Conductor jacket and its manufacturing process
Patent Information
- Application Number
- JP2019530129
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2016-12-19
- Filing Date
- 2017-12-18
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2037-12-18
AI Technical Summary
Ethylene-based solution resins (SR resins) used for cable jackets exhibit poor processability and surface smoothness when extruded at typical line speeds, compared to gas phase polymerized resins (GP resins) with broader molecular weight distribution (MWD), leading to unacceptable surface quality in cable jackets.
A manufacturing process that blends ethylene-based polymers with wide and narrow MWD ratios, optionally including carbon black, and extrudes the blend at high velocities to produce conductor jackets with improved surface smoothness and tensile properties.
The process achieves surface smoothness of 20-80 μinches and enhances tensile strength and elongation, while allowing extrusion at speeds exceeding 1.02 m/sec, improving the overall quality and processability of conductor jackets.
Abstract
Description
[Background technology]
[0001] Cables, such as power cables or communication cables, are a type of conductor that includes internal conductive elements such as metal wires or glass fibers, and one or more external layers for shielding and protection. The outermost layer of a cable is typically a protective layer called the outer sheath or outer covering.
[0002] Ethylene-based polymers are known for the manufacture of cable sheaths. Ethylene-based polymers for use in cable sheaths need to have good processability, such as good extrusion characteristics over a wide processing temperature range. Furthermore, such ethylene-based cable sheaths generally need to have good mechanical properties. However, cable sheath compounds made from ethylene-based solution resins (SR resins) do not process well in extruders and result in unacceptable surface smoothness at typical extrusion line speeds when compared to equivalent compounds based on gas-phase polymerized resins (GP resins) with a broader molecular weight distribution (MWD).
[0003] In this technical field, there is a recognized need to diversify and expand the types of polymer resins available for use in cable sheathing applications while maintaining appropriate processability and suitable mechanical and performance characteristics. [Overview of the project]
[0004] This disclosure relates to a manufacturing process for conductive sheaths, such as cable sheaths. The process improves the processability of SR resin by blending it with GP resin and then extruding the blend to produce a conductive sheath having acceptable surface smoothness and improved tensile properties.
[0005] This disclosure provides a process. In one embodiment, the process comprises blending an ethylene polymer with a broad molecular weight distribution (MWD) having an I21 / I2 ratio of 55 to 85 with an ethylene polymer with a narrow MWD having an I21 / I2 ratio of 20 to 50. The process comprises forming a blend component comprising 20% to 45% by weight of the broad MWD ethylene polymer, 80% to 55% by weight of the narrow MWD ethylene polymer, and optional carbon black. The blend component has a density of 0.925 g / cc to 0.955 g / cc and an I21 / I2 ratio of 30 to 55. The process comprises extruding the blend component onto a conductor at a speed greater than 1.02 m / s and forming a conductor sheath having a surface smoothness of 30 μm to 80 μm.
[0006] This disclosure provides an alternative process. In one embodiment, the process comprises blending an ethylene polymer with a broad molecular weight distribution (MWD) having an I21 / I2 ratio of 55 to 85 with an ethylene polymer with a narrow MWD having an I21 / I2 ratio of 20 to 50. The process comprises forming a blend component comprising 20% to 70% by weight of the broad MWD ethylene polymer, 80% to 20% by weight of the narrow MWD ethylene polymer, and optional carbon black. The blend component has a density of 0.925 g / cc to 0.955 g / cc and an I21 / I2 ratio of 15 to 65. The process comprises extruding the blend component onto a conductor at a speed greater than 1.02 m / s and forming a conductor sheath having a surface smoothness of 20 μm to 80 μm.
[0007] definition All references to the periodic table of elements in this specification refer to the periodic table of elements published and copyrighted by CRC Press, Inc., 2003. Similarly, all references to groups refer to the groups reflected in this periodic table of elements, which use the IUPAC system for group numbering. Unless otherwise stated, suggested by the context, or customary in the art, all parts and percentages are based on weight. For the purposes of U.S. patent practice, any patents, patent applications, or publications referenced herein are incorporated herein by reference in their entirety (or their equivalent U.S. editions are incorporated by reference in the same way) with respect to the disclosure of synthesis techniques, definitions (to the extent that they do not conflict with any definitions provided herein), and general knowledge in the art.
[0008] Numerical ranges disclosed herein include all values from and including the lower and upper limits. For ranges containing explicit numbers (e.g., 1, or 2, or 3 to 5, or 6, or 7), any subrange between any two explicit numbers is included (e.g., 1 to 2, 2 to 6, 5 to 7, 3 to 7, 5 to 6, etc.).
[0009] Unless otherwise stated, all parts and proportions are based on weight, and all testing processes are current as of the filing date of this disclosure, unless implicitly stated in the context or customary in the art.
[0010] As used herein, the term “composition” refers to a mixture of materials comprising the composition, as well as reaction and decomposition products formed from the materials of the composition.
[0011] The terms “comprising,” “including,” “having,” and their derivatives are not intended to exclude the existence of any additional components, steps, or procedures, whether or not they are specifically disclosed. To avoid any doubt, all compositions claimed through the use of the term “comprising” may include any additional additives, adjuvants, or compounds, whether polymeric or otherwise, unless otherwise stated. In contrast, the term “essentially consisting of” excludes any other components, steps, or procedures from any subsequent citation except those not essential to the operability. The term “consisting of” excludes any components, steps, or procedures not specifically described or enumerated.
[0012] A "conductor" is one or more wires or one or more fibers for conducting heat, light, and / or electricity. A conductor may be a single wire / fiber or multiple wires / fibers, or may be in the form of stranded wires or tubular wires. Non-limiting examples of suitable conductors include various metals such as carbon, silver, gold, copper, and aluminum. A conductor may also be an optical fiber made from either glass or plastic. A conductor may or may not be housed in a protective sheath. A "cable" is a conductor consisting of two or more wires or two or more optical fibers bundled together and optionally bundled within a common insulating sheath. Individual wires or fibers within the sheath may be exposed, covered, or insulated. Combined cables may contain both electrical wires and optical fibers. Cables may be designed for low, medium, and / or high voltage applications.
[0013] Density is reported as grams per cubic centimeter and measured according to ASTM D 792 (g / cc or g / cm³). 3 ).
[0014] An "ethylene-based polymer" is a polymer containing more than 50 weight percent polymerizable ethylene monomers (based on the total weight of polymerizable monomers) and optionally containing at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymer" and "polyethylene" can be used interchangeably. Non-limiting examples of ethylene-based polymers (polyethylene) include low-density polyethylene (LDPE) and linear polyethylene. Non-limiting examples of linear polyethylene include linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (ULDPE), very low-density polyethylene (VLDPE), multi-component ethylene-based copolymers (EPE), ethylene / α-olefin multiblock copolymers (also known as olefin block copolymers (OBC)), single-site catalyst linear low-density polyethylene (m-LLDPE), substantially linear or linear plastomers / elastomers, medium-density polyethylene (MDPE), and high-density polyethylene (HDPE). Generally, polyethylene can be produced in gas-phase fluidized bed reactors, liquid-phase slurry process reactors, or liquid-phase solution process reactors using heterogeneous catalytic systems such as Ziegler-Natta catalysts, or homogeneous catalytic systems containing ligand structures such as Group IV transition metals and metallocenes, non-metallocene metal centers, heteroaryls, heteroatomic aryloxyethers, and phosphine imines. Combinations of heterogeneous and / or homogeneous catalysts can also be used in either single-reactor or double-reactor configurations.
[0015] "Ethylene plastomer / elastomer" is an ethylene-derived unit and at least one C3-C 10The ethylene plastomer / elastomer is substantially linear, or linear, ethylene / α-olefin copolymer containing a uniform short-chain branched distribution of units derived from α-olefin comonomers, or at least one C4-C8α-olefin comonomer, or at least one C6-C8α-olefin comonomer. The ethylene plastomer / elastomer has a density of 0.870 g / cc, or 0.880 g / cc, or 0.890 g / cc to 0.900 g / cc, or 0.902 g / cc, or 0.904 g / cc, or 0.909 g, or 0.910 g / cc, or 0.917 g / cc. Non-exclusive examples of ethylene plastomers / elastomers include AFFINITY® plastomers and elastomers (available from The Dow Chemical Company), EXACT® plastomers (available from ExxonMobil Chemical), Tafmer® (available from Mitsui), Nexlene® (available from SK Chemicals Co.), and Lucene® (available from LG Chem Ltd.).
[0016] "High-density polyethylene" (or "HDPE") is an ethylene homopolymer, or at least one C4-C 10 The HDPE is an ethylene / α-olefin copolymer having an α-olefin comonomer or C4α-olefin comonomer, and having a density greater than 0.94 g / cc, or 0.945 g / cc, or 0.95 g / cc, or 0.955 g / cc to 0.96 g / cc, or 0.97 g / cc, or 0.98 g / cc. HDPE can be a unimodal copolymer or a multimodal copolymer. A "unimodal ethylene copolymer" has one distinct peak in gel permeation chromatography (GPC) showing the molecular weight distribution of ethylene / C4-C4-Olefin Comonomer. 10 It is an α-olefin copolymer.
[0017] The "coating" is a coating on the conductor.
[0018] "Linear low-density polyethylene" (or "LLDPE") is a unit derived from ethylene and at least one C3-C 10 LLDPE is a linear ethylene / α-olefin copolymer containing a heterogeneous short-chain branching distribution, comprising units derived from α-olefin comonomers, or at least one C4-C8α-olefin comonomer, or at least one C6-C8α-olefin comonomer. In contrast to conventional LDPE, LLDPE is characterized by little, if any, long-chain branching. LLDPE has a density of 0.916 g / cc to 0.925 g / cc. Non-limiting examples of LLDPE include TUFLIN® linear low-density polyethylene resin (available from The Dow Chemical Company), DOWLEX® polyethylene resin (available from Dow Chemical Company), and MARLEX® polyethylene (available from Chevron Phillips).
[0019] "Low-density polyethylene" (or "LDPE") is an ethylene homopolymer or at least one C3-C polymer containing long-chain branches with a density of 0.915 g / cc to 0.925 g / cc and broad MWD. 10 LDPE is an ethylene / α-olefin copolymer containing α-olefins or C3-C4α-olefins. LDPE is typically produced by high-pressure free-radical polymerization (tubular reactors or autoclaves with free-radical initiators). Non-exclusive examples of LDPE include MarFlex® (Chevron Phillips), LUPOLEN® (LyondellBasell), and LDPE products from Borealis, Ineos, ExxonMobil, and others.
[0020] Medium-density polyethylene (or "MDPE") is an ethylene homopolymer, or at least one C3-C polymer, having a density of 0.926 g / cc to 0.940 g / cc. 10 It is an ethylene / α-olefin copolymer containing α-olefin or C3-C4α-olefin.
[0021] The melt index (I2) is measured at 190 °C under a load of 2.16 kg in accordance with ASTM D1238.
[0022] The melt index (I0.5) is measured at 190 °C under a load of 0.5 kg in accordance with ASTM D 1238.
[0023] The melt index (I10) is measured at 190 °C under a load of 10.0 kg in accordance with ASTM D-1238.
[0024] The melt index (I21) is measured at 190 °C under a load of 21.0 kg in accordance with ASTM D 1238.
[0025] Index I21 / I2 or "I21 / I2 ratio". The I21 / I2 ratio is an indirect measure of the viscosity ratio at high and low shear rates and exhibits shear-thinning behavior related to both the molecular weight distribution (MWD) and the presence of long-chain branching, each of which significantly affects processability. Generally, polyethylene containing long-chain branching has high melt strength, exhibits low viscosity under high shear rate conditions, and allows for higher processing speeds compared to polyethylene having little or no long-chain branching.
[0026] "Multi-component ethylene copolymer" (or "EPE") refers to units derived from ethylene and at least one C3-C as described in patent documents USP6,111,023, USP5,677,383, and USP6,984,695. 10It contains units derived from an α-olefin comonomer, or at least one C4-C8 α-olefin comonomer, or at least one C6-C8 α-olefin comonomer. The EPE resin has a density of 0.905 g / cc, or 0.908 g / cc, or 0.912 g / cc, or 0.920 g / cc to 0.926 g / cc, or 0.929 g / cc, or 0.940 g / cc, or 0.962 g / cc. Non-limiting examples of the EPE resin include ELITE™ enhanced polyethylene (available from The Dow Chemical Company), ELITE AT™ advanced technology resin (available from The Dow Chemical Company), SURPASS™ polyethylene (PE) resin (available from Nova Chemicals), and SMART™ (available from SK Chemicals Co.).
[0027] A "multimodal ethylene copolymer" is an ethylene / C4-C α-olefin copolymer having at least two different peaks in GPC showing the molecular weight distribution. 10 It is an α-olefin copolymer. Multimodality includes copolymers having two peaks (bimodal) and copolymers having three or more peaks. Non-limiting examples of HDPE include DOW™ high density polyethylene (HDPE) resin (available from The Dow Chemical Company), ELITE™ enhanced polyethylene resin (available from The Dow Chemical Company), CONTINUUM™ bimodal polyethylene resin (available from Dow Chemical Company), LUPOLEN™ (available from LyondellBasell), and HDPE products from Borealis, Ineos, and ExxonMobil.
[0028] As used herein, “olefin polymer” is a polymer containing more than 50 mol percent of polymerizable olefin monomers (based on the total amount of polymerizable monomers) and optionally containing at least one comonomer. Non-limiting examples of olefin polymers include ethylene polymers and propylene polymers.
[0029] A "polymer" is a compound prepared by polymerizing monomers, whether of the same or different types, resulting in multiple and / or repeating "units" or "mer units" that constitute the polymer in its polymeric form. Therefore, the general term polymer includes the term homopolymer and is typically used to refer to polymers prepared from only one type of monomer, while the term copolymer typically refers to polymers prepared from at least two types of monomers. It also encompasses all forms of copolymers, including random, block, etc. The terms "ethylene / α-olefin polymer" and "propylene / α-olefin polymer" refer to the aforementioned copolymers and one or more additional polymerizable α-olefin monomers prepared by polymerizing ethylene or propylene, respectively. While polymers are often referred to as being "made from" one or more specific monomers, such as "based on" a particular monomer or type of monomer, or "containing" a particular monomer content, it should be noted that in this context, the term "monomer" is understood to refer to the polymerization residue of a specified monomer and does not refer to non-polymerized species. In general, polymers as used herein refer to those based on "units," which are the polymerized forms of the corresponding monomers.
[0030] A "propylene-based polymer" is a polymer that contains more than 50 mole percent of polymerized propylene monomer (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer.
[0031] "Single-site catalyst linear low-density polyethylene" (or "m-LLDPE") is an ethylene-derived unit and at least one C3-C 10m-LLDPE is a linear ethylene / α-olefin copolymer containing a uniform short-chain branched distribution, comprising units derived from α-olefin comonomers, or at least one C4-C8α-olefin comonomer, or at least one C6-C8α-olefin comonomer. m-LLDPE has densities of 0.913 g / cc, or 0.918 g / cc, or 0.920 g / cc to 0.925 g / cc, or 0.940 g / cc. Non-limiting examples of m-LLDPE include EXCEED® metallocene PE (available from ExxonMobil Chemical), LUFLEXEN® m-LLDPE (available from LyondellBasell), and ELTEX® PF m-LLDPE (available from Ineos Olefins & Polymers).
[0032] Surface smoothness. The surface smoothness of the conductive sheath is measured in accordance with ANSI 1995 using a Surftest SV-400 series 178 surface texture measuring instrument. The wire sample is placed in a V-block, and the stylus (10urn) is lowered to a specific starting position (applying a force of approximately 1 gram to the wire). Measurement is taken by moving the stylus laterally at a fixed speed of 2 (millimeters per second). Four readings are taken per wire sample, and four samples are tested, then averaged to the reported value in microinches.
[0033] Tensile properties. The compositions can be characterized by their tensile strength at break (megapascals, MPa) and elongation at break (%) ("TE"). Tensile strength ("TS") and elongation at break are measured according to the ASTM D638 test procedure for compression molded specimens prepared in accordance with ASTM D4703. Elongation at break, or elongation to break, is the strain of the specimen at break, expressed as a percentage.
[0034] Where used herein, Tm or “melting point” (also referred to as the melting peak in relation to the shape of the plotted DSC curve) is measured by DSC (Differential Scanning Calorimetry) techniques for measuring the melting point or melting peak of polyolefins, as described in USP 5,783,638. Note that many blends containing two or more polyolefins have one or more melting points or melting peaks, and many individual polyolefins have only one melting point or melting peak.
[0035] "Ultra low density polyethylene" (or "ULDPE") and "very low density polyethylene" (or "VLDPE") are defined as having ethylene-derived units and at least one C3-C group, respectively. 10 These are linear ethylene / α-olefin copolymers containing a heterogeneous short-chain branched distribution, comprising α-olefin comonomers, or units derived from at least one C4-C8α-olefin comonomer, or at least one C6-C8α-olefin comonomer. ULDPE and VLDPE have densities of 0.885 g / cc, or 0.90 g / cc to 0.915 g / cc, respectively. Non-limiting examples of ULDPE and VLDPE include ATTANE® ultra-low density polyethylene resin (available from The Dow Chemical Company) and FLEXOMER® ultra-low density polyethylene resin (available from The Dow Chemical Company). [Modes for carrying out the invention]
[0036] This disclosure provides a process for manufacturing a conductor sheath. In one embodiment, the process comprises blending an ethylene polymer with a broad molecular weight distribution (MWD) having an I21 / I2 ratio of 55 to 85 with an ethylene polymer with a narrow MWD having an I21 / I2 ratio of 20 to 50. The process comprises forming a blend component comprising 20% to 45% by weight of the broad MWD ethylene polymer, 80% to 55% by weight of the narrow MWD ethylene polymer, and optional carbon black. The blend component has a density of 0.925 g / cc to 0.955 g / cc and an I21 / I2 ratio of 30 to 55. The process comprises extruding the blend component onto a conductor at a speed exceeding 1.02 meters per second (m / s) (i.e., 200 feet / minute (ft / min)). The process comprises forming a conductor sheath having a surface smoothness of 30 μinch to 80 μinch.
[0037] This disclosure provides an alternative manufacturing process for a conductor sheath. In one embodiment, the process comprises blending an ethylene polymer with a broad molecular weight distribution (MWD) having an I21 / I2 ratio of 55 to 85 with an ethylene polymer with a narrow MWD having an I21 / I2 ratio of 20 to 50. The process comprises forming a blend component comprising 20% to 70% by weight of the broad MWD ethylene polymer, 80% to 20% by weight of the narrow MWD ethylene polymer, and optionally, 0% to 10% by weight of carbon black. The blend component has a density of 0.925 g / cc to 0.955 g / cc and an I21 / I2 ratio of 15 to 65. The process comprises extruding the blend component onto a conductor at a speed exceeding 1.02 meters per second (m / s) (i.e., 200 feet / minute (ft / min)). The process comprises forming a conductor sheath having a surface smoothness of 20 μinch to 80 μinch.
[0038] 1. Ethylene-based polymers of broad and narrow MWD. This process involves blending broad-molecular-weight-distribution (MWD) ethylene polymers with narrow-molecular-weight-distribution (MWD) ethylene polymers. A "broad-molecular-weight-distribution ethylene polymer" or "broad-molecular-weight-distribution ethylene polymer" is an ethylene polymer having an I21 / I2 ratio of 55 to 85. A "narrow-molecular-weight-distribution ethylene polymer" or "narrow-molecular-weight-distribution ethylene polymer" is an ethylene polymer having an I21 / I2 ratio of 20 to 50.
[0039] Ethylene-based polymers may be ethylene homopolymers or ethylene / α-olefin copolymers. Non-limiting examples of α-olefin comonomers suitable for ethylene-based polymers include C3-C 20 α-olefin, or C4-C 12 Examples include α-olefins or C4-C8 α-olefins. Further non-limiting examples of suitable α-olefin comonomers include propylene, butene, methyl-1-pentene, hexene, octene, decene, dodecene, tetradecene, hexadecene, octadecene, cyclohexyl-1-propene (allylcyclohexane), vinylcyclohexane, and combinations thereof. In one embodiment, the α-olefin comonomer for ethylene-based polymers is selected from butene, hexene, or octene.
[0040] In one embodiment, the broad MWD ethylene-based elastomer is an ethylene / C4-C8α-olefin copolymer having one, some, or all of the following properties:
[0041] (i) a density of 0.915 g / cc, or 0.920 g / cc, or 0.925 g / cc, or 0.930 g / cc, or 0.933 g / cc to 0.935 g / cc, or 0.937 g / cc, and / or
[0042] (ii) I2 of 0.5g / 10 min, or 0.6g / 10 min, or 0.65g / 10 min, or 0.7g / 10 min to 0.8g / 10 min, or 0.9g / 10 min, and / or
[0043] (iii) I21 of 35g / 10 min, or 40g / 10 min, or 45g / 10 min, or 50g / 10 min to 55g / 10 min, or 60g / 10 min, or 65g / 10 min, or 70g / 10 min, or 75g / 10 min, and / or
[0044] (iv) I21 / I2 at 55, or 60, or 65–70, or 75, or 80, or 85.
[0045] In one embodiment, the broad MWD ethylene polymer is an ethylene / C4-C8α-olefin copolymer, which is medium-density polyethylene or "broad MWD MDPE". The broad MDPE has one, some, or all of the following properties:
[0046] (i) a density of 0.933 g / cc, or 0.935 g / cc to 0.937 g / cc, and / or
[0047] (ii) I2 of 0.5g / 10 min, or 0.65g / 10 min, or 0.8g / 10 min to 1.0g / 10 min, or 1.5g / 10 min, and / or
[0048] (iii) I21 of 45g / 10 min, or 49g / 10 min, or 50g / 10 min to 52g / 10 min, or 54g / 10 min, or 55g / 10 min, and / or
[0049] (iv) I21 / I2 at 60, or 65, or 70–75, or 80.
[0050] In one embodiment, the broad MWD ethylene polymer is an ethylene / C4-C8α-olefin copolymer, which is linear low-density polyethylene or "broad MWD LLDPE". The broad LLDPE has one, some, or all of the following properties:
[0051] (i) a density of 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, and / or
[0052] (ii) I2 of 0.5g / 10 min, or 0.65g / 10 min, or 0.8g / 10 min to 1.0g / 10 min, or 1.5g / 10 min, and / or
[0053] (iii) I21 of 45g / 10 min, or 49g / 10 min, or 50g / 10 min to 52g / 10 min, or 54g / 10 min, or 55g / 10 min, and / or
[0054] (iv) I21 / I2 at 60, or 65, or 70–75, or 80.
[0055] In one embodiment, the ethylene-based polymer of narrow MWD is an ethylene / C4-C8α-olefin copolymer, which is linear low-density polyethylene or "LLDPE of narrow MWD". LLDPE of narrow MWD has one, some, or all of the following properties:
[0056] (i) Density of 0.915 g / cc, or 0.917 g / cc, or 0.918 g / cc to 0.919 g / cc,
[0057] (ii) I2 of 0.5g / 10 min, 0.9g / 10 min, 1.0g / 10 min, or 1.5g / 10 min, 2.0g / 10 min to 2.3g / 10 min, or 2.5g / 10 min, or 2.9g / 10 min, or 3.0g / 10 min, and / or
[0058] (iii) I21 of 35g / 10 min, or 40g / 10 min, or 50g / 10 min, or 60g / 10 min, or 61g / 10 min to 70g / 10 min, or 71g / 10 min, or 80g / 10 min, or 85g / 10 min, or 87g / 10 min, or 90g / 10 min, and / or
[0059] (iv) I21 / I2 ratio of 20, or 25, or 27, or 30, or 31–35, or 39, or 40, or 45, or 50.
[0060] In one embodiment, the ethylene-based polymer of narrow MWD is an ethylene / C4-C8α-olefin copolymer, which is medium-density polyethylene or "MDPE". The MDPE of narrow MWD has one, some, or all of the following properties:
[0061] (i) a density of 0.933 g / cc, or 0.935 g / cc to 0.937 g / cc, and / or
[0062] (ii) I2 of 2.2g / 10 min, or 2.3g / 10 min, or 2.5g / 10 min to 2.8g / 10 min, and / or
[0063] (iii) I21 of 30g / 10 min, or 33g / 10 min to 35g / 10 min, or 37g / 10 min, or 40g / 10 min, and / or
[0064] (iv) I21 / I2 from 25, or 27, or 28, or 30.
[0065] 2. Blending ingredients This process involves blending broad-MWD ethylene polymers and narrow-MWD ethylene polymers to form a blended component. In one embodiment, the blending is carried out by melt blending. "Melted blending" is a process by which at least two components are combined or otherwise mixed together, with at least one of the components in a molten state. Melted blending can be achieved by batch mixing, extrusion blending, extrusion molding, and any combination thereof.
[0066] In one embodiment, the blend component comprises 20% by weight, or 25% by weight, or 30% to 30% by weight, or 35% by weight, or 40% by weight, or 45% by weight, of a broad MWD ethylene polymer, and 80% by weight, or 75% by weight, or 79% to 65% by weight, or 60% by weight, or 55% by weight, of a narrow MWD ethylene polymer. The blend component also comprises 1% by weight, or 2% by weight, or 3% by weight, or 5% to 7% by weight, or 9% by weight, or 10% by weight, of carbon black. A non-limiting example of a suitable carbon black is DFNA-0037BK. The blended components have a density of 0.925 g / cc, or 0.930 g / cc, or 0.935 g / cc, or 0.940 g / cc to 0.945 g / cc, or 0.950 g / cc, or 0.955 g / cc, and an I21 / I2 ratio of 30, or 32, or 34, or 36, or 38, or 40, or 42, or 45 to 46, or 48, or 50, or 52, or 55.
[0067] In another embodiment, the blend component comprises 20% by weight, or 25% by weight, or 30% by weight, or 35% by weight, or 40% by weight, or 45% to 50% by weight, or 55% by weight, or 60% by weight, or 65% by weight, or 70% by weight of an ethylene polymer with a broad MWD, and 80% by weight, or 75% by weight, or 79% by weight, or 65% by weight, or 60% by weight, or 55% by weight, or 50% by weight, or 49% by weight, or 45% to 40% by weight, or 35% by weight, or 30% by weight, or 25% by weight, or 20% by weight of an ethylene polymer with a narrow MWD. The blended components have a density of 0.925 g / cc, or 0.930 g / cc, or 0.933 g / cc, or 0.935 g / cc, or 0.940 g / cc to 0.945 g / cc, or 0.948 g / cc, or 0.950 g / cc, or 0.955 g / cc, and an I21 / I2 ratio of 15, or 17, or 20, or 30, or 32, or 34, or 36, or 38, or 40, or 45 to 50, or 52, or 55, or 60, or 62, or 65.
[0068] In another embodiment, the blend components include 20% by weight, or 25% by weight, or 30% by weight, or 35% by weight, or 40% by weight, or 45% to 50% by weight, or 55% by weight, or 60% by weight, or 65% by weight, or 70% by weight of a broad MWD ethylene polymer, 80% by weight, or 75% by weight, or 79% by weight, or 65% by weight, or 60% by weight, or 55% by weight, or 50% by weight, or 49% by weight, or 45% to 40% by weight, or 35% by weight, or 30% by weight, or 25% by weight, or 20% by weight of a narrow MWD ethylene polymer, and 1% by weight, or 2% by weight, or 3% by weight, or 5% to 7% by weight, or 9% by weight, or 10% by weight of carbon black. The individual weight percentages of broad MWD ethylene polymers, narrow MWD ethylene polymers, and carbon black are considered to be 100% by weight of the blend components (including any additives). The blend components have a density of 0.925 g / cc, or 0.930 g / cc, or 0.933 g / cc, or 0.935 g / cc, or 0.940 g / cc to 0.945 g / cc, or 0.948 g / cc, or 0.950 g / cc, or 0.955 g / cc, and an I21 / I2 ratio of 15, or 17, or 20, or 30, or 32, or 34, or 36, or 38, or 40, or 45 to 50, or 52, or 55, or 60, or 62, or 65.
[0069] The blended components may contain one or more optional additives. Non-limiting examples of suitable additives include antioxidants, colorants, ultraviolet (UV) absorbers or stabilizers, anti-blocking agents, flame retardants, compatibilizers, plasticizers, fillers, processing aids, and combinations thereof.
[0070] In one embodiment, the blend component includes an antioxidant. Non-limiting examples of suitable antioxidants include phenolic antioxidants, thio antioxidants, phosphoric acid antioxidants, and hydrazine-based metal deactivators. In further embodiments, the blend component includes an antioxidant such as IRGANOX 1035, present in an amount of 0.1% by weight, or 0.2% to 0.3% by weight, based on the total weight of the blend component.
[0071] In one embodiment, the blend components include a filler. Non-limiting examples of suitable fillers include zinc oxide, zinc borate, zinc molybdate, zinc sulfide, organic clay, and combinations thereof. The filler may or may not have flame-retardant properties.
[0072] In one embodiment, the blend component includes processing aids. Non-limiting examples of suitable processing aids include oils, organic acids (such as stearic acid), and metal salts of organic acids (such as zinc stearate). In further embodiments, the blend component includes processing aids such as DYNAMAR FX 5912, present in an amount of 0.01% by weight, or 0.05% by weight, or 0.1% to 0.15% by weight, or 0.17% by weight, or 0.2% by weight, based on the total weight of the blend component.
[0073] In one embodiment, the blend component comprises 20% to 45% by weight of a broad MWD ethylene polymer, 80% to 55% by weight of a narrow MWD ethylene polymer, and 1% to 10% by weight of carbon black, wherein the broad MWD ethylene polymer, the narrow MWD ethylene polymer, and the carbon black constitute 100% by weight of the blend component (including any additives). The blend component has a density of 0.925 g / cc, or 0.930 g / cc, or 0.935 g / cc to 0.940 g / cc, or 0.950 g / cc, or 0.955 g / cc, and an I21 / I2 ratio of 30, or 34 to 37, or 40, or 43, or 45, or 47, or 49, or 50, or 52, or 55.
[0074] In one embodiment, the blend components include 20% to 45% by weight, or 55% by weight, or 70% by weight of broad MWD ethylene polymers, 80% to 55% by weight, or 49% by weight, or 45% by weight, or 30% by weight, or 25% by weight, or 20% by weight of narrow MWD ethylene polymers, and 0% by weight, or 1% to 10% by weight of carbon black, wherein the broad MWD ethylene polymers, narrow MWD ethylene polymers, and carbon black constitute 100% by weight of the blend components (including any additives). The blended components have a density of 0.925 g / cc, or 0.930 g / cc, or 0.933 g / cc, or 0.935 g / cc, or 0.940 g / cc to 0.945 g / cc, or 0.948 g / cc, or 0.950 g / cc, or 0.955 g / cc, and an I21 / I2 ratio of 15, or 17, or 20, or 30, or 32, or 34, or 36, or 38, or 40, or 45 to 50, or 52, or 55, or 60, or 62, or 65.
[0075] In one embodiment, the blend component is either propylene-free or otherwise does not contain propylene.
[0076] In one embodiment, the blend component is either devoid of high-density ethylene or "HDPE," or otherwise does not contain high-density ethylene or "HDPE."
[0077] 3. Extrusion This process includes extruding the blended components onto the conductor at a speed exceeding 1.02 meters per second (m / s) (200 feet per minute (ft / min)), and forming a conductor sheath with a surface smoothness of 25 microinches, 30 microinches, 35 microinches, 40 microinches, 50 to 60 microinches, or 70 microinches, 80 microinches.
[0078] The extrusion process is carried out by an extruder. The extruder has a crosshead die, which provides the desired thickness of the layer (wall or coating). Non-limiting examples of extruders that can be used include single-screw extruders modified with a crosshead die, cooler, and continuous winding device. A typical single-screw extruder can be described as having a hopper at its upstream end and a die at its downstream end. The hopper feeds into the barrel containing the screw. At the downstream end, between the end of the screw and the die, there is a screen pack and a breaker plate. The screw section of the extruder can be considered to be divided into three sections: a feed section, a compression section, and a metering section, as well as multiple heating zones from the rear heating zone to the front heating zone, associated with multiple sections from upstream to downstream. The barrel length-to-diameter ratio is in the range of 16:1 to 30:1. Grooved barrel extruders or twin-screw extruders can also be used in core material coating processes. The extrusion process can be carried out at temperatures ranging from 160°C, 180°C, 200°C–220°C, 240°C, or 260°C. The crosshead die distributes the blend components into the flow channels so that the molten blend components exit at a uniform rate and are applied to the conductor. In this way, blending (molten blending) and extrusion are performed in the same single extruder. As the conductor passes through the center of the crosshead and exits, a uniform layer of the blend components is applied circumferentially using either tube-on tool pressure or half-pressure. One or more layers of the blend components (or other materials) can be applied using multiple crossheads. The coated conductor is then thoroughly cooled in a water trough to prevent deformation of the applied blend component layer on the winding reel and to obtain the conductor sheath.
[0079] The molten blend may be carried out sequentially before extrusion. Alternatively, the molten blend may be carried out simultaneously with or substantially simultaneously with extrusion (i.e., the molten blend and extrusion are carried out in the same extruder). Carbon black may be added during the molten blend and / or during extrusion.
[0080] The extrusion speed is greater than 1.02 m / sec (>200 feet / min). In one embodiment, the extrusion speed is greater than 1.02 m / sec, or 1.14 m / sec, or 1.27 m / sec, or 1.40 m / sec to 1.52 m / sec, or 1.65 m / sec.
[0081] This process involves forming a conductor sheath. The conductor sheath consists of blended components. The conductor sheath has a surface smoothness of 25 μinch, or 30 μinch, or 35 μinch, or 40 μinch, or 50 μinch to 60 μinch, or 70 μinch, or 80 μinch.
[0082] In one embodiment, the cable sheath, consisting of a blended component, has a thickness of approximately 0.508 mm, or 0.762 mm, or 1.016 mm, or 1.27 mm to 1.524 mm, or 1.778 mm, or 2.032 mm, or 2.286 mm, or 2.54 mm, and has an extrusion rate greater than 1.02 m / s, or 1.14 m / s, or 1.27 m / s to 1.40 m / s, or 1.52 m / s, or 1.65 m / s. In further embodiments, the conductor sheath lacks a propylene-based polymer and / or HDPE.
[0083] In one embodiment, the process involves blending linear low-density polyethylene (LLDPE) with a broad MWD having a density of 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, and an I21 / I2 ratio of 73, or 75 to 77, with LLDPE with a narrow MWD having a density of 0.915 g / cc, or 0.920 g / cc to 0.924 g / cc, and an I21 / I2 ratio of 30, or 33 to 35. The process involves forming a blended component comprising 20% by weight, or 25% by weight, or 30% by weight, or 35% to 40% by weight, or 45% by weight of broad MWD LLDPE, 70% by weight, or 65% by weight, or 60% to 55% by weight, or 50% by weight of narrow MWD LLDPE, and 1% by weight, or 2% by weight, or 3% by weight, or 4% to 5% by weight, or 6% or 7% by weight of carbon black. The blended component has a density of 0.925 g / cc, or 0.930 g / cc to less than 0.935 g / cc, and an I21 / I2 ratio of 30, or 35, or 40, or 45 to 50, or 55. This process includes extruding the blended components onto the conductor at a speed exceeding 1.02 m / s (or 1.52 m / s) and forming a conductor sheath with a surface smoothness of 30 μinch, 40 μinch, 50 μinch to 60 μinch, 70 μinch, or 80 μinch.
[0084] In one embodiment, the process involves blending linear low-density polyethylene (LLDPE) with a broad MWD having a density of 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, and an I21 / I2 ratio of 73, or 75 to 77, with LLDPE with a narrow MWD having a density of 0.915 g / cc, or 0.920 g / cc to 0.924 g / cc, and an I21 / I2 ratio of 20, or 24, or 30, or 33 to 35. The process involves forming a blend component comprising 20% by weight, or 25% by weight, or 30% by weight, or 35% to 40% by weight, or 45% by weight, or 50% by weight, or 55% by weight, or 60% by weight, or 65% by weight, or 70% by weight of broad MWD LLDPE; 70% by weight, or 65% by weight, or 60% to 55% by weight, or 50% by weight, or 49% by weight, or 45% by weight, or 40% by weight, or 35% by weight, or 30% by weight, or 25% by weight, or 20% by weight of narrow MWD LLDPE; and 1% by weight, or 2% by weight, or 3% by weight, or 4% to 5% by weight, or 6% by weight, or 7% by weight of carbon black. The blended component has a density of 0.925 g / cc, or 0.930 g / cc, or 0.933 g / cc to 0.935 g / cc, or 0.940 g / cc, or 0.945 g / cc, or 0.948 g / cc, or 0.950 g / cc, or 0.955 g / cc, and an I21 / I2 ratio of 30, or 32, or 34, or 36, or 38, or 40, or 45 to 50, or 52, or 55, or 60, or 62, or 65. The process includes extruding the blended component onto a conductor at a speed exceeding 1.02 m / s (or 1.52 m / s) and forming a conductor sheath having a surface smoothness of 30 μinch, or 40 μinch, or 50 μinch to 60 μinch, or 70 μinch, or 80 μinch.
[0085] In one embodiment, the process involves blending linear low-density polyethylene (LLDPE) with a broad MWD having a density of 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, and an I21 / I2 ratio of 73, or 75 to 77, with LLDPE with a narrow MWD having a density of 0.915 g / cc, or 0.917 g / cc to 0.920 g / cc, and an I21 / I2 ratio of 30, or 31 to 33. The process involves forming a blended component comprising 23 wt%, or 25 wt%, or 30 wt%, or 35 wt% to 40 wt%, or 45 wt% of broad MWD LLDPE, 70 wt%, or 65 wt%, or 60 wt% to 55 wt%, or 50 wt% of narrow MWD LLDPE, and 1 wt%, or 2 wt%, or 3 wt%, or 4 wt% to 5 wt%, or 6 wt%, or 7 wt% of carbon black. The blended component has a density of 0.925 g / cc, or 0.930 g / cc to less than 0.935 g / cc, and an I21 / I2 ratio of 33, or 35, or 37 to 39, or 40, or 42. This process includes extruding the blended components onto the conductor at a speed exceeding 1.02 m / s (or 1.52 m / s) and forming a conductor sheath with a surface smoothness of 45 μinch, 50 μinch, 55 μinch, 60 μinch, 65 μinch to 70 μinch, 75 μinch, or 80 μinch (hereinafter referred to as Process A).
[0086] In one embodiment, process A includes forming a conductive sheath having a tensile strength of 20.0 MPa, or 21 MPa to 22.0 MPa, and a tensile elongation of 825%, or 850%, or 870% to 900%, or 910%.
[0087] In one embodiment, the process involves blending linear low-density polyethylene (LLDPE) with a broad MWD having a density of 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, and an I21 / I2 ratio of 73, or 75 to 77, with LLDPE with a narrow MWD having a density of 0.915 g / cc, or 0.917 g / cc to 0.920 g / cc, and an I21 / I2 ratio of 30, or 31 to 33. The process involves forming a blended component comprising 23 wt%, or 25 wt%, or 30 wt%, or 35 wt% to 40 wt%, or 45 wt% of broad MWD LLDPE, 70 wt%, or 65 wt%, or 60 wt% to 55 wt%, or 50 wt% of narrow MWD LLDPE, and 1 wt%, or 2 wt%, or 3 wt%, or 4 wt% to 5 wt%, or 6 wt%, or 7 wt% of carbon black. The blended component has a density of 0.925 g / cc, or 0.930 g / cc to less than 0.935 g / cc, and an I21 / I2 ratio of 35, or 40, or 45 to 50, or 55. This process includes extruding the blended components onto the conductor at a speed exceeding 1.02 m / s (or 1.52 m / s) and forming a conductor sheath with a surface smoothness of 35 μm, or 40 μm to 45 μm, or 50 μm (hereafter referred to as Process B).
[0088] In one embodiment, process B includes forming a conductive sheath having a tensile strength of 19.0 MPa, or 20.0 MPa to 21.0 MPa, or 23.0 MPa, and a tensile elongation of 780%, or 800% to 820%, or 850%, or 870%.
[0089] In one embodiment, the process involves blending a broad-MWD medium-density polyethylene (MDPE) having a density of 0.933 g / cc, or 0.935 g / cc to less than 0.937 g / cc, and an I21 / I2 ratio of 55, or 60, or 65 to 70, or 75, with a narrow-MWD ethylene polymer having a density of 0.920 g / cc, or 0.925 g / cc to 0.930 g / cc, or 0.935 g / cc, and an I21 / I2 ratio of 25, or 30 to 35, or 40. This process involves forming a blended component comprising 35 wt% or 40 wt% to 50 wt% or 55 wt% broad MWD MDPE, 50 wt% or 45 wt% to 40 wt% narrow MWD ethylene polymer, and 1 wt% or 2 wt% or 3 wt% or 4 wt% to 5 wt% or 6 wt% or 7 wt% carbon black. The blended component has a density of 0.935 g / cc or 0.940 g / cc to less than 0.945 g / cc and an I21 / I2 ratio of 35 or 40 to 50 or 55. This process also includes extruding the blended component onto a conductor at a speed greater than 1.02 m / s (or 1.52 m / s) and forming a conductor sheath having a surface smoothness of 40 μinch or 45 μinch or 50 μinch to 55 μinch or 60 μinch (hereafter referred to as Process C).
[0090] In one embodiment, process C includes forming a conductive sheath having a tensile strength of 27 MPa, or 29 MPa to 30 MPa, and a tensile elongation of 830%, or 850%, or 880%, 900%, to 920%, or 950%, or 970%.
[0091] In one embodiment, the process comprises blending broad-MWD medium-density polyethylene (MDPE) having a density of 0.933 g / cc, or 0.935 g / cc to 0.937 g / cc, and an I21 / I2 ratio of 63, or 65 to 67, with narrow-MWD MDPE having a density of 0.933 g / cc, or 0.935 g / cc to 0.937 g / cc, and an I21 / I2 ratio of 25, or 27 to 30. The process comprises forming a blend component comprising 35 wt%, or 40 wt% to 45 wt%, or 50 wt%, of broad-MWD MDPE, 65 wt%, or 60 wt%, or 55 wt% to 50 wt%, or 45 wt%, of narrow-MWD MDPE, and 1 wt%, or 2 wt%, or 3 wt%, or 4 wt% to 5 wt%, or 6 wt%, or 7 wt%, of carbon black. The blended components have a density of 0.935 g / cc, or 0.937 g / cc, or 0.940 g / cc to less than 0.945 g / cc, and an I21 / I2 ratio of 40, or 43 to 45. This process includes extruding the blended components onto the conductor at a speed greater than 1.02 m / s (or 1.52 m / s) and forming a conductor sheath with a surface smoothness of 50 μinch, or 55 μinch to 60 μinch (hereafter referred to as Process D).
[0092] In one embodiment, process D includes forming a conductive sheath having a tensile strength of 27 MPa, or 29 MPa to 30 MPa, and a tensile elongation of 860%, or 880%, or 900% to 920%, or 950%, or 970%.
[0093] In one embodiment, the process involves blending linear low-density polyethylene (LLDPE) with a broad MWD having a density of 0.915 g / cc, or 0.920 g / cc to 0.925 g / cc, and an I21 / I2 ratio of 73, or 75 to 77, with LLDPE with a narrow MWD having a density of 0.915 g / cc, or 0.917 g / cc to 0.920 g / cc, and an I21 / I2 ratio of 20, or 24 to 25, or 30, or 35. This process involves forming a blend component containing 30% by weight, or 35% by weight, or 40% by weight, or 45% by weight, or 50% by weight, or 55% to 60% by weight, or 65% by weight, or 70% by weight of broad MWD LLDPE; 70% by weight, or 65% by weight, or 60% by weight, or 55% by weight, or 50% by weight, or 49% by weight, or 45% to 40% by weight, or 35% by weight, or 30% by weight, or 25% by weight, or 20% by weight of narrow MWD LLDPE; and 1% by weight, or 2% by weight, or 3% by weight, or 4% to 5% by weight, or 6% by weight, or 7% by weight of carbon black. The blended component has a density of 0.925 g / cc, or 0.930 g / cc to 0.933 g / cc, or 0.934 g / cc, and an I21 / I2 ratio of 35, or 40, or 43 to 58, or 60, or 65. This process includes extruding the blended component onto the conductor at a speed exceeding 1.02 m / s (or 1.52 m / s) and forming a conductor sheath having a surface smoothness of 45 μinch, or 50 μinch, or 55 μinch, 60 μinch, or 65 μinch to 70 μinch, or 75 μinch, or 80 μinch (hereafter referred to as Process E).
[0094] In one embodiment, process E includes forming a conductive sheath having a tensile strength of 15.0 MPa, or 16.0 MPa, or 16.2 MPa to 18.0 MPa, or 20.0 MPa, or 25.0 MPa, and a tensile elongation of 625%, or 650%, or 651% to 665%, or 670%, or 680%, or 700%.
[0095] In one embodiment, the process involves blending broad-MWD medium-density polyethylene (MDPE) having a density of 0.933 g / cc, or 0.935 g / cc to 0.937 g / cc, and an I21 / I2 ratio of 63, or 65 to 67, with narrow-MWD MDPE having a density of 0.933 g / cc, or 0.935 g / cc to 0.937 g / cc, and an I21 / I2 ratio of 25, or 27 to 30. The process involves forming a blend component comprising 35% by weight, or 40% by weight, or 45% by weight, or 50% to 55% by weight, or 60% by weight, or 65% by weight, or 70% by weight of broad MWD MDPE; 65% by weight, or 60% by weight, or 55% by weight, or 50% by weight, or 49% to 45% by weight, or 40% by weight, or 35% by weight, or 30% by weight, or 25% by weight, or 20% by weight of narrow MDPE; and 1% by weight, or 2% by weight, or 3% by weight, or 4% to 5% by weight, or 6% by weight, or 7% by weight of carbon black. The blended component has a density of 0.935 g / cc, or 0.937 g / cc, or 0.940 g / cc to 0.945 g / cc, or 0.950 g / cc, and an I21 / I2 ratio of 15, or 17 to 18, or 20, or 25, or 30, or 35. This process includes extruding the blended component onto a conductor at a speed exceeding 1.02 m / s (or 1.52 m / s) and forming a conductor sheath having a surface smoothness of 20 μinch, or 25 μinch to 30 μinch, or 40 μinch (hereafter referred to as Process F).
[0096] In one embodiment, process F includes forming a conductive sheath having a tensile strength of 25 MPa, or 26 MPa, or 27 MPa, or 29 MPa to 30 MPa, and a tensile elongation of 800%, or 807% to 810%, or 820%, or 860%, or 880%, or 900%.
[0097] In one embodiment, the process involves blending broad-MWD medium-density polyethylene (MDPE) having a density of 0.933 g / cc, or 0.935 g / cc to 0.937 g / cc, and an I21 / I2 ratio of 63, or 65 to 67, with narrow-MWD LLDPE having a density of 0.915 g / cc, or 0.917 g / cc to 0.920 g / cc, or 0.921 g / cc, or 0.925 g / cc, and an I21 / I2 ratio of 30, or 31 to 33, or 39, or 40. This process involves forming a blend component comprising 35% by weight, or 40% by weight, or 45% by weight, or 50% to 55% by weight, or 60% by weight, or 65% by weight, or 70% by weight of broad MWD MDPE; 65% by weight, or 60% by weight, or 55% by weight, or 50% by weight, or 49% to 45% by weight, or 40% by weight, or 35% by weight, or 30% by weight, or 25% by weight, or 20% by weight of narrow LLDPE; and 1% by weight, or 2% by weight, or 3% by weight, or 4% to 5% by weight, or 6% by weight, or 7% by weight of carbon black. The blended component has a density of 0.935 g / cc, or 0.937 g / cc, or 0.940 g / cc to 0.945 g / cc, or 0.948 g / cc, or 0.950 g / cc, and an I21 / I2 ratio of 30, or 40, or 50, or 55, or 60 to 62, or 65. This process includes extruding the blended component onto a conductor at a speed exceeding 1.02 m / s (or 1.52 m / s) and forming a conductor sheath having a surface smoothness of 20 μinch, or 25 μinch to 30 μinch, or 40 μinch (hereafter, Process G).
[0098] In one embodiment, process G includes forming a conductive sheath having a tensile strength of 25 MPa, or 26 MPa, or 27 MPa, or 29 MPa to 30 MPa, and a tensile elongation of 800%, or 805% to 810%, or 820%, or 860%, or 880%, or 900%.
[0099] This process, utilizing two polymer blend components, simultaneously achieves acceptable surface smoothness (30–80 μ-inches) for the conductor sheath, improving the sheath's tensile strength and elongation, while advantageously providing improved processability (i.e., the ability to extrude at line speeds exceeding 1.02 m / s).
[0100] A surface smoothness of 20–80 μm provides aesthetic value and customer satisfaction. This process, utilizing two polymer blend components, minimizes variations in the diameter of the conductor sheath. Smoothness of 20–80 μm, or 30–80 μm, minimizes defects at the internal interface.
[0101] Examples of the present disclosure are provided, but are not limited to them. [Examples]
[0102] The materials used in the examples and comparative examples of the present invention are shown in Table 1A below.
[0103] [Table 1A-1]
[0104] [Table 1A-2]
[0105] CS1-9 and IE1-12 Melt Blending Process The Banbury mixer / molten-feed pelletizing extruder blending line is used for the production of CS1-9 and IE1-12 blends. The Banbury system typically provides very good control of the blending temperature. A three-stage mixing cycle with a drop-off temperature of 175°C is used.
[0106] Extrusion Insulated wire extrusion tests CS1–9 and IE1–12 are completed on a 6.35 cm (2.5 inch) Davis Standard wire line. The 6.35 cm Davis Standard wire and cable extruder is equipped with a 24:1 L / D barrel. The extruder is set up with a polyethylene-type Maddox mixed head screw with a compression ratio of 3:1. The extruder flows through a 9 / 32 inch × 5 / 8 inch Guill die in an adjustable central crosshead, and through specific tube tip and coating dies to form a molten flow for sample extrusion. Using this apparatus, samples with a final diameter of approximately 2.9 mm (0.114 inch) and a wall thickness of approximately 0.635 mm (0.025 inch) are produced on a 14 American Wire Gauge (AWG) solid copper conductor (1.63 mm diameter / 0.064 inch).
[0107] CS10–15 and IE13–16 Melt Blending Process Before preparing the wire samples, CS10–15 and IE13–16 are first mixed in a laboratory-scale Brabender mixer. The samples are melted and mixed using a Brabender mixing bowl with a capacity of 250cc and a cam-type mixing blade. The mixer temperature is set to 180°C. The mixing process first involves adding the resin to the mixing bowl at a mixing rate of 15 revolutions per minute (rpm). Both heating zones are set to 180°C. After the resin begins to melt, the carbon black masterbatch (DFNA-0037BK), processing aid (Dynamar FX 5912), and antioxidant (Irganox 1035) are added and mixed at 50 rpm for 6 minutes. The molten material is then removed and placed between Mylar sheets and pressed onto the sheets at room temperature (23°C) using a Wabash compression molding press. A Berlyn pelletizer is used to pelletize the samples.
[0108] Mini wire extrusion Using the Brabender Mini-Wire line, coated wires are extruded onto 14-gauge copper wire for each material. The machine settings are shown in Table 1B. Using this apparatus, samples with a final diameter of approximately 0.086 inches and a wall thickness of approximately 0.01 inches are produced on a 1.63 mm (0.064 inch) diameter 14 AWG solid copper conductor. After extrusion, the surface smoothness is measured with a profilometer.
[0109] [Table 1B]
[0110] The characteristics of comparative samples of the conductor sheath and the examples of the present invention are shown in Tables 2 to 4 below.
[0111] Qualitative smoothness is determined visually. In Tables 2-4, a "++" qualitative smoothness indicates a very smooth wire surface, while a "--" qualitative smoothness indicates a very rough wire surface.
[0112] [Table 2]
[0113] [Table 3]
[0114] [Table 4]
[0115] Tables 2-4 show that mixing components with different I21 / I2 viscosity profiles is possible to achieve and / or exceed the specifications of conventional conductive sheathing compounds, particularly with respect to final I21 / I2, melt index, density, mechanical properties, environmental stress cracking, and surface smoothness.
[0116] This disclosure advantageously expands the range of base resins suitable for forming conductor sheaths with a surface smoothness of 20 to 80 microinches at high speeds (i.e., extrusions exceeding 1.02 m / s).
[0117] The extrusion characteristics of Examples 1 to 15 of the present invention exhibit unexpected extrusion behavior. Polyethylene resins with a broad MWD and long-chain branching are known to exhibit excellent processability; that is, such polyethylenes have excellent surface smoothness and can be extruded at high line speeds. In contrast, polyethylene resins with a narrow MWD exhibit a viscosity profile that is relatively lacking in both melt strength and shear viscosity reduction behavior. Therefore, polyethylene polymers with a narrow MWD have limited extrusion performance and generally result in a conductive sheath with poor surface smoothness (i.e., surface smoothness greater than 80 μm) when processed at speeds exceeding 1.02 m / s.
[0118] Surprisingly, the blend components of the present invention maintain good surface smoothness (20–80 μm in) even at high content levels of narrow MWD polyethylene (up to 70 wt%). It is unexpected that surface smoothness is not a linear function of the weight percentage of narrow MWD polyethylene content, as shown by the data in Tables 2, 3, and 4, where the addition of narrow MWD polyethylene improves surface smoothness. Furthermore, the blend components of the present invention, as a whole, exhibit improved mechanical properties across the range of proposed compositions.
[0119] This disclosure is not limited to the embodiments and figures contained herein, and is particularly intended to include modifications of these embodiments, such as parts of the embodiments and combinations of elements of different embodiments contained in the following claims.
Claims
1. A process for manufacturing a conductor jacket, comprising the steps of: 55 to 85 I 21 / I 2 a first ethylene-based polymer having an I ratio of 20 to 50; 21 / I 2 a second ethylene-based polymer having a ratio of forming a blend component comprising 20% to 45% by weight of the first ethylene-based polymer, 80% to 55% by weight of the second ethylene-based polymer, and optional carbon black; The blend components have a density of 0.925 g / cc to 0.955 g / cc and an I 21 / I 2 extruding the blend components onto a conductor at a velocity of greater than 1.02 m / sec. forming a conductor jacket having a surface smoothness of 30 μinch to 80 μinch (0.76 μm to 2.03 μm).
2. Density of 0.915 g / cc to 0.925 g / cc and I of 73 to 77 21 / I 2 a first linear low density polyethylene (LLDPE) having a ratio of 0.915 g / cc to 0.925 g / cc and an I 21 / I 2 and blending a second LLDPE having a ratio of forming a blend component comprising 20% to 45% by weight of said first LLDPE, 70% to 55% by weight of said second LLDPE, and 1% to 10% by weight of carbon black; The blend components have a density of from 0.925 g / cc to less than 0.935 g / cc and an I 21 / I 2 forming a ratio of extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 30 μinch to 80 μinch (0.76 μm to 2.03 μm).
3. Density of 0.915 g / cc to 0.925 g / cc and I of 73 to 77 21 / I 2 a first linear low density polyethylene (LLDPE) having a ratio of 0.915 g / cc to 0.920 g / cc and an I of 30 to 33; 21 / I 2 and blending a second LLDPE having a ratio of forming a blend component comprising 23% to 45% by weight of said first LLDPE, 70% to 55% by weight of said second LLDPE, and 1% to 7% by weight of carbon black, said blend component having a density of from 0.925 g / cc to less than 0.935 g / cc and an I of from 33 to 42; 21 / I 2 forming a ratio of extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 45 μinch to 80 μinch (1.14 μm to 2.03 μm).
4. 4. The process of claim 3 including forming a conductor jacket having a tensile strength of 20.0 MPa to 22.0 MPa and a tensile elongation of 825% to 910%.
5. Density of 0.915 g / cc to 0.925 g / cc and I of 73 to 77 21 / I 2 a first linear low density polyethylene (LLDPE) having a ratio of 0.915 g / cc to 0.920 g / cc and an I of 30 to 33; 21 / I 2 and blending a second LLDPE having a ratio of forming a blend component comprising 23% to 45% by weight of said first LLDPE, 70% to 55% by weight of said second LLDPE, and 1% to 7% by weight of carbon black, said blend component having a density of from 0.925 g / cc to less than 0.935 g / cc and an I of from 35 to 55; 21 / I 2 forming a extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 35 μinch to 50 μinch (0.89 μm to 1.27 μm).
6. 6. The process of claim 5, comprising forming a conductor jacket having a tensile strength of 19.0 MPa to 23.0 MPa and a tensile elongation of 780% to 870%.
7. A density of 0.933 g / cc to less than 0.937 g / cc and an I of 55 to 75 21 / I 2 and a first medium density polyethylene (MDPE) having a density of 0.933 g / cc to 0.935 g / cc and an I 21 / I 2 a second ethylene-based polymer having a ratio of forming a blend component comprising 35 wt% to 45 wt% of the first MDPE, 60 wt% to 55 wt% of the second ethylene-based polymer, and 1 wt% to 7 wt% carbon black, wherein the blend component has a density of from 0.935 g / cc to less than 0.945 g / cc and an I of from 35 to 55. 21 / I 2 forming a extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 40 μinch to 60 μinch (1.02 μm to 1.52 μm).
8. 8. The process of claim 7 including forming a conductor jacket having a tensile strength of 27 MPa to 30 MPa and a tensile elongation of 830% to 970%.
9. Density of 0.933 g / cc to 0.937 g / cc and I of 63 to 67 21 / I 2 and a first medium density polyethylene (MDPE) having a density of 0.933 g / cc to 0.935 g / cc and an I of 25 to 30. 21 / I 2 and blending a second MDPE having a ratio of forming a blend component comprising 35% to 45% by weight of said first MDPE, 60% to 55% by weight of said second MDPE, and 1% to 7% by weight of carbon black, said blend component having a density of 0.935 g / cc to less than 0.945 g / cc and an I of 40 to 45; 21 / I 2 forming a extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 50 μinch to 60 μinch (1.27 μm to 1.52 μm).
10. 10. The process of claim 9, comprising forming a conductor jacket having a tensile strength of 27 MPa to 30 MPa and a tensile elongation of 860% to 970%.
11. A process for manufacturing a conductor jacket, comprising the steps of: 55 to 85 I 21 / I 2 a first ethylene-based polymer having an I ratio of 20 to 50; 21 / I 2 a second ethylene-based polymer having a ratio of forming a blend component comprising 20% to 70% by weight of the first ethylene-based polymer, 80% to 20% by weight of the second ethylene-based polymer, and optional carbon black; The blend components have a density of 0.925 g / cc to 0.955 g / cc and an I 21 / I 2 forming a ratio of extruding the blend components onto a conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 20 μinch to 80 μinch (0.51 μm to 2.03 μm).
12. Density of 0.915 g / cc to 0.925 g / cc and I of 73 to 77 21 / I 2 a first linear low density polyethylene (LLDPE) having a ratio of 0.915 g / cc to 0.925 g / cc and an I 21 / I 2 and blending a second LLDPE having a ratio of forming a blend component comprising 50% to 70% by weight of said first LLDPE, 49% to 20% by weight of said second LLDPE, and 1% to 10% by weight of carbon black, said blend component having a density of from 0.925 g / cc to less than 0.935 g / cc and an I of from 33 to 60; 21 / I 2 forming a ratio of extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 30 μinch to 80 μinch (0.76 μm to 2.03 μm).
13. A density of 0.933 g / cc to less than 0.937 g / cc and an I of 55 to 75 21 / I 2 and a first medium density polyethylene (MDPE) having a density of 0.935 g / cc to 0.940 g / cc and an I 21 / I 2 and blending a second medium density polyethylene (MDPE) having a ratio of forming a blend component comprising 50% to 70% by weight of said first MDPE, 49% to 20% by weight of said second MDPE, and 1% to 10% by weight of carbon black, said blend component having a density of 0.935 g / cc to 0.950 g / cc and an I of 35 to 50; 21 / I 2 forming a extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 20 μinch to 60 μinch (0.51 μm to 1.52 μm).
14. A density of 0.933 g / cc to less than 0.937 g / cc and an I of 55 to 75 21 / I 2 and a first medium density polyethylene (MDPE) having a density of 0.915 g / cc to 0.925 g / cc and an I of 20 to 40. 21 / I 2 a second linear low density polyethylene (LLDPE) having a ratio of forming a blend component comprising 50% to 70% by weight of said broad first MDPE, 49% to 20% by weight of said second LLDPE, and 1% to 10% by weight of carbon black, said blend component having a density of 0.935 g / cc to 0.950 g / cc and an I of 40 to 65; 21 / I 2 forming a extruding the blend components onto the conductor at a velocity of greater than 1.02 m / sec; forming a conductor jacket having a surface smoothness of 20 μinch to 60 μinch (0.51 μm to 1.52 μm).