Resin composition with high biomass level
A resin composition combining polyamide 11 with glass fiber and natural materials like eggshells or marble improves mechanical strength and maintains high biomass content, addressing the limitations of conventional polyamide 11 in pipe joints.
Patent Information
- Application Number
- JP2023088696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional polyamide 11 resin compositions used in pipe joints lack sufficient mechanical strength while maintaining a high biomass content.
A resin composition comprising polyamide 11 blended with glass fiber and natural materials like eggshells, seashells, calcite, or marble, which enhances mechanical strength without significantly reducing biomass content.
The composition achieves a high degree of biomass and excellent mechanical strength, suitable for applications requiring robustness.
Smart Images

Figure 2024171602000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition having a high biomass content. [Background technology]
[0002] 2. Description of the Related Art Pipe joints have been used to connect piping for water supply, hot water supply, or air conditioning equipment in a building.
[0003] Traditionally, resins such as polyamide resins have been used as materials for pipe joints, with polyamide 6 and polyamide 66 being widely used due to their advantageous performance and cost. However, in response to growing environmental awareness in recent years, there is also a growing need for polyamide resins made entirely or partially from biomass raw materials, such as polyamide 56, polyamide 510, polyamide 610, polyamide 1010, and polyamide 11. Of these, polyamide 11 has a high biomass content and is excellent in cold resistance, fatigue resistance, solvent resistance, etc., and is therefore used in engine components, etc.
[0004] Patent Document 1 describes a joint using a single raw material of polyamide 11. Patent Document 2 also describes polyamide 11 as a joint material, but does not specifically describe a joint using polyamide 11.
[0005] However, molded articles made using polyamide 11 as a single raw material generally have low mechanical strength and cannot function as molded articles that require mechanical strength, such as joints. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2001-50463 A (Examples 1, 3, 5 and 7) [Patent Document 2] JP 2005-193614 A (e.g., claim 24) Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a resin composition having a high biomass content and excellent mechanical strength. [Means for solving the problem]
[0008] In order to solve the above problems, the present inventors have investigated various materials that can improve the mechanical strength, which is a drawback of polyamide 11, and have found that blending glass fibers into polyamide 11 improves the mechanical strength, but is not sufficient, and also reduces the biomass ratio, making it impossible to obtain a product that has a satisfactory biomass ratio and excellent mechanical strength. Therefore, the present inventors have conducted extensive research to find a 100% natural material that can further improve the mechanical strength, and have found that the above problems can be solved by blending powders of natural materials such as eggshells, seashells, calcite, limestone, and marble, and have completed the present invention.
[0009] That is, the gist of the present invention is as follows. (1) A resin composition comprising 25 to 90 parts by mass of polyamide 11 (A), 1 to 65 parts by mass of glass fiber (B), and 1 to 65 parts by mass of powder of at least one natural material selected from eggshells, seashells, calcite, limestone, and marble (C) (the total amount of components (A), (B), and (C) is 100 parts by mass). (2) The resin composition according to (1) above, which is used for injection molding. (3) A molded article obtained by molding the resin composition described in (1) above. (4) The molded article according to (3) above, which is a pipe joint. Effect of the Invention
[0010] According to the present invention, it is possible to provide a resin composition having a high biomass content and excellent mechanical strength. [Brief description of the drawings]
[0011] [Figure 1]FIG. 1 is a diagram showing the structures of a pipe joint and a connecting jig used in the examples and comparative examples. [Diagram 2] FIG. 2 is a diagram showing the results of breaking torque measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The polyamide 11 used in the present invention is an aliphatic polyamide obtained by condensation polymerization of 11-aminoundecanoic acid, which is obtained solely from castor oil, a vegetable oil derived from biomass (biological resource), as a raw material.
[0013] The glass fibers used in the present invention have a fiber diameter of usually 0.01 to 20 μm, preferably 0.03 to 15 μm, and a fiber cut length of usually 0.5 to 10 mm, preferably 0.7 to 5 mm.
[0014] The powder of natural material used in the present invention may be a powder obtained by crushing eggshell, shell, calcite, limestone, or marble, and is generally called eggshell calcium, shell calcium (borei powder), etc. Two or more of these may also be used in combination. Such powder of natural material is generally available on the market, for example, under the trade name "Eggshell Calcium" (manufactured by Taiyo Kagaku), the trade name "Hisea-S" (calcined shell calcium), the trade name "Hisea 2200" (uncalcined shell calcium) (all manufactured by Kaiho Products), the trade name "Shell Powder 120" (manufactured by Furusato Bussan), the trade name "Caused Scallop Shell Powder" (manufactured by Takada Kagakuten), etc., and these commercially available products may be used in the present invention.
[0015] The resin composition of the present invention comprises 25 to 90 parts by mass of polyamide 11 (A), 1 to 65 parts by mass of glass fiber (B), and 1 to 65 parts by mass of powder (C) of at least one kind of natural material selected from eggshell, shell, calcite, limestone, and marble (the total amount of components (A), (B), and (C) is 100 parts by mass), and preferably comprises 35 to 90 parts by mass of polyamide 11 (A), 5 to 50 parts by mass of glass fiber (B), and 5 to 50 parts by mass of powder (C) of at least one kind of natural material selected from eggshell, shell, calcite, limestone, and marble (the total amount of components (A), (B), and (C) is 100 parts by mass), and further Most preferably, it contains 35 to 80 parts by mass of polyamide 11 (A), 10 to 35 parts by mass of glass fiber (B), and 5 to 35 parts by mass of powder (C) of at least one natural material selected from eggshell, shell, calcite, limestone, and marble (the total amount of components (A), (B), and (C) is 100 parts by mass), and particularly preferably, it contains 35 to 60 parts by mass of polyamide 11 (A), 10 to 35 parts by mass of glass fiber (B), and 25 to 35 parts by mass of powder (C) of at least one natural material selected from eggshell, shell, calcite, limestone, and marble (the total amount of components (A), (B), and (C) is 100 parts by mass). By blending components (A), (B), and (C) in the above ratio, a resin composition having a high biomass degree and excellent mechanical strength can be obtained.
[0016] If the proportion of polyamide 11 (A) is less than 25 parts by mass, injection molding becomes difficult, while if it exceeds 90 parts by mass, the mechanical strength decreases. If the proportion of glass fiber (B) is less than 1 part by mass, the mechanical strength decreases, while if it exceeds 65 parts by mass, the biomass degree decreases. If the proportion of natural material powder (C) is less than 1 part by mass, the mechanical strength and biomass degree decrease, while if it exceeds 65 parts by mass, the mechanical strength decreases.
[0017] In addition to the polyamide 11 (A), the glass fiber (B) and the powder of the natural material (C), other additives may be added to the resin composition of the present invention, provided that the effects of the present invention are not impaired. Such additives are not particularly limited, but include known additives used in the field of resin compositions, such as softeners, fillers, ultraviolet absorbers, antioxidants, heat stabilizers, light stabilizers, weather stabilizers, and antistatic agents.
[0018] In the resin composition of the present invention, the amount of additives other than polyamide 11 (A), glass fiber (B), and powder of the natural material (C) is not particularly limited as long as the effects of the present invention are achieved. However, the total amount of the other additives is usually 10 parts by mass or less, and preferably 3 parts by mass or less, per 100 parts by mass of the total amount of components (A), (B), and (C).
[0019] The resin composition of the present invention can be molded into a molded article by various known molding methods, specifically, various molding methods such as injection molding, extrusion molding, etc., and is particularly preferably molded by injection molding. Furthermore, the molded article such as a sheet obtained by the above molding method can be secondary processed by thermoforming, etc.
[0020] The molded article of the present invention is not particularly limited in its application, but is suitable for various well-known applications such as pipe joints, automobile parts, civil engineering and building materials, electrical and electronic parts, sanitary products, and films and sheets.
[0021] For example, when the molded article of the present invention is a pipe joint, it has a high biomass content and the fastening fracture strength of the fastened portion of the joint is excellent. EXAMPLES
[0022] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these.
[0023] (Examples 1-2 and Comparative Examples 1-2) (1) Materials used (A) Polyamide 11: Rilsan manufactured by Arkema TM BMNO LTD-PA11 was used. (B) Glass fiber and polyamide 11: glass fiber-containing polyamide 11 Rilsan manufactured by Arkema Co., Ltd. TM BZM30 OTL PA11-GF30 was used. (C) As a powder of natural material, fired scallop shell powder manufactured by Takada Chemical was used. The resin compositions shown in Table 1 were prepared by blending the above materials (A), (B) and (C).
[0024] (2) Molding The materials of Examples 1 and 2 and Comparative Examples 1 and 2 shown in Table 1 were dry-blended and dried in a dehumidifying dryer at 80° C. for 5 hours. Thereafter, a pipe joint mold was mounted on an injection molding machine (NEX80II from Nissei Plastic Industrial Co., Ltd.) and molding was performed to produce the pipe joint shown in FIG.
[0025] (3) Screw tightening breaking torque measurement test The threaded portion of the molded pipe fitting was wrapped with sealing tape three times and then hand-tightened to the connection jig shown in Figure 1. The jig with the molded pipe fitting attached was then fixed, and the threaded portion was tightened using a torque wrench to confirm the torque at which it broke. The results are shown in Table 1 and Figure 2. In Table 1 and Figure 2, Sample A shows the breaking torque of a two-part thread, and Sample B shows the breaking torque of a three-part thread.
[0026] [Table 1]
[0027] It can be seen from Table 1 and FIG. 2 that the molded bodies of Examples 1 and 2 have a high biomass content and are excellent in mechanical strength.
Claims
1. A resin composition comprising 25 to 90 parts by mass of polyamide 11 (A), 1 to 65 parts by mass of glass fiber (B), and 1 to 65 parts by mass of powder of at least one natural material selected from eggshells, seashells, calcite, limestone, and marble (C) (the total amount of components (A), (B), and (C) is 100 parts by mass).
2. The resin composition according to claim 1, which is used for injection molding.
3. A molded article obtained by molding the resin composition according to claim 1.
4. 4. The molded article according to claim 3, which is a pipe joint.
Citation Information
Patent Citations
Piping joint
JP2001050463A
Method for joining pipe-shaped article
JP2005193614A
Cited By
Polyarylene sulfide resin composition and molded article made therefrom
JP2026165606A