Electrode Catalyst

By optimizing the microstructure and composition of tin oxide-based particles with mesopores, the electrode catalyst supports Pt-based fine particles, addressing the trade-off issues and achieving high ORR mass activity and reduced ionomer poisoning.

JP7573942B2Active Publication Date: 2024-10-28KK TOYOTA CHUO KENKYUSHO +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021063422
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-02
Publication Date
2024-10-28
Estimated Expiration
2041-04-02

AI Technical Summary

Technical Problem

Existing electrode catalysts for polymer electrolyte fuel cells face challenges in achieving both high specific surface area and high oxygen reduction reaction (ORR) mass activity due to the trade-off between surface area and electrical conductivity when using tin oxide-based carriers, leading to decreased performance and catalyst degradation.

Method used

The electrode catalyst supports Pt-based fine particles on tin oxide-based particles with optimized microstructure and composition, including mesopores and specific surface area, to enhance ORR mass activity.

Benefits of technology

This configuration achieves high ORR mass activity of 150A/g at 0.9V and 650A/g at 0.85V, with reduced ionomer poisoning and improved catalyst performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573942000004
    Figure 0007573942000004
  • Figure 0007573942000005
    Figure 0007573942000005
  • Figure 0007573942000006
    Figure 0007573942000006
Patent Text Reader

Abstract

To provide a novel electrode catalyst including tin oxide-based particles with Pt-based fine particles supported on its surface.SOLUTION: An electrode catalyst comprises tin oxide-based particles of 30 m2 / g or more in a specific surface area, and Pt-based fine particles supported on the tin oxide-based particles. The electrode catalyst is 150 A / gPt or more in oxygen reductive reaction mass activity at 0.9 V, and / or 650 A / gPt or more in oxygen reductive reaction mass activity at 0.85 V. The tin oxide-based particles preferably have pores of 50 nm or smaller in a pore size. The tin oxide-based particles are preferably made of SnO2 doped with Sb, Nb, Ta and / or W.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode catalyst, and more specifically to an electrode catalyst in which Pt-based fine particles are supported on the surfaces of tin oxide-based particles. [Background technology]

[0002] A polymer electrolyte fuel cell (PEFC) comprises a membrane electrode assembly (MEA) in which catalyst layers are bonded to both sides of an electrolyte membrane. A gas diffusion layer is usually arranged on the outside of the catalyst layer. Furthermore, a current collector (separator) with a gas flow path is arranged on the outside of the gas diffusion layer. A PEFC usually comprises a structure (fuel cell stack) in which a plurality of unit cells each consisting of such an MEA, gas diffusion layer, and current collector are stacked.

[0003] In PEFCs, the catalyst layer generally consists of a mixture of an electrode catalyst in which catalytic metal particles such as platinum are supported on the surface of a support, and a catalyst layer ionomer. Carbon materials such as carbon black and acetylene black are usually used for the catalyst support. However, it is known that carbon supports are oxidized and corroded when exposed to a high potential, causing the catalytic metal particles supported on the support to fall off, which in turn reduces the electrode performance. For this reason, it has been proposed to use conductive metal oxides, which are stable at high potentials, as support materials.

[0004] For example, Non-Patent Document 1 states: (a) Among various conductive metal oxides, nonstoichiometric titanium oxide (TiO x ) or tin oxide doped with other elements (Nb, Sb, etc.) is promising as a catalyst support, and (b) In particular, tin oxide, which is stable in a highly acidic and high-potential environment, is promising as a catalyst support for the cathode of PEFC. is stated.

[0005] Non-Patent Document 2 states: (a) Sn 0.96 Nb 0.04 O2-δ The catalyst was made of Pt supported on a support (the BET specific surface area of ​​the support is 37 m 2 / g, Pt loading is 10.0 wt%), and (b) Sn 0.96 Sb 0.04 O 2-δ The catalyst was made of Pt supported on a support (the BET specific surface area of ​​the support is 33 m 2 / g, Pt loading is 12.3 wt%) has been disclosed. The literature also reports that the oxygen reduction reaction (ORR) mass activity of these catalysts at 0.85 V is 515-608 A / g PT It is stated that:

[0006] Non-Patent Document 3 discloses a catalyst in which Pt is supported on a support made of Sb-SnO2 xerogel. The same paper states that the ORR mass activity of this catalyst at 0.9 V is 92 A / g Pt It is stated that:

[0007] Non-Patent Document 4 discloses a catalyst in which Pt is supported on a support made of Sb-SnO2 xerogel. The same paper states that the ORR mass activity of this catalyst at 0.9 V is 32 A / g Pt It is stated that:

[0008] Non-Patent Document 5 discloses a catalyst in which Pt is supported on a support made of Nb-SnO2, and this is further supported on carbon (VGCF). The same paper also reports that the ORR mass activity of this catalyst at 0.9 V is 141 A / g Pt and the ORR mass activity at 0.85 V is 541 A / g Pt It is stated that:

[0009] Furthermore, Non-Patent Document 6 describes a support made of Ta-SnO2 nanofibers (the BET specific surface area of ​​the support is 27 m 2 A catalyst in which Pt is supported on a Cr-Al-Fe-O-Pt alloy (CuO / g) is disclosed. The same literature states that the ORR mass activity of this catalyst at 0.9 V is 307 to 465 A / g Pt It is stated that:

[0010] PEFC cathode electrode catalysts are required to have high ORR activity. In addition, it is better for the loading rate of Pt, which is the active species, to be high. This is because when a catalyst layer is made with a catalyst with a low Pt loading rate, the thickness of the catalyst layer is thicker than when a catalyst layer with the same Pt ​​weight (Pt amount per electrode area) is made with a catalyst with a high Pt loading rate, which is disadvantageous in terms of electronic resistance, proton transfer resistance, and gas diffusion resistance within the catalyst layer.

[0011] In order to increase the Pt loading rate, it is necessary to increase the surface area of ​​the support. If Pt is loaded at a high loading rate on the surface of a support with a small specific surface area, the Pt fine particles will aggregate on the support, or Pt will be loaded as coarse particles. As a result, the specific surface area of ​​Pt will decrease, and the ORR mass activity will decrease.

[0012] However, in the case of oxide supports such as tin oxide supports, there is a trade-off between the specific surface area and electrical conductivity. Generally, to increase the specific surface area, it is necessary to reduce the particle size of the oxide support particles. However, as the particle size decreases, the number of contact points between the particles increases, increasing the total contact resistance and decreasing the electrical conductivity of the compact. If the electrical conductivity of the support is low, the utilization rate of the supported Pt decreases, or the ORR activity (specific activity) per surface area of ​​Pt decreases, resulting in a decrease in the ORR mass activity.

[0013] Among the Pt / M-SnO2 described in the above Non-Patent Documents 1 to 6, the Pt / Ta-SnO2 nanofiber described in Non-Patent Document 6 has been reported to have the highest ORR mass activity. However, this Ta-SnO2 nanofiber support has a specific surface area of ​​27 m 2 / g, increasing the Pt loading rate from 7 mass% to 34 mass% reduces the electrochemical specific surface area (ECSA) of Pt to 73 m 2 / g Pt 48m from 2 / g Ptand the ORR mass activity at 0.9 V was 465 A / g Pt to 307A / g Pt It decreases to.

[0014] On the other hand, the Sb-SnO2 aerogel support in Non-Patent Document 4 has a specific surface area of ​​85 m 2 / g, but the ORR specific activity and mass activity at 0.9 V are 100 μA / cm 2 Pt , and 32A / g Pt is low. Thus, there have been no previously reported Pt / M-SnO2 catalysts that have both a high specific surface area and high ORR mass activity. [Prior art documents] [Non-patent literature]

[0015] [Non-Patent Document 1] T. Arai et al., SAE Int. J. Alt. Power., 2017, 6, 145 [Non-Patent Document 2] K. Kakinuma et al., Electrochim. Acta, 2013, 110, 316 [Non-Patent Document 3] VK Ramani, DOE 2020 Annual Merit Review, #FC145 [Non-Patent Document 4] G. Ozouf et al., J. Electrochem. Soc., 2018, 165, F3036 [Non-Patent Document 5] S. Matsumoto et al., J. Electrochem. Soc., 2018, 165, F1164 [Non-Patent Document 6] I. Jimenez-Morales et al., ACS Catal., 2020, 10, 10399 Summary of the Invention [Problem to be solved by the invention]

[0016] An object of the present invention is to provide a novel electrode catalyst in which Pt-based fine particles are supported on the surfaces of tin oxide-based particles. Another problem to be solved by the present invention is to achieve both a large specific surface area and high ORR mass activity in an electrode catalyst in which Pt-based fine particles are supported on the surfaces of tin oxide-based particles. [Means for solving the problem]

[0017] In order to solve the above problems, the electrode catalyst according to the present invention has the following configuration. (1) The electrode catalyst is Specific surface area is 30m 2 / g or more, and Pt-based fine particles supported on the tin oxide-based particles; It is equipped with: (2) The electrode catalyst is Oxygen reduction reaction mass activity at 0.9V is 150A / g Pt or more; and / or Oxygen reduction reaction mass activity at 0.85V is 650A / g Pt That's all. Effect of the Invention

[0018] In an electrocatalyst in which Pt-based particles are supported on the surface of tin oxide-based particles, by optimizing the microstructure and / or composition of the tin oxide-based particles, it is possible to achieve both a high specific surface area and high ORR mass activity. In particular, when the tin oxide-based particles have mesopores, they exhibit high ORR mass activity despite their high specific surface area. This is believed to be because ionomer poisoning is reduced by supporting Pt-based particles in the mesopores. [Brief description of the drawings]

[0019] [Figure 1] 1 is a SEM image (backscattered electron image) of Pt / Sb—SnO 2 obtained in Example 1 (ALD method). [Diagram 2] 1 is a SEM image (backscattered electron image) of Pt / Sb—SnO 2 obtained in Example 2 (colloid method). [Diagram 3] 1 shows XRD patterns of Pt / Sb—SnO2 obtained in Example 1 (ALD method) and Example 3 (colloid method). [Figure 4] 1 shows cyclic voltammograms of Pt / Sb-SnO2 obtained in Examples 2 and 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] An embodiment of the present invention will be described in detail below. [1. Electrocatalyst] The electrode catalyst according to the present invention is Specific surface area is 30m 2 / g or more, and Pt-based fine particles supported on the tin oxide-based particles; It is equipped with:

[0021] [1.1. Tin oxide particles] [1.1.1. Composition] "Tin oxide based particles" refers to particles made of SnO2 or particles made of SnO2 containing a dopant. In the present invention, the type of dopant is not particularly limited. Examples of dopants include Nb, Sb, W, Ta, and Al. SnO2 may contain any one of these dopants, or may contain two or more of them.

[0022] Among these, the tin oxide particles are preferably SnO2 doped with Sb, Nb, Ta, and / or W. In particular, the tin oxide particles are preferably SnO2 doped with Sb. SnO2 doped with Sb has a higher electrical conductivity than SnO2 containing other dopants, and is therefore suitable as a catalyst support for supporting Pt-based fine particles.

[0023] In SnO2 doped with Sb, the more the doping amount of Sb, the higher the electrical conductivity. To obtain such an effect, the doping amount of Sb is preferably 2.5 at% or more. The doping amount of Sb is more preferably 5.0 at% or more. On the other hand, if the doping amount of Sb is excessive, the carrier concentration becomes excessive and the electrical conductivity may decrease. Therefore, the doping amount of Sb is preferably 15.0 at% or less. The doping amount of Sb is more preferably 10.0 at% or less.

[0024] [1.1.2. Specific surface area] In general, the larger the specific surface area of ​​the tin oxide particles, the more highly dispersed the Pt-based particles can be supported, and the higher the ORR mass activity. Therefore, the larger the specific surface area of ​​the tin oxide particles, the better. To obtain high ORR mass activity, the specific surface area of ​​the tin oxide particles should be 30 m 2 The specific surface area should be at least 50 m 2 / g or more, more preferably 100m 2 / g or more.

[0025] [1.1.3. Pore diameter] The tin oxide based particles preferably have pores therein with a pore size of 50 nm or less (hereinafter also referred to as "mesopores"). Here, "mesopores" generally refer to pores having a diameter of 2 nm or more and 50 nm or less. However, in the present invention, unless otherwise specified, "mesopores" includes pores having a diameter of less than 2 nm (so-called "micropores") in addition to pores having a diameter of 2 nm or more and 50 nm or less. "Pore size" refers to the average diameter of the mesopores. The pore diameter can be obtained by analyzing the adsorption side data of the nitrogen adsorption isotherm of the tin oxide particles by the BJH method and determining the pore diameter at which the pore volume is maximum (the most frequent peak value or the mode pore diameter).

[0026] In the case where the tin oxide-based particles have mesopores, when the tin oxide-based particles are supported with Pt-based fine particles, the proportion of the Pt-based fine particles present in the mesopores increases. Therefore, when the Pt-based fine particles are supported in the mesopores of the tin oxide-based particles to form an electrode catalyst, and a catalyst layer is produced using such an electrode catalyst and an ionomer, it is possible to suppress the poisoning of the Pt-based fine particles by the ionomer and the resulting performance degradation.

[0027] When the tin oxide particles have mesopores, the pore diameter (size of the mesopores) affects the performance of the electrode catalyst. In general, if the pore diameter is too small, it becomes difficult to support Pt-based fine particles in the mesopores. As a result, when a catalyst layer is produced using the electrode catalyst according to the present invention and an ionomer, the Pt-based fine particles may be poisoned by the ionomer. Therefore, the pore diameter is preferably 1 nm or more. The pore diameter is more preferably 2 nm or more. On the other hand, if the pore diameter is too large, the ionomer may enter the mesopores and the Pt-based fine particles supported in the mesopores may be poisoned by the ionomer. Therefore, the pore diameter is preferably 20 nm or less. The pore diameter is more preferably 10 nm or less, and even more preferably 5 nm or less.

[0028] [1.1.4. Shape] In the present invention, the shape of the tin oxide based particles is not particularly limited as long as the above-mentioned conditions are satisfied. The tin oxide based particles may be isolated particles or may be particles having a beaded structure in which porous primary particles are fused together. Here, the term "beaded structure" refers to a structure in which primary particles are fused together in a beaded shape.

[0029] By using the method described below, tin oxide particles having a beaded structure in which porous primary particles are fused together can be obtained. In particles having a beaded structure (i.e., secondary particles), the primary particles are loosely connected to each other, so there are relatively large voids between the primary particles. Therefore, when an electrode catalyst is produced using tin oxide particles having a beaded structure and a catalyst layer is produced using this and an ionomer, appropriate voids are formed in the catalyst layer. As a result, the gas diffusion resistance of the catalyst layer is reduced. In addition, because the primary particles are made up of an aggregate of minute crystallites, there are relatively minute voids (mesopores) inside the primary particles, and therefore, when these are used as catalyst supports, it is possible to suppress the poisoning of Pt-based fine particles by the ionomer.

[0030] The shape of the primary particles is not particularly limited. When tin oxide-based particles are produced using the method described below, the primary particles are usually not perfectly spherical, but have an irregular shape with an aspect ratio of about 1.1 to 3.

[0031] As described below, the tin oxide-based particles according to the present invention are produced using mesoporous carbon as a template. Also, the mesoporous carbon is produced using mesoporous silica as a template. Mesoporous silica is usually synthesized by condensation polymerization of a silica source in a reaction solution containing a silica source, a surfactant, and a catalyst.

[0032] In this case, by limiting the concentration of the surfactant and the concentration of the silica source in the reaction solution to specific ranges, respectively, it is possible to obtain mesoporous silica having a beaded structure and having a specific range of specific surface area, pore size, etc. When such mesoporous silica having a beaded structure is used as a first template, mesoporous carbon having a beaded structure can be obtained.Furthermore, when mesoporous carbon having a beaded structure is used as a second template, tin oxide particles having a beaded structure can be obtained.

[0033] [1.1.5. Average particle size of primary particles] The term "average particle size of primary particles" refers to the average value of the maximum dimension of primary particles measured by observation with a scanning electron microscope (SEM). When the tin oxide-based particles are particles having a beaded structure in which porous primary particles are fused together, the average particle size of the primary particles is not particularly limited, and an optimal value can be selected depending on the purpose.

[0034] Generally, if the average particle size of the primary particles is too small, it becomes difficult to support Pt-based fine particles. Therefore, the average particle size of the primary particles is preferably 0.05 μm or more. The average particle size is more preferably 0.06 μm or more, and even more preferably 0.07 μm or more. On the other hand, if the average particle size of the primary particles is too large, the thickness of the catalyst layer becomes thick, and the ionic resistance and electronic resistance in the catalyst layer become large. Therefore, the average particle size of the primary particles is preferably 2 μm or less. The average particle size is more preferably 1 μm or less, and even more preferably 0.5 μm or less.

[0035] 1.1.6. Electrical conductivity of powder compacts "Conductivity of green compact" means (a) Tin oxide particles are molded using two stainless steel disks and a plastic jig with a cylindrical hole. (b) The value obtained by applying a pressure of 2.4 MPa to the obtained green compact while passing a constant current through it and measuring the voltage. The electrical conductivity of the compact (i.e., tin oxide-based particles) depends mainly on the type and amount of dopant. When the composition of the tin oxide-based particles is optimized, the electrical conductivity of the compact is 1×10 -3 When the manufacturing conditions are optimized, the conductivity is 1×10 -2 S / cm or more. By using the method described below, it is possible to synthesize tin oxide particles even when the powder compact has an electrical conductivity of about 10 S / cm.

[0036] 1.1.7. Pore volume "Pore volume" refers to the volume of the mesopores contained in the primary particles, and does not include the volume of the voids between the primary particles. The pore volume can be obtained by analyzing the adsorption data of the nitrogen adsorption isotherm of the tin oxide particles by the BJH method and calculating the value of P / P0 = 0.03 to 0.99.

[0037] When the tin oxide particles according to the present invention are used as a catalyst carrier for PEFC, if the pore volume is too small, the ratio of catalyst particles supported in the pores will be small. Therefore, the pore volume is preferably 0.1 mL / g or more. The pore volume is preferably 0.15 mL / g or more, and more preferably 0.2 mL / g or more. On the other hand, if the pore volume is too large, the ratio of the pore walls of the tin oxide particles will be small, and the electronic conductivity will be low. Also, the amount of ionomer penetration will be large, and the activity may decrease due to catalyst poisoning. Therefore, the pore volume is preferably 1 mL / g or less. The pore volume is preferably 0.7 mL / g or less, and more preferably 0.5 mL / g or less.

[0038] [1.1.8. Tap density] "Tap density" refers to a value measured in accordance with JIS Z 2512. When the tin oxide-based particles according to the present invention are used in the catalyst layer of a PEFC, if the tap density of the tin oxide-based particles is too small, the thickness of the resulting catalyst layer becomes too large, and the proton conductivity decreases. Therefore, the tap density is preferably 0.005 g / cm 3 The tap density is preferably 0.01 g / cm or more. 3 More preferably, 0.05 g / cm 3 That's all. On the other hand, if the tap density is too high, when a catalyst layer is produced using this, it becomes difficult to secure voids in the catalyst layer that are capable of suppressing flooding. Therefore, the tap density is set to 1.0 g / cm 3 The tap density is preferably 0.75 g / cm 3 The following is the result.

[0039] [1.2. Pt-based fine particles] [1.2.1. Composition] "Pt-based fine particles" refers to fine particles made of Pt or a Pt alloy. The Pt-based fine particles are supported on the outer surface of the tin oxide-based particles or on the inner surface of the mesopores. When the Pt-based fine particles are made of a Pt alloy, the composition of the Pt alloy (i.e., the type and content of alloying elements) is not particularly limited, and an optimal composition can be selected depending on the purpose. (a) Alloys containing Pt and one or more precious metal elements other than Pt (e.g., Pt-Pd alloys, Pt-Ru alloys, Pt-Ir alloys, etc.); (b) Alloys containing Pt and one or more base metal elements (e.g., Fe, Co, Ni, Cr, V, Ti, etc.) (e.g., Pt-Fe alloys, Pt-Co alloys, Pt-Ni alloys, Pt-Cr alloys, Pt-V alloys, Pt-Ti alloys, etc.); etc.

[0040] [1.2.2. Average particle size] The term "average particle size of Pt-based fine particles" refers to the average value of the maximum dimension of Pt-based fine particles measured by observation with a scanning electron microscope (SEM). The average particle size of the Pt-based particles affects the mass activity. In general, if the average particle size of the Pt-based particles becomes too large, the mass activity of the Pt-based particles decreases. Therefore, the average particle size of the Pt-based particles is preferably 5 nm or less. The average particle size is more preferably 4 nm or less. On the other hand, if the average particle size of the Pt-based fine particles is too small, the components constituting the fine particles such as Pt are likely to dissolve. Therefore, the average particle size of the Pt-based fine particles is preferably 1 nm or more. The average particle size is more preferably 2 nm or more.

[0041] 1.2.3. Loading amount The amount of Pt-based fine particles supported is not particularly limited, and an optimal amount can be selected depending on the purpose. In general, if the amount of Pt-based fine particles supported is too small, the thickness of the catalyst layer required to obtain a predetermined basis weight becomes large, and the electronic resistance, proton transfer resistance, and / or gas diffusion resistance of the catalyst layer increase. Therefore, the amount of Pt-based fine particles supported is preferably 5 mass% or more. The amount is more preferably 10 mass% or more, and even more preferably 15 mass% or more. On the other hand, if the amount of Pt-based fine particles supported is excessive, the Pt-based fine particles will aggregate on the support surface, and the activity of the electrode catalyst will decrease. Therefore, the amount of Pt-based fine particles supported is preferably 60 mass% or less. The amount is more preferably 50 mass% or less, and even more preferably 40 mass% or less.

[0042] [1.3. Characteristics] [1.3.1. Oxygen reduction reaction (ORR) mass activity at 0.9 V] In the electrocatalyst according to the present invention, when the composition and / or structure (particularly the composition and / or structure of the tin oxide-based particles) are optimized, the ORR mass activity at 0.9 V is 150 A / g Pt By further optimizing the composition and / or structure of the electrocatalyst, the ORR mass activity at 0.9 V can be increased to 300 A / g Pt or more than 400A / g Pt That's all.

[0043] [1.3.2. Oxygen reduction reaction (ORR) mass activity at 0.85 V] In the electrocatalyst according to the present invention, by optimizing the composition and / or structure (particularly the composition and / or structure of the tin oxide-based particles), in addition to or instead of the ORR mass activity at 0.9 V falling within the above range, the ORR mass activity at 0.85 V can be increased to 650 A / g Pt By further optimizing the composition and / or structure of the electrocatalyst, the ORR mass activity at 0.85 V can be increased to 1500 A / g Pt or more than 2000A / g Pt That's all.

[0044] [2. Manufacturing method of mesoporous silica (first mold)] Tin oxide particles can be produced by various methods. Among these, in order to produce tin oxide particles having a beaded structure, it is first necessary to produce mesoporous silica (first template) having a beaded structure. Such mesoporous silica can be produced by: (a) preparing precursor particles by condensation polymerization of the silica source in a reaction solution containing a silica source, a surfactant, and a catalyst; (b) separating the precursor particles from the reaction solution and drying; (c) optionally subjecting the dried precursor particles to a diameter enlarging treatment; (d) Calcining the precursor particles This is obtained by:

[0045] [2.1. Polycondensation process] First, in a reaction solution containing a silica source, a surfactant, and a catalyst, the silica source is condensation-polymerized to obtain precursor particles (condensation polymerization step).

[0046] 2.1.1. Silica source In the present invention, the type of silica source is not particularly limited. Examples of the silica source include (a) tetraalkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetraisopropoxysilane, tetrabutoxysilane, dimethoxydiethoxysilane, and tetraethyleneglycoxysilane; (b) trialkoxysilanes such as 3-mercaptopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-(2-aminoethyl)aminopropyltrimethoxysilane; As the silica source, any one of these may be used alone or two or more of them may be used in combination.

[0047] [2.1.2. Surfactants] When a silica source is polycondensed in a reaction solution, the surfactant forms micelles in the reaction solution. Hydrophilic groups are gathered around the micelles, so the silica source is adsorbed to the surface of the micelles. Furthermore, the micelles to which the silica source is adsorbed self-organize in the reaction solution, and the silica source is polycondensed. As a result, mesopores due to the micelles are formed inside the primary particles. The size of the mesopores can be controlled (1 to 50 nm) mainly by the molecular length of the surfactant.

[0048] In the present invention, an alkyl quaternary ammonium salt is used as the surfactant. The alkyl quaternary ammonium salt refers to a compound represented by the following formula (a). CH3-(CH2) n -N + (R1)(R2)(R3)X - (a)

[0049] In formula (a), R1, R2, and R3 each represent an alkyl group having 1 to 3 carbon atoms. R1, R2, and R3 may be the same or different. In order to facilitate aggregation (micelle formation) of alkyl quaternary ammonium salts, it is preferable that R1, R2, and R3 are all the same. Furthermore, it is preferable that at least one of R1, R2, and R3 is a methyl group, and it is preferable that all of them are methyl groups. In formula (a), X represents a halogen atom. The type of halogen atom is not particularly limited, but X is preferably Cl or Br in view of availability.

[0050] In formula (a), n represents an integer of 7 to 21. In general, the smaller n is, the smaller the central pore diameter of the mesopores is, resulting in a spherical mesoporous body. On the other hand, the larger n is, the larger the central pore diameter is, but if n is too large, the hydrophobic interaction of the alkyl quaternary ammonium salt becomes excessive. As a result, a layered compound is formed, and a mesoporous body cannot be obtained. n is preferably 9 to 17, more preferably 13 to 17.

[0051] Among those represented by formula (a), alkyltrimethylammonium halides are preferred. Examples of alkyltrimethylammonium halides include hexadecyltrimethylammonium halide, octadecyltrimethylammonium halide, nonyltrimethylammonium halide, decyltrimethylammonium halide, undecyltrimethylammonium halide, and dodecyltrimethylammonium halide. Among these, alkyltrimethylammonium bromide or alkyltrimethylammonium chloride is particularly preferred.

[0052] In the case of synthesizing mesoporous silica, one kind of alkyl quaternary ammonium salt may be used, or two or more kinds may be used. However, since the alkyl quaternary ammonium salt serves as a template for forming mesopores in the primary particles, the type of alkyl quaternary ammonium salt has a large effect on the shape of the mesopores. In order to synthesize silica particles with more uniform mesopores, it is preferable to use one kind of alkyl quaternary ammonium salt.

[0053] 2.1.3. Catalyst When the silica source is polycondensed, a catalyst is usually added to the reaction solution. When synthesizing particulate mesoporous silica, it is preferable to use an alkali such as sodium hydroxide or aqueous ammonia as the catalyst.

[0054] 2.1.4. Solvents The solvent used may be water, an organic solvent such as alcohol, or a mixed solvent of water and an organic solvent. Alcohol is (1) Monohydric alcohols such as methanol, ethanol, and propanol, (2) Dihydric alcohols such as ethylene glycol, (3) Trihydric alcohols such as glycerin, Either is fine. When a mixed solvent of water and an organic solvent is used, the content of the organic solvent in the mixed solvent can be selected arbitrarily depending on the purpose. In general, adding an appropriate amount of an organic solvent to the solvent makes it easier to control the particle size and particle size distribution.

[0055] [2.1.5. Composition of reaction solution] The composition of the reaction solution affects the external shape and pore structure of the synthesized mesoporous silica. In particular, the concentrations of the surfactant and silica source in the reaction solution have a large effect on the average primary particle size, pore size, pore volume, and tap density of the mesoporous silica particles.

[0056] [A. Surfactant concentration] If the concentration of the surfactant is too low, the particle precipitation speed is slowed down, and a structure in which the primary particles are connected cannot be obtained. Therefore, the concentration of the surfactant must be 0.03 mol / L or more. The concentration of the surfactant is preferably 0.035 mol / L or more, more preferably 0.04 mol / L or more.

[0057] On the other hand, if the concentration of the surfactant is too high, the particle precipitation speed becomes too fast, and the primary particle size easily exceeds 300 nm. Therefore, the concentration of the surfactant must be 1.0 mol / L or less. The concentration of the surfactant is preferably 0.95 mol / L or less, more preferably 0.90 mol / L or less.

[0058] [B. Concentration of Silica Source] If the concentration of the silica source is too low, the particle precipitation rate will be slow, and a structure in which primary particles are connected will not be obtained. Alternatively, the surfactant will be excessive, and uniform mesopores may not be obtained. Therefore, the concentration of the silica source must be 0.05 mol / L or more. The concentration of the silica source is preferably 0.06 mol / L or more, and more preferably 0.07 mol / L or more.

[0059] On the other hand, if the concentration of the silica source is too high, the particle precipitation speed becomes too fast, and the primary particle size easily exceeds 300 nm. Alternatively, sheet-like particles may be obtained instead of spherical particles. Therefore, the concentration of the silica source must be 1.0 mol / L or less. The concentration of the silica source is preferably 0.95 mol / L or less, more preferably 0.9 mol / L or less.

[0060] [C. Catalyst Concentration] In the present invention, the catalyst concentration is not particularly limited. In general, if the catalyst concentration is too low, the particle precipitation speed becomes slow. On the other hand, if the catalyst concentration is too high, the particle precipitation speed becomes fast. It is preferable to select the optimum catalyst concentration according to the type of silica source, the type of surfactant, the target physical property value, etc.

[0061] [2.1.6 Reaction conditions] A silica source is added to a solvent containing a predetermined amount of a surfactant, and hydrolysis and polycondensation are carried out, whereby precursor particles containing silica and the surfactant are obtained with the surfactant acting as a template. The optimum reaction conditions are selected depending on the type of silica source, the particle size of the precursor particles, etc. In general, the reaction temperature is preferably −20 to 100° C. The reaction temperature is more preferably 0 to 90° C., and further preferably 10 to 80° C.

[0062] [2.2. Drying process] Next, the precursor particles are separated from the reaction solution and dried (drying step). Drying is carried out in order to remove the solvent remaining in the precursor particles. The drying conditions are not particularly limited as long as the solvent can be removed.

[0063] [2.3. Expansion process] Next, if necessary, the dried precursor particles may be subjected to a diameter expansion treatment (diameter expansion step). The "diameter expansion treatment" refers to a treatment for expanding the diameter of mesopores in the primary particles. Specifically, the diameter-enlarging treatment is carried out by subjecting the synthesized precursor particles (from which the surfactant has not been removed) to a hydrothermal treatment in a solution containing a diameter-enlarging agent, which can enlarge the pore size of the precursor particles.

[0064] Examples of the diameter expanding agent include: (a) Hydrocarbons such as trimethylbenzene, triethylbenzene, benzene, cyclohexane, triisopropylbenzene, naphthalene, hexane, heptane, octane, nonane, decane, undecane, and dodecane; (b) Acids such as hydrochloric acid, sulfuric acid, and nitric acid, etc.

[0065] The reason why the pore size increases by hydrothermal treatment in the presence of a hydrocarbon is believed to be that rearrangement of silica occurs when the diameter-expanding agent is introduced from the solvent into the pores of the more hydrophobic precursor particles. In addition, the pore size increases when hydrothermal treatment is performed in the presence of an acid such as hydrochloric acid. This is thought to be due to the dissolution and reprecipitation of silica inside the primary particles. When the manufacturing conditions are optimized, radial pores are formed inside the silica. When this is hydrothermal treated in the presence of an acid, silica dissolves and reprecipitation occurs, and the radial pores are converted into interconnected pores.

[0066] The conditions for the diameter-enlarging treatment are not particularly limited as long as the desired pore diameter can be obtained. Usually, it is preferable to add about 0.05 mol / L to 10 mol / L of a diameter-enlarging agent to the reaction solution and perform hydrothermal treatment at 60 to 150°C.

[0067] [2.4. Firing process] Next, after carrying out a diameter expansion treatment as necessary, the precursor particles are calcined (calcination step), thereby obtaining mesoporous silica particles having a beaded structure. The calcination is carried out in order to dehydrate and crystallize the precursor particles with residual OH groups, and to thermally decompose the surfactant remaining in the mesopores. The calcination conditions are not particularly limited as long as they allow dehydration, crystallization, and thermal decomposition of the surfactant. The calcination is usually carried out by heating in the air at 400°C to 700°C for 1 hour to 10 hours.

[0068] [3. Manufacturing method of mesoporous carbon (second mold)] Next, the mesoporous silica having a beaded structure is used as a template to produce mesoporous carbon having a beaded structure (second template). Such mesoporous carbon is (a) preparing mesoporous silica as a first template; (b) depositing carbon in the mesopores of the mesoporous silica to produce a silica / carbon composite; (c) removing silica from the composite. This is obtained by: In order to promote graphitization of the obtained mesoporous carbon, the mesoporous carbon may be heat-treated at a temperature higher than 1500° C. after removing the silica.

[0069] [3.1. First mold preparation process] First, mesoporous silica that will become the first template is prepared (first template preparation step). Details of the method for producing mesoporous silica are as described above, and therefore will not be described here.

[0070] [3.2. Carbon deposition process] Next, carbon is precipitated in the mesopores of the mesoporous silica to produce a silica / carbon composite (carbon precipitation step). Specifically, the deposition of carbon into mesopores is as follows: (a) introducing a carbon precursor into the mesopores; (b) Polymerizing and carbonizing the carbon precursor within the mesopores This is done by:

[0071] [3.2.1. Introduction of carbon precursor] The term "carbon precursor" refers to a material capable of producing carbon by pyrolysis. Specific examples of such carbon precursors include: (1) A polymer precursor that is liquid at room temperature and is thermally polymerizable (e.g., furfuryl alcohol, aniline, etc.), (2) A mixture of aqueous carbohydrate solutions and acids (e.g., mixtures of monosaccharides such as sucrose, xylose, glucose, etc., or disaccharides or polysaccharides with acids such as sulfuric acid, hydrochloric acid, nitric acid, or phosphoric acid), (3) A mixture of two-component curing polymer precursors (e.g., phenol and formalin, etc.), etc. Among these, polymer precursors can be impregnated into the mesopores without diluting them with a solvent, so that a relatively large amount of carbon can be produced in the mesopores with a relatively small number of impregnations. In addition, they have the advantage that they do not require a polymerization initiator and are easy to handle.

[0072] When a liquid or solution carbon precursor is used, the amount of liquid or solution adsorbed per one time is preferably as large as possible, and is preferably such an amount that the entire mesopores are filled with the liquid or solution. When a mixture of an aqueous solution of a carbohydrate and an acid is used as the carbon precursor, the amount of acid is preferably the minimum amount capable of polymerizing the organic matter. Furthermore, when a mixture of two-liquid curing type polymer precursors is used as the carbon precursor, the optimum ratio is selected depending on the type of polymer precursor.

[0073] [3.2.2. Polymerization and carbonization of carbon precursors]

[0074] The polymerized carbon precursor is then carbonized within the mesopores. The carbon precursor is carbonized by heating the mesoporous silica containing the carbon precursor to a predetermined temperature in a non-oxidizing atmosphere (for example, in an inert atmosphere, in a vacuum, etc.). Specifically, the heating temperature is preferably 500°C or more and 1200°C or less. If the heating temperature is less than 500°C, the carbon precursor is not sufficiently carbonized. On the other hand, if the heating temperature exceeds 1200°C, silica and carbon react with each other, which is not preferable. The optimal heating time is selected depending on the heating temperature.

[0075] The amount of carbon generated in the mesopores may be equal to or greater than the amount that allows the carbon particles to maintain their shape when the mesoporous silica is removed. Therefore, when the amount of carbon generated in one filling, polymerization, and carbonization is relatively small, it is preferable to repeat these steps multiple times. In this case, the conditions for each repeated step may be the same or different. Furthermore, when each of the steps of filling, polymerization, and carbonization is repeated multiple times, each carbonization step may be performed at a relatively low temperature, and after the final carbonization step is completed, another carbonization step may be performed at a higher temperature. If the final carbonization step is performed at a higher temperature than the previous carbonization steps, the carbon introduced into the pores in multiple steps is more likely to be integrated.

[0076] [3.3. First mold removal process] Next, the mesoporous silica serving as the first template is removed from the composite (first template removal step), thereby obtaining mesoporous carbon (second template) having a beaded structure. Specific examples of methods for removing mesoporous silica include: (1) A method of heating the complex in an alkaline aqueous solution such as sodium hydroxide, (2) Etching the composite with an aqueous solution of hydrofluoric acid; etc.

[0077] [3.4. Graphitization process] Next, if necessary, the mesoporous carbon is heat-treated at a temperature higher than 1500°C (graphitization step). When carbonizing a carbon source in the mesopores of mesoporous silica, the heat treatment temperature must be low in order to suppress the reaction between silica and carbon. Therefore, the degree of graphitization of the carbon after carbonization is low. In order to obtain a high degree of graphitization, it is preferable to heat-treat the mesoporous carbon at a high temperature after removing the first template.

[0078] If the heat treatment temperature is too low, graphitization becomes insufficient. Therefore, the heat treatment temperature is preferably higher than 1500° C. The heat treatment temperature is preferably 1700° C. or higher, and more preferably 1800° C. or higher. On the other hand, if the heat treatment temperature is made higher than necessary, there is no difference in the effect and no practical benefit. Therefore, the heat treatment temperature is preferably 2300° C. or less. The heat treatment temperature is preferably 2200° C. or less.

[0079] [4. Manufacturing method of tin oxide particles] A method for producing tin oxide particles having a beaded structure includes the steps of: A first step of preparing mesoporous carbon having a bead-like structure; a second step of precipitating tin oxide or tin oxide containing a dopant (hereinafter, these are also collectively referred to as "Sn-containing oxide") in the mesopores of the mesoporous carbon to obtain a Sn-containing oxide / carbon composite; A third step of removing carbon from the Sn-containing oxide / carbon composite. It is equipped with:

[0080] [4.1. 1st step] First, mesoporous carbon having a bead-like structure is prepared (first step). Details of the method for producing mesoporous carbon are as described above, and therefore will not be described here.

[0081] [4.2. 2nd process] Next, a Sn-containing oxide is precipitated in the mesopores of the mesoporous carbon (second step), thereby obtaining a Sn-containing oxide / carbon composite. Specifically, the deposition of the Sn-containing oxide in the mesopores is carried out by introducing a precursor of the Sn-containing oxide into the mesopores and converting the precursor into the Sn-containing oxide.

[0082] [4.2.1. Precursors] Specific examples of precursors for forming Sn-containing oxides in mesopores include: (1) A compound that contains a metal element constituting a Sn-containing oxide, is soluble in a solvent, and can be oxidized by dissolved oxygen in the solvent to cause precipitation. (2) A compound that contains a metal element constituting an Sn-containing oxide and is capable of forming a metal oxide by thermal decomposition or hydrolysis; etc.

[0083] Compounds that can be oxidized and precipitated by dissolved oxygen include: (1) Salts containing divalent Sn, such as SnCl2, (2) Salts containing Nb, Sb, W, Ta, or Al, such as NbCl5, SbCl3, WCl6, TaCl5, and AlCl3; etc.

[0084] Compounds capable of forming metal oxides by thermal decomposition or hydrolysis include: (1) Chlorides such as SnCl4, SnCl2, NbCl5, SbCl3, WCl6, TaCl5, and AlCl3, (2) Alkoxides such as tungsten ethoxide (W(OC2H5)6), Sn(OC2H5)2, Sn(OC(CH3)3)4, Nb(OC2H5)5, Ta(OC2H5)5, Sb(OC2H5)3, and Al(OC2H5)3; (3) Acetylacetonate salts such as tin acetylacetonate (Sn(CH3COCHCOCH3)2) and Al(CH3COCHCOCH3)3, (4) Acetates such as Sn(CH3COO)2 and Sb(CH3COO)3, etc.

[0085] [4.2.2. Introduction of precursors into pores] When the precursor is a liquid, it may be adsorbed directly into the pores of the mesoporous carbon. Alternatively, the precursor may be dissolved in a suitable solvent, and the solution may be adsorbed into the pores of the mesoporous carbon. When the precursor is dissolved in a solvent, the type of solvent and the concentration of the precursor are not particularly limited, and an optimum solvent may be selected depending on the purpose.

[0086] [4.2.3. Conversion of precursors to oxides] After the precursor is adsorbed, the precursor is converted into an Sn-containing oxide by any method, and the most suitable method is selected depending on the type of precursor. For example, when a chloride is used as a precursor, mesoporous carbon is dispersed in a solution containing dissolved chloride and stirred in air. With continued stirring, the chloride is eventually adsorbed into the mesopores of the mesoporous carbon, and the chloride in the mesopores gradually becomes an Sn-containing oxide due to the dissolved oxygen.

[0087] For example, when an alkoxide is used as a precursor, the alkoxide or a solution in which the alkoxide is dissolved is added to mesoporous carbon, and the alkoxide or the solution is impregnated into the mesopores. When this is heated to a predetermined temperature, polycondensation of the alkoxide occurs, and Sn-containing oxides are produced in the mesopores. When a sufficient amount of Sn-containing oxide cannot be formed in the mesopores by one cycle of adsorption of the precursor and conversion to the Sn-containing oxide, the adsorption and conversion may be repeated multiple times.

[0088] [4.3. Third step] Next, carbon is removed from the Sn-containing oxide / carbon composite (third step), thereby obtaining the tin oxide-based particles according to the present invention. The method for removing carbon is not particularly limited, and various methods can be used. Examples of the carbon removal method include: (1) A method of heating a Sn-containing oxide / carbon composite in an oxidizing atmosphere, (2) Oxygen plasma etching of a Sn-containing oxide / carbon composite; etc. The removal conditions, such as the heating temperature and heating time, are not particularly limited as long as the conditions are such that the carbon is completely removed without causing the crystallites of the Sn-containing oxide to become coarse.

[0089] [5. Effect] In an electrode catalyst in which Pt-based fine particles are supported on the surface of tin oxide-based particles, by optimizing the microstructure and / or composition of the tin oxide-based particles, it is possible to achieve both a high specific surface area and high ORR mass activity. In particular, when the tin oxide-based particles have mesopores, they exhibit high ORR mass activity despite their high specific surface area. This is believed to be because ionomer poisoning is reduced by supporting Pt-based fine particles in the mesopores.

[0090] In particular, when porous carbon with a beaded structure is used as a template and a Sn source is precipitated in the pores of the template, porous SnO2 particles with a high specific surface area and a beaded structure are obtained. In addition, when an appropriate amount of dopant M (e.g., Sb) is added to the Sn source, porous M-SnO2 particles with high electrical conductivity are obtained. When Pt or a Pt alloy is supported on the surface of the porous M-SnO2 particles by a colloidal method, the high specific surface area of ​​the porous M-SnO2 particles allows Pt-based fine particles with a particle size of about 2 to 3 nm to be supported on the surface in a highly dispersed manner.

[0091] The electrode catalyst thus obtained has a high ORR area specific activity of the Pt-based fine particles due to the high conductivity of the support, and as a result, it exhibits high ORR mass activity. More specifically, the ORR mass activity at 0.9 V is 150 A / g Pt and / or an ORR mass activity at 0.85 V of 650 A / g or more. Pt Thus, an electrode catalyst having the formula: EXAMPLES

[0092] (Examples 1 to 4) [1. Preparation of Sb-SnO2 support] [1.1. Preparation of bead-like mesoporous silica (radial pores)] To a mixed solvent of 4.6 g of methanol (MeOH) and 4.6 g of ethylene glycol (EG), 56.3 g of 30 mass% aqueous cetyltrimethylammonium chloride solution was added and stirred at room temperature. 8.8 g of 1 M NaOH was added and heated to 50° C. Hereinafter, this is referred to as the “first solution.” Next, 12.3 g of tetraethoxysilane (TEOS) was dissolved in a mixed solvent of 6.5 g of MeOH and 6.5 g of EG, hereinafter referred to as "second solution."

[0093] The second solution was added to the first solution heated to 50°C. After the mixture became cloudy, the heating was stopped and the mixture was stirred for another 4 hours or more. After filtering and redispersing in purified water twice, the mixture was dried at 45°C. The dried powder was then calcined in air at 550°C for 6 hours to obtain connected starburst mesoporous silica (radial pores, CSS, Connected Starburst Silica).

[0094] [1.2. Preparation of bead-like mesoporous carbon (radial pores)] 0.5g of CSS was placed in a PFA container, and furfuryl alcohol (FA) was added in an amount equal to the pore volume of the CSS, allowing it to penetrate into the pores of the CSS. This was heat-treated at 150°C for 24 hours to polymerize the FA. This was then heat-treated in a nitrogen atmosphere for 6 hours at 500°C to advance the carbonization of the FA. This was repeated twice, and then further heat-treated in a nitrogen atmosphere for 6 hours at 900°C to obtain a CSS / carbon composite.

[0095] This composite was immersed in a 12% HF solution for 4 hours to dissolve the silica component. After dissolution, it was repeatedly filtered and washed, and then dried at 45°C to obtain connected starburst mesoporous carbon (radial pores, CSC, Connected Starburst Carbon). The resulting porous body had a BET specific surface area of ​​2122 m 2 / g, pore volume: 1.3 mL / g, and pore diameter: 2.2 nm.

[0096] [1.3. Preparation of bead-like mesoporous Sb-SnO2] 0.03 g of SbCl3 was dissolved in 4 mL of concentrated hydrochloric acid (35 mass%), diluted with 36 mL of purified water, and then 5.0 g of SnCl2 was added and dissolved. 0.1 g of beaded mesoporous carbon (CSC) was added to this solution and dispersed. This dispersion was stirred in air at room temperature for 2 hours, after which 200 mL of purified water was added and stirred in air for another 4 hours. Filtration and redispersion in purified water were repeated twice, and the mixture was dried at 45°C to obtain a beaded Sb-SnO2 / carbon composite. This beaded Sb-SnO2 / carbon composite was treated in an air atmosphere at 320℃ for 24 hours to obtain beaded mesoporous Sb-SnO2 (Sb doping amount: 2.5 at%).

[0097] Furthermore, except that the amount of SbCl3 dissolved in concentrated hydrochloric acid was 0.06 g, 0.12 g, or 0.18 g, the same procedure as above was repeated to obtain mesoporous Sb-SnO2 with different Sb doping amounts (Sb doping amount: 3.2 at%, 5.6 at%, or 8.1 at%). Note that the "Sb doping amount" refers to the value obtained by ICP analysis.

[0098] 2. Preparation of electrode catalysts [2.1. Example 1: Pt / Sb-SnO2 by ALD] Using an ALD device, Pt was vapor-deposited onto Sb-SnO2 support particles. MeCpPtMe3 (methylcyclopentadienyltrimethylplatinum) was used as the Pt precursor. A sample tube containing 100 mg of Sb-SnO2 support particles (Sb doping amount: 2.5 at%) was heated to 150°C, and a container containing the Pt precursor was heated to 60°C using a mantle heater. The following ALD cycle (1-4) was repeated 18 times to obtain Pt / Sb-SnO2 (Pt loading rate: 35 mass%). 1.Pt precursor supply: MeCpPtMe3 / Ar, 50ccm, 20min 2. Purge: Ar, 200ccm, 5min 3.Pt precursor reduction: H2, 100 ccm, 5 min 4. Purge: Ar, 200ccm, 5min

[0099] [2.2. Example 2: Pt / Sb-SnO2 by colloidal method (1)] 6 mL of 0.4 M NaOH / EG solution and 6 mL of 0.04 mM H2PtCl6 / EG solution were mixed. This mixture was heated at 160 °C for 3 min while stirring in a microwave synthesis apparatus (Monowabe 400, manufactured by Anton Paar) to obtain a Pt nanoparticle colloidal solution. Next, 94 mg of Sb-SnO2 carrier particles (Sb doping amount: 2.5 at%) was added to 6 mL of Pt nanoparticle colloidal solution, and stirred at room temperature for 2 h. Then, 0.15 mL of 1 M HNO3 was added, and the stirring at room temperature for 1 h was repeated twice. Furthermore, 0.375 mL of 1 M HNO3 was added, and the stirring at room temperature for 1 h was repeated. After that, filtration and redispersion in purified water were repeated twice. The solid was vacuum dried at 70°C, and Pt / Sb-SnO2 (Pt loading rate: 20 mass%) was obtained.

[0100] [2.3. Example 3: Pt / Sb-SnO2 by colloidal method (2)] Pt / Sb-SnO2 (Pt loading: 20 mass%) was obtained in the same manner as in Example 2, except that Sb-SnO2 support particles (Sb doping amount: 5.6 at%) were used instead of Sb-SnO2 support particles (Sb doping amount: 2.5 at%).

[0101] [2.4. Example 4: Pt / Sb-SnO2 by colloidal method (3)] Pt / Sb-SnO2 (Pt loading: 30 mass%) was obtained in the same manner as in Example 2, except that Sb-SnO2 support particles (Sb doping amount: 5.6 at%) were used instead of Sb-SnO2 support particles (Sb doping amount: 2.5 at%) and the amount of Pt nanoparticle colloidal solution was 10 mL.

[0102] 3. Test Method [3.1. Evaluation of bead-like mesoporous Sb-SnO2] [3.1.1. N2 adsorption measurement] The prepared bead-like mesoporous Sb-SnO2 was subjected to N2 adsorption measurement. The pore size distribution was calculated from the N2 adsorption isotherm by the BJH method, and the mode pore size (the most frequent value of the pore size) was taken as the pore size of the sample.

[0103] [3.1.2. Conductivity measurement] The electrical conductivity of the prepared bead-like mesoporous Sb-SnO2 was measured by making a green compact and measuring the voltage when a direct current was applied while applying a pressure of 2.4 MPa.

[0104] [3.2. Evaluation of Pt / Sb-SnO2] [3.2.1. SEM observation] The prepared Pt / Sb-SnO2 was observed using a SEM. [3.2.2. XRD measurement] XRD measurements were carried out on the prepared Pt / Sb-SnO2.

[0105] [3.2.3. Electrochemical evaluation] Electrochemical measurements were performed on the prepared Pt / Sb-SnO2 using the rotating disk electrode (RDE) method. RDE measurements were performed at room temperature in 0.1 M perchloric acid. The electrochemical surface area (ECSA) of Pt was calculated from the charge of the hydrogen adsorption / desorption peak of the cyclic voltammogram recorded in the electrolyte purged with Ar. Linear sweep voltammetry (20 mV / s, forward sweep) was also performed in an electrolyte saturated with O2. The ORR activity at 0.9 V or 0.85 V (based on the reversible hydrogen electrode (RHE)) was calculated by performing background correction, solution resistance correction, and limiting current correction on the obtained voltammogram. The ORR activity was calculated as the activity per Pt mass (mass activity, MA) and the activity per Pt surface area (specific activity, SA).

[0106] [4. Results] [4.1. Evaluation of bead-like mesoporous Sb-SnO2] Table 1 shows the Sb doping amount, specific surface area, pore size, and electrical conductivity of the bead-like mesoporous Sb-SnO2. It was found that the electrical conductivity was highest when the Sb doping amount was 5.6 at%. On the other hand, the particles with an Sb doping amount of 8.1 at% had a slightly larger specific surface area than the other particles, but no significant difference was observed in the pore size compared to the other particles.

[0107] [Table 1]

[0108] [4.2. Evaluation of Pt / Sb-SnO2] [4.2.1. SEM Observation] Fig. 1 shows an SEM image (backscattered electron image) of Pt / Sb-SnO2 obtained in Example 1 (ALD method). Fig. 2 shows an SEM image (backscattered electron image) of Pt / Sb-SnO2 obtained in Example 2 (colloid method). Figs. 1 and 2 show that Pt nanoparticles of about 2 to 3 nm are highly dispersed and supported on the Sb-SnO2 support, regardless of whether the ALD method or the colloid method is used.

[0109] [4.2.2. XRD measurement] FIG. 3 shows the XRD patterns of Pt / Sb-SnO2 obtained in Example 1 (ALD method) and Example 3 (colloid method). In the electrode catalyst in which Pt is supported by the colloid method (Example 3), a diffraction peak derived from Pt(200) can be confirmed near 2θ=47°. On the other hand, in the electrode catalyst in which Pt is supported by the ALD method (Example 1), the corresponding peak is shifted to the low angle side, and it was found to be a peak attributed to PtSb3. From this, it was found that when the ALD method is used, Pt is supported on the support surface and at the same time, alloying of Pt with Sn of the support progresses.

[0110] [3.2.3. Electrochemical evaluation] FIG. 4 shows the cyclic voltammograms of Pt / Sb-SnO2 obtained in Example 2 and Example 3. Comparing Example 2 (Sb doping amount: 2.5 at%, colloid method) and Example 3 (Sb doping amount: 5.6 at%, colloid method), no difference was observed between the two at 0.6 V or less. However, the peak due to Pt oxidation-reduction at 0.6 V or more was smaller in Example 2 (Sb doping amount: 2.5 at%) than in Example 3 (Sb doping amount: 5.6 at%). This indicates that when the Sb doping amount is small, the electronic conductivity of the carrier decreases in the high potential region, and the proportion of electrochemically usable Pt particles decreases.

[0111] Table 2 shows the carrier properties, Pt loading rate, and electrochemical evaluation results of Pt / Sb-SnO2 in Examples 1 to 4. Example 1 (ALD method) had the lowest values ​​for ECSA, SA, and MA. This is believed to be due to the fact that Pt was alloyed with Sn of the carrier when Pt was supported using the ALD method. In general, it is known that Pt alloys have a smaller hydrogen adsorption amount than pure Pt, and that a low value is obtained when ECSA is estimated from the hydrogen adsorption / desorption peak of a cyclic voltammogram. In addition, it is believed that the ORR activity was also reduced by alloying. Therefore, it was found that the colloidal method is more suitable than the ALD method for supporting Pt on the bead-like mesoporous Sb-SnO2.

[0112] Among the electrode catalysts supported by the colloidal method, the MA of Examples 3 and 4, in which the Sb doping amount of the support is 5.6 at %, is about 15% higher than that of Example 2, in which the Sb doping amount of the support is 2.5 at %. This is thought to be because when the Sb doping amount is small, the electronic conductivity of the support decreases in the region of 0.6 V or more. No difference in MA due to the difference in Pt support rate (Example 3 and Example 4) was observed.

[0113] [Table 2]

[0114] Table 3 shows a comparison of ECSA and ORR activity between Pt / Sb-SnO2 obtained in Example 3 and Pt / M-SnO2 (M=Sb, Nb, Ta) reported in Non-Patent Documents 2 to 6. The ORR mass activity (MA) of Example 3 is more than three times higher than the MA of Pt / M-SnO2 reported in Non-Patent Documents 2 to 5. In addition, for Pt / Ta-SnO2 in Non-Patent Document 6, an MA that is about 10% higher than that in Example 3 is reported. However, the specific surface area of ​​the Ta-SnO2 support in Non-Patent Document 6 is 1 / 6 of the specific surface area of ​​the Sb-SnO2 support used in Example 3. Therefore, if the specific surface area of ​​the M-SnO2 support is 30m 2 A Pt / M-SnO2 catalyst with a Pt / SnO2 mass activity of 150 A / g (@0.9 V) or 650 A / g (@0.85 V) and an ORR mass activity of 150 A / g (@0.9 V) or 650 A / g (@0.85 V) has not been reported so far, and this was achieved for the first time by the present invention.

[0115] [Table 3]

[0116] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications are possible without departing from the gist of the present invention. [Industrial Applicability]

[0117] The electrode catalyst according to the present invention can be used as an electrode catalyst for an air electrode catalyst layer of a polymer electrolyte fuel cell, or an electrode catalyst for an anode catalyst layer.

Claims

1. An electrode catalyst comprising: (1) The electrode catalyst is Specific surface area is 30m 2 / g or more, and Pt-based fine particles supported on the tin oxide-based particles; Equipped with The tin oxide particles have a structure in which porous primary particles are fused together in a beaded shape (a beaded structure). (2) The electrode catalyst is and / or an oxygen reduction reaction mass activity at 0.9 V of 300 A / g Pt or more; The oxygen reduction reaction mass activity at 0.85 V is 1500 A / g Pt or more.

2. 2. The electrode catalyst according to claim 1, wherein the tin oxide based particles have pores therein with a pore diameter of 50 nm or less.

3. The tin oxide particles are SnO doped with Sb, Nb, Ta, and / or W. 2 The electrode catalyst according to claim 1 or 2, comprising:

4. The tin oxide particles are Sb-doped SnO 2 It consists of: The doping amount of Sb is 2.5 at % or more and 15.0 at % or less.

4. The electrode catalyst according to claim 1 .

5. The tin oxide particles have a powder conductivity of 1×10 -3 5. The electrode catalyst according to claim 1, wherein the electrochemical conductivity is 1.0 S / cm or more.

6. 6. The electrode catalyst according to claim 1, wherein the pore size of the tin oxide based particles is from 1 nm to 20 nm.

7. 7. The electrode catalyst according to claim 1, wherein the Pt-based fine particles have an average particle size of 5 nm or less.

Citation Information

Patent Citations

  • Alloy electrode catalyst and fuel cell using the same

    JP2017157353A

  • Electrode catalyst, carrier used therefor and method for manufacturing the same, and fuel battery using the electrode catalyst

    JP2017162572A

  • Manufacturing method of electrode material

    JP2020161273A

  • Tantalum-containing tin oxide for fuel cell electrode material

    WO2014136908A1

  • Electrode catalyst and method for producing electrode catalyst

    WO2015146454A1