Method for converting combustible or flame retardant substrate or part into non-combustible substrate or part
A coating of metal nanoparticles with a melting point above 840°C forms an airtight film that addresses the challenge of maintaining non-flammability and safety at high temperatures by providing heat and fire resistance, mechanical strength, and airtightness.
Patent Information
- Application Number
- JP2021180703
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-11-04
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2041-11-04
AI Technical Summary
Existing coatings fail to provide both heat resistance and fire resistance at temperatures up to 840°C, leading to potential ignition and spread of fires, and do not maintain airtightness to prevent oxygen supply, thus failing to ensure non-flammability and safety in high-temperature conditions.
A coating composed of metal nanoparticles with a melting point above 840°C, bonded to each other and laminated, is applied to form an airtight film that withstands temperatures up to 840°C, using a paste made by crushing metal compound crystals and mixing them with organic compounds to ensure adhesion and thermal decomposition.
The coating provides heat resistance, fire resistance, and airtightness, preventing ignition and spread of fires, maintaining mechanical strength, electrical conductivity, and ensuring non-flammability even at extreme temperatures.
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating having a structure in which metal nanoparticles made of a metal having a melting point of higher than 840°C are bonded to each other and the metal nanoparticles bonded to each other are laminated together, and the coating covers the entire outer surface of a substrate or part that is exposed to the outside world, and the coating provides the substrate or part with airtightness that isolates it from the outside world, and the substrate or part that is flammable or flame-retardant is: It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. Pertaining to the way in which a material is transformed into a substrate or part. Prior to the present invention, the present inventor has filed a patent application No. 2019-169866 (filed on September 18, 2019) for a method of covering a flammable or flame-retardant substrate or part with a collection of two types of particles consisting of aluminum oxide particles and maghemite particles to make the substrate or part non-flammable. Here, the difference between the two will be explained. The prior application relates to a method for covering a substrate or part with an assembly of two types of fine particles, aluminum oxide and maghemite, to change a flammable or flame-retardant substrate or part into a non-flammable substrate or part. In contrast, the present invention relates to a method for covering a substrate or part with a coating having a structure in which nanoparticles of a metal having a melting point higher than 840°C are metallically bonded to each other, and an assembly of metallic nanoparticles that are metallically bonded to each other are laminated, to change a flammable or flame-retardant substrate or part into a non-flammable substrate or part. It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. It involves the process of converting a material into a substrate or component. That is, in the prior application, a magnetic attraction force acting between ferromagnetic maghemite particles is applied to a group of nonmagnetic aluminum oxide particles, and a coating is formed from a group of two types of particles. For this purpose, a group of two types of particles, aluminum oxide and ferrous oxide, is precipitated at the same time, and the ferrous oxide particles are oxidized to maghemite particles. Furthermore, in order to increase the magnetic attraction force acting on the maghemite particles, a magnetization process is performed to saturate the magnetization of the maghemite particles. In contrast, in the present invention, regardless of whether the metal is ferromagnetic or nonmagnetic, metal nanoparticles made of a metal with a melting point higher than 840°C are metallically bonded to each other, and a coating in which the group of metallic nanoparticles that are metallically bonded are laminated covers the substrate or part. Therefore, in the present invention, it is sufficient to precipitate a group of metal particles only once. As will be described in detail in paragraph 7, the regulations for the insulating performance of the fire-resistant layer of a fire-resistant electric wire or fire-resistant cable are based on the idea that the most stringent heat resistance is specified, and the maximum temperature in the event of a fire is set at 840°C. In this invention, non-flammability is defined as a property that combines heat resistance capable of withstanding 840°C and fire resistance capable of withstanding temperatures of 840°C. In addition, in aluminum oxide, which is a non-magnetic material made of metal oxide, the particles do not bond metallically to each other at the contact area, and the particles do not magnetically attract each other. On the other hand, when maghemite exceeds 530°C, a phase transition to weakly ferromagnetic hematite begins, and the phase transition ends at 640°C, when all maghemite is replaced by hematite. Furthermore, when the temperature exceeds 675°C, the magnetism emitted by the hematite particles disappears, and the magnetic attraction force that bonds the particles together disappears. For this reason, in the prior application, after simultaneously depositing a collection of aluminum oxide and ferrous oxide particles, a compressive stress is applied to the substrate or part, and the particles are bonded together by frictional heat, and the collection of particles deposited on the surface of the substrate or part is bonded to the surface of the substrate or part by frictional heat, and a coating consisting of the collection of particles bonded by frictional heat is bonded to the surface of the substrate or part. Therefore, if the substrate or part is not planar, the substrate or part is placed in a mold having a groove with dimensions equivalent to the outer shape of the substrate or part, and after two types of fine particle clusters are precipitated, compressive stress is applied to the substrate or part in the mold, the fine particles are bonded to each other by frictional heat, and the cluster of fine particles precipitated on the surface of the substrate or part is bonded to the surface of the substrate or part by frictional heat. However, if the outer surface of the substrate or part exposed to the outside world is uneven, it is difficult to bond the cluster of fine particles precipitated on the surface of the substrate or part to the entire surface of the substrate or part by frictional heat. Furthermore, vibration acceleration is applied to the mold in three directions, the substrate or part is peeled off from the mold, and the substrate or part is removed from the mold. In contrast, in the present invention, a coating formed by stacking clusters of metal nanoparticles bonded with each other forms an airtight coating that blocks the outside world, and the airtight coating covers the entire outer surface of the substrate or part exposed to the outside world, so there is no need to apply compressive stress to the metal fine particles. This allows a flammable substrate or part to be converted into a non-flammable substrate or part even if it has weak mechanical strength. Furthermore, in the present invention, a substrate or a part is immersed in a paste, the paste is absorbed by the substrate or the part, and then the substrate or the part is heat-treated to thermally decompose the metal compound, and the entire outer surface of the substrate or the part is covered with a coating of a laminate of aggregates of metal nanoparticles bonded with each other. Therefore, even if the substrate or the part is not flat, the paste is absorbed by the entire outer surface of the substrate or the part. Therefore, a process of applying compressive stress to the substrate or the part is not required. Furthermore, in the prior application, the size of the two types of fine particles, aluminum oxide and maghemite, is 40-60 nm. In contrast, in the present invention, the size of the metal fine particles is around 10 nm. Since the size of the fine particles is about 1 / 5 smaller, the size of the gaps formed between adjacent fine particles follows the size of the fine particles and is nearly 1 / 5 narrower. Therefore, by randomly stacking more than 10 layers of metal-bonded metal fine particles, there are no gaps penetrating the collection of metal fine particles, and the coating consisting of the collection of stacked metal fine particles becomes an airtight coating that blocks the outside world. Therefore, the thickness of the airtight coating in the present invention is more than 1 / 2 thinner than that of the prior application. Therefore, the airtight coating has almost no mass. As a result, there is almost no increase in weight of the substrate or parts that have been converted to non-flammable. As explained above, the present invention has various advantages over the prior art applications. Next, prior to the present invention, the present inventor has registered a patent (Patent No. 6792834, filed on October 7, 2016) for a non-flammable paint in which an inner coating is made of a multilayer structure of stacked clusters of metallically bonded metal particles, and an outer coating is made of an organic compound coating with a boiling point higher than the thermal decomposition temperature of a metal compound that precipitates a metal upon thermal decomposition, covering a flammable substance with this double-layer coating, thereby turning the flammable substance into a non-flammable substance. In addition, the present invention proposes an invention relating to a method for producing a paste that covers a flammable or flame-retardant substance with an airtight coating before the invention for converting a flammable or flame-retardant substrate or part into a non-flammable substrate or part. Here, the difference between the two will be explained. As described above, in the present invention, the maximum temperature in the event of a fire is set to 840°C, and the non-combustibility in the present invention is a property that combines heat resistance that can withstand 840°C and fire resistance that can withstand a temperature of 840°C. For this reason, a substrate or part is covered with a collection of metal nanoparticles that are laminated with a collection of metal nanoparticles that are made of a metal with a melting point higher than 840°C, and a flammable or flame-retardant substrate or part is changed into a non-combustible substrate or part. In contrast, the registered patent does not have the idea of combining heat resistance and fire resistance at 840°C as non-combustibility. That is, the organic compound forming the outer coating in the registered patent has a boiling point 50°C or more higher than the thermal decomposition temperature of the metal compound. Specifically, since the metal compound is an octylic acid metal compound that thermally decomposes at 290°C and precipitates metal, an organic compound belonging to aromatic carboxylate esters with a boiling point of 340°C or more and an ignition point of 390°C or more was used as the organic compound. Therefore, at temperatures higher than 390°C, the vaporized organic compound ignites. Therefore, the non-flammability of the registered patent is non-flammability at temperatures lower than 390°C. In contrast, in the present invention, the substrate or part is covered only with a collection of metal nanoparticles in which the collection of metal-bonded metal nanoparticles is layered. Therefore, the organic compound in the present invention has a boiling point lower than the thermal decomposition temperature of the metal compound and vaporizes before the metal compound thermally decomposes. In other words, the organic compound vaporizes before the substrate or part is covered with the coating. As a result, the coating made of the collection of metal nanoparticles in the present invention has a non-flammability that can withstand 840°C. Furthermore, the size of the metal microparticles in the present invention is about 1 / 5 of the size of the metal microparticles in the registered patent. Therefore, the gaps formed between adjacent metal microparticles are also about 1 / 5 of the size of the registered patent. Therefore, by randomly stacking more than 10 layers of metal-bonded metal microparticles, there are no gaps penetrating the collection of metal microparticles, and the coating made of the collection of metal microparticles becomes an airtight coating that blocks the outside world. Therefore, even if the layer of metal microparticles to be stacked is thinner than the layer of metal microparticles in the registered patent, an airtight coating can be formed. Therefore, in the present invention, a coating made of an organic compound is not formed. On the other hand, in the registered patent, in order to make the coating airtight, the thickness of the organic compound coating is about twice as thick as the coating made of the collection of metal microparticles. The thickness of the airtight coating that blocks the outside world in the present invention is thinner than the layer of metal particles in the registered patent. Therefore, the viscosity of the paste in the present invention is set to be lower than 2 mPa·s at 20°C, and the thickness of the paste to be adsorbed on the substrate or part is set to be thinner than 1 μm. Therefore, the organic compound used in the present invention has a lower viscosity than the organic compound in the registered patent, and a lower boiling point than the organic compound in the registered patent. As explained above, the present invention has various advantages over issued patents. [Background technology]
[0002] The regulations related to fire protection equipment that blocks flames are stipulated in Article 109-2 of the Enforcement Order of the Building Standards Act, which stipulates that the 20 minutes during which heat from a fire is applied is the flame-blocking time, and stipulates the requirements that the fire protection equipment must not emit flames on any surface other than the heated surface during the flame-blocking time. Examples of such fire protection equipment include fire doors, fire and smoke shutters, fire and smoke dampers, fire and smoke hanging walls, fire and smoke sheets, fire and smoke screens, fire and smoke panels, and drenchers. The requirements for this fire protection equipment are that it must be flame retardant, that is, it must not emit flames on any surface other than the heated surface, for the first 20 minutes after a fire breaks out, but it is not a requirement that the fire protection equipment itself must be non-flammable. However, it is not always possible for everyone to evacuate from a burning building within 20 minutes of the start of a fire. Also, if fire protection equipment burns after 20 minutes of the start of a fire, its fire protection function will be impaired, leading to the spread of the fire. Therefore, regardless of the scale of the fire, if fire prevention equipment is non-flammable, it will continue to perform its fire prevention function during a fire, and its effectiveness will be great.
[0003] On the other hand, in terms of flame resistance, which indicates difficulty in burning, non-flammable is used as the property of not burning continuously, flame retardant is used as the property of burning only for a short time with a slow burning speed, self-extinguishing is used as the property of burning while exposed to flame but extinguishing when removed from the flame, and retarded flame is used as the property of not self-extinguishing but having a slow burning speed. However, since there are few cases where these properties are specified as performance, there are cases where retarded flame is used in the same way as non-flammable, as mentioned above. As a provision related to flame resistance, for example, there is a certification standard for non-flammable materials among fire-resistant materials (based on Ministry of Land, Infrastructure, Transport and Tourism Notification No. 1178), which stipulates that when exposed to fire, the material will not burn for 20 minutes after the start of the application of fire force, will not cause damage harmful to fire prevention, and will not emit smoke or gas harmful to evacuation. This provision, like Article 109-2 of the Enforcement Order of the Building Standards Act mentioned above, is a provision for retardation of fire limited to the 20 minutes after the application of fire force, and is not a provision for non-flammability. JIS-K6911 also defines the non-combustibility of thermosetting resins, stating that a flame is applied to a 5 x 0.5 x 0.5 inch test piece for 30 seconds, and the burning of the test piece should be extinguished within 180 seconds after the flame is removed, and the length of the burned test piece should be 1 inch or less. JIS-K6911 also defines self-extinguishing as the burning of the test piece should be extinguished within 180 seconds after the flame is removed, and the length of the burned test piece should be 1 inch or more and 4 inches or less. This definition of the non-combustibility of thermosetting resins is the property that combustion does not continue once the flame is removed, and it is not the non-combustibility property of thermosetting resins that does not burn when exposed to flames. Furthermore, fire-resistant electric wires or cables maintain the insulating performance of the fire-resistant layer to ensure emergency power supply in the event of a fire, and are capable of carrying electricity for a certain period of time, and are used for wiring in various emergency equipment (emergency elevators, indoor fire hydrant equipment, smoke exhaust equipment, etc.) specified by the Fire Service Act and the Building Standards Act. The insulation performance of the fire-resistant layer is required to be certified by testing at the Japan Electric Wire & Cable Makers' Association (JCS) based on the Fire and Disaster Management Agency regulations (technical standards based on the Ministry of Home Affairs Fire and Disaster Management Agency Notification No. 10, December 18, 1997), and to have insulating performance that can withstand heating according to a fire temperature curve that reaches 840°C in 30 minutes. Furthermore, heat-resistant electric wires or heat-resistant cables are required to have insulating performance that can withstand heating according to a fire temperature curve that reaches 380°C in 15 minutes, and to be certified by testing at the Japan Electric Wire & Cable Makers' Association (JCS) based on the Fire and Disaster Management Agency regulations. Therefore, although the regulations for the insulating performance of the fire-resistant layer in fire-resistant electric wires or fire-resistant cables are the strictest, they are not regulations for incombustibility that means the fire-resistant layer does not burn in the event of a fire.
[0004] Meanwhile, various flame retardants made of materials different from conventional flame retardants are being developed. Patent Document 1 proposes a flame retardant paint mainly composed of high-purity bentonite and soap-free emulsion resin. However, the molecular structure of bentonite becomes unstable at 400°C or higher, so the gas barrier properties of bentonite decrease in high-temperature environments of 400°C or higher. In addition, the manufacturing cost of refining bentonite into fine powder with a montmorillonite content of 85% by weight or more is not cheap. In addition, emulsion resin is non-combustible according to the Building Standards Act mentioned above, that is, even if it does not burn for 20 minutes after heating begins, it will burn if heated for a longer period of time. Note that bentonite is an inorganic substance made of a type of clay mineral, and has been used conventionally as a precipitation inhibitor for paints. In addition, Patent Document 2 proposes an inorganic and organic hybrid type fireproof paint consisting mainly of a powder made by mixing white cement with inorganic aggregate and fireproofing agent, and a liquid agent made of aqueous emulsion resin. However, in order to increase the fireproofness of a paint consisting of such a composition, the mixing ratio of white cement, inorganic aggregate, and fireproofing agent in the paint must be increased. However, the higher the inorganic fireproofing agent, the higher the viscosity of the paint, and the worse the workability of forming the coating film. In addition, the adhesion to the base is poor, and the deterioration of the coating film properties over time is accelerated. In addition, even if the aqueous emulsion resin has the fireproofness of the Building Standards Act mentioned above, that is, the property of not burning for 20 minutes after the start of heating, it will burn if heated for a longer period of time. The acrylic resin used in the emulsion resin begins to thermally decompose at approximately 370°C, the temperature of the atmosphere, and decomposes into methyl methacrylate, which has a boiling point of 101°C and an ignition point of 421°C, methyl acrylate, which has a boiling point of 80°C and an ignition point of 468°C, and related compounds. Dibutyl phthalate, a representative plasticizer, has a boiling point of 340°C and an ignition point of 402°C. Therefore, when a flammable material is coated with a non-flammable paint containing emulsion resin and a plasticizer as ingredients, the coating film thermally decomposes at temperatures below 400°C, losing its non-flammability, and the flammable material produced by the thermal decomposition ignites. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 20016-117810 A [Patent Document 2] JP 20013-043891 A [Non-patent literature]
[0006] [Non-Patent Document 1] Japanese Journal of Mineralogy, Vol. 16, No. 3, 253-264, November 1983 [Non-Patent Document 2] Journal of Industrial Chemistry, Vol. 66, No. 11 (1963) 92-96 [Non-Patent Document 3] Journal of the Mining Industry of Japan, Vol. 98, No. 1133 (July 1982) 575-578 Summary of the Invention [Problem to be solved by the invention]
[0007] The non-combustible nature of the paint stipulated in the Building Standards Act is a regulation that satisfies the three requirements only for the first 20 minutes of a fire outbreak, and more precisely, it is a regulation that is not non-combustible but flame retardant. However, it is not always possible for all people to evacuate from a burning building within 20 minutes of the fire outbreak. Also, if a non-combustible paint burns after 20 minutes of a fire outbreak, flammable substances will ignite from the paint film on which the non-combustible paint is applied, causing the fire to spread and generating smoke or gas that is harmful to evacuation. Therefore, if non-combustible paint could be changed to a truly non-combustible paint that does not self-ignite or catch fire, it would continue to be non-combustible in any fire, and would have a great effect on disaster prevention. Here, the properties of fire resistance, flame resistance, flame retardancy, self-extinguishing, and flame retardancy are compared with the property of non-flammability. If the substrate or part does not burn in any scale of fire or fire caused by any material, that is, in a fire in which flammable or inflammable gas, flammable or inflammable liquid, or flammable or inflammable solid is burning, that is, if the substrate or part has non-flammability, the substrate or part has all the properties of fire resistance, flame resistance, flame retardancy, self-extinguishing, and flame retardancy. Therefore, properties such as fire resistance, flame resistance, flame retardancy, self-extinguishing, and flame retardancy are included in non-flammability. Therefore, a non-flammable substrate or part has all the properties of fire resistance, flame resistance, flame retardancy, self-extinguishing, and flame retardancy. Therefore, the realization of non-flammability is technically more difficult than the realization of fire resistance, flame resistance, flame retardancy, self-extinguishing, and flame retardancy. Next, let us consider the maximum temperature during a fire. The standard that specifies the maximum temperature during a fire is the insulation performance of the fire-resistant layer of a fire-resistant electric wire or cable. In other words, fire-resistant electric wires or cables maintain the insulation performance of the fire-resistant layer to ensure emergency power supply during a fire, and are capable of carrying electricity for a certain period of time, and are used for wiring various emergency equipment (emergency elevators, indoor fire hydrant equipment, smoke exhaust equipment, etc.) specified by the Fire Service Act and the Building Standards Act. The insulation performance of the fire-resistant layer is required to be certified by testing at the Japan Electric Wire & Cable Makers' Association (JCS) based on the Fire and Disaster Management Agency regulations (technical standards based on the Ministry of Home Affairs Fire and Disaster Management Agency Notification No. 10, December 18, 1997), and to have insulation performance that can withstand heating according to a fire temperature curve that reaches 840°C in 30 minutes. Furthermore, heat-resistant electric wires or heat-resistant cables are required to be certified by testing at the Japan Electric Wire & Cable Makers' Association (JCS) based on the Fire and Disaster Management Agency regulations mentioned above, and to have insulation performance that can withstand heating according to a fire temperature curve that reaches 380°C in 15 minutes. Therefore, although the regulations for the insulating performance of the fire-resistant layer in a fire-resistant electric wire or cable are the strictest, they do not regulate the incombustibility of the fire-resistant layer so that it will not burn in the event of a fire. The insulation performance of the fire-resistant layer of this fire-resistant wire or cable Regulations Based on this, the maximum temperature in the event of a fire is set to 840°C, and the non-combustibility in this invention is defined as a property that combines heat resistance and fire resistance at 840°C. Here, we consider the technical issues involved in realizing a substrate or part that is non-combustible even at 840°C during a fire. The first task is to cover a flammable or flame-retardant substrate or part with a coating that is heat-resistant and fire-resistant to 840°C. In other words, the flammable or flame-retardant substrate or part is sure to decompose at a temperature lower than 840°C. On the other hand, if the substrate or part is covered with a coating that is heat-resistant and fire-resistant to 840°C, all substances generated by pyrolysis are not discharged to the outside. Therefore, black smoke and harmful gases are not discharged, black smoke obstructs visibility, and harmful gases do not cause disasters. In addition, flammable substances generated by pyrolysis do not self-ignite or ignite. Therefore, the starting point of a fire is not created and the fire does not spread. The second problem is that the coating has airtightness that blocks the outside world. Therefore, even at 840°C, oxygen gas is not supplied to the substrate or part. On the other hand, combustion is an oxidation reaction with oxygen gas. If the substrate or part is blocked from the outside world by a coating that has heat resistance and fire resistance at 840°C, the substrate or part will not self-ignite or ignite even if it is heated to a temperature exceeding the ignition point and flash point. In addition, even if the substrate or part is thermally decomposed, the combustible material generated by the thermal decomposition will not self-ignite or ignite. Furthermore, the thermally decomposed combustible material will not be discharged to the outside, and will not self-ignite or ignite. In other words, by covering the substrate or part with a coating that has heat resistance and fire resistance at 840°C and has airtightness that blocks the outside world even at 840°C, the substrate or part becomes non-flammable. Therefore, the first objective of the present invention is to find a method for producing a coating that has heat resistance and fire resistance up to 840°C and that has airtightness to block out the outside world even at 840°C, and a method for covering a flammable or flame-retardant substrate or part with said coating. Incidentally, all buildings use a large number of flammable or flame-retardant substrates or parts, that is, products whose main components are organic substances such as synthetic resins, wood, and paper, or products that are composited with organic substances. For this reason, it would be extremely effective to cover flammable or flame-retardant substrates or parts with a coating that has heat resistance and fire resistance up to 840°C, and also has airtightness that blocks the outside world even at 840°C. However, there is currently no coating that provides such an effect. On the other hand, flammable or flame-retardant substrates or parts are used as various products in buildings, and have a wide variety of surface conditions, shapes, sizes, and materials. Therefore, all flammable or flame-retardant substrates or parts must be covered with an airtight coating that has heat resistance and fire resistance at 840°C and blocks the outside world even at 840°C. Therefore, the second object of the present invention is to cover a substrate or part with a coating that has heat resistance and fire resistance at 840°C and is airtight even at 840°C, regardless of the surface condition, material, shape, and size of the flammable or flame-retardant substrate or part. [Means for solving the problem]
[0008] The flammable or flame-retardant substance of the present invention It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. The method for producing a paste for converting the material to a substance is as follows: To methanol In molecular state a metal compound having both a first property of being dispersed but not dissolved in methanol and a second property of precipitating a metal having a melting point higher than 840°C upon thermal decomposition is dispersed in methanol to prepare a methanol dispersion of the metal compound, and then the methanol is evaporated from the methanol dispersion of the metal compound to precipitate a crystal mass of the metal compound; The collection of crystals of the metal compound is then filled into a container, and a plate material covering the entire surface of the collection of crystals of the metal compound is placed on the collection of crystals of the metal compound. A compressive load is then applied to the entire surface of the plate material to crush the crystals of the metal compound in the container. Impact acceleration is then repeatedly applied to the sides and bottom of the container in three directions, namely, front-back, left-right, and up-down, to rearrange the crushed collection of crystals of the metal compound in the container. The compressive load is then applied again to the entire surface of the plate material to further crush the crystals of the metal compound. The impact acceleration in the three directions is then repeatedly applied again to the sides and bottom of the container. A pair of processes consisting of the process of applying the compressive load and the process of applying the impact acceleration are repeated, and when the plate material stops moving when the compressive load is applied to the plate material, it is determined that the crushing of the crystals of the metal compound is completed, and the pair of processes are stopped. The plate material is then removed from the container. Further, a second organic compound having a first property of being soluble in a first organic compound having a viscosity at 20°C of less than 1 mPa·sec, a second property of not dissolving or dispersing crystals of the metal compound, a third property of having a boiling point higher than that of the first organic compound and lower than the thermal decomposition temperature of the metal compound, and a fourth property of having a viscosity at 20°C of 4-7 mPa·sec is prepared. sticky The metal compound is dissolved in the first organic compound so that the viscosity of the metal compound is less than 2 mPa·sec, and the solution is applied to the crushed metal compound in the container. Consists of a size of about 20 nm mixing the crushed crystal mass with the metal compound to form a suspension in which the crushed crystal mass of the metal compound is dispersed in the dissolving solution; The suspension produced by the above process is treated with a flammable or flame-retardant material. It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. A paste that converts flammable or flame-retardant materials into It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. A method for producing a paste that can be converted into a substance.
[0009] The paste of the present invention is prepared by the following three simple processes. Each process and the action and effect of each process will be explained below. In the first process, a collection of crystals of the metal compound is precipitated. For this purpose, the metal compound is dispersed in methanol, and then the methanol is evaporated to precipitate a collection of crystals of the metal compound. In other words, when a metal compound that precipitates a metal having a melting point higher than 840°C by thermal decomposition is dispersed in methanol, which is the most commonly used organic solvent, the metal compound becomes a molecular state and disperses in the methanol. In contrast, when a metal compound dissolves in methanol, the metal constituting the metal compound becomes a metal ion and dissolves in the methanol, and the dissolved metal compound cannot return to the metal compound before dissolution. For this reason, even if methanol is evaporated from a methanol solution of the metal compound, crystals of the metal compound before dissolution do not precipitate. Therefore, a metal compound that does not dissolve in methanol but disperses in methanol is used as a metal compound that precipitates a metal by thermal decomposition. As a result, when methanol is evaporated from a methanol dispersion of the metal compound, the metal compound precipitates as crystals of the metal compound smaller than 100 nm. This crystal is a collection of crystals formed by the accumulation of crystals formed by single molecules of the metal compound, since the metal compound dispersed in methanol in a molecular state precipitates as crystals. Therefore, when stress is applied to the crystals, the crystals are broken down into fine crystals. On the other hand, the finer the crystals, the more difficult it is to apply stress to them, and there is a limit to how fine the crystals can be made. In addition, common metals with melting points lower than 840°C are tin, lead, zinc, magnesium, and aluminum, in order of decreasing melting point. Therefore, the metal compounds used in the present invention precipitate metals other than these five types of metals by thermal decomposition. In addition, the vaporized methanol is recovered by a recovery machine and reused. In the second process, the crystals of the metal compound are crushed to about 1 / 5 of their original size. For this purpose, a container is filled with a collection of crystals of the metal compound, a plate material is placed over the collection of crystals of the metal compound in the container, the collection of crystals of the metal compound is constrained within the container, and the collection of crystals of the metal compound is compressed through the plate material. At this time, the crystals with a relatively large size are more likely to be crushed. For this reason, the relatively large crystals are crushed preferentially, and the crushing of the crystals progresses while the compressive load is applied. Meanwhile, in the collection of crystals in the container, new voids are formed by the crushing of the crystals, and while the compressive load is applied, the crystals move to fill the voids. After this, the applied compressive load is stopped, and the container is repeatedly subjected to impact acceleration in three directions, front and back, left and right, and up and down. At this time, the crystals do not scatter because they are constrained within the container by the plate material, but the crystals move to fill the voids, and the crushed collection of crystals is rearranged within the container. Furthermore, after the applied impact acceleration is stopped, a compressive load is again applied to the collection of crushed crystals through the plate material. At this time, the crushing of the crushed crystals advances against the cluster of finer crystals. After this, the container is again repeatedly subjected to impact acceleration in three directions to advance the rearrangement of the cluster of finer crystals. A pair of processes consisting of a process of applying a compressive load and a process of applying an impact acceleration in three directions is repeated. On the other hand, the finer the crystals, the more difficult it becomes to apply compressive stress to the crystals even when a compressive load is applied, and there is a limit to the refinement of the crystals. When the refinement of the crystals reaches its limit, the crushing of the crystals does not advance even when a compressive load is applied to the plate material, and no movement is observed in the plate material to which the compressive load is applied. At this point, the pair of processes is stopped. As a result, the size of the crystals becomes approximately 20 nm, which is close to 1 / 5 of the size at the time of precipitation. The compressive load applied to the plate material is a compressive load equivalent to 10-50 kg weight, depending on the size of the container. The impact acceleration applied to the container is an impact acceleration of 0.2-0.5 G, depending on the size of the container. In the third process, a second organic compound having a viscosity of 4-7 mPa·sec at 20°C is dissolved in a first organic compound having a viscosity of less than 1 mPa·sec at 20°C so that the viscosity of the solution at 20°C is less than 2 mPa·sec, and the solution is mixed with the aggregate of crushed crystals of the metal compound to prepare a suspension. The crushed crystals of the metal compound are extremely fine, about 20 nm in size, and the crushed crystals have almost no mass. The viscosity of the solution is less than 2 mPa·sec at 20°C. Therefore, even if the weight of the solution is less than the weight of the aggregate of crushed crystals, the aggregate of crushed crystals is easily dispersed uniformly in the solution. The metal compound is not dissolved or dispersed in both the first organic compound and the second organic compound. Therefore, in the suspension, the fine crystals of the metal compound are not dissolved or dispersed in the solution. In other words, the organic compound in which the metal compound disperses is limited to a straight-chain aliphatic alcohol having four or less carbon atoms. The suspensions prepared by the three processes described above are used as pastes to convert flammable or flame-retardant materials into non-flammable materials. Since the viscosity of the solution is less than 2 mPa·s at 20°C, the thickness of the paste applied to the substrate or part is less than 1 μm. In addition, the metal compound, the first organic compound, and the second organic compound used in the production of the paste are all general-purpose industrial chemicals. Furthermore, the above-mentioned three processes are all simple. Therefore, the paste can be produced at low cost.
[0010] As stated in paragraph 8 The suspension is not It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. It is used as a paste to convert a substrate or part made of a flammable or flame-retardant material into a material. It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. The method of converting it into a substrate or part is as follows: The paste is filled into a container, and a substrate or a part made of a flammable or flame-retardant material is entirely immersed in the paste in the container, and then the substrate or the part is removed from the container, and a coating having a thickness of less than 1 μm and made of the paste is adsorbed onto the entire outer surface of the substrate or the part exposed to the outside. Thereafter, the substrate or the part is As stated in paragraph 8 Exposing the metal compound to an atmosphere in which it thermally decomposes, and then Applicable The temperature is raised to a temperature at which the metal compound decomposes, As stated in paragraph 8 A first organic compound; As stated in paragraph 8 The second organic compound and the second organic compound are vaporized in order according to their boiling points, and then the metal compound is thermally decomposed, and a metal having a melting point of more than 840° C. is deposited on the entire outer surface of the substrate or the part exposed to the outside world. Consists of a size of about 10 nm A collection of metal nanoparticles , in the active state as intrinsic metal nanoparticles The metal nanoparticles are simultaneously deposited, and metal bonds are formed at the sites where the deposited metal nanoparticles come into contact with each other, and the metal-bonded metal nanoparticles are stacked together, so that the entire outer surface of the substrate or the part exposed to the outside world is made up of a stack of metal nanoparticles of the metal that are metal-bonded together. Airtight to block out the outside world Covered with a membrane As a result, the entire outer surface of the substrate or the part made of a flammable or flame-retardant material exposed to the outside world is covered with an airtight coating that blocks the outside world and is made of a collection of metal nanoparticles laminated with the collection of metal-bonded metal nanoparticles, and the substrate or the part made of a flammable or flame-retardant material is It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. A substrate or part made of a flammable or flame-retardant material that is to be converted into the substrate or part, It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. How it is transformed into a substrate or component.
[0011] The substrate or part made of flammable or flame-retardant material in the present invention is It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. There are two simple processes for converting it into a substrate or part. Each process and its effect are explained below. In the first treatment, the entire substrate or part is immersed in the paste, the substrate or part is removed from the container, and the paste having a thickness less than 1 μm is adsorbed onto the entire outer surface of the substrate or part exposed to the outside world. To achieve this, the viscosity of the solution in which the second organic compound is dissolved in the first organic compound is made lower than 2 mPa·sec at 20°C so that the thickness of the paste adsorbed onto the substrate or part is less than 1 μm. Note that because the viscosity of the solution is low, the paste having a thickness less than 1 μm is adsorbed onto the entire outer surface of the substrate or part exposed to the outside world, regardless of the surface irregularities or the size or shape of the substrate or part. In the second process, the substrate or part to which the paste is adsorbed is exposed to an atmosphere in which the metal compound is thermally decomposed, and the temperature is raised to a temperature at which the metal compound is thermally decomposed. At this time, the first organic compound and the second organic compound are vaporized in order according to their boiling points. The vaporized first organic compound and second organic compound are recovered and reused. After this, the thermal decomposition of the metal compound begins, and the fine crystals of the metal compound are decomposed into inorganic or organic molecules and metal molecules, and the inorganic or organic molecules take the heat of vaporization and vaporize. The vaporized inorganic or organic molecules are recovered and reused. At the moment when the vaporization of the inorganic or organic molecules is completed, the collection of metal molecules forms metal nanoparticles with a size of about 10 nm, and a collection of metal nanoparticles made of a metal with a melting point higher than 840 ° C. is precipitated all at once on the entire outer surface of the substrate or part exposed to the outside world. Therefore, a huge number of metal nanoparticles are precipitated according to the number of moles of the metal compound to be thermally decomposed. In addition, when the metal compound is thermally decomposed, all impurities contained in the paste, such as moisture, organic matter, and hydroxides, whose boiling points are lower than the thermal decomposition temperature of the metal compound, are vaporized, and genuine metal nanoparticles are precipitated in an active state. When the clusters of active metal nanoparticles are precipitated all at once, the metal nanoparticles are metallically bonded at the sites where they come into contact with each other, and the metallically bonded clusters of metal nanoparticles are layered, so that the entire outer surface of the substrate or part exposed to the outside world is covered with an airtight coating that is thicker than 100 nm and blocks the outside world, and is made up of the clusters of metallically bonded metal nanoparticles. Here, we will explain the effect of covering the entire outer surface of a substrate or component exposed to the outside world with a coating consisting of a layered structure of metal nanoparticles that are metallically bonded to each other and are made of metal with a melting point of higher than 840°C. First, the substrate or part can be covered with an airtight coating that blocks the outside world, regardless of the surface irregularities, size, or shape of the substrate or part. It has both heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃. It can be transformed into a substrate or part. Secondly, the coating has mechanical strength based on the metallic bonding force between the metal particles. That is, each metal particle that composes the coating comes into contact with and metallically bonds with a total of 16-18 metal particles, consisting of six adjacent metal particles on the same layered surface and five or six adjacent metal particles on the upper and lower layers. Therefore, the coating has enough mechanical strength to not be destroyed even if the substrate or part is dropped from a height of about 2m. Third, the coating has airtightness that blocks the outside world. In other words, the coating is made of granular metal nanoparticles with a size of about 10 nm that are randomly stacked without gaps, and adjacent metal nanoparticles are metallically bonded to each other. At this time, gaps are formed between adjacent nanoparticles, but when metal-bonded nanoparticles are randomly stacked, the gaps are filled, and when more than 10 metal-bonded nanoparticles are randomly stacked, there are no communicating gaps in the nanoparticle clusters of metal-bonded nanoparticles. Therefore, a coating made of a structure in which a cluster of metal-bonded nanoparticles is stacked has airtightness that blocks the outside world. Fourth, the coating has metallic properties. In other words, since the coating is composed of a collection of metal particles, the coating has the properties of the metal that composes the metal particles. This gives the substrate or part covered with the coating the electrical conductivity and thermal conductivity of a metal. The coating also functions as an electromagnetic wave shielding film and an antistatic film. Fifth, the coating repels all liquids. In other words, the surface of the coating is made up of metal particles with a size of about 10 nm that are metallically bonded. Therefore, due to the surface tension of the liquid, the liquid is repelled by the surface of the coating and cannot penetrate into the coating. Therefore, the substrate or part that has been made non-flammable can be used for a long period of time, both in liquid and outdoors. Sixth, the coating is both water-repellent and stain-resistant. That is, the surface of the coating is extremely flat because metal particles of about 10 nm in size are bonded together. Therefore, the coating is both water-repellent and stain-resistant, and foreign matter does not adhere to the coating. Therefore, the substrate or part that has been made non-flammable can be used outdoors for a long period of time. Seventh, the coating has excellent sliding properties. In other words, the surface of the coating has extremely high flatness and excellent smoothness because the metal nanoparticles with a size of about 10 nm are metallically bonded. Therefore, when other substrates or parts slide on the coating, the other substrates or parts slide on the surface of the coating. In addition, the contact area of the metal nanoparticles with the other substrates or parts is extremely small. Therefore, the coating acts as a lubricating coating with a small friction coefficient. On the other hand, the thickness of the coating is thicker than 100 nm, but it is very thin. However, the wear rate of the coating is slow, so the effect of the coating lasts a long time. Eighth, even if the temperature to which the substrate or parts covered with the coating are exposed changes suddenly during a fire, the bonding strength between the particles does not change. In other words, the thermal expansion and contraction of particles with a size of around 10 nm is extremely small. For this reason, even if the temperature to which the substrate or parts are exposed changes suddenly during a fire, the coating hardly undergoes any thermal expansion or contraction. For this reason, the metallic bonding strength between the metal particles does not change, and the coating is not destroyed even by the sudden temperature change during a fire. Ninth, the coating has heat resistance and fire resistance close to the melting point of the metal that constitutes the metal microparticles. On the other hand, general-purpose metals with melting points lower than 840°C include tin, lead, zinc, magnesium, and aluminum, in order of lowest melting point. If metal compounds that precipitate by thermal decomposition are used for metals other than these five types of metals, the coating will have both heat resistance that can withstand temperatures higher than 840°C and close to the melting point of the metal, and fire resistance that can withstand temperatures higher than 840°C and close to the melting point of the metal. Therefore, since the maximum temperature during a fire is 840°C, the coating will have both heat resistance and fire resistance no matter what kind of fire it encounters. In addition, in the event of a fire, the coating may be exposed to a temperature higher than the temperature at which the metal compound is thermally decomposed and the metal nanoparticles are precipitated. At this time, the metal nanoparticles, except for the surface of the substrate or part, are isolated from the outside world, so the metal nanoparticles without impurities are reactivated. The metal nanoparticles gradually change their particle shape from granular particles to flat particles as the temperature rises, and the particles become coarser. Therefore, the higher the temperature at which the temperature rises, the more the nanoparticles become flat. On the other hand, as the nanoparticles become flatter, the volume of the contact parts between the metal nanoparticles that are in contact with each other from above and below and from the left and right increases, and the volume of the metal bonded parts increases. This increases the mechanical strength of the coating and improves the airtightness of the coating that blocks the outside world. Furthermore, when the temperature approaches the melting point of the metal, the flattened particles bond with each other metallically, and the coating approaches a thin film with an extremely thin metallic bond thickness. Therefore, the airtightness of the coating that blocks the outside world is continuously maintained, and the coating is not destroyed even when it is subjected to an impact during a fire. As a result, the coating maintains its airtightness and can withstand temperatures of 840°C. Tenth, the surface of the coating has a metallic luster, which imparts flame retardancy and metallic luster to the substrate or part, thereby adding new value to the substrate or part. Eleventh, the coating has almost no weight. In other words, the coating is made up of more than 10 metal nanoparticles of about 10 nm each, so the coating has almost no weight. Therefore, by imparting non-combustibility to the substrate or part, there is almost no increase in the weight of the substrate or part. Twelfth, the coating can be formed in two simple steps using a cheap paste made from cheap materials and simple processes. Therefore, the coating that provides various functions and effects is inexpensive. As a result, all of the problems described in paragraph 7 are resolved. As described above, the coating that covers the entire outer surface of the substrate or part in the present invention is Heat resistance that can withstand 840℃ and fire resistance that can withstand temperatures of 840℃ Not only does it provide a good effect, it also provides many excellent effects.
[0012] As stated in paragraph 8 The metal compound is an inorganic metal compound composed of an inorganic salt having a metal complex ion in which an inorganic molecule or an inorganic ion serves as a ligand and is coordinately bonded to a metal ion, and the inorganic metal compound is As stated in paragraph 8 As metal compound, according to the method described in paragraph 8 P This is the method of making the paste described in paragraph 8 of Making the Paste.
[0013] In other words, when an inorganic metal compound consisting of an inorganic salt having a metal complex ion coordinated to a metal ion, in which an inorganic molecule or an inorganic ion is a ligand, is heat-treated in a reducing atmosphere, the coordinate bond is first broken and the compound is decomposed into the inorganic substance and the metal. When the temperature is further increased, the inorganic substance absorbs the heat of vaporization and vaporizes, and the vaporization of the inorganic substance is completed in the temperature range of 180-220℃, and the metal molecules gather together and the metal is precipitated. As described in paragraph 9, when the crystals of a metal compound are repeatedly crushed, they are crushed to crystals of about 20 nm in size. Therefore, when fine crystals of an inorganic metal compound of about 20 nm in size are thermally decomposed, after the inorganic matter is vaporized, metal nanoparticles of about 10 nm in size are precipitated. That is, among the ions constituting the inorganic metal compound, the metal ion located at the center of the molecule is the largest, and the distance between the metal ion and the ligand is the longest. When this inorganic metal compound is heat-treated in a reducing atmosphere, the coordinate bond where the metal ion is bonded to the ligand is first broken, and the compound is decomposed into the metal and the inorganic substance. When the temperature is further increased, the inorganic substance absorbs the heat of vaporization and vaporizes, and when the vaporization of the inorganic substance is completed, the metal precipitates and the thermal decomposition is completed. The temperature at which the metal precipitates is the lowest among the temperatures at which metal precipitates in the thermal decomposition of metal compounds. Therefore, the cost of the heat treatment is low. In addition, an inorganic metal compound made of an inorganic salt having a metal complex ion is dispersed in methanol at nearly 10% by weight, and is not dissolved in methanol. For this reason, the inorganic metal compound can be used as a metal compound having both of the two properties described in paragraph 8. That is, metal complex ions in which inorganic molecules or inorganic ions act as ligands and are coordinated to metal ions are easier to synthesize than other metal complex ions. Examples of such metal complex ions include ammine metal complex ions in which ammonia (NH3) acts as a ligand and is coordinated to metal ions, aqua metal complex ions in which water (H2O) acts as a ligand and is coordinated to metal ions, and hydroxyl groups (OH) ― Hydroxometal complex ion in which the ligand is coordinated to the metal ion, chloride ion Cl - Or chloride ion Cl - and chlorometal complex ions in which ammonia NH3 acts as a ligand and is coordinated to a metal ion. Furthermore, inorganic metal compounds made of inorganic salts such as chlorides, sulfates, and nitrates that have such metal complex ions are easy to synthesize, and because the molecular weight of the inorganic salt is small, the inorganic substances are vaporized and the metal is precipitated in the temperature range of 180-220°C. This temperature at which metals precipitate is the lowest of all temperatures at which metal compounds precipitate through thermal decomposition. These inorganic metal compounds are general-purpose industrial chemicals.
[0014] As stated in paragraph 8 The metal compound is an octylic acid metal compound, As stated in paragraph 8 As metal compound, according to the method described in paragraph 8 P This is the method of making the paste described in paragraph 8 of Making the Paste.
[0015] That is, when metal octylate compounds are heat-treated at 290°C in an air atmosphere, they precipitate metal. They also disperse in methanol at nearly 10% by weight, but do not dissolve in methanol. Therefore, metal octylate compounds can be used as metal compounds that combine the two properties described in paragraph 8. As described in paragraph 9, when the crystals of the metal compound are repeatedly crushed, they are crushed to crystals of about 20 nm in size. Therefore, when fine crystals of the metal octylate compound of about 20 nm in size are thermally decomposed, after the octylate is vaporized, metal nanoparticles of about 10 nm in size are precipitated. That is, among the ions constituting the metal octylate compound, the metal ion is the largest. Therefore, in the metal octylate compound in which the oxygen ion constituting the carboxyl group of octylic acid is covalently bonded to the metal ion, the distance between the oxygen ion constituting the carboxyl group and the metal ion is longer than the distance between other ions. When the metal octylate compound having such molecular structure is heat-treated in an air atmosphere, the bond between the oxygen ion constituting the carboxyl group and the metal ion is first broken when the temperature exceeds 228°C, the boiling point of octylic acid, and the compound is separated into octylic acid and metal. Furthermore, since octylic acid is a saturated fatty acid, it does not have an unsaturated structure in which carbon atoms are in excess of hydrogen atoms, so that the octylic acid takes the heat of vaporization and vaporizes, and the metal precipitates at 290°C when the vaporization is completed. When the metal octylate compound is heat-treated in a nitrogen atmosphere, the metal precipitates at 340°C. On the other hand, when a synthetic resin, which has a relatively low thermal decomposition temperature, is heated in a nitrogen atmosphere, the thermal decomposition temperature of the synthetic resin shifts to a higher temperature because the thermal decomposition reaction of the synthetic resin is an endothermic decomposition reaction rather than an exothermic decomposition reaction. Therefore, when the substrate or part is made of a synthetic resin, it is preferable to thermally decompose the metal octylate compound in a nitrogen atmosphere. In other words, the carboxylate anion (R-COO -), but metal carboxylate compounds that are covalently bonded to metal ions precipitate the metal through thermal decomposition. Such metal carboxylate compounds are, in order of decreasing thermal decomposition temperature at which they precipitate the metal, metal octylate compounds, metal laurate compounds, and metal stearates compounds. Therefore, by using metal octylate compounds, which have the lowest thermal decomposition temperature, the suspension described in paragraph 7 can be produced inexpensively. Note that metal laurate compounds and metal stearates compounds, like metal octylate compounds, are dispersed in methanol at nearly 10% by weight and do not dissolve in methanol. That is, the boiling point of lauric acid is 296°C, and the thermal decomposition temperature of metal laurate compound is 360°C. However, the thermal decomposition temperatures of metal laurate compound and metal stearate compound are higher than that of metal octylate compound. Therefore, it is desirable to use metal octylate compound as a raw material for depositing metal. In addition, compared to carboxylate metal compounds made from saturated fatty acids, carboxylate metal compounds made from unsaturated fatty acids have an excess of carbon atoms relative to hydrogen atoms, and therefore, when thermally decomposed, metal oxides, for example, in the case of copper oleate, cuprous oxide Cu2O and cupric oxide CuO are precipitated simultaneously, and processing costs are required to reduce the cuprous oxide and cupric oxide to copper. In particular, cuprous oxide must be oxidized to cupric oxide in an atmosphere richer in oxygen than the air atmosphere, and then reduced to copper in a reducing atmosphere, which increases processing costs. For this reason, the carboxylate anion (R-COO) of carboxylate of saturated fatty acids is used as a metal compound that precipitates metals when thermally decomposed. - ), but metal carboxylate compounds which are covalently bonded to a metal ion are preferred. Furthermore, metal octylate compounds are inexpensive industrial chemicals that can be easily synthesized. That is, when octylic acid is reacted with a strong alkali, an alkali metal octylate compound is produced. When the alkali metal octylate compound is then reacted with an inorganic metal compound, metal octylate compounds made of various metals are produced. Also, octylic acid is a versatile organic acid. Therefore, metal octylate compounds are the cheapest organometallic compounds among organometallic compounds. For this reason, although their thermal decomposition temperature is higher than that of the complexes made of inorganic metal compounds described in paragraph 13, they are cheaper metal compounds than the complexes.
[0016] As stated in paragraph 8 The second organic compound is an organic compound belonging to an alcoholic group, As stated in paragraph 8 as the second organic compound, As stated in paragraph 8 The first organic compound is an organic compound belonging to acetate esters, and the organic compound belonging to acetate esters is As stated in paragraph 8 as the first organic compound and according to the method described in paragraph 8. P This is the method of making the paste described in paragraph 8 of Making the Paste.
[0017] The second organic compound having the four properties described in paragraph 8 is an organic compound belonging to an alcohol family. Also, the first organic compound having a viscosity of less than 1 mPa·s at 20°C described in paragraph 8 is an organic compound belonging to an acetate family. First, the metal compound described in paragraph 8 is an inorganic metal compound described in paragraph 13, and an organic compound belonging to alcohols having a boiling point lower than 180°C is described. 3-Methyl-1-butanol (CH3)2CH(CH2)2OH has a viscosity of 3.7 mPa·s at 20°C and a boiling point of 131°C. Tertiary amyl alcohol, CH3CH2COH(CH3)2, has a viscosity of 3.8 mPa·s at 20°C and a boiling point of 103°C. 2-butanol, CH3CH2CH(OH)CH3, has a viscosity of 3.9 mPa·s at 20°C and a boiling point of 99°C. 2-Methyl-1-butanol, CH3CH2CH(CH3)CH2OH, has a viscosity of 4.0 mPa·s at 20°C and a boiling point of 108°C. 2-Heptanol, CH3(CH2)4CH(OH)CH3, has a viscosity of 4.0 mPa·s at 20°C and a boiling point of 159°C. Isobutyl alcohol (CH3)2CHCH2OH has a viscosity of 4.0 mPa·s at 20°C and a boiling point of 108°C. 4-Methyl-2-pentanol (CH3)2CHCH2CHOHCH3 has a viscosity of 4.1 mPa·s at 20°C and a boiling point of 132°C. 2-Octanol, CH3(CH2)5CH(OH)CH3, has a viscosity of 6.2 mPa·s at 20°C and a boiling point of 178°C. 3-Pentanol, CH3CH2CH(OH)CH2CH3, has a viscosity of 6.4 mPa·s at 20°C and a boiling point of 116°C. 1-Heptanol, CH3(CH2)6OH, has a viscosity of 7.4 mPa·s at 20°C and a boiling point of 176°C. 。 These ten types of alcohols have the following characteristics: (1) they are soluble in acetate esters; (2) they do not dissolve or disperse crystals of metal compounds; (3) they have a boiling point higher than that of acetate esters and lower than the thermal decomposition temperature of inorganic metal compounds; and (4) they have a viscosity of 4-7 mPa·sec at 20°C. Next, the metal compound described in paragraph 8 is the metal octylate compound described in paragraph 15, which is an organic compound belonging to alcohols having a boiling point higher than 180°C and lower than 290°C. 1-Octanol, CH3(CH2)7OH, has a boiling point of 194°C and a viscosity of 7.3 mPa·s at 25°C. 1-Octanol has the first property of being soluble in acetate esters, the second property of not dissolving or dispersing crystals of metal compounds, the third property of having a boiling point higher than that of acetate esters and lower than the thermal decomposition temperature of metal octylate compounds, and the fourth property of having a viscosity of 4-7 mPa·sec at 20°C. Next, the above-mentioned alcohol-soluble acetates having a viscosity of less than 1 mPa·sec at 20°C and a viscosity of 4-7 mPa·sec at 20°C will be described. Methyl acetate, CH3COOCH3, has a viscosity of 0.366 mPa·s at 21°C and a boiling point of 57°C. Ethyl acetate, CH3COOCH2CH3, has a viscosity of 0.462 mPa·s at 25°C and a boiling point of 77°C. Isopropyl acetate, CH3COOCH(CH3)2, has a viscosity of 0.525 mPa·s at 20°C and a boiling point of 89°C. Normal propyl acetate, CH3COO(CH2)2CH3, has a viscosity of 0.6 mPa·s at 20°C and a boiling point of 101°C. Isobutyl acetate is CH3COOCH2CH(CH3)2, its viscosity at 20°C is 0.68 mPa·s and its boiling point is 118°C. Normal butyl acetate, CH3COOC4H9, has a viscosity of 0.738 mPa·s at 20°C and a boiling point of 126°C. These six organic compounds belonging to the acetate ester group have a viscosity of less than 1 mPa·s at 20°C, and the above alcohols have a viscosity of 4-7 mPa·s at 20°C. kind Dissolves in 。 [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a cross-sectional view illustrating a melamine decorative board covered with a cluster of copper particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Example 1 This is an example of a melamine laminate covered with a cluster of copper particles. The melting point of copper is 1085°C, which is higher than the maximum temperature of 840°C during a fire as mentioned in paragraph 1. Melamine laminates are a type of surface material used in areas where strength is required, such as furniture, fixtures, and fittings. They are made by impregnating printed paper or kraft paper with melamine resin and phenolic resin, respectively, and then layering the dried impregnated papers together. They are then applied with a pressure of 100 kg / cm at 150°C. 2The laminate is molded by applying a pressure of 10000000000000000. Melamine resin decomposes into low molecular weight charcoal at 230-320℃ in the atmosphere, and the thermal decomposition of the charred residue proceeds slowly at 320-475℃, and the charred residue is burned at 475-570℃. Novolac phenolic resin also begins to release flammable plasticizers at around 260℃, continuing up to around 360℃, after which the polymer begins to thermally decompose with endothermic heat at 390℃, producing flammable gases such as phenol and cresol, and finishing at around 700℃, leaving behind 65% solid residue (ash). Therefore, phenolic resin also burns as it decomposes in the atmosphere. Tetraammine copper nitrate [Cu(NH3)4](NO3)2 (e.g., a product of Mitsuwa Chemical Industries, Ltd.) was used as the copper compound. 3-methyl-1-butanol (e.g., a product of Fujifilm Wako Pure Chemical Industries, Ltd.), which has a viscosity of 3.7 mPa·s at 20°C and a boiling point of 131°C, was used as the second organic compound. Also, isobutyl acetate (e.g., a product of Fujifilm Wako Pure Chemical Industries, Ltd.), which has a viscosity of 0.68 mPa·s at 20°C and a boiling point of 118°C, was used as the first organic compound. First, 51 g (equivalent to 0.2 moles) of tetraammine copper nitrate was dispersed in methanol to a concentration of 10% by weight, and then the methanol dispersion of tetraammine copper nitrate was heated to 65°C, the methanol was evaporated, and a cluster of tetraammine copper nitrate crystals was precipitated. The cluster of tetraammine copper nitrate crystals was then transferred to a 6 cm x 6 cm x 2 cm container. A 6 cm x 6 cm x 1 cm plate was placed on top of the cluster of tetraammine copper nitrate crystals, and five 1 kg weights were placed on the plate at equal intervals. After removing the weight, an impact acceleration of 0.2 G was repeatedly applied to the sides and bottom of the container in three directions: front-back, left-right, and up-down. After repeating the process of applying a compressive load and the process of applying an impact acceleration three times, a weight was placed on the plate, but since there was no movement of the plate, it was considered that the crushing of the tetraammine copper nitrate crystals was completed. Furthermore, 35 cc of 3-methyl-1-butanol was dissolved in 65 cc of isobutyl acetate to give a viscosity of 1.7 mPa·sec at 20°C. A mass of crushed crystals of tetraammine copper nitrate was mixed into this solution to make a suspension, which was then filled into a container. After this, five pieces measuring 5 cm x 5 cm were cut out from a 0.95 mm thick melamine decorative board (Aica Kogyo Co., Ltd. product XJN2085KV04), the cut melamine decorative boards were immersed in the above-mentioned suspension, and the cut melamine decorative boards were removed from the suspension. The five melamine decorative boards were then passed through a heat treatment device in a hydrogen atmosphere heated to 200°C, and five samples were created. Next, one sample was cut in the center, and the surface and cross section of the sample were observed using an electron microscope. An extremely low accelerating voltage SEM owned by JFE Techno-Research Corporation was used as the electron microscope. This device allows surface observation at extremely low accelerating voltages starting from 100V, and allows the surface to be observed directly without forming a conductive coating. First, a secondary electron beam between 900-1000V of the reflected electron beam was extracted and image-processed to observe the surface of the sample. The surface of the sample was covered evenly with granular particles with a size of about 10 nm. Next, the energy and intensity of the characteristic X-rays were image-processed to analyze the type of elements that make up the particles formed on the surface. They were found to be copper particles. Therefore, the surface of the sample was covered with copper particles. Next, the cross section of the sample was observed under an electron microscope. Clusters of around 15 particles were stacked tightly together, covering the melamine laminate. Figure 1 shows a schematic diagram of the cross section of the sample. 1 is the cluster of copper particles, and 2 is the melamine laminate. When the sample was cut, the cluster of copper particles adjacent to the cut area did not separate from the surface of the sample. This meant that the cluster of copper particles was bonded to the melamine laminate with a certain strength. Furthermore, five samples were allowed to drop to the floor from a height of 2m, but there was no change in the sample surface. This meant that the cluster of copper particles was bonded to the laminate with a certain strength. Furthermore, the four samples were left in a heat treatment device consisting of an air atmosphere at 840°C for two minutes. During this time, no flames, black smoke, or strange odors were generated from the samples. Furthermore, no abnormalities such as cracks were found on the surface of the samples. After this, one sample was cut. When the sample was cut, the clusters of copper particles covering the surface of the sample did not crumble, but the ash of the melamine decorative board crumbled. From these results, it was found that the clusters of copper particles had both heat resistance and fire resistance at 840°C, and also covered the melamine decorative board with airtightness, making the melamine decorative board non-flammable.
[0020] Example 2 This is an example of covering natural wood veneer decorative plywood with a cluster of copper particles. Natural wood veneer decorative boards are used as building materials such as flooring and fittings, and as surface decorative materials for furniture. Several sheets of veneer, thinly sliced wood with a thickness of 0.2-0.6 mm, are glued to plywood, and the adhesive is dried at a temperature exceeding 100°C. Note that wood ignites at temperatures of 400-460°C in the air. The copper compound used was copper octylate [CH3(CH2)3CH(C2H5)COO]2Cu (e.g., a product of Mitsuwa Chemical Industries, Ltd.). The second organic compound used was 1-octanol (e.g., a product of Fujifilm Wako Pure Chemical Industries, Ltd.), which has a boiling point of 194°C and a viscosity of 7.3 mPa·sec at 25°C. The first organic compound used was n-butyl acetate (e.g., a product of Fujifilm Wako Pure Chemical Industries, Ltd.), which has a viscosity of 0.738 mPa·sec at 20°C and a boiling point of 126°C. First, 70 g (equivalent to 0.2 moles) of copper octylate was dispersed in methanol to a concentration of 10% by weight, and then the methanol dispersion of copper octylate was heated to 65°C, the methanol was evaporated, and a cluster of copper octylate crystals was precipitated. The cluster of copper octylate crystals was then transferred to a 6 cm x 6 cm x 2 cm container. A 6 cm x 6 cm x 1 cm plate was placed on top of the cluster of copper octylate crystals, and five 1 kg weights were placed on the plate at equal intervals. After removing the weight, an impact acceleration of 0.2 G was repeatedly applied to the sides and bottom of the container in three directions: front-back, left-right, and up-down. After repeating the process of applying a compressive load and the process of applying an impact acceleration three times, the weight was placed on the plate, but since there was no movement of the plate, it was considered that the crushing of the tetraammine copper nitrate crystals was completed. After this, 10 cc of 1-octanol was dissolved in 90 cc of n-butyl acetate to give a viscosity of 1.4 mPa·sec at 20°C. A cluster of crushed copper octoate crystals was mixed into this solution to make a suspension, which was then filled into a container. Five pieces measuring 5 cm x 5 cm were cut out from a 2.5 mm thick natural wood veneer decorative plywood (a straight grain ash product from Matsumoto Plywood Co., Ltd.), immersed in the suspension as in Example 1, and then passed through a heat treatment device in an air atmosphere at 290°C to create five samples. The surface and cross section of the sample were observed under an electron microscope in the same manner as in Example 1. Clusters of copper particles were precipitated on the surface of the sample. Clusters of about 12 copper particles were layered and covered the natural wood veneer decorative plywood. When the sample was cut, the cluster of copper particles adjacent to the cut area did not separate from the surface of the sample. The cluster of copper particles was bonded to the natural wood veneer plywood with a certain strength. Five samples were allowed to fall to the floor from a height of 2m, but there was no change in the sample surface. This shows that the cluster of copper particles was bonded with a certain strength. Furthermore, as in Example 1, the four samples were left in a heat treatment device consisting of an air atmosphere at 840°C for two minutes. At this time, no flames, black smoke, or strange odors were generated from the samples. Furthermore, no abnormalities such as cracks were observed on the surface of the samples. After this, one sample was cut. When the sample was cut, the cluster of copper particles did not crumble, but the ash of the natural wood veneer decorative plywood crumbled. Therefore, the cluster of copper particles had both heat resistance and fire resistance at 840°C, and covered the natural wood veneer decorative plywood with airtightness, providing non-flammability to the natural wood veneer decorative plywood.
[0021] The two examples are only a part of the examples. In other words, by immersing a substrate or a part in the suspension and then thermally decomposing the copper compound adsorbed on the substrate or the part, the surface of the flammable or flame-retardant substrate or part can be covered with a collection of copper fine particles. In addition, the metal fine particles are not limited to copper fine particles, and the surface of the flammable or flame-retardant substrate or part can be covered with a collection of various metal fine particles precipitated by thermal decomposition of the metal compound. That is, regardless of the material, shape, size, or surface condition of the substrate or part, if the substrate or part is immersed in the suspension, the suspension will adhere to the surface of the substrate or part depending on the viscosity of the suspension. In the two examples, a flat plate material was used, but even in the case of a part, if the part is immersed in the suspension, the suspension will adhere to the surface of the part depending on the viscosity of the suspension, regardless of the material, shape, size, or surface condition of the part. In addition, the thickness of the suspension attached to the substrate or part is determined by the viscosity of the suspension. As a result, the number of copper particles that are stacked without gaps to cover the substrate or part can be freely changed by the viscosity of the suspension. In the two examples, the number of copper particles stacked without gaps was about 12 and about 15, but all the copper particles were bonded to each other, and the copper particle group was bonded to the substrate or part, so the copper particle group exhibited airtightness. Therefore, regardless of the material, shape, size, and surface condition of the substrate or part, the substrate or part can be covered with the airtight metal particle group. Therefore, even at a high temperature of 840°C, the airtight metal particle group provides non-flammability to the substrate or part. This non-flammability can be imparted to all flammable or flame-retardant substrates or parts. [Explanation of symbols]
[0022] 1. A cluster of copper particles stacked together 2. Melamine laminate
Claims
1. The method for producing a paste for converting a flammable or flame-retardant material into a material having both heat resistance to withstand 840°C and fire resistance to withstand a temperature of 840°C comprises the steps of: A metal compound having both a first property of being dispersed in methanol in a molecular state but not dissolved in methanol and a second property of precipitating a metal having a melting point higher than 840°C by thermal decomposition is dispersed in methanol to prepare a methanol dispersion of the metal compound, and then the methanol is evaporated from the methanol dispersion of the metal compound to precipitate a crystal cluster of the metal compound. The collection of crystals of the metal compound is then filled into a container, and a plate material covering the entire surface of the collection of crystals of the metal compound is placed on the collection of crystals of the metal compound. A compressive load is then applied to the entire surface of the plate material to crush the crystals of the metal compound in the container. Impact acceleration is then repeatedly applied to the side and bottom of the container in three directions, namely, front-back, left-right, and up-down, to rearrange the crushed collection of crystals of the metal compound in the container. The compressive load is then applied again to the entire surface of the plate material to further crush the crystals of the metal compound. Impact acceleration is then repeatedly applied again in the three directions to the side and bottom of the container. A pair of processes consisting of the process of applying the compressive load and the process of applying the impact acceleration are repeated, and when the plate material stops moving when the compressive load is applied to the plate material, it is determined that the crushing of the crystals of the metal compound is completed, and the pair of processes is stopped. The plate material is then removed from the container. a second organic compound having a first property of being soluble in a first organic compound having a viscosity at 20°C of less than 1 mPa·sec, a second property of not dissolving or dispersing crystals of the metal compound, a third property of having a boiling point higher than the boiling point of the first organic compound and lower than the thermal decomposition temperature of the metal compound, and a fourth property of having a viscosity at 20°C of 4-7 mPa·sec, is dissolved in the first organic compound so that the viscosity at 20°C is lower than 2 mPa·sec, and the solution is mixed with the collection of crushed crystals of the metal compound in the container to prepare a suspension in which the collection of crushed crystals of the metal compound is dispersed in the solution; A method for producing a paste for converting a flammable or flame-retardant substance into a substance having both heat resistance and fire resistance to a temperature of 840°C, the method using the suspension produced by the above-mentioned treatment as a paste for converting a flammable or flame-retardant substance into a substance having both heat resistance and fire resistance to a temperature of 840°C.
2. A method for converting a flammable or flame-retardant substance into a substance having both heat resistance and fire resistance to a temperature of 840°C by using the suspension according to claim 1 as a paste for converting the flammable or flame-retardant substance into a substrate or part having both heat resistance and fire resistance to a temperature of 840°C, the method comprising the steps of: The paste is filled into a container, and a substrate or a part made of a flammable or flame-retardant material is entirely immersed in the paste in the container, and then the substrate or the part is removed from the container, and a coating having a thickness of less than 1 μm and made of the paste is adsorbed onto the entire outer surface of the substrate or the part exposed to the outside. Thereafter, the substrate or the part is exposed to an atmosphere in which the metal compound described in claim 1 is thermally decomposed, and the temperature is raised to a temperature at which the metal compound is thermally decomposed. As a result, the first organic compound described in claim 1 and the second organic compound described in claim 1 are vaporized in order according to their boiling points, and then the metal compound is thermally decomposed, and a collection of metal nanoparticles of about 10 nm in size made of a metal having a melting point higher than 840° C. precipitates all at once in an active state as true metal nanoparticles on the entire outer surface of the substrate or the part exposed to the outside world, and the precipitated metal nanoparticles are metallically bonded at the sites where they come into contact with each other, and the metallically bonded metal nanoparticles are stacked, and the entire outer surface of the substrate or the part exposed to the outside world is covered with an airtight coating that blocks the outside world and is made of the metallic nanoparticles that are stacked together. As a result, the entire outer surface of the substrate or part made of a flammable or flame-retardant substance that is exposed to the outside world is covered with an airtight coating that blocks the outside world and is made of a collection of metal nanoparticles laminated with collections of metal-bonded metal nanoparticles, and the substrate or part made of a flammable or flame-retardant substance is transformed into a substrate or part that has both heat resistance capable of withstanding 840°C and fire resistance capable of withstanding temperatures of 840°C. This is a method for transforming a substrate or part made of a flammable or flame-retardant substance into a substrate or part that has both heat resistance capable of withstanding 840°C and fire resistance capable of withstanding temperatures of 840°C.
3. A method for creating a paste as described in claim 1, wherein the metal compound described in claim 1 is an inorganic metal compound composed of an inorganic salt having a metal complex ion in which an inorganic molecule or an inorganic ion serves as a ligand and is coordinately bonded to a metal ion, and the inorganic metal compound is used as the metal compound described in claim 1, and a paste is created according to the method described in claim 1.
4. A method for creating a paste as described in claim 1, comprising using the metal compound as described in claim 1 which is an octylic acid metal compound, and creating a paste according to the method as described in claim 1.
5. A method for creating a paste as recited in claim 1, wherein the second organic compound as recited in claim 1 is an organic compound belonging to alcohols, and the organic compound belonging to alcohols is used as the second organic compound as recited in claim 1, and the first organic compound as recited in claim 1 is an organic compound belonging to acetates, and the organic compound belonging to acetates is used as the first organic compound as recited in claim 1, and a paste is created according to the method as recited in claim 1.
Citation Information
Patent Citations
JP20016-117810A
JP20013-043891A