Foam stabilizers for phenolic foam

Acrylate and methacrylate copolymers stabilize phenolic foams without siloxanes, addressing the issue of cyclic siloxane formation, resulting in improved thermal insulation and stability.

JP2024156630APending Publication Date: 2024-11-06EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024069653
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-23
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

The decomposition of polyether-modified siloxanes in the presence of acids as catalysts during phenolic foam production leads to the formation of cyclic siloxanes like D4, D5, and D6, which negatively impact the foam's properties, particularly thermal insulation.

Method used

A composition for phenolic foam production using acrylate and/or methacrylate copolymers as foam stabilizers, along with alkoxylated vegetable oils, to stabilize the foam without siloxanes, thereby minimizing the formation of cyclic siloxanes and maintaining excellent thermal insulation properties.

Benefits of technology

The solution achieves phenolic foams with superior thermal insulation, long-term stability, and high surface quality without compromising other properties, while eliminating or reducing the formation of D4, D5, and D6.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156630000001
    Figure 2024156630000001
  • Figure 2024156630000002
    Figure 2024156630000002
  • Figure 2024156630000003
    Figure 2024156630000003
Patent Text Reader

Abstract

To provide a composition for producing a phenolic foam containing a new foaming stabilizer having no adverse effect on emission due to formation of a decomposition product, which is a drawback of a polyether-modified siloxane as a foaming stabilizer conventionally used for a phenolic foam.SOLUTION: There is provided a composition for producing phenolic foam, comprising at least one phenolic resin, at least one blowing agent, and at least one catalyst, wherein the composition comprises at least one acrylate and / or methacrylate copolymer as a foaming stabilizer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of phenolic foams. The present invention relates in particular to compositions for producing phenolic foams, to a method for producing phenolic foams, to phenolic foams produced according to the invention and their use. In the context of the present invention, phenolic foams are understood to mean in particular foams obtained by reacting phenolic resins with acids as catalysts with the addition of blowing agents and foam stabilizers. Phenolic foams are known to the person skilled in the art and are described, for example, in EP 3830174, EP 602004006376 (German translation), EP 2898005, EP 1922357, WO 2022043561, EP 4073155, AUS 2021238847 or WO 2006114777. Phenolic foams are also known by the name phenolic resin foams. This also applies to the present invention.

[0002] In the production of phenolic foams, cell stabilizing additives or foam stabilizing additives can generally be used, which are aimed at obtaining a homogeneous and less turbulent foam structure with fine cells, and thus have a significant positive effect on the use properties of the foam, in particular, for example, on the thermal insulation performance. For this purpose, foam stabilizers can usually be used, for example, foam stabilizers based on ethoxylated vegetable oils, for example, castor oil, as described, for example, in EP-A-3830174. The use of polyether-modified siloxanes (PES), as described, for example, in WO-A-2022043561, has proven to be particularly effective in further improving the use properties. In particular, the combination of ethoxylated vegetable oils and polyether-modified siloxanes results in excellent use properties. This combination is therefore a generally preferred type of foam stabilizer in the production of phenolic foams.

[0003] The use of polyether-modified siloxanes as foam stabilizers in the presence of acids as catalysts can lead to the decomposition of the polyether-modified siloxanes and the subsequent formation of cyclic siloxanes, especially octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5) and dodecamethylcyclohexasiloxane (D6), which have a negative effect on the properties of phenolic foams, especially emissions.

[0004] Against this background, the object of the present invention was to provide a phenolic foam which has similar use properties, in particular heat insulating properties, as phenolic foams produced using conventional polyether-modified siloxanes, but which does not or only little form D4, D5 and / or D6 in terms of emissions related to the formation of cyclic siloxanes.

[0005] This problem is solved by the subject matter of the present invention, which is a composition for producing phenolic foam, comprising at least one phenolic resin, at least one blowing agent and at least one catalyst, said composition comprising at least one acrylate and / or methacrylate copolymer as foam stabilizer.

[0006] The subject matter according to the invention has various advantages. For example, it makes it possible to provide a phenolic foam that meets the known requirements. In particular, the phenolic foam has very good heat insulating properties, shows excellent long-term behavior and high surface quality. Advantageously, this is possible without impairing the other properties of the material and with no or only little formation of cyclic siloxanes, especially D4, D5 and / or D6. Furthermore, a homogeneous, less disturbed foam structure is possible, especially with fine cells. The invention basically makes it possible to carry out siloxane-free foam stabilization, i.e., it makes it possible to completely dispense with siloxane-based additives, such as, for example, known polyether-modified siloxanes. Furthermore, the invention also makes it possible to use in combination with alkoxylated vegetable oils known from the prior art.

[0007] At least one acrylate and / or methacrylate copolymer is selected from the group consisting of H2C=CR 1 -COOR 2 and at least one comonomer of the type H2C=CR 1 -COOR 3 and at least one comonomer of the type: R 1 = each independently of the other is -H or -CH3 and the different substituents R 1 It is possible for different comonomers to be present in the copolymer, having the following structure: R 2 = each independently of the others, identical or different radicals from the group of saturated or unsaturated, linear, cyclic or branched, aliphatic or aromatic hydrocarbons having 1 to 25 carbon atoms, preferably methyl, ethyl, n-butyl, i-butyl, t-butyl, 2-ethylhexyl, isodecyl, cyclohexyl, benzyl, phenyl, isobornyl or allyl R 3 =Each independently of the other, Eq. (1) [ka] are identical or different polyether groups having a general average composition according to Where: x=1 to 500, advantageously 1 to 250, in particular 3 to 80, R 4 = each independently of one another is an identical or different group -CH2-O-, -CH2-CH2-O-, -CH2-CH2-CH2-O-, -CH2-CH2-CH2-CH2-CH2-O-, or -CH2-CH2-CH2-CH2-CH2-CH2-O-, R 4 may be omitted, R 5= each independently of the others, identical or different alkyl groups having 1 to 18 carbon atoms, optionally having an ether function, or identical or different aryl groups having 6 to 18 carbon atoms, optionally having an ether function, or H, preferably H, methyl, ethyl or benzyl, with the group R 3 Within each, different substituents R 5 may be present in any order or sequence, R 6 = each independently of the others, identical or different alkyl groups having 1 to 18 carbon atoms, optionally having an ether function, or identical or different aryl groups having 6 to 18 carbon atoms, optionally having an ether function, or H, preferably H, methyl, ethyl or benzyl, with the group R 3 Within each, different substituents R 6 may be present in any order or sequence, For the monomer repeat unit, preferably there are two groups R 5 and R 6 =H or two groups R 5 and R 6 one of which is H and the other is methyl; R 7 = each independently of the other: R 8 、 C(O)R 8 , -CH2-CH(OH)-CH2OH, and -CH2-C(CH2OH)2-CH2-CH3, preferably methyl, butyl, H or C(O)Me; 7 It is possible for different comonomers to be present in the copolymer, having the following structure: R 8 = each independently of the other, the same or different alkyl groups having 1 to 16 carbon atoms, the same or different aryl groups having 6 to 16 carbon atoms, or H A particularly preferred embodiment of the present invention is when the composition according to the invention is characterized in that

[0008] Particularly preferred examples of acrylate and / or methacrylate monomers that can be used in the context of the present invention include, but are not limited to, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, hexyl (meth)acrylate, ethylhexyl (meth)acrylate, isodecyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobutyl ... runyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, phenylethyl (meth)acrylate), 3,3,5-trimethylcyclohexyl (meth)acrylate, hydroxyalkyl (meth)acrylates, such as 3-hydroxypropyl methacrylate, 3,4-dihydroxybutyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2,5-dimethyl-1,6-hexanediol (meth)acrylate, 1,10-decanediol (meth)acrylate; Lithium dimethacrylates, such as 1,4-butanediol methacrylate, 2-butoxyethyl methacrylate, 2-ethoxyethoxymethyl methacrylate, 2-ethoxyethyl methacrylate; methacrylates of ether alcohols, such as tetrahydrofurfuryl methacrylate, vinyloxyethoxyethyl methacrylate, methoxyethoxyethyl methacrylate, 1-butoxypropyl methacrylate, 1-methyl(2-vinyloxy)ethyl methacrylate, cyclohexyloxymethyl methacrylate, methoxymethoxyethyl Methacrylate, benzyloxymethyl methacrylate, furfuryl methacrylate, 2-butoxyethyl methacrylate, 2-ethoxyethoxymethyl methacrylate, 2-ethoxyethyl methacrylate, allyloxymethyl methacrylate, 1-ethoxybutyl methacrylate, methoxymethyl methacrylate, 1-ethoxyethyl methacrylate, ethoxymethyl methacrylate and / or ethoxylated or propoxylated (meth)acrylates, preferably having 1 to 20, in particular 2 to 8, ethoxy or propoxy groups.

[0009] In this specification, the term (meth)acrylate means methacrylates, such as methyl methacrylate, ethyl methacrylate, and acrylates, such as methyl acrylate, ethyl acrylate, and mixtures of both.

[0010] Furthermore, processes for the preparation of usable acrylate and / or methacrylate copolymers are known to the person skilled in the art from the prior art: these are described, for example, in EP 1 070 730 A or US 9 349 500 B1.

[0011] At least one blowing agent is selected from the group consisting of: - Hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclo-, iso- and / or n-pentane And - halogenated hydrocarbons having 3, 4 or 5 carbon atoms, preferably isopropyl chloride, hydrofluoroolefins and / or hydrohaloolefins, preferably 1234ze, 1234yf, 1224yd, 1233zd(E) and / or 1336mzz There is a further particularly preferred embodiment of the present invention, when the composition according to the invention is characterized in that it is selected from the group consisting of:

[0012] There is also a further particularly preferred embodiment of the present invention, when the at least one acrylate and / or methacrylate copolymer has a number-average molecular weight Mn, determined by gel permeation chromatography according to DIN 55672-1:2016-03 (eluent: THF; standard: PMMA), in the range from 500 to 100,000 g / mol, particularly preferably from 1,000 to 40,000 g / mol and in particular from 1,000 to 25,000 g / mol.

[0013] According to a further particularly preferred embodiment of the invention, the at least one acrylate and / or methacrylate copolymer is present in the composition according to the invention in a total amount of 0.1 to 15 parts by weight, advantageously 0.5 to 10 parts by weight, particularly preferably 0.5 to 8 parts by weight, based on 100 parts by weight of the total phenolic resin used.

[0014] Advantageously, the composition according to the invention may further comprise at least one Si-containing foam stabilizer, preferably in a total amount of less than 50 wt.%, more preferably less than 25 wt.%, even more preferably less than 10 wt.%, relative to the total amount of all foam stabilizers contained.

[0015] According to a further preferred embodiment of the present invention, the composition according to the present invention does not comprise a Si-containing foam stabilizer.

[0016] According to a further preferred embodiment of the present invention, the composition according to the present invention further comprises at least one silicon-free surfactant and / or silicon-free foam stabilizer, each of which is not an acrylate and / or methacrylate copolymer, in a total amount of 0.1 to 15 parts by weight, preferably 1 to 10 parts by weight, based on 100 parts by weight of the total phenolic resin used.

[0017] If the composition according to the invention further comprises at least one alkoxylated, preferably ethoxylated vegetable oil, in particular castor oil, in a total amount of 0.1 to 15 parts by weight, advantageously 1 to 10 parts by weight, relative to 100 parts by weight of the total phenolic resin used, this corresponds to a further preferred embodiment of the invention.

[0018] As initiators, in principle, compounds which decompose under the polymerization conditions into radicals, such as peroxides, hydroperoxides, hydrogen peroxide, persulfates, azo compounds and so-called redox initiators, can be used for the preparation of the acrylate and / or methacrylate copolymers usable according to the invention. In some cases, it may also be advantageous to use mixtures of different initiators, for example mixtures of hydrogen peroxide with sodium or potassium peroxodisulfate. Possible organic peroxides are, for example, acetylacetone peroxide, methyl ethyl ketone peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, tert-amyl perpivalate, tert-butyl perpivalate, tert-butyl perneohexanoate, tert-butyl perisobutyrate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl perisonanoate, tert-butyl permaleate, tert-butyl perbenzoate, di-(2-ethylhexyl)-2-methyl-1,2-propanediol, tert-butyl perisopropyl peroxypropane ... peroxydicarbonate, dicyclohexyl peroxydicarbonate, di-(4-tert-butylcyclohexyl) peroxydicarbonate, dimyristyl peroxydicarbonate, diacetyl peroxydicarbonate, allyl perester, cumyl peroxyneodecanoate, tert-butylper-3,5,5-trimethylhexanoate, acetylcyclohexylsulfonyl peroxide, dilauryl peroxide and / or tert-amylperoxy-2-ethylhexanoate. Other possible initiators are azo compounds, such as 2,2'-azobis-isobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile) and / or 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile).

[0019] Surprisingly, it has been found within the scope of the present invention that when the acrylate and / or methacrylate copolymers usable according to the present invention are produced preferably with tert-butylperoxy-2-ethylhexanoate (TBPEH) or tert-amylperoxy-2-ethylhexanoate (APO) or a combination of TBPEH and APO as initiators, even better results can be achieved in terms of the properties required according to the present invention.Thus, when at least one acrylate and / or methacrylate copolymer is produced with TBPEH (tert-butylperoxy-2-ethylhexanoate) and / or APO (tert-amylperoxy-2-ethylhexanoate) as initiators, this corresponds to a particularly preferred embodiment of the present invention.

[0020] Furthermore, if at least one acrylate and / or methacrylate copolymer has a residual monomer content of less than 1% by weight based on the total acrylate and / or methacrylate copolymers involved, this corresponds to a particularly preferred embodiment of the present invention. The residual monomer content can be determined using conventional methods, in particular by solid content or by GC or HPLC. The corresponding composition allows for a particularly advantageous foam according to the present invention.

[0021] In addition to the at least one acrylate and / or methacrylate copolymer which can be used according to the invention, in principle all foam-stabilizing components known from the prior art can additionally be used.

[0022] The composition according to the invention comprises at least one catalyst. According to a particularly preferred embodiment of the invention, the at least one catalyst is selected from the group consisting of organic and inorganic acids, advantageously the at least one catalyst is selected from the group consisting of sulfuric acid, phosphoric acid, benzenesulfonic acid, xylenesulfonic acid, p-toluenesulfonic acid, ethylbenzenesulfonic acid, naphtholsulfonic acid, cumenesulfonic acid and phenolsulfonic acid.

[0023] If the at least one catalyst is present in the composition according to the invention in a total amount of 1 to 30 parts by weight, advantageously 1 to 25 parts by weight, particularly preferably 3 to 20 parts by weight, based on 100 parts by weight of the total phenolic resin used, this corresponds to a further particularly preferred embodiment of the invention.

[0024] Advantageously, the at least one acrylate and / or methacrylate copolymer usable according to the invention can be used both in bulk and in a solvent. All suitable substances usable for the production of phenolic foams can be used here.

[0025] Particularly preferred phenolic foam formulations in the sense of the present invention have a melting point of 5 to 900 kg / m 3 and advantageously has the composition shown in Table 1, which corresponds to a preferred embodiment of the invention: [Table 1]

[0026] A further subject of the present invention is a process for the preparation of phenolic foam, which is carried out using a reaction mixture comprising a composition according to the invention as defined above, in particular as defined in any one of claims 1 to 12.

[0027] For further preferred embodiments and configurations of the method according to the invention, reference is also made to the explanations already given above in connection with the composition according to the invention.

[0028] A further subject of the present invention is a phenolic foam produced by the process according to the invention as described above, advantageously using the composition according to the invention, in particular as defined in any one of claims 1 to 12.

[0029] Phenolic foam is rated at 5-500kg / m according to ASTM D1622-2020 3 , preferably 10 to 200 kg / m 3 , particularly preferably 12 to 100 kg / m 3Particularly preferred phenolic foams exist when the foam has a density of 0.1 to 0.5% by weight, which corresponds to a particularly preferred embodiment of the present invention.

[0030] A further subject of the invention is the use of the phenolic foam according to the invention for thermal insulation.

[0031] Particularly preferred compositions according to the invention are described in more detail below.

[0032] Particularly preferred compositions according to the invention comprise the following components: - at least one phenolic resin, at least one blowing agent, - at least one catalyst, at least one acrylate and / or methacrylate copolymer as foam stabilizer, - optionally further additives etc.

[0033] The production of phenolic foams (also called phenolic resin foams; these terms are synonymous within the scope of the present invention) is known per se. To produce phenolic foams, one or more phenolic resins, advantageously one or more so-called resole resins, are used. The phenolic resins, advantageously resole resins, which can be used accordingly, are known per se. In particular, they can be produced in a known manner, advantageously by condensation of phenol or phenolic compounds, such as cresol, xylenol, p-alkylphenols, p-phenylphenol, resorcin, etc., and aldehydes, such as formaldehyde, furfural, acetaldehyde, etc., under basic conditions, for example by using catalytic amounts of alkali metal hydroxides, such as sodium hydroxide, potassium hydroxide or calcium hydroxide, or aliphatic amines, such as trimethylamine or triethylamine, preferably together with an excess of aldehyde. This is the usual route for the production of phenolic resins, advantageously resole resins, but the invention is not limited to the chemicals listed above.

[0034] Here, the molar ratio of phenolic groups to aldehyde groups is not particularly limited. Preferably, the ratio is in the range of 1:1 to 1:3, particularly preferably in the range of 1:1.5 to 1:2.5. Advantageously, but not limited to, the phenolic resin has a free aldehyde content of 0.1% to 0.5% by weight. This can be determined by potentiometric titration according to ISO 11402:2004 with hydroxylamine hydrochloride.

[0035] The phenolic resins which can be preferably used in the production of foams are liquid at 25° C. and normal pressure, advantageously have a water concentration of about 1 to 25% by weight, preferably 5 to 20% by weight, and have methylol groups as reactive substituents, as described, for example, in EP 0 170 357. If desired, the viscosity of the phenolic resin can be adjusted, in particular by the water content. A high water content usually results in a low viscosity, which makes the resin easier to handle and mix during the production of foams.

[0036] The viscosity of the preferably usable phenolic resins at 25° C. and normal pressure is advantageously in the range of 1000 to 28000 mPa·s and can be measured by the usual methods known to the skilled artisan, for example with a Brookfield viscometer. Basic information on the production and composition of phenolic resins can be obtained from the prior art and is described in particular in, for example, EP 3830174, EP 2898005, WO 2022043561 or EP 4073155.

[0037] Blowing agents and their use in the production of phenolic foams are known to those skilled in the art. The use of one or more blowing agents depends essentially on the type of system and the application of the resulting phenolic foam. Depending on the amount of blowing agent used, high or low density foams can be produced. For example, advantageously 5 kg / m according to ASTM D1622-20. 3 ~900kg / m 3 , preferably 5 to 500 kg / m3 , particularly preferably 10 to 200 kg / m 3 , especially 12 to 100 kg / m 3 It is possible to produce foams having densities of

[0038] As blowing agents it is advantageous to use one or more corresponding compounds having a suitable boiling point, for example hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclo-, iso- or n-pentane, halogenated hydrocarbons, for example chlorinated hydrocarbons, for example dichloroethane, 1,2-dichloroethene, n-propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, isopentyl chloride, 1,1-dichloroethene, trichloroethene or chloroethene, or hydrofluorocarbons (HFCs), for example HFC245fa, HFC134a or HFC365mfc, hydrofluoroolefins (HFOs) or hydrohaloolefins, preferably 1234ze, 1234yf, 1224yd, 1233zd(E) or 1336mzz, and mixtures thereof.

[0039] Catalysts which can be used for the production of phenolic foams are known to the skilled person from the prior art and are described, for example, in EP 0170357 A1 or the German translation of EP 602004006376 A1. Advantageously, here, the usual organic and inorganic acids known from the prior art can be used. One or more acids can be used. Particularly preferably usable are sulfuric acid, phosphoric acid, benzenesulfonic acid, xylenesulfonic acid, p-toluenesulfonic acid, ethylbenzenesulfonic acid, naphtholsulfonic acid, cumenesulfonic acid and / or phenolsulfonic acid. In particular, mixtures of several of these compounds can be used as catalysts. The preferred amount of catalyst used for the complete reaction is in particular also influenced by the water content of the phenolic resin and / or the water content of the catalyst if it is present as an aqueous solution. For example, a higher water content may require a higher acid concentration.

[0040] Phenolic foams can be formed in a known manner, i.e., by reaction of a mixture containing, inter alia, a phenolic resin, a blowing agent, a foam stabilizer and a catalyst. When a catalyst is added to a mixture of a phenolic resin, a blowing agent and a foam stabilizer, an exothermic reaction occurs between the methylol groups and the phenol, forming methylene bridges and crosslinking. Water is eliminated by condensation. Here, the type and amount of acid used, the properties of the blowing agent and the structure of the foam stabilizer influence the exothermicity of the reaction and the foam formation.

[0041] Foam stabilizers and their use in the production of phenolic foams are generally known to those skilled in the art, as mentioned above. According to the present invention, at least one foam stabilizer based on acrylate and / or methacrylate copolymers is used. Additional foam stabilizers can also be used to assist in the production of foam. These compounds are well known from the prior art. For example, the use of ethoxylated castor oil is described in EP 3830174.

[0042] As optional additives, one or more substances known from the prior art that are commonly used in the production of phenolic foams can be used, such as viscosity reducers, plasticizers, hardeners, flame retardants, cell refining additives, fillers, colorants, pigments and / or fragrances. Suitable optional additives are described, for example, in EP-A-3830174, US-A-4444912 and EP-A-1922357.

[0043] As optional solid fillers, for example, metal hydroxides, such as aluminum hydroxide, magnesium hydroxide, metal carbonates, such as calcium carbonate, magnesium carbonate, barium carbonate or zinc carbonate, metal oxides, such as aluminum oxide or zinc oxide, or metal powders, such as zinc, can be used. To reduce the viscosity of the phenolic resin, for example, monoethylene glycol or polyester polyols can be used. As hardeners, for example, compounds with amino groups, such as urea or dicyandiamide, can be used. Urea is preferably used. These can be used optionally not only during foaming, but also already during the production of the phenolic resin.

[0044] The process for producing the phenolic foam according to the invention can be carried out using any known method, which is known to the person skilled in the art and is described, for example, in EP-A-3830174.

[0045] Unless otherwise apparent from the specification, all preferred or particularly preferred embodiments of the invention can be combined with one or more other preferred or particularly preferred embodiments of the invention.

[0046] The subject matter according to the present invention will be described below by way of example, but the scope of the present invention is clear from the entire specification and the claims, and the present invention is not limited to these exemplary embodiments. When ranges, general formulas or compound classes are given, these are intended to include not only the corresponding ranges or compound groups explicitly mentioned, but also all subranges and subcompound groups that can be obtained by extracting the individual values ​​(ranges) or compounds. When documents are cited within the present specification, their contents are fully incorporated into the disclosure of the present invention, in particular with regard to the subject matter in the context in which the documents are cited. Unless otherwise stated, percentages are data in weight percent. When average values ​​are given, these are numerical averages, unless otherwise stated. When parameters determined by measurement are given, the measurements were carried out at a temperature of 23° C. and at normal pressure, unless otherwise stated.

[0047] Working Example: Example 1: Synthesis of copolymers A to J Copolymer A: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 30.01 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.2 g of TBPEH (tert-butyl peroxy-2-ethylhexanoate), 56.18 g of isobutyl methacrylate (i-BMA), 67.29 g of MPEG500 methacrylate (MPEG500MA) and 2.21 g of 2-mercaptoethanol was added over 4 hours using a peristaltic pump. The mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C. and 0.13 g of TBPEH dissolved in 10 g of n-butyl acetate was added for post-reaction and post-stirred at 80 ° C. for 2 hours. An additional 5 g of n-butyl acetate was added and this was stirred for an additional 30 minutes without heating.

[0048] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard material: PMMA): Mw = 5630 g / mol; Mn = 2560 g / mol; PDI (polydispersity) = 2.2.

[0049] Copolymer B: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 30.09 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.18 g of TBPEH (tert-butyl peroxy-2-ethylhexanoate), 76.75 g of isobutyl methacrylate (i-BMA), 46.58 g of MPEG500 methacrylate (MPEG500MA) and 2.21 g of 2-mercaptoethanol was added over 4 hours using a peristaltic pump. The mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C. and 0.13 g of TBPEH dissolved in 10 g of n-butyl acetate was added for post-reaction and post-stirred at 80 ° C. for 2 hours. An additional 5 g of n-butyl acetate was added and this was stirred for an additional 30 minutes without heating.

[0050] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PS): Mw = 7373 g / mol; Mn = 3156 g / mol; PDI = 2.3.

[0051] Copolymer C: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 30.15 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.02 g of TBPEH (tert-butyl peroxy-2-ethylhexanoate), 53.77 g of isobutyl methacrylate (i-BMA), 70.92 g of MPEG500 methacrylate (MPEG500MA) and 1.15 g of 2-mercaptoethanol was added over 4 hours using a peristaltic pump. The mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C. and 0.12 g of TBPEH dissolved in 10 g of n-butyl acetate was added for post-reaction and post-stirred at 80 ° C. for 2 hours. An additional 5 g of n-butyl acetate was added and this was stirred for an additional 30 minutes without heating.

[0052] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PS): Mw = 11290 g / mol; Mn = 3536 g / mol; PDI = 3.2.

[0053] Copolymer D: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 30.01 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.2 g of TBPEH, 54.69 g of isodecyl methacrylate (IDMA), 68.77 g of MPEG500MA and 2.21 g of 2-mercaptoethanol was added over 4 hours using a peristaltic pump. The mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C. and 0.13 g of TBPEH dissolved in 10 g of n-butyl acetate was added for post-reaction and post-stirred at 80 ° C. for 2 hours. An additional 5 g of n-butyl acetate was added and this was further stirred for 30 minutes without heating.

[0054] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PMMA): Mw = 5250 g / mol; Mn = 2410 g / mol; PDI = 2.2.

[0055] Copolymer E: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 30.08 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.23 g of TBPEH (tert-butylperoxy-2-ethylhexanoate), 76.93 g of isobutyl methacrylate (i-BMA), 46.54 g of MPEG500 methacrylate (MPEG500MA) and 2.25 g of 2-mercaptoethanol was added over 4 hours using a peristaltic pump. The mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C. and 0.14 g of TBPEH dissolved in 10 g of n-butyl acetate was added for post-reaction and post-stirred at 80 ° C. for 2 hours. An additional 5 g of n-butyl acetate was added and this was stirred for an additional 30 minutes without heating.

[0056] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PS): Mw = 6202 g / mol; Mn = 2427 g / mol; PDI = 2.6.

[0057] Copolymer F: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 29.85 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.12 g of TBPEH (tert-butyl peroxy-2-ethylhexanoate), 52.38 g of isobutyl methacrylate (i-BMA), 68.67 g of MPEG500 methacrylate (MPEG500MA) and 4.45 g of 2-mercaptoethanol was added over 4 hours using a peristaltic pump. The mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C. and 0.13 g of TBPEH dissolved in 10 g of n-butyl acetate was added for post-reaction and post-stirred at 80 ° C. for 2 hours. An additional 5 g of n-butyl acetate was added and this was stirred for an additional 30 minutes without heating.

[0058] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PS): Mw = 5103 g / mol; Mn = 2127 g / mol; PDI = 2.4.

[0059] Copolymer G: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 30.01 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 20.75 g of BP-50-FT (dibenzoyl peroxide), 50.92 g of i-BMA, 60.99 g of MPEG500MA and 2.21 g of 2-mercaptoethanol was added over 4 hours using a peristaltic pump. The mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C and 0.13 g of BP-50-FT dissolved in 10 g of n-butyl acetate was added for post-reaction and post-stirred at 80 ° C for 2 hours. An additional 5 g of n-butyl acetate was added and this was further stirred for 30 minutes without heating.

[0060] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PMMA): Mw = 6350 g / mol; Mn = 4080 g / mol; PDI = 1.6.

[0061] Copolymer H: A 1000 mL four-neck flask equipped with a reflux condenser and N2 conduit, a sabre stirrer (100 rpm) and a Pt100 digital internal thermometer was charged with a mixture of 265.05 g of petroleum benzine (bp 100-120 ° C) and 265.05 g of toluene, and the oil bath was heated to 135 ° C. A mixture of 4.43 g of BP-50-FT (dibenzoyl peroxide), 90.59 g of C17.4MA (stearyl methacrylate), 55.02 g of MPEG350MA (MPEG350 methacrylate) and 19.06 g of i-BMA was added over 5 hours using a peristaltic pump. After the end of the addition, 0.40 g of BP-50-FT was added for post-reaction and further stirred for 2 hours. It was cooled to room temperature and the batch was left overnight in the flask without stirring. The oil bath was heated to 130° C. again, and 0.40 g of BP-50-FT was added and stirred for 3 hours.

[0062] The batch was concentrated on a rotary evaporator to completely remove the solvent mixture. 150 g of the solvent-free polymer was dissolved in 150 g of n-butyl acetate.

[0063] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PMMA): Mw = 14900 g / mol; Mn = 8610 g / mol; PDI = 1.7.

[0064] Copolymer I: A 500 mL four-neck flask equipped with a reflux condenser and N2 conduit, a dropping funnel, a KPG stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 29.9 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.8 g of APO (tert-amylperoxy-2-ethylhexanoate), 56.0 g of i-BMA, 67.1 g of MPEG500MA and 2.2 g of 2-mercaptoethanol was added dropwise over 4 hours, first at a rate of 1 drop per 4 seconds over 1.5 hours and then at a rate of 1 drop per 2 seconds over a further 2.5 hours, and the mixture was stirred at this temperature for a further 30 minutes. It was cooled to 80 ° C. and 0.14 g of APO dissolved in 10 g of n-butyl acetate was added for post-reaction. An additional 15 g of i-butyl acetate was added and this was stirred for an additional 30 minutes without heating.

[0065] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PMMA): Mw = 8474 g / mol; Mn = 2426 g / mol; PDI = 3.5.

[0066] Copolymer J: A 550 mL four-neck flask equipped with a reflux condenser and N2 conduit, a dropping funnel, a KPG stirrer (200 rpm) and a Pt100 digital internal thermometer was charged with 29.9 g of n-butyl acetate and the oil bath was heated to 145 ° C. A mixture of 9.8 g of APO (tert-amylperoxy-2-ethylhexanoate), 56.0 g of i-BMA, 67.1 g of MPEG500MA and 2.2 g of 2-mercaptoethanol was continuously added dropwise at a rate of 1 drop per 2 seconds over a period of 4 hours and the mixture was stirred at this temperature for another 30 minutes. It was cooled to 80 ° C and 0.14 g of APO dissolved in 10 g of n-butyl acetate was added for post-reaction. Another 15 g of i-butyl acetate was added and it was further stirred for 30 minutes without heating.

[0067] GPC according to DIN 55672-1:2016-03 (eluent: THF; standard: PMMA): Mw = 6181 g / mol; Mn = 2276 g / mol; PDI = 2.7.

[0068] Example 2: Preparation of phenolic foam For application technical comparison the formulations in Table 2 were selected.

[0069] [Table 2]

[0070] Comparative foaming was performed by hand mixing. For this, the phenolic resin (batch amount 180±5 g) and foam stabilizer were weighed into a beaker and mixed with a plate stirrer (diameter 6 cm) at 20° C. and 500 rpm for 30 seconds. The foaming agent was then added, mixed at 1500 rpm for 30 seconds and cooled to 18° C. The acid was then added and the mixture was stirred at 2000 rpm for 45 seconds and transferred to an aluminum mold with dimensions 25 cm×25 cm×7 cm, covered with a polyethylene film and thermostated at 60° C. After 1 hour, the foam was demolded and cured in an oven heated to 60° C. for 18 hours.

[0071] The pore structure was subjectively rated on a scale of 1 to 10, with 10 representing a very fine foam without any (ideal) disturbances and 1 representing an extremely disturbed and coarse foam. Thermal conductivity (λ value, in mW / m K) was measured on 2.5 cm thick panels at an average temperature of 10 °C using a Hesto Lambda Control instrument, type HLC X206, as specified in standard EN12667:2001. To determine the change in thermal conductivity over time, specimens were stored at 70 °C for 7 days and then measured again. Density was measured according to ASTM D1622-2020.

[0072] The foam stabilizer according to the invention was likewise tested with a polyether-modified siloxane as single component and in combination with an alkoxylated castor oil. In the comparative example, TEGOSTAB® B 84905 from Evonik Operations GmbH was used as the polyether-modified siloxane suitable for phenolic foams, and TAGAT® CH 40 from Evonik Operations GmbH was used as the ethoxylated castor oil.

[0073] The results are shown in Tables 3 and 4.

[0074] [Table 3]

[0075] These results show that copolymers A-F, I and J can achieve foam quality at the same level or slightly higher than polyether-modified siloxanes. Copolymers G and H showed slightly inferior foam quality compared to polyether-modified siloxanes. However, these are still at the level of conventional alkoxylated vegetable oils, and therefore it is also possible to produce usable foams without the use of polyether-modified siloxanes. All other foam properties relevant for use are not or only slightly affected by the copolymers according to the invention.

[0076] [Table 4]

[0077] These results show that all copolymers in combination with ethoxylated castor oil achieve foam quality at the same level or slightly higher than that of polyether modified siloxanes in combination with ethoxylated castor oil, all other use-relevant foam properties are not or only slightly affected by the copolymers according to the invention.

Claims

1. A composition for producing phenolic foam comprising at least one phenolic resin, at least one blowing agent and at least one catalyst, characterized in that the composition comprises at least one acrylate and / or methacrylate copolymer as a foam stabilizer.

2. The at least one acrylate and / or methacrylate copolymer is 2 C=CR 1 -COOR 2 and at least one comonomer of the type H 2 C=CR 1 -COOR 3 and at least one comonomer of the type: R 1 = each independently represents -H or -CH 3 and the substituents R 1 It is possible for different comonomers to be present in the copolymer, having the following structure: R 2 = each independently of the others, identical or different radicals from the group of saturated or unsaturated, linear, cyclic or branched, aliphatic or aromatic hydrocarbons having 1 to 25 carbon atoms, preferably methyl, ethyl, n-butyl, i-butyl, t-butyl, 2-ethylhexyl, isodecyl, cyclohexyl, benzyl, phenyl, isobornyl or allyl R 3 = each independently of the formula (1) [Formula 1] are identical or different polyether groups having a general average composition according to Where: x=1 to 500, preferably 1 to 250, in particular 3 to 80, R 4 = each independently of the other the same or different radicals -CH 2 -O-, -CH 2 -CH 2 -O-, -CH 2 -CH 2 -CH 2 -O-, -CH 2 -CH 2 -CH 2 -CH 2 -O- or -CH 2 -CH 2 -CH 2 -CH 2 -CH 2 -O-, and R 4 may be omitted, R 5 = each independently of the others identical or different alkyl groups having 1 to 18 carbon atoms, optionally having an ether function, or identical or different aryl groups having 6 to 18 carbon atoms, optionally having an ether function, or H, preferably H, methyl, ethyl or benzyl, with the radical R 3 Within each of the groups, different substituents R 5 may be present in any order or sequence, R 6 = each independently of the others identical or different alkyl groups having 1 to 18 carbon atoms, optionally having an ether function, or identical or different aryl groups having 6 to 18 carbon atoms, optionally having an ether function, or H, preferably H, methyl, ethyl or benzyl, with the radical R 3 Within each of the groups, different substituents R 6 may be present in any order or sequence, For the monomer repeat unit, preferably there are two groups R 5 and R 6 =H or two groups R 5 and R 6 one of which is H and the other is methyl; R 7 = each independently of the other: R 8 、 C(O)R 8 , -CH 2 -CH(OH)-CH 2 OH, and -CH 2 -C(CH 2 O.H. 2 -CH 2 -CH 3 are identical or different groups selected from the group consisting of: 7 It is possible for different comonomers to be present in the copolymer, having the following structure: R 8 = each independently of the other is the same or different alkyl group having 1 to 16 carbon atoms, the same or different aryl group having 6 to 16 carbon atoms, or H The composition according to claim 1 .

3. The at least one blowing agent is selected from the group consisting of: - hydrocarbons having 3, 4 or 5 carbon atoms, preferably cyclo-, iso- and / or n-pentane; And halogenated hydrocarbons having 3, 4 or 5 carbon atoms, preferably isopropyl chloride, hydrofluoroolefins and / or hydrohaloolefins, preferably 1234ze, 1234yf, 1224yd, 1233zd(E) and / or 1336mzz 3. The composition according to claim 1 or 2, characterized in that it is selected from the group consisting of:

4. 4. The composition according to claim 1 , wherein the at least one acrylate and / or methacrylate copolymer has a number-average molecular weight Mn in the range from 500 to 100,000 g / mol, particularly preferably from 1,000 to 40,000 g / mol, in particular from 1,000 to 25,000 g / mol, determined by gel permeation chromatography according to DIN 55672-1:2016-03 (eluent: THF; standard: PMMA).

5. 5. The composition according to claim 1, wherein the at least one acrylate and / or methacrylate copolymer is present in a total amount of 0.1 to 15 parts by weight, preferably 0.5 to 10 parts by weight, particularly preferably 0.5 to 8 parts by weight, based on 100 parts by weight of the total phenolic resins used.

6. 6. The composition according to claim 1, characterized in that the at least one Si-containing foam stabilizer is present in a total amount of advantageously less than 50 wt.-%, more preferably less than 25 wt.-%, even more preferably less than 10 wt.-%, based on the total amount of all foam stabilizers present.

7. The composition according to any one of claims 1 to 6, further comprising at least one silicon-free surfactant and / or silicon-free foam stabilizer, each of which is not an acrylate and / or methacrylate copolymer, in a total amount of 0.1 to 15 parts by weight, preferably 1 to 10 parts by weight, based on 100 parts by weight of the total phenolic resin used.

8. 8. The composition according to claim 1, further comprising at least one alkoxylated, preferably ethoxylated vegetable oil, in particular castor oil, in a total amount of 0.1 to 15 parts by weight, preferably 1 to 10 parts by weight, based on 100 parts by weight of the total phenolic resins used.

9. 9. The composition according to claim 1, characterized in that the at least one catalyst is selected from the group consisting of organic and inorganic acids, advantageously the at least one catalyst is selected from the group consisting of sulfuric acid, phosphoric acid, benzenesulfonic acid, xylenesulfonic acid, p-toluenesulfonic acid, ethylbenzenesulfonic acid, naphtholsulfonic acid, cumenesulfonic acid and phenolsulfonic acid.

10. 10. The composition according to claim 1, wherein the at least one catalyst is present in a total amount of 1 to 30 parts by weight, preferably 1 to 25 parts by weight, particularly preferably 3 to 20 parts by weight, based on 100 parts by weight of the total phenolic resin used.

11. 11. The composition according to claim 1, characterized in that the at least one acrylate and / or methacrylate copolymer is prepared using TBPEH (tert-butylperoxy-2-ethylhexanoate) and / or APO (tert-amylperoxy-2-ethylhexanoate) as initiator.

12. 12. The composition according to claim 1, characterized in that the residual monomer content is less than 1% by weight, based on the total acrylate and / or methacrylate copolymers contained.

13. A process for the preparation of phenolic foam, characterized in that it is carried out using a reaction mixture comprising a composition according to any one of claims 1 to 12.

14. A phenolic foam produced by the method of claim 13.

15. The phenol foam has a compressive strength of 5 to 500 kg / m according to ASTM D1622-2020. 3 , preferably 10 to 200 kg / m 3 , particularly preferably 12 to 100 kg / m 3 The phenolic foam of claim 14, characterized in that it has a density of

16. 16. Use of the phenolic foam according to claim 14 or 15 for thermal insulation.