Optoelectronic devices based on multi-period micro / nano grating substrates, their fabrication methods, and applications.

By constructing multi-period micro/nano grating structures in one step using femtosecond lasers, the problems of complex fabrication processes and interface damage in existing technologies have been solved, achieving efficient light management and improved stability, thereby enhancing the photoelectric conversion performance of perovskite optoelectronic devices.

CN123124574APending Publication Date: 2026-11-17NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611123667.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for fabricating multi-period grating structures suffer from complex processes, strong alignment dependence, and a tendency to introduce interface defects and cumulative errors, which limits the performance improvement of perovskite optoelectronic devices.

Method used

Multi-period micro-nano gratings can be constructed in one step using femtosecond lasers. By combining micron-scale and nano-scale grating structures, and through the synergistic effect of femtosecond laser ablation and laser-induced periodic surface structures, multi-period micro-nano gratings can be directly constructed on conductive substrates, avoiding the lengthy process and interface damage of traditional multi-step processes.

Benefits of technology

It achieves efficient light management, improves light absorption efficiency and carrier generation rate, enhances photoelectric conversion performance and device stability, and reduces fabrication cost and time cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124574A_ABST
    Figure CN123124574A_ABST
Patent Text Reader

Abstract

This invention discloses an optoelectronic device based on a multi-period micro / nano grating substrate, its fabrication method, and its applications, relating to the field of semiconductor device technology. The optoelectronic device comprises, from bottom to top, a conductive substrate, a hole transport layer, a perovskite active layer, an electron transport layer, and a metal electrode, stacked sequentially. A multi-period micro / nano grating structure is disposed on the conductive substrate. This multi-period micro / nano grating structure includes multiple equally spaced strip grooves on the conductive substrate, and multiple arrayed strip protrusions at the bottom of each strip groove, forming a target grating structure corresponding to the multi-period micro / nano grating structure. This invention achieves broadband and efficient light management by constructing a multi-period micro / nano grating including micrometer-scale and nanometer-scale gratings on a substrate, and by using a femtosecond laser to construct the multi-period micro / nano grating in one step. Furthermore, morphology optimization ensures the electrical integrity of the perovskite film and interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor device technology, specifically to an optoelectronic device based on a multi-period micro / nano grating substrate, its fabrication method, and its applications. Background Technology

[0002] Perovskite materials, due to their excellent light absorption, long carrier diffusion length, and low-temperature solution processing capabilities, have shown broad application prospects in photodetectors, solar cells, and other fields. However, the development of perovskite-based optoelectronic devices faces numerous challenges, including low photoelectric conversion efficiency, poor stability, and light loss due to strong Fresnel reflection, which seriously affect the improvement of device performance. Currently, the manipulation of the light field using micro / nano grating structures has become one of the important research directions for improving the performance of perovskite optoelectronic devices. By constructing micro / nano grating structures with specific periodicity and morphological characteristics on the surface of transparent electrodes or functional layers, the propagation behavior of light can be significantly altered, including enhancing light scattering, inducing multiple reflections, extending the propagation path of light in the active layer, and exciting local electromagnetic field enhancement effects. These effects work synergistically to improve light absorption efficiency, enhance carrier generation, and ultimately improve the photoelectric conversion performance of the device. Gu et al. fabricated nanogratings on the surface of MAPbI3 thin films using nanoimprint technology, which improved the detection performance of the detector (Adv. Opt. Mater. 2022,10, 2201516.). Liu et al. used nanoimprinting to imprint nanoscale grating patterns on the surface of perovskite thin films. These linear nanograting patterns can detect polarized light and enhance light absorption, effectively improving device performance (Adv. Opt. Mater. 2024, 2302411.). Song et al. constructed a charge transport interface array structure with controllable height and period, achieving a photodetector responsivity of 30.1 A / W (Adv. Mater. 2024, 36, 2408448.). However, the physical contact pressure during the imprinting process can damage the perovskite lattice structure, introduce defects, and reduce photoelectric performance. Demolding can easily cause template contamination and film residue, affecting pattern accuracy and repeatability. Soft templates are prone to pattern distortion and thickness unevenness during large-area imprinting. High-precision template preparation is expensive, and the imprinting cycle is long, which is not conducive to large-scale production. Meanwhile, compared with single-period grating structures, stacked or dual-grating architectures have been proven to provide a more efficient and flexible approach to optimizing photodetector performance due to their significant advantages in light capture efficiency and spectral response modulation. Song et al. fabricated a highly efficient corrugated perovskite photodetector with a stacked double shallow grating structure using a multi-step nanoimprinting method, achieving sensitive digital polarization imaging. In the double grating structure, the perovskite exhibits superior light collection capabilities through the synergistic effect of reflection, diffraction, and waveguide mode excitation (Adv. Energy Mater. 2021, 11, 2100742.).Li et al. fabricated an in-situ encapsulated corrugated lattice perovskite photodetector using two nanograting soft templates with relative rotation angles. The confined growth of the two nanograting templates led to the growth of a crystal with a moiré lattice structure, thereby improving the trapping ability of the perovskite crystal and thus enhancing device performance (Adv. Mater. 2023, 35, 2207771.). Li et al. also used two PDMS templates to introduce dual nanogratings via nanoimprinting to enhance the stability of MAPbBr3 and extend its spectral response to the near-infrared range (Adv. Mater. 2025, e15848.). Constructing multi-scale, multi-period structures has become an important development trend in this field. However, from a fabrication process perspective, realizing multi-period micro / nano structures remains highly complex. Traditional techniques, such as nanoimprinting, electron beam lithography, dry / wet etching, and multiple photolithography stacking processes, typically require multiple steps, including template preparation, pattern transfer, multi-layer alignment, and repeated processing. These multi-step processes are not only cumbersome and time-consuming, but also place stringent demands on equipment. In large-area fabrication, they are susceptible to cumulative errors, leading to decreased structural consistency. Furthermore, multiple processing steps may introduce additional interface defects, stress concentrations, or material damage, adversely affecting the sensitive interfacial electrical properties of perovskite devices and limiting their practical application potential. Summary of the Invention

[0003] To address the shortcomings of the aforementioned background technology, this invention tackles the bottlenecks caused by the complex fabrication process and strong alignment dependence of existing multi-period grating structures. This invention constructs multi-period micro-nano gratings, including micron-scale and nano-scale gratings, on a substrate, and uses femtosecond lasers to construct the multi-period micro-nano gratings in one step, achieving broadband and efficient light management. Furthermore, morphology optimization ensures the perovskite film formation and the electrical integrity of the interface.

[0004] This invention utilizes the synergistic effect of femtosecond laser ablation and laser-induced periodic surface structures (LIPSS) to directly construct multi-periodic micro / nano gratings on the surface of a conductive substrate using a single-step dry fabrication process: low spatial frequency (LSFL) or high spatial frequency (HSFL) periodic structures are nested within the inner walls of a micrometer-scale ablation trench. During subsequent solution deposition of perovskite films, the substrate morphology induces conformal coverage, forming a photoactive layer with multi-periodic characteristics. This method eliminates the need for templates and multiple alignments, avoiding the bottlenecks of traditional substrate patterning processes such as lengthy processes, error accumulation, and interface damage. Furthermore, the cold processing characteristics of femtosecond lasers effectively protect the electrical properties of the substrate surface and the charge transport characteristics of the perovskite-substrate interface.

[0005] The first objective of this invention is to provide an optoelectronic device based on a multi-period micro / nano grating substrate, which includes a conductive substrate, a hole transport layer, a perovskite active layer, an electron transport layer, and a metal electrode stacked sequentially from bottom to top. A multi-period micro / nano grating structure is disposed on the conductive substrate; The multi-period micro / nano grating structure includes multiple equally spaced strip grooves on a conductive substrate, and multiple arrayed strip protrusions at the bottom of each strip groove. Each groove and its internal multiple protrusions form a grating unit; Each of the strip protrusions has a triangular cross-sectional shape; the long side of each of the strip grooves and the long side of each strip protrusion are parallel to the long side of the conductive substrate. Multiple equally spaced strip grooves form a micrometer-scale grating structure; multiple strip protrusions within each strip groove form a nanometer-scale grating structure; the distance between adjacent strip grooves is 1.0~2.0μm; The distance between the bottoms of adjacent strip protrusions is zero, and the distance between the tops is 150~250nm; the depth of each strip groove is 25~35nm; the height of each protrusion is 20~30nm; The bottom of the perovskite active layer extends downward in the region corresponding to the multi-period micro / nano grating structure to form a target grating structure corresponding to the multi-period micro / nano grating structure; the target grating structure is formed by embedding the bottom of the perovskite active layer downward into a strip groove; The hole transport layer is provided between the multi-period micro / nano grating structure and the corresponding target grating structure.

[0006] In one embodiment, the thickness of the perovskite active layer is 350~450 nm; the material of the perovskite active layer is tin-lead perovskite. In one embodiment, the substrate thickness is 0.5~1.5mm; the conductive substrate thickness is 100~150nm; the hole transport layer thickness is 2~7nm; the electron transport layer thickness is 25~30nm; and the metal electrode thickness is 80~120nm.

[0007] In one embodiment, the two side walls of each of the strip grooves are inclined, so that the cross-sectional shape of the strip groove is an inverted trapezoid.

[0008] In one embodiment, the conductive substrate is an ITO or FTO substrate; the hole transport layer is PTAA or MeO-6PACz; and the electron transport layer is PCBM or C 60 The metal electrode is made of silver, copper, aluminum, or gold.

[0009] In one embodiment, a substrate, which is glass or silicon, is further disposed at the bottom of the conductive substrate.

[0010] The second objective of this invention is to provide a method for fabricating optoelectronic devices on multi-period micro / nano grating substrates, comprising the following steps: A multi-period micro / nano grating structure was fabricated in a single step on a conductive substrate using a femtosecond laser-induced method. During the fabrication process, the energy density of the laser beam was determined based on the damage threshold of the conductive substrate. After cleaning the conductive substrate containing the multi-period micro-nano grating structure, a hole transport layer and a perovskite active layer are sequentially prepared by spin coating and then bonded to the outer surface of the multi-period micro-nano grating structure on the conductive substrate, so that the interface between the perovskite active layer and the conductive substrate forms the target grating structure. An electron transport layer is bonded onto the perovskite active layer by spin coating or thermal evaporation. Metal electrodes bonded to the electron transport layer are deposited on the outer surface of the electron transport layer using a photomask via thermal evaporation.

[0011] In one embodiment, when fabricating a multi-period micro / nano grating structure on a conductive substrate using a femtosecond laser-induced method in a single step, the process includes: The conductive substrate is placed on the displacement platform of the femtosecond laser processing system and leveled. Adjust the parameters of the laser beam according to its energy density; A grating unit is obtained by laser-induced laser on a conductive substrate. The conductive substrate is then moved to process the next grating unit, thus forming a multi-period micro / nano grating structure.

[0012] In one embodiment, the laser beam output power is 2 mW to 18 mW, the laser beam pulse width is 100 fs to 500 fs, the repetition frequency is 100 kHz to 500 kHz, and the laser wavelength is 1030 nm.

[0013] The third objective of this invention is to provide an application of a multi-period micro / nano grating substrate optoelectronic device in a photodetector.

[0014] Compared with existing technologies, the optoelectronic device based on a multi-period micro / nano grating substrate, its fabrication method, and its application provided by this invention have the following main advantages: This invention constructs a multi-period micro / nano grating structure on a substrate, comprising micrometer-scale and nanometer-scale gratings. The micrometer-scale grating serves as the master grating, determined by the femtosecond laser-induced trajectory, while the nanometer-scale grating is determined by the LIPSS self-organization mechanism. The micrometer-scale master grating acts as a macroscopic diffraction trapping structure and a micro-optical waveguide, utilizing diffraction to alter the propagation direction of incident light and converting photons into waveguide modes that propagate at large angles, significantly extending the effective optical path length of photons in the active layer. The nanometer-scale grating embedded within it, due to its size being much smaller than the incident wavelength, satisfies the effective medium theory in terms of optical properties. A continuously gradient refractive index transition layer is constructed at the material interface, achieving an ultra-wideband anti-reflection effect by disrupting Fresnel reflection. The synergistic regulation of these two elements improves the light absorption limit of thin-film detectors constrained by physical thickness, achieving efficient photon injection and complete interception without increasing the active layer thickness to avoid carrier recombination. In terms of electromagnetic field localization enhancement and exciton manipulation, this multi-period micro / nano grating structure triggers a cross-scale second-order field strength amplification effect. The micron-scale master grating first macroscopically converges the light field space and guides it into the trench, while the nanoscale grating embedded in it further excites strong local surface plasmon resonance or guided mode resonance within the trench. This extreme localization of photons at the nano gaps forms a high-density near-field optical hotspot, resulting in a leap of several orders of magnitude in the local electromagnetic field strength. This extreme near-field enhancement directly acts on the adjacent light-absorbing active layer, which not only significantly improves the optical absorption coefficient of the material but also greatly accelerates the exciton generation rate by utilizing the strong electromagnetic field pumping effect and effectively reduces the exciton binding energy. This improves the pure generation rate and separation efficiency of photogenerated carriers at the source, systematically enhancing the external quantum efficiency of the detector.

[0015] In this invention, during the direct writing of micron-scale master gratings using femtosecond lasers, the material surface undergoes intense non-thermal phase transitions, plasma jets, and localized material redistribution. This strong macroscopic energy gradient and stress field easily disrupts the physical boundaries of the self-organized nanoscale structure, leading to severe disordered bifurcation and fracture of the embedded nanoscale gratings within it, and even complete melting and flattening due to transient energy overload. However, this invention, through precise design of the spatial energy distribution and temporal pulse train modulation of the femtosecond laser, effectively constrains and guides the self-organized growth of the nanostructure using the transient electromagnetic boundaries constructed from the micron-scale structure, thus solving the manufacturing bottleneck of lost spatial coherence of micro / nano structures in cross-scale processing.

[0016] In this invention, the induced fabrication of the micrometer-scale master grating involves macroscopic energy flow manipulation with strong ablation and large removal, while the induction of the nanometer-scale grating relies on the weak coherent interference between ultrafast transient surface plasmons and local material properties. In actual manufacturing, these two processing mechanisms with different energy densities are prone to vicious competition in spatial modes and energy distribution, making it impossible to fabricate a composite structure with regularity at both scales in situ within the same process window. This invention, however, achieves efficient coordination between macroscopic geometric boundaries and microscopic dynamic interference fields in a single laser scan by precisely modulating the dynamic balance of energy flow during processing. This enables stable, integrated, in-situ fabrication of high-quality, high-fidelity embedded multi-scale structures, allowing the construction of embedded multi-period micro / nano grating structures without multiple complex processes.

[0017] This invention selects a single-step formation of a multi-period micro / nano grating structure on a conductive substrate using laser-induced technology, improving production efficiency. Subsequently, a perovskite active layer is bonded to the outer surface of the multi-period micro / nano grating using a spin-coating method. Due to the uniform thickness of the spin-coating, the interface of the perovskite active layer forms a target grating structure that matches the grating structure of the substrate. This method avoids directly processing the perovskite active layer during the formation of the grating structure, which could affect the structure and quality of the perovskite active layer. Therefore, this method is simple, low-cost, and can improve the accuracy and performance of perovskite devices, meeting practical application requirements. Attached Figure Description

[0018] Figure 1 This is a schematic diagram of the cross-section of an optoelectronic device containing a multi-period micro / nano grating substrate; Figure 2 This is a schematic diagram of a cross-section of a multi-period micro / nano grating structure on a conductive substrate; Figure 3 The images show the AFM diagram (a) of the multi-period micro / nano grating on the conductive substrate and the distribution curve of the multi-period micro / nano grating structure (b). Figure 4 This is a SEM image of a multi-period micro / nano grating on a conductive substrate. Figure 5 This is a comparison chart of the external quantum efficiency of perovskite optoelectronic devices with multi-period micro / nano grating structures fabricated by femtosecond laser single-step induction. Figure 6 This is a comparison chart of the responsivity of perovskite optoelectronic devices with multi-period micro / nano grating structures fabricated by femtosecond laser single-step induction. Figure 7 This is a comparison chart of the specific detectivity of perovskite optoelectronic devices with multi-period micro / nano grating structures fabricated by femtosecond laser single-step induction. Detailed Implementation

[0019] To enable those skilled in the art to better understand and implement the technical solutions of the present invention, the present invention will be further described below in conjunction with specific embodiments and accompanying drawings. However, the embodiments described are not intended to limit the present invention.

[0020] This invention addresses the numerous challenges facing the development of perovskite optoelectronic devices, including low photoelectric conversion efficiency, poor stability, and light loss due to strong Fresnel reflection, which severely impact device performance. Based on constructing micro / nano grating structures with specific periodicity and morphological characteristics on the surface of transparent electrodes or functional layers, this invention significantly alters light propagation behavior, including enhancing light scattering, inducing multiple reflections, extending the light propagation path in the active layer, and stimulating local electromagnetic field enhancement. These effects work synergistically to improve light absorption efficiency, enhance carrier generation, and ultimately improve the device's photoelectric conversion performance. However, from a fabrication process perspective, realizing multi-period micro / nano structures remains technically complex. Traditional techniques, such as nanoimprint lithography, electron beam lithography, dry / wet etching, and multiple photolithography stacking processes, typically involve multiple steps including template preparation, pattern transfer, multi-layer alignment, and repeated processing. These multi-step processes are not only cumbersome and time-consuming but also demand stringent equipment precision requirements; during large-area fabrication, they are susceptible to cumulative errors, leading to decreased structural consistency. More importantly, multiple processing steps may introduce additional interface defects, stress concentrations, or thermal damage to the material, which can adversely affect the sensitive interface electrical properties of perovskite devices, thereby limiting their photoelectric conversion efficiency and long-term stability, and restricting their practical application potential.

[0021] Femtosecond laser direct writing technology has become an important technique for fabricating micro and nanostructures due to its non-contact, maskless, "cold" processing, and high resolution characteristics. However, existing femtosecond laser-based perovskite surface structuring methods mostly focus on the construction of single-period uniform gratings, and have not yet achieved single-step fabrication of micro and nano grating structures with multi-scale and multi-period characteristics.

[0022] The present invention aims to provide an optoelectronic device based on a multi-period micro / nano grating substrate, its fabrication method, and its applications. This optoelectronic device constructs a multi-period micro / nano grating structure on a substrate, including micrometer-scale and nanometer-scale gratings. This multi-period micro / nano grating structure triggers a cross-scale second-order field amplification effect. The micrometer-scale master grating first macroscopically converges the light field space and guides it into the trench, while the embedded nanometer-scale grating further excites strong localized surface plasmon resonances or guided mode resonances within the trench. This results in extreme localization of photons at the nanometer gaps, forming high-density near-field optical hotspots, leading to a leap of several orders of magnitude in the local electromagnetic field intensity. This extreme near-field enhancement directly acts on the adjacent light-absorbing active layer, significantly improving the material's optical absorption coefficient and greatly accelerating the exciton generation rate using the strong electromagnetic field pumping effect, while effectively reducing the exciton binding energy. This fundamentally improves the pure generation rate and separation efficiency of photogenerated carriers, systematically enhancing the external quantum efficiency of the detector.

[0023] This invention utilizes the nonlinear absorption effect and transient energy deposition characteristics generated during the interaction between femtosecond lasers and materials to induce the in-situ formation of laser-induced periodic surface structures (LIPSS) on functional substrates such as ITO without the need for masks or complex alignment. By precisely controlling laser processing parameters (such as pulse energy, repetition frequency, scanning speed, and polarization direction), low spatial frequency LIPSS (LSFL) or high spatial frequency LIPSS (HSFL) structures can be generated. Notably, the LIPSS formation process is accompanied by directional thinning and surface reconstruction of the material. Therefore, by optimizing the femtosecond laser direct writing parameters, the synergistic control of the micrometer-scale main grating period and the nanometer-scale sub-periodic structure can be achieved, thereby enabling precise modulation of the light-material interaction at different scales and providing a new technical approach for optimizing the performance of perovskite optoelectronic devices.

[0024] To achieve the above objectives, see Figure 1 As shown, an optoelectronic device based on a multi-period micro / nano grating substrate is disclosed. The optoelectronic device includes a substrate 1, a conductive substrate 2, a hole transport layer 3, a perovskite active layer 4, an electron transport layer 5, and a metal electrode 6 stacked sequentially from bottom to top. A multi-period micro / nano grating structure is disposed on the conductive substrate 2; See Figure 2 As shown, the multi-period micro-nano grating structure includes multiple equally spaced strip grooves 2-1 on a conductive substrate 2, and multiple arrayed strip protrusions 2-2 at the bottom of each strip groove. Each strip groove 2-1 and the multiple strip protrusions 2-2 arranged inside it form a grating unit; Each of the strip protrusions 2-2 has a triangular cross-sectional shape; the long side of each of the strip grooves 2-1 and the long side of each strip protrusion 2-2 are parallel to the long side of the conductive substrate. Multiple equally spaced strip grooves 2-1 form a micrometer-scale grating structure; multiple strip protrusions 2-2 within each strip groove 2-1 form a nanometer-scale grating structure 7; The distance between adjacent strip grooves is 1.0~2.0μm; The distance between the bottoms of adjacent strip protrusions is zero, and the distance between the tops is 150~250nm; the depth of each strip groove is 25~35nm; the height of each protrusion is 20~30nm; wherein, the height of the protrusion is less than the depth of the strip groove, which can play a role in thinning the conductive substrate.

[0025] Preferably, the distance between adjacent grooves is 1 μm; the distance between the bottoms of adjacent protrusions is zero, and the distance between the tops is 200 nm; the depth of each groove is 30 nm; and the height of each protrusion is 25 nm. The bottom of the perovskite active layer extends downward in the region corresponding to the multi-period micro-nano grating structure to form a target grating structure 8 corresponding to the multi-period micro-nano grating structure; the target grating structure 8 is formed by embedding the bottom of the perovskite active layer downward into the strip groove 2-1. The hole transport layer is provided between the multi-period micro / nano grating structure and the corresponding target grating structure.

[0026] See Figure 2 As shown, the width of a strip groove 2-1 and the sum of the distances between it and its adjacent strip grooves 2-1 are defined as the main micron-level grating period; the distance between the tops of adjacent strip protrusions 2-2 is defined as the secondary nanon-level grating period.

[0027] The thickness of the perovskite active layer is 350~450 nm; preferably, the thickness is 400 nm; the material of the perovskite active layer is tin-lead perovskite. The substrate thickness is 0.5~1.5mm; the conductive substrate thickness is 100~150nm; the hole transport layer thickness is 2~7nm; the electron transport layer thickness is 25~30nm; and the metal electrode thickness is 80~120nm.

[0028] Preferably, the substrate thickness is 1 mm; the conductive substrate thickness is 140 nm; the hole transport layer thickness is 5 nm; the electron transport layer thickness is 28 nm; and the metal electrode thickness is 100 nm.

[0029] The two side walls of each of the strip grooves 2-1 are inclined, so that the cross-sectional shape of the strip groove is an inverted trapezoid. That is, the side wall of the strip groove 2-1 forms an angle with the adjacent strip protrusion 2-2, and this angle corresponds to the top angle of the strip protrusion 2-2, thereby forming a periodic nanoscale grating.

[0030] The conductive substrate is indium tin oxide (ITO) or fluorine-doped tin oxide (FTO) substrate; the hole transport layer is poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) or methoxy-substituted hexaphenylazapyrene (MeO-6PACz); the electron transport layer is methyl phenyl C61-butyrate (PCBM) or fullerene C 60 The metal electrode is made of silver, copper, aluminum, or gold; the substrate is made of glass or silicon.

[0031] The single-step embedded multi-period micro / nano grating structure provided by this invention exhibits significant synergistic effects and structural advantages in improving the overall physical properties and interface dynamics of the electrode surface. In precision optical or optoelectronic applications, this micro / nano nested structure, as a subwavelength / micrometer-scale composite grating, exhibits unique optical diffraction, light-trapping effects, and surface plasmon resonance characteristics, greatly enhancing the ability to capture and modulate photons in specific wavelength bands. Regarding the mechanical stability and service life of the electrode, traditional two-step processing methods, due to the step-by-step high-energy etching and low-energy induction, often result in severe residual stress concentration at the micro / nano interface due to overlapping heat-affected zones or lattice distortion. During mechanical bending, thermal cycling, or service in complex environments, this interface stress easily leads to the pulverization and detachment of the surface nanostructure. In contrast, the nested structure formed by the single-step self-organization of this invention features homogeneous in-situ growth between the micrometer-scale substrate and the nano-stripes, with good lattice continuity and no obvious non-uniform stress abrupt changes at the interface transition. This micro / nano integrated topological configuration exhibits extremely excellent mechanical toughness and anti-peeling ability under the coupling effect of multi-physics fields, thereby ensuring the structural stability of the electrode during long-term service.

[0032] The present invention provides a method for fabricating an optoelectronic device on a multi-period micro / nano grating substrate, comprising the following steps: A multi-period micro / nano grating structure was fabricated in a single step on a conductive substrate using a femtosecond laser-induced method. During the fabrication process, the energy density of the laser beam was determined based on the damage threshold of the conductive substrate. After cleaning the conductive substrate containing the multi-period micro-nano grating structure, a hole transport layer and a perovskite active layer are sequentially prepared by spin coating and then bonded to the outer surface of the multi-period micro-nano grating structure on the conductive substrate, so that the interface between the perovskite active layer and the conductive substrate forms the target grating structure. An electron transport layer is bonded onto the perovskite active layer by spin coating or thermal evaporation. Metal electrodes bonded to the electron transport layer are deposited on the outer surface of the electron transport layer using a photomask via thermal evaporation.

[0033] Among them, the single-step fabrication of multi-period micro / nano grating structures on conductive substrates using femtosecond laser-induced methods includes: The conductive substrate is placed on the displacement platform of the femtosecond laser processing system and leveled. Adjust the parameters of the laser beam according to its energy density; A grating unit is obtained by laser-induced laser on a conductive substrate. Then, the conductive substrate is moved to process the next grating unit, and a multi-period micro-nano grating structure is formed. The laser beam output power is 2 mW~18 mW, the pulse width of the laser beam is 100 fs~500 fs, the repetition frequency is 100 kHz~500 kHz, and the laser wavelength is 1030 nm.

[0034] An exemplary method for fabricating an optoelectronic device on a multi-period micro / nano grating substrate includes: S1. Determine the energy density of the laser beam based on the damage threshold of the conductive substrate; S2. A multi-period micro / nano grating is fabricated in a single step on the top face of a conductive substrate using femtosecond laser-induced technology. This multi-period micro / nano grating comprises micrometer-scale and nanometer-scale gratings, which are combined. Specifically, it includes: S21. Place the conductive substrate on the displacement platform of the femtosecond laser processing system and level it. S22. Adjust the parameters of the laser beam according to the energy density of the laser beam obtained in step S1; S23. The laser beam obtained in step S22 is used to laser induce the conductive substrate to obtain a grating unit; S24. The laser beam is turned off. It is determined whether the processing of all grating units has been completed. If yes, the processing of multi-period micro-nano gratings on the substrate is completed; if not, step S25 is executed. S25. After moving the conductive substrate according to the distance between two adjacent grating units, proceed to step S23.

[0035] S3. Clean the conductive substrate obtained in step S2, specifically including: S31. Use an aqueous solution with added cleaning agent to perform a rough cleaning of the conductive substrate containing multi-period micro / nano gratings. S32. Perform ultrasonic cleaning on the conductive substrate containing multi-period micro-nano gratings after rough cleaning; wherein, during ultrasonic cleaning, the substrate is ultrasonically cleaned sequentially using a mixture of water and glass water, deionized water, ethanol, acetone and isopropanol solution, wherein each ultrasonic cleaning time is 20 min and the ultrasonic power is 100 W.

[0036] S33. The conductive substrate containing multi-period micro-nano gratings, which has been ultrasonically cleaned, is dried in an oven at 100°C for 12 hours, and then cleaned by an ultraviolet light cleaner for 20 minutes.

[0037] S4. A hole transport layer and a perovskite active layer are sequentially prepared using a spin-coating method, and then bonded to the outer surface of a conductive substrate containing a multi-period micro / nano grating, so that the interface between the perovskite active layer and the substrate forms the target grating. Specifically, this includes: S41. A hole transport layer is prepared on the outer surface of a conductive substrate containing a multi-period micro / nano grating by spin coating. S42. A perovskite active layer is prepared on the outer surface of the hole transport layer by spin coating, so that the interface between the perovskite active layer and the hole transport layer forms a target grating. S43. An electron transport layer is bonded to the outer surface of the target grating by spin coating or thermal evaporation.

[0038] S5. A metal electrode bonded to the electron transport layer is deposited on the outer surface of the electron transport layer by means of a photomask using a thermal evaporation method.

[0039] This invention proposes a single-step in-situ shaping method based on the multi-period self-organizing nonlinear effect of femtosecond lasers. Under specific laser energy density, pulse overlap rate, and beam morphology modulation, a strong nonlinear coupling occurs between the spatially coherent light field and plasmon polaritons on the electrode material surface. This triggers both micrometer-level ablation behavior and nanometer-level self-organizing evolution on the material surface during a single scan. Ultimately, a nested multi-period micro / nano grating structure with high spatial coaxiality and structural integrity is constructed on the electrode surface in one step. The micrometer-level grating period in this structure is precisely controlled within the 1–20 μm scale, and the nanometer-level grating is directly embedded in-situ within the periodic units of the micrometer grating. This fundamental difference in mechanism allows this invention to fundamentally eliminate the dependence of traditional two-step methods on multi-channel energy switching and sub-micrometer-level secondary alignment accuracy.

[0040] This invention enables the simultaneous construction of multi-level periodic grating structures on a conductive substrate using a single laser scan, eliminating the need for multiple exposures, step-by-step laser parameter adjustments, or mask replacements. Compared to traditional multi-step processing strategies, this invention completes the fabrication of multi-period structures in a single step, significantly reducing process complexity and time costs, and improving the throughput and consistency of large-area fabrication. The single-step nesting technique of this invention cleverly utilizes the high peak power characteristics of ultrafast lasers, enabling spatial redistribution of energy within an extremely short timescale. Within the overlapping region of a single pulse or continuous pulse, the material simultaneously undergoes micron-level precision ablation and nano-level surface self-organization reconstruction. Energy utilization efficiency is significantly improved, and by avoiding repeated thermal effects of secondary light fields on the processed area, the heat-affected zone of the electrode material substrate is compressed to its limit, ensuring high morphological consistency and process repeatability of the micro / nano nested gratings over a large macroscopic area.

[0041] In this invention, because the multi-period structure is formed synchronously in situ during a single scan, structural drift and alignment deviations caused by thermal cycling accumulation during multi-step processing are avoided. The spatial position of each periodic structure is precisely defined by the same laser scanning trajectory, ensuring high-precision registration between the main periodic and sub-periodic structures, which is beneficial for achieving a synergistic enhancement effect of optical field modulation.

[0042] The single-step processing strategy in this invention reduces multiple interactions between the laser and the material, lowers the risk of thermal damage at the buried interface, and helps maintain the quality of the thin film and the electrical properties of the interface. The fabricated multi-period micro / nano grating structure can simultaneously control the light-harvesting efficiency and carrier generation / transmission behavior over a wide spectral range, providing a structural basis for improving the external quantum efficiency, response speed, and long-term stability of the device.

[0043] This invention eliminates the need for precision alignment equipment, multiple sets of photomasks, or complex optical modulation systems. It enables the fabrication of multi-period structures using only a conventional femtosecond laser-induced platform, significantly reducing equipment investment and process maintenance costs. Furthermore, the single-step scanning strategy is compatible with large-area, fast direct-write technology, demonstrating excellent potential for large-scale production.

[0044] This invention provides an application of a multi-period micro / nano grating substrate optoelectronic device in photodetectors or solar cells.

[0045] It should be noted that, unless otherwise specified, the experimental methods used in this invention are all conventional methods; and the reagents and materials used, unless otherwise specified, are all commercially available.

[0046] Example 1 See Figure 1As shown, an optoelectronic device based on a multi-period micro / nano grating substrate includes a substrate 1, a conductive substrate 2, a hole transport layer 3, a perovskite active layer 4, an electron transport layer 5, and a metal electrode 6 stacked sequentially from bottom to top. A multi-period micro / nano grating structure is disposed on the conductive substrate 2; The multi-period micro / nano grating structure includes multiple equally spaced strip grooves on a conductive substrate 2, and multiple arrayed strip protrusions at the bottom of each strip groove; Each groove and its internal multiple protrusions form a grating unit; Each of the strip protrusions has a triangular cross-sectional shape; the long side of each of the strip grooves and the long side of each strip protrusion are parallel to the long side of the conductive substrate. Multiple equally spaced strip grooves form a micron-scale grating structure; multiple strip protrusions within each strip groove form a nano-scale grating structure; the distance between adjacent strip grooves is 1 μm; The distance between the bottoms of adjacent strip protrusions is zero, and the distance between their tops is 200 nm; The depth of each groove is 30nm; Each protrusion is 25nm high; The bottom of the perovskite active layer extends downward in the region corresponding to the multi-period micro / nano grating structure to form a target grating structure 8 corresponding to the multi-period micro / nano grating structure; the target grating structure 8 is formed by embedding the bottom of the perovskite active layer downward into a strip groove. The hole transport layer is provided between the multi-period micro / nano grating structure and the corresponding target grating structure.

[0047] The perovskite active layer has a thickness of 400 nm; the perovskite active layer is made of tin-lead perovskite; the substrate has a thickness of 1 mm; the conductive substrate has a thickness of 140 nm; the hole transport layer has a thickness of 5 nm; the electron transport layer has a thickness of 28 nm; and the metal electrode has a thickness of 100 nm.

[0048] The two side walls of each of the strip grooves are inclined, so that the cross-sectional shape of the strip groove is an inverted trapezoid.

[0049] The conductive substrate is an ITO substrate; the hole transport layer is PTAA; the electron transport layer is PCBM; the metal electrodes are all gold; and the substrate is silicon.

[0050] Example 2 A method for fabricating an optoelectronic device on a multi-period micro / nano grating substrate, as provided in Embodiment 1, includes the following steps: S1. Determine the energy density of the laser beam based on the damage threshold of the conductive substrate 2; The conductive substrate 2 is disposed on the upper surface of the substrate 1, which is selected as glass according to requirements. Specifically, the conductive substrate 2 is illustrated using an ITO substrate as an example. Before etching the multi-period micro / nano grating structure on the conductive substrate 2, it is necessary to determine the damage threshold of the conductive substrate 2. Typically, a scribing method is chosen to determine the damage threshold of the conductive substrate 2. The damage threshold of the conductive substrate 2 is selected such that the energy density of the laser beam is greater than the measured damage threshold; in this embodiment, the measured damage threshold laser energy density is 215.4 mJ / cm². 2 The corresponding power is 2.6 mW. Therefore, the actual laser energy density for processing is set to 232.0 mJ / cm². 2 The corresponding laser power is 2.8mW, the pulse width of the laser beam is 200fs, the repetition frequency is 200kHz, and the laser wavelength is 1030nm.

[0051] S2. Using laser-induced technology, multi-period micro / nano gratings are fabricated on the top end face of conductive substrate 2, including micron-scale grating structures and nano-scale grating structures. S3. Clean the conductive substrate 2 obtained in step S2. S4. Using spin coating, the hole transport layer 3 and the perovskite active layer 4 are bonded to the outer surface of the substrate grating 7, so that the interface of the perovskite active layer 4 forms the target grating structure 8.

[0052] Step S2 includes the following steps: S21. Level the conductive substrate 2; Typically, a substrate 1 with a conductive substrate 2 is fixed on a 3D displacement processing platform. This platform can move the substrate 1 along the x-axis, y-axis, and z-axis directions by adjustment. Therefore, after determining the height of the substrate 1, the imaging of the conductive substrate 2 is observed by a CCD, and the substrate 1 is adjusted in the x-axis and y-axis directions according to the imaging, until the conductive substrate 2 is in a horizontal state by adjusting the substrate 1, so that the distance between the surface of the conductive substrate 2 and the laser output end is constant during subsequent processing, ensuring the accurate processing of the grating depth.

[0053] S22. Adjust the parameters of the laser beam according to the laser beam output power obtained in step S1; In practical use, the laser is focused by a focusing objective lens, and the energy density of the focused laser is then adjusted by a combination of a Glan Taylor prism and a half-wave plate to achieve the predetermined energy density.

[0054] S23. The laser beam obtained in step S22 is used to laser induce the conductive substrate 2 to obtain a grating unit. Specifically, according to the structural size of the target grating structure 8 and its distribution on the conductive substrate 2, the first grating unit in the conductive substrate is processed by laser direct writing technology, and multiple grating units are processed in sequence.

[0055] S24. The laser beam is turned off. It is determined whether the processing of all grating units has been completed. If yes, the processing of the multi-period micro-nano grating on the conductive substrate is completed. If not, step S25 is executed. Specifically, after processing one grating unit, the laser beam is turned off. At this time, it is necessary to determine whether the processing of all grating units on the conductive substrate 2 has been completed. If not, the processing of the next grating unit needs to be carried out. At this time, step S25 is executed. If all are completed, the processing of the grating units on the conductive substrate 2 is ended, and the upper surface of the conductive substrate 2 is obtained as a conductive substrate containing a multi-period micro-nano grating.

[0056] S25. After moving the conductive substrate 2 according to the distance between two adjacent grating units, proceed to step S23. Specifically, before processing the next grating unit, the conductive substrate 2 needs to be moved horizontally by the processing platform, or the output end of the laser can be moved. The moving distance is determined according to the distance between two adjacent grating units.

[0057] After the adjustment is completed, step S23 is executed again to process the new grating unit with the laser beam. This process is repeated until all grating units on the conductive substrate 2 are processed.

[0058] Alternatively, the positions of the grating units to be processed on the conductive substrate 2 can be pre-set. After processing one grating unit, the processing platform moves the conductive substrate 2 to the position of the next grating unit via the substrate 1, and then laser induction is performed again. This cycle continues until the last grating unit is processed, and all grating units on the conductive substrate 2 are processed.

[0059] Step S3 includes the following steps: S31. Use an aqueous solution with added cleaning agent to perform a rough cleaning of the conductive substrate containing multi-period micro / nano gratings. In this process, the surface of a conductive substrate containing multi-period micro / nano gratings is roughly cleaned by adding detergent to an aqueous solution.

[0060] S32. Perform ultrasonic cleaning on the conductive substrate containing multi-period micro / nano gratings after rough cleaning, specifically including: S321. Pour water and glass cleaner into a beaker, then place the roughly washed conductive substrate containing multi-period micro-nano gratings into the beaker. Cover and seal the beaker with plastic wrap, then place the beaker into an ultrasonic cleaner. Set the temperature of the ultrasonic cleaner to 35°C, the ultrasonic time to 20 min, and the power to 100 W for ultrasonic treatment.

[0061] S322. Then, the conductive substrate containing the multi-period micro-nano grating is taken out and placed in a new beaker. Deionized water is injected into the beaker through an ultrapure water device. After covering and sealing the beaker with plastic wrap again, the beaker is placed in an ultrasonic cleaner. The temperature of the ultrasonic cleaner is set to 35°C, the ultrasonic time is set to 20 min, and the power is set to 100 W for ultrasonic treatment.

[0062] S323. Next, pour out the deionized water from the beaker, add anhydrous ethanol to the beaker, cover and seal the beaker with plastic wrap again, and then place the beaker in an ultrasonic cleaner. Set the temperature of the ultrasonic cleaner to 35°C, the ultrasonic time to 20 min, and the power to 100 W for ultrasonic treatment.

[0063] S324. Finally, pour the anhydrous ethanol in the beaker into the waste liquid bucket, add acetone to the beaker, cover and seal the beaker with plastic wrap again, and then put the beaker into the ultrasonic cleaner. Set the temperature of the ultrasonic cleaner to 35℃, the ultrasonic time to 20 min, and the power to 100 W for ultrasonic treatment.

[0064] S325. Finally, pour the acetone in the beaker into the waste liquid bucket, add isopropanol solution to the beaker, cover and seal the beaker with plastic wrap again, and then put the beaker into the ultrasonic cleaner. Set the temperature of the ultrasonic cleaner to 35℃, the ultrasonic time to 20 min, and the power to 100 W for ultrasonic treatment.

[0065] S33. The conductive substrate containing multi-period micro-nano gratings, which has been ultrasonically cleaned, is dried in an oven at 100°C for 12 hours, and then cleaned by an ultraviolet light cleaner for 20 minutes.

[0066] Step S4 includes: S41. A hole transport layer 3 is attached to the outer surface of a conductive substrate containing a multi-period micro / nano grating by spin coating. Specifically, the substrate 1 is placed in a glove box, and the hole transport layer 3 is first spin-coated onto the conductive substrate 2 using spin coating. The hole transport layer 3 has a uniform thickness. When spin-coated onto the conductive substrate 2, since the conductive substrate 2 is fabricated with a multi-period micro / nano grating structure, the hole transport layer 3 is attached to the outer surface of the multi-period micro / nano grating structure, that is, the hole transport layer 3 is attached to the inner wall of the multi-period micro / nano grating structure. The hole transport layer 3 covers the surface of the conductive substrate 2 and the inner wall of the multi-period micro / nano grating structure.

[0067] S42. A perovskite active layer 4 is attached to the surface of the hole transport layer 3 by spin coating, so that the interface of the perovskite active layer 4 forms the target grating structure 8. Specifically, the perovskite active layer 4 is spin-coated on the outer surface of the hole transport layer 3. Similarly, the perovskite active layer 4 is attached to the outer surface of the hole transport layer 3, forming a similar multi-period micro-nano grating structure. The interface of the perovskite active layer 4 forms the target grating structure 8.

[0068] S43. An electron transport layer 5 is bonded to the outer surface of the perovskite active layer 4 by spin coating.

[0069] S5. A metal electrode 6 is deposited on the outer surface of the electron transport layer 5 using a photomask via thermal evaporation; wherein the metal electrode is gold.

[0070] Example 3 Same as Example 1, except that, The distance between adjacent grooves is 1.5 μm; The distance between the bottoms of adjacent strip protrusions is zero, and the distance between their tops is 150 nm; The depth of each groove is 25nm; Each protrusion is 20nm high; The thickness of the perovskite active layer is 350 nm; The thickness of the substrate is 0.5 mm; The conductive substrate is 100 nm thick; The hole transport layer is 2nm thick; The electron transport layer is 25 nm thick; The metal electrode thickness is 80 nm; The conductive substrate is an FTO substrate; The hole transport layer is MeO-6PACz; The electron transport layer is C 60 ; All metal electrodes are made of gold.

[0071] The optoelectronic device provided in this embodiment is prepared using the same method as in Embodiment 2.

[0072] Example 4 Same as Example 1, except that, The distance between adjacent grooves is 2.0 μm; The distance between the bottoms of adjacent strip protrusions is zero, and the distance between their tops is 250 nm; The depth of each groove is 35 nm; Each protrusion is 30nm high; The thickness of the perovskite active layer is 450 nm; The thickness of the substrate is 1.5 mm; The conductive substrate is 150 nm thick; The hole transport layer is 7nm thick; The electron transport layer is 30 nm thick; The metal electrode thickness is 120 nm; The conductive substrate is an ITO substrate; The hole transport layer is PTAA; The electron transport layer is a PCBM; All metal electrodes are made of silver.

[0073] The optoelectronic device provided in this embodiment is prepared using the same method as in Embodiment 2.

[0074] Comparative Example Similar to Example 1, except that there are no multi-period micro / nano gratings on the conductive substrate.

[0075] To illustrate the relevant performance of the optoelectronic device on the multi-period micro / nano grating substrate prepared in Example 2, a comparison with the comparative example is provided in conjunction with the accompanying drawings.

[0076] See Figure 3 As shown, the AFM plot (a) of the multi-period micro / nano grating on the conductive substrate and the structure distribution curve (b) of the multi-period micro / nano grating are presented; from Figure 3 The fabricated multi-period micro / nano grating structure parameters are as follows: the main micron-scale grating period is 2.0 μm, the average groove depth is 30 nm, the groove width is approximately 1.0 μm, and the groove wall slope angle is approximately 97°. Inside the groove, the secondary nanon-scale grating period is 200 ± 30 nm, and the protrusion height is approximately 25 nm.

[0077] See Figure 4 As shown, SEM images of multi-period micro / nano gratings on a conductive substrate are displayed; from Figure 4 As can be seen, the structure exhibits typical multi-period characteristics, with two parallel micron-sized master grating grooves laterally traversing the field of view. The grooves are uniform in width and have continuous edges. In the inner wall and bottom region of the grooves, high spatial frequency laser-induced periodic surface structures (HSFLs) induced by femtosecond lasers can be clearly observed. The nanofibers are densely arranged along the direction of the master grating grooves, exhibiting a quasi-regular periodic distribution.

[0078] Figure 5 , Figure 6 , Figure 7 In this context, "multi-period grating" refers to the optoelectronic device on the multi-period micro / nano grating substrate provided in Example 2; "without multi-period grating" refers to the optoelectronic device provided in the comparative example.

[0079] See Figure 5 As shown, this is a comparison of the external quantum efficiency of perovskite optoelectronic devices with multi-period micro / nano grating structures fabricated using femtosecond laser single-step induction; from Figure 5 It can be seen that the multi-period micro / nano grating structure device exhibits a wide-band EQE enhancement compared to the reference device provided in the comparative example. This enhancement effect can be attributed to the synergistic optical management mechanism of the multi-period structure: the micron-scale grating extends the optical path through diffraction coupling, and the nano-scale LIPSS grating enhances the local optical field. Together, they broaden the effective spectral response range of the device, thereby significantly improving the photoelectric conversion efficiency.

[0080] See Figure 6 As shown, this is a comparison of the responsivity of perovskite optoelectronic devices with multi-period micro / nano grating structures fabricated using femtosecond laser single-step induction; from Figure 6 As can be seen, compared with the reference device provided in the comparative example, the device with the femtosecond laser single-step induced multi-period micro / nano grating structure achieves a significant improvement in responsivity in the visible to near-infrared range. This enhancement effect can be attributed to the synergistic optical management mechanism of the multi-period structure. The micron-scale grating extends the optical path through diffraction coupling, while the nano-scale grating enhances the local optical field. Together, they improve the photon absorption efficiency and photogenerated carrier generation rate of the perovskite photoactive layer, thereby enhancing the device's photoresponse capability.

[0081] See Figure 7 As shown, this is a comparison of the specific detectivity of perovskite optoelectronic devices with multi-period micro / nano grating structures fabricated using femtosecond laser single-step induction; from Figure 7 As can be seen, compared with the reference device provided in the comparative example, the device with the femtosecond laser single-step induced multi-period micro / nano grating structure achieves a significant improvement in specific detectivity in the visible to near-infrared range. The multi-period micro / nano grating structure improves both light capture efficiency and the generation and collection efficiency of photogenerated carriers, allowing the device to maintain its advantage in signal-to-noise ratio and comprehensively optimize its overall photoelectric detection performance.

Claims

1. An optoelectronic device based on a multi-period micro / nano grating substrate, characterized in that, The optoelectronic device comprises, from bottom to top, a conductive substrate, a hole transport layer, a perovskite active layer, an electron transport layer, and a metal electrode stacked in sequence; A multi-period micro / nano grating structure is disposed on the conductive substrate; The multi-period micro / nano grating structure includes multiple equally spaced strip grooves on a conductive substrate, and multiple arrayed strip protrusions at the bottom of each strip groove. Each groove and its internal multiple protrusions form a grating unit; Each of the strip protrusions has a triangular cross-sectional shape; the long side of each of the strip grooves and the long side of each strip protrusion are parallel to the long side of the conductive substrate. Multiple equally spaced strip grooves form a micrometer-scale grating structure; multiple strip protrusions within each strip groove form a nanometer-scale grating structure; the distance between adjacent strip grooves is 1.0~2.0μm; The distance between the bottoms of adjacent strip protrusions is zero, and the distance between the tops is 150~250nm; the depth of each strip groove is 25~35nm; the height of each protrusion is 20~30nm; The bottom of the perovskite active layer extends downward in the region corresponding to the multi-period micro / nano grating structure to form a target grating structure corresponding to the multi-period micro / nano grating structure; the target grating structure is formed by embedding the bottom of the perovskite active layer downward into a strip groove; The hole transport layer is provided between the multi-period micro / nano grating structure and the corresponding target grating structure.

2. The optoelectronic device based on a multi-period micro / nano grating substrate according to claim 1, characterized in that, The thickness of the perovskite active layer is 350~450nm; the material of the perovskite active layer is tin-lead perovskite.

3. The optoelectronic device based on a multi-period micro / nano grating substrate according to claim 1, characterized in that, The thickness of the substrate is 0.5~1.5mm; the thickness of the conductive substrate is 100~150nm; The hole transport layer has a thickness of 2-7 nm; the electron transport layer has a thickness of 25-30 nm; and the metal electrode has a thickness of 80-120 nm.

4. The optoelectronic device based on a multi-period micro / nano grating substrate according to claim 1, characterized in that, The two side walls of each of the strip grooves are inclined, so that the cross-sectional shape of the strip groove is an inverted trapezoid.

5. The optoelectronic device based on a multi-period micro / nano grating substrate according to claim 1, characterized in that, The conductive substrate is an ITO or FTO substrate; the hole transport layer is PTAA or MeO-6PACz; the electron transport layer is PCBM or C 60 The metal electrode is made of silver, copper, aluminum, or gold.

6. The optoelectronic device based on a multi-period micro / nano grating substrate according to claim 1, characterized in that, The conductive substrate is further provided with a base at its bottom, the base being glass or silicon.

7. A method for fabricating an optoelectronic device on a multi-period micro / nano grating substrate as described in any one of claims 1 to 6, characterized in that, Includes the following steps: A multi-period micro / nano grating structure was fabricated in a single step on a conductive substrate using a femtosecond laser-induced method. During the fabrication process, the energy density of the laser beam was determined based on the damage threshold of the conductive substrate. After cleaning the conductive substrate containing the multi-period micro-nano grating structure, a hole transport layer and a perovskite active layer are sequentially prepared by spin coating and then bonded to the outer surface of the multi-period micro-nano grating structure on the conductive substrate, so that the interface between the perovskite active layer and the conductive substrate forms the target grating structure. An electron transport layer is bonded onto the perovskite active layer by spin coating or thermal evaporation. Metal electrodes bonded to the electron transport layer are deposited on the outer surface of the electron transport layer using a photomask via thermal evaporation.

8. The method for fabricating an optoelectronic device on a multi-period micro / nano grating substrate according to claim 7, characterized in that, When fabricating multi-period micro / nano grating structures on a conductive substrate in a single step using a femtosecond laser-induced method, the process includes: The conductive substrate is placed on the displacement platform of the femtosecond laser processing system and leveled. Adjust the parameters of the laser beam according to its energy density; A grating unit is obtained by laser-induced laser on a conductive substrate. The conductive substrate is then moved to process the next grating unit, thus forming a multi-period micro / nano grating structure.

9. The method for fabricating an optoelectronic device on a multi-period micro / nano grating substrate according to claim 8, characterized in that, The laser beam output power is 2mW~18mW, the laser beam pulse width is 100fs~500fs, the repetition frequency is 100kHz~500kHz, and the laser wavelength is 1030nm.

10. The application of a photoelectric device based on a multi-period micro / nano grating substrate as described in any one of claims 1 to 6 in a photodetector.