substrate 903 on the photoluminescent layer preform is peeled off, the excess photoluminescent layer 501 in the area outside the second strip groove 50 is removed, and the fourth release substrate 904 is peeled off. After curing treatment, a functional layer in which the silver-gray composite adhesive layer 30, the fluorescent layer 401 and the photoluminescent layer 501 are periodically arranged along the width direction of the heat-bonded film is obtained.
[0144] For details, see Figure 6 This step involves precisely transferring and filling the pre-fabricated light-gathering layer 501 into the second strip groove 50, while removing the light-gathering material from non-target areas to form an independent embedded light-gathering functional area. The photoluminescent layer preform consists of a second release film 802, a photoluminescent layer 501, and a third release substrate 903. First, the second release film 802 is peeled off to expose the photoluminescent layer 501. The exposed photoluminescent layer 501 is then bonded to the heat-bonded film structure with the second strip groove 50 already formed. Heat and pressure are provided by hot pressing, and the resin in the photoluminescent layer 501 softens under heat, flows under pressure, and fills into the second strip groove 50. After cooling, it solidifies, so that the photoluminescent layer 501 is stably embedded in the second strip groove 50. Then, the third release substrate 903 is peeled off to remove the photoluminescent layer 501 located in the area outside the second strip groove 50. Subsequently, the fourth release substrate 904 is peeled off, thereby forming a functional layer in which the silver-gray composite adhesive layer 30, the fluorescent layer 401, and the photoluminescent layer 501 are periodically arranged along the width direction of the heat-bonded film.
[0145] As an example, the hot pressing in step S6 is hot roller pressing, and the pressing temperature is 110℃~120℃ (110℃, 112℃, 114℃, 116℃, 118℃, 120℃, etc.).
[0146] Next, refer to Figure 7 In step S7, the white cover layer preform after peeling off the third release film 803 is attached to the side of the functional layer away from the fourth release film 804 to form a photoluminescent thermal adhesive film.
[0147] Specifically, this step is mainly used to form the white cover layer 60 and to complete the protection and stabilization treatment of each functional area. The white cover layer preform consists of a third release film 803, the white cover layer 60, and a flame-retardant adhesive film layer 70. First, the third release film 803 is peeled off, and the exposed white cover layer 60 is bonded to the formed functional layer. The main functions of the white cover layer 60 are to cover the underlying color, improve the display effect of the fluorescent layer 401 and the phosphorescent layer 501, improve optical contrast, and provide protection for the functional layer. After bonding, it is cured again to ensure that the white cover layer 60 is firmly bonded to the functional layer, improve the overall washability, and form a stable heat-bonded film structure.
[0148] Finally, see Figure 8In step S8, the fourth release film 804 on the phosphorescent fluorescent heat-sensitive film described in step S7 is peeled off and bonded to the reflective substrate from which the first release substrate 901 was peeled off in step S1, resulting in a composite phosphorescent reflective fluorescent heat-sensitive film. As an example, in the composite phosphorescent reflective fluorescent heat-sensitive film obtained in step S8, the projected area of the metal reflective layer 105 in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer 30 is located, and does not overlap with the areas where the fluorescent layer 401 and the phosphorescent layer 501 are located.
[0149] Specifically, this step involves combining the photoluminescent heat-bonded film formed in step S7 with the reflective substrate formed in step S1. After the first release substrate 901 is peeled off from the reflective substrate in step S1, a transparent adhesive layer 20 is exposed. The transparent adhesive layer 20 is used to connect the reflective structural layer 10 and the functional layer. At the same time, it ensures that the projection area of the metal reflective layer 105 in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer 30 is located, and does not overlap with the areas where the fluorescent layer 401 and the photoluminescent layer 501 are located. This achieves physical separation of the retroreflective luminescent area from the fluorescent layer 401 and the photoluminescent layer 501 in the width direction of the film surface, so that the heat-bonded film has three optical functions at the same time: retroreflection, fluorescence color rendering, and photoluminescence afterglow. Each function works independently, achieving high visibility in all weather conditions.
[0150] Comparative Example 1
[0151] This comparative example provides a photoluminescent and reflective fluorescent heat-adhesive film, which is prepared using a traditional manufacturing process. Specifically, an adhesive mixed with fluorescent pigments and photoluminescent powder is directly coated onto the back of an anodized aluminum film. After drying and curing, a white cover layer 60 and a flame-retardant adhesive film layer 70 are then laminated to obtain the photoluminescent and reflective fluorescent heat-adhesive film.
[0152] The heat-adhesive films in Example 1 and Comparative Example 1 were subjected to the following tests:
[0153] 1. Washability: Using ISO 6330: Textiles - Household washing and drying procedures for testing textiles, garments with heat-adhesive films were washed 25 and 50 times, and the retroreflective coefficient and appearance of the heat-adhesive film were measured. Using ISO 15797: Textiles - Industrial washing and finishing procedures for testing work clothes, work clothes with heat-adhesive films were washed 25 times, and the retroreflective coefficient and appearance of the heat-adhesive film after 25 washes were measured. The test results are shown in Table 1.
[0154] 2. Photoluminescence performance: The photoluminescence performance of the heat-bonded film was tested using DIN 67510-1:2020-05 "Long afterglow pigments and products - Part 1: Manufacturer's measurement and marking". The characteristics of the afterglow brightness (luminous intensity) of the heat-bonded film in a dark environment after being excited by light were evaluated. The test results are shown in Table 2.
[0155] Table 1. Test results of the washability of the heat-bonded films in Example 1 and Comparative Example 1
[0156]
[0157] The results in Table 1 show that before washing, the heat-adhesive films of Example 1 and Comparative Example 1 have similar retroreflective properties. According to ISO 6330 standards, after 25 and 50 washes, the retroreflective coefficient of Example 1 is significantly higher than that of Comparative Example 1, especially after 50 household washes, Example 1 still maintains 273 cd·lx. -1 ·m -2 The retroreflection coefficient of Comparative Example 1 is only 56 cd·lx. -1 ·m -2 The results no longer meet the standard requirements. According to ISO 15797 standard, after 25 washes, the retroreflection coefficient retention rate of Example 1 is significantly higher than that of Comparative Example 1. Furthermore, under both standards, Example 1 showed intact surface structure after washing, with no obvious cracking or light transmission, indicating that the present invention, through its functional layer embedded structure and washable composite system, improves the structural stability and optical performance retention of the heat-adhesive film during long-term use.
[0158] Table 2. Photoluminescence performance test results of the heat-bonded films in Example 1 and Comparative Example 1
[0159]
[0160] The minimum afterglow value (Grade B) in Table 2 represents the minimum brightness value that the photoluminescent material should achieve at a specific time point to meet the Grade B standard for long afterglow performance. That is, after excitation by specified light, the brightness should be ≥210 mcd / m² at 2 minutes. 2 The brightness should be ≥50 mcd / m² after 10 minutes. 2 The brightness should be ≥15mcd / m² after 30 minutes. 2 The brightness should be ≥7mcd / m² after 60 minutes. 2 The light-storing performance in Comparative Example 1 does not meet the requirements. The afterglow brightness of the heat-bonded film in Example 1 is higher than the minimum afterglow value. Compared with Comparative Example 1, which does not increase the thickness of the light-storing layer 501 and the proportion of light-storing powder, it has a higher afterglow retention capability. This shows that the present invention reduces optical interference and effectively improves the light-storing performance of the heat-bonded film by independently setting the fluorescent layer 401 and the light-storing layer 501.
[0161] In summary, the heat-bonding film of this invention achieves physical isolation between fluorescence and light-gathering functions, effectively enhancing nighttime afterglow brightness and enriching daytime warning colors, while also possessing excellent washability and flame retardant properties. The fluorescent layer and the light-gathering layer are adjacent and parallel on the film surface without overlapping, avoiding the problems of reduced fluorescence brightness and shortened afterglow time caused by mutual interference in traditional mixed coating processes. Through selective vacuum evaporation, the metal reflective layer is distributed only in the area corresponding to the silver-gray composite adhesive layer. While the areas containing the fluorescent and light-gathering layers retain the glass microsphere layer and focusing layer, the absence of a metal reflective layer prevents retroreflection of light, instead allowing it to be transmitted to the underlying fluorescent and light-gathering layers for laser emission. This achieves physical separation of the retroreflective luminescent area from the corresponding areas of the fluorescent and phosphorescent layers along the width of the film, enabling the heat-bonded film to simultaneously possess three optical functions: retroreflection, fluorescence color rendering, and phosphorescent afterglow. Each function operates independently, achieving high visibility in all weather conditions. The silver-gray composite adhesive layer, fluorescent layer, phosphorescent layer, and white cover layer all use washable resin as the matrix material, giving each functional layer excellent resistance to hydrolysis and detergent corrosion. At the same time, the fluorescent layer and phosphorescent layer are embedded in the strip-shaped grooves formed by the silver-gray composite adhesive layer, improving the interlayer bonding strength and effectively preventing detachment during long-term washing. This allows the heat-bonded film to maintain stable optical performance and structural integrity even after multiple washes. This invention employs a two-step selective removal and hot-pressing transfer filling process for the fluorescent layer preform and the phosphorescent layer preform. First, a first strip-shaped groove is formed to fill the fluorescent layer. Then, a second selective removal process is performed within the fluorescent layer region to form a second strip-shaped groove to fill the phosphorescent layer. This achieves precise positioning of the fluorescent layer and the phosphorescent layer in the width direction, ensuring they are adjacent and non-overlapping. Furthermore, this process can be completed using die-cutting or laser equipment, making it suitable for continuous industrial production. It boasts low manufacturing costs, simple processes, and high yield. Therefore, this invention effectively overcomes the various shortcomings of existing technologies and possesses high industrial application value.
[0162] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A composite photoluminescent and reflective fluorescent heat-adhesive film, characterized in that: It includes a reflective structural layer, a transparent adhesive layer, a functional layer and a white cover layer stacked in sequence, wherein a flame-retardant adhesive film layer is provided on the side of the white cover layer away from the functional layer; The reflective structure layer comprises a base film layer, a beaded adhesive layer, a glass microsphere layer, a focusing layer, and a metal reflective layer stacked sequentially. The beaded adhesive layer is formed on one side of the base film layer. The glass microsphere layer comprises a plurality of glass microspheres, some of which are embedded in the beaded adhesive layer and fixed by the beaded adhesive layer. The focusing layer is disposed on the side of the glass microsphere layer away from the base film layer. The metal reflective layer is disposed on the side of the focusing layer away from the glass microsphere layer and is spaced apart along the width direction of the heat-bonded film. The transparent adhesive layer is disposed on the side of the reflective structural layer away from the base film layer and is used to connect the reflective structural layer and the functional layer; The functional layer includes a silver-gray composite adhesive layer, a fluorescent layer, and a light-gathering layer arranged periodically along the width direction of the heat-adhesive film. The fluorescent layer and the light-gathering layer are embedded in the silver-gray composite adhesive layer, and the fluorescent layer and the light-gathering layer are adjacent to each other without overlapping. The projection area of the metal reflective layer in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer is located, and does not coincide with the areas where the fluorescent layer and the light-gathering layer are located. The white cover layer is disposed on the side of the functional layer away from the transparent adhesive layer.
2. The composite light-storing and reflecting and fluorescent heat-paste film according to claim 1, characterized in that: The silver-gray composite adhesive layer is provided with a first strip-shaped groove arranged at intervals along the width direction of the film surface, and the fluorescent layer is disposed in the first strip-shaped groove; and the fluorescent layer is provided with a second strip-shaped groove arranged at intervals along the width direction of the film surface, and the photoluminescent layer is disposed in the second strip-shaped groove.
3. The composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 1, characterized in that: The material of the beaded adhesive layer includes one of PP, PE, EVA, EBA, and EAA, as well as a mixture with an opening agent; And / or, the thickness of the bead adhesive layer is 25% to 35% of the diameter of the glass microspheres; And / or, the diameter of the glass microspheres is 45μm~95μm, and the refractive index of the glass microspheres is 1.9~1.95; And / or, the material of the focusing layer includes one or a combination of polyurethane, polyester, and epoxy-modified acrylic resin, and the thickness of the focusing layer is 5μm to 20μm; And / or, the material of the metal reflective layer includes at least one of aluminum, silver, and chromium.
4. The composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 1, characterized in that: The thickness of the transparent adhesive layer is 10μm~20μm.
5. The composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 1, characterized in that: The thickness of the silver-gray composite adhesive layer is 30μm~70μm; And / or, the material of the silver-gray composite adhesive layer includes one or a combination of epoxy resin, polyurethane, modified acrylic resin, and a mixture with silver-gray pigment, flame retardant, and crosslinking agent.
6. The composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 1, characterized in that: The thickness of the fluorescent layer is 30 μm to 80 μm; And / or, the material of the fluorescent layer includes one or a combination of EVA, polyolefin, and polyurethane, and a mixture with fluorescent pigment, flame retardant, and crosslinking agent, wherein the fluorescent pigment includes one or a combination of yellow, orange, and red pigments.
7. The composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 1, characterized in that: The thickness of the light-generating layer is 30μm to 80μm; And / or, the material of the photoluminescent layer includes one or a combination of EVA, polyolefin, and polyurethane, as well as a mixture with photoluminescent powder, flame retardant, and crosslinking agent.
8. The composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 1, characterized in that: The thickness of the white covering layer is 30μm~70μm; And / or, the white covering layer comprises one or a combination of epoxy resin, polyurethane, modified acrylic resin, and a mixture with white pigment, flame retardant, and crosslinking agent.
9. The composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 1, characterized in that: The base layer of the flame-retardant adhesive film is selected from one of TPU, PU, PES, and PVC, and the thickness of the base layer is 30-150μm.
10. A method for preparing a composite photoluminescent and reflective fluorescent heat-adhesive film as described in any one of claims 1 to 9, characterized in that: The preparation method includes the following steps: S1. A beaded adhesive layer is formed on the surface of the base film layer. Glass microspheres are partially embedded in the beaded adhesive layer to form a glass microsphere layer. A focusing layer is formed on the side of the glass microsphere layer away from the beaded adhesive layer. Selective vacuum evaporation is performed on the side of the focusing layer away from the glass microsphere layer to form a metal reflective layer that is spaced apart along the width direction of the film surface, thus obtaining a reflective structure layer. Subsequently, a transparent adhesive layer is formed on the side of the reflective structure layer away from the base film layer, and a first release substrate is bonded to it to form a reflective substrate. S2. Pre-fabricate the fluorescent layer, the phosphorescent layer, and the white opaque layer respectively: A fluorescent layer is formed on the surface of the first release film, and after drying, it is bonded to the second release substrate to obtain a fluorescent layer preform. A light-gathering layer is formed on the surface of the second release film, and after drying, it is bonded to the third release substrate to obtain a light-gathering layer preform. A white masking layer is formed on the surface of the third release film. After drying, a flame-retardant adhesive film layer is bonded to obtain a white masking layer preform. S3. Provide a fourth release film and form a silver-gray composite adhesive layer on the surface of the fourth release film. Perform a first selective removal on the area where the silver-gray composite adhesive layer is located on the side of the silver-gray composite adhesive layer to form a first strip groove that is spaced apart along the width direction of the heat-bonding film. The first strip groove penetrates the silver-gray composite adhesive layer and extends to the fourth release film to form a receiving area for filling the fluorescent layer. S4. After peeling off the first release film, the fluorescent layer preform is bonded together, and the fluorescent layer is filled into the first strip groove by hot pressing. After cooling, the second release substrate on the fluorescent layer preform is peeled off, and the excess fluorescent layer in the area outside the first strip groove is removed. Then, the fourth release substrate is bonded together. S5. After curing, on the side of the fourth release substrate away from the fluorescent layer, a second selective removal is performed on the area where the fluorescent layer is located to form a second strip groove that is spaced apart along the width direction of the heat-bonding film. The second strip groove penetrates the fluorescent layer and extends to the fourth release film to form a receiving area for filling the light-gathering layer. S6. After peeling off the second release film, the photoluminescent layer preform is bonded together, and the photoluminescent layer is filled into the second strip groove by hot pressing. After cooling, the third release substrate on the photoluminescent layer preform is peeled off, the excess photoluminescent layer in the area outside the second strip groove is removed, and the fourth release substrate is peeled off. After curing treatment, a functional layer in which the silver-gray composite adhesive layer, fluorescent layer and photoluminescent layer are periodically arranged along the width direction of the heat-bonded film is obtained. S7. The white cover layer preform after peeling off the third release film is attached to the side of the functional layer away from the fourth release film to form a photoluminescent thermal adhesive film. S8. Peel off the fourth release film on the phosphorescent fluorescent heat-adhesive film described in step S7, and bond it with the reflective substrate from which the first release substrate was peeled off in step S1 to obtain a composite phosphorescent reflective fluorescent heat-adhesive film.
11. The method for preparing the composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 10, characterized in that: In step S1, the beaded adhesive layer is formed by extrusion casting. And / or, before embedding the glass microspheres into the bead adhesive layer in step S1, the bead adhesive layer needs to be baked to a molten state; And / or, in step S1, a focused layer is formed by extrusion or scraping.
12. The method for preparing the composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 10, characterized in that: The hot pressing mentioned in steps S4 and S6 is hot roller pressing, and the pressing temperature is 110℃~120℃.
13. The method for preparing the composite photoluminescent and reflective fluorescent heat-adhesive film according to claim 10, characterized in that: In step S8, the projection area of the metal reflective layer in the composite photoluminescent and reflective thermal adhesive film in the direction perpendicular to the film surface corresponds to the area where the silver-gray composite adhesive layer is located, and does not overlap with the areas where the fluorescent layer and photoluminescent layer are located.