Glass for magnetic recording medium substrates, magnetic recording medium substrate, magnetic recording medium, and glass spacer for magnetic recording / reproducing apparatuses

LAP665AUndetermined Publication Date: 2022-10-28HOYA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP665
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-11-14
Filing Date
2017-11-14
Publication Date
2022-10-28

AI Technical Summary

Technical Problem

Conventional aluminum alloy substrates for magnetic recording media are prone to deformation and have insufficient surface smoothness, leading to thermal expansion mismatches with spindle materials, which can cause deformation and reliability issues in magnetic recording devices. Additionally, there is a need for substrates with high heat resistance, rigidity, low specific gravity, and appropriate thermal expansion coefficients to reduce warping and power consumption.

Method used

A glass composition for magnetic recording medium substrates with a specific oxide-based formulation, including SiO2, Al2O3, B2O3, MgO, CaO, and SnO2/CeO2, providing a glass transition temperature of 625°C or higher, Young's modulus of 83 GPa or more, specific gravity of 2.85 or less, and an average linear expansion coefficient of 48×10^-7/°C, ensuring excellent heat resistance, rigidity, and thermal stability.

Benefits of technology

The glass composition achieves high heat resistance, rigidity, low specific gravity, and appropriate thermal expansion, reducing substrate deformation, warping, and power consumption while maintaining surface smoothness and stability, enhancing the reliability and efficiency of magnetic recording media.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a glass for magretic recording medium substrate, which is an amorphousoxide glass, wherein, in terms of mol%, ao SiOz content ranges from 45 to 68%; an AlzOrcontent ranges from 5 to 20yo; atotal content of SiO2 and AlzO: ranSes from 60 to 80%; aB2O3 content ranges from 0 to 5%; an MgO content ranges from3 to 28Yo; a CaO contentratrges from 0 to I 8%; a total content of BaO and Sr0 ranges from 0 to 2%o; a total content ofalkali earth metal oxides ranges fro m 12to 30o / o; a total content of alkali metal oxides rangesfrom 3.5 to 15%; and at least one kind selected from the group consisting ofSn oxide and Ceoxide being included, a total content of Sn oxide and Ce oxide ranges from 0.05 to 2.00%, aglass transition temperature is equal to or higher than 625oC; a Young's modulus is equal to ormore than 83 GPa; a specific gravity is equal to or less than 2.85; and an average linearexpansion coefficient at 100 to 300'C is equal to or more than 48"10-? / oC
Need to check novelty before this filing date? Find Prior Art

Description

Glass for magnetic recording medium substrates, magnetic recording medium substrates, magnetic recording media, and glass spacers for magnetic recording and playback devices.

[0001] The present invention relates to glass for magnetic recording medium substrates, magnetic recording medium substrates, magnetic recording media, and glass spacers for magnetic recording and playback devices.

[0002] Conventionally, aluminum alloy substrates have been used as substrates for magnetic recording media such as hard disks (magnetic recording media substrates). However, aluminum alloy substrates have been criticized for being prone to deformation and for not having sufficient surface smoothness after polishing. For this reason, glass magnetic recording media substrates are now widely used (see, for example, Patent Document 1).

[0003] Japanese Patent Publication No. 2010-64921

[0004] In the process of forming a magnetic recording layer on a magnetic recording medium substrate, film deposition is usually performed at high temperatures, or heat treatment is performed at high temperatures after film deposition. Therefore, the glass used for magnetic recording medium substrates is required to have high heat resistance to withstand high-temperature treatment, specifically a high glass transition temperature.

[0005] On the other hand, magnetic recording and playback devices (generally called HDDs (hard disk drives)) that incorporate magnetic recording media have a structure in which the central part is held in place by the spindle and clamp of a spindle motor, causing the magnetic recording media itself to rotate. Therefore, if there is a large difference in the thermal expansion coefficients of the magnetic recording media substrate and the spindle material that constitutes the spindle, a discrepancy will occur in the thermal expansion and contraction of the spindle and the magnetic recording media substrate in response to ambient temperature changes during use, resulting in the deformation of the magnetic recording media. When such a phenomenon occurs, the head will not be able to read the written information, which will impair the reliability of recording and playback. Therefore, the glass for the magnetic recording media substrate is required to have a moderate thermal expansion coefficient similar to that of the spindle material (e.g., stainless steel).

[0006] Furthermore, with the thinning of magnetic recording media and the increasing density of recording, there is a growing demand for further reduction of warping and deflection of the magnetic recording media during spindle motor rotation, as well as for practical strength of the magnetic recording media. To meet these demands, it is desirable for the glass used for the magnetic recording media substrate to have high rigidity, specifically a high Young's modulus.

[0007] In addition, it is desirable to have a low specific gravity for the glass used for magnetic recording media substrates. This is because a lower specific gravity allows for a lighter magnetic recording media substrate. A lighter substrate leads to a lighter magnetic recording medium, which reduces the power required to rotate the magnetic recording medium and thus lowers the power consumption of the HDD.

[0008] Furthermore, it is desirable that the glass used for magnetic recording medium substrates exhibits excellent glass stability. Here, glass stability refers to the resistance to crystal precipitation in molten glass. For example, it can be evaluated by the presence and degree of crystal precipitation after holding molten glass at a holding temperature near the liquidus temperature for a long period of time. Moreover, the less likely crystals are to precipitate even when the holding temperature is lowered, the better the glass stability. Glass with excellent glass stability can be molded at lower molding temperatures, thus extending the lifespan of components of the molding apparatus such as heating elements, furnace bodies, and pipes. In addition, to suppress volatilization, striations, and the generation of molding bubbles, it is desirable to increase the glass viscosity by lowering the molding temperature. However, with glass that has poor glass stability, crystals will precipitate when the molding temperature is lowered. In contrast, with glass that has excellent glass stability, it is possible to lower the molding temperature while suppressing crystal precipitation.

[0009] As described above, it is desirable for glass used for magnetic recording medium substrates to have excellent heat resistance, rigidity, and glass stability, as well as a low specific gravity and a suitable coefficient of thermal expansion.

[0010] Therefore, one aspect of the present invention aims to provide a glass for magnetic recording medium substrates that is excellent in heat resistance, rigidity and glass stability, has a low specific gravity and an appropriate coefficient of thermal expansion.

[0011] One aspect of the present invention is SiO, expressed in mole percent. 2The content of is 45 to 68%, Al 2 O 3 The content of is 5 to 20%, SiO 2 and Al 2 O 3 The total content of (SiO 2 +Al 2 O 3 ) is 60 to 80%, B 2 O 3 The content of is 0 to 5%, the content of MgO is 3 to 28%, the content of CaO is 0 to 18%, the total content of BaO and SrO (BaO + SrO) is 0 to 2%, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is 12 to 30%, the total content of alkali metal oxides (Li 2 O + Na 2 O + K 2 O) is 3.5 to 15%, and it contains at least one selected from the group consisting of Sn oxide and Ce oxide, the total content of Sn oxide and Ce oxide is 0.05 to 2.00%, the glass transition temperature is 625°C or higher, the Young's modulus is 83 GPa or higher, the specific gravity is 2.85 or lower, and the average linear expansion coefficient at 100 to 300°C is 48×10 -7 / °C or higher, and it is an amorphous oxide glass for a magnetic recording medium substrate,

[0012] By having the above glass composition, the glass for a magnetic recording medium substrate can have high heat resistance with a glass transition temperature of 625°C or higher, high rigidity with a Young's modulus of 83 G or higher, a specific gravity of 2.85 or lower, and the above appropriate thermal expansion coefficient, and can exhibit excellent glass stability.

[0013] According to one aspect of the present invention, it is possible to provide a glass for a magnetic recording medium substrate that is excellent in heat resistance and rigidity, has a low specific gravity, has an appropriate thermal expansion coefficient, and is excellent in glass stability. Furthermore, according to one aspect, it is also possible to provide a magnetic recording medium substrate made of the above glass for a magnetic recording medium substrate and a magnetic recording medium including this substrate. Furthermore, according to one aspect, it is possible to provide a glass spacer for a magnetic recording device.

[0014] [Glass for Magnetic Recording Medium Substrates] One aspect of the present invention provides a glass having the above-mentioned glass composition, with a glass transition temperature of 625°C or higher, a Young's modulus of 83 GPa or higher, a specific gravity of 2.85 or lower, and an average coefficient of linear expansion of 48 × 10⁻¹⁶ at 100 to 300°C. -7 This relates to amorphous oxide glass for magnetic recording medium substrates (hereinafter also simply referred to as "glass") having a temperature of 1°C or higher.

[0015] The glass described above is amorphous glass and oxide glass. Unlike crystallized glass, amorphous glass does not contain a crystalline phase and exhibits a glass transition phenomenon upon heating. Oxide glass is glass in which the main network-forming component is an oxide. The glass described above will be explained in more detail below.

[0016] <Glass Composition> In this invention and specification, the glass composition is expressed as oxide-based glass composition. Here, "oxide-based glass composition" refers to the glass composition obtained by calculating it assuming that all glass raw materials decompose during melting and exist as oxides in the glass. Unless otherwise specified, the glass composition is expressed in molar terms (mol %, molar ratio). The glass composition in this invention and specification can be determined by methods such as ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Quantitative analysis is performed separately for each element using ICP-AES. The analytical values ​​are then converted to oxide notation. Analytical values ​​obtained by ICP-AES may contain a measurement error of approximately ±5% of the analytical value. Therefore, the oxide notation values ​​converted from the analytical values ​​may also contain an error of approximately ±5%. Furthermore, in the present invention and this specification, a component content of 0% or not present or introduced means that the component is substantially absent, and that the component content is below the level of an impurity. Below the level of an impurity means, for example, less than 0.01%.

[0017] The glass composition of the above glass is described below.

[0018] SiO 2 It is a network-forming component of glass and has the function of improving glass stability. Also, SiO 2 This is a component that also contributes to improving chemical durability. SiO in the above glass 2 The content of is preferably 68% or less, more preferably 65% ​​or less, more preferably 64% or less, even more preferably 63% or less, and even more preferably 62% or less, from the viewpoint of improving the coefficient of thermal expansion and maintaining melting and moldability. 2 The content of is 45% or more, preferably 48% or more, more preferably 50% or more, even more preferably 52% or more, even more preferably 53% or more, and even more preferably 54% or more, from the viewpoint of maintaining heat resistance and chemical durability.

[0019] Al 2 O 3 It is also a component that forms the network of glass and has the function of improving heat resistance. 2 O 3 It also has the function of improving chemical durability. From the viewpoint of improving heat resistance and chemical durability, Al in the above glass 2 O 3 The content of is 5% or more, preferably 8% or more, more preferably 10% or more, even more preferably 12% or more, and even more preferably 13% or more. Furthermore, from the viewpoint of improving glass stability, the Al content in the above glass is 2 O 3 The content is 20% or less, preferably 18% or less, more preferably 17% or less, and even more preferably 16% or less.

[0020] SiO 2 and Al 2 O 3 The respective contents of each are as described above. Furthermore, in the above glass, SiO 2 and Al 2 O 3 Total content (SiO 2 +Al2 O 3 ) is 60% or more, more preferably 65% ​​or more, even more preferably 67% or more, even more preferably 69% or more, and even more preferably 70% or more, from the viewpoint of stabilizing the glass structure. Also, from the viewpoint of the viscosity characteristics of the glass during melting, the SiO in the above glass is 2 and Al 2 O 3 Total content (SiO 2 +Al 2 O 3 The percentage is 80% or less, preferably 78% or less, more preferably 77% or less, even more preferably 76% or less, and even more preferably 75% or less.

[0021] B 2 O 3 It is also a component that forms the network of glass, a component that lowers the specific gravity of glass, and a component that improves fusion properties. However, B 2 O 3 It is highly volatile during melting and tends to destabilize the glass component ratio. Furthermore, excessive introduction tends to reduce chemical durability. For these reasons, B in the above glass 2 O 3 The content should be 0-5%. B 2 O 3 The content is preferably 3% or less, more preferably 2% or less, even more preferably 1% or less, even more preferably 0.5% or less, and even more preferably 0.3% or less.

[0022] Among the alkaline earth metal oxides MgO, CaO, SrO, and BaO, MgO has the effect of increasing the Young's modulus and specific modulus of glass, increasing the coefficient of thermal expansion, and improving the meltability and formability of glass. Details regarding specific modulus will be described later. From the viewpoint of obtaining the above effects well, the MgO content in the glass is 3% or more, preferably 5% or more, more preferably 6% or more, even more preferably 7% or more, and even more preferably 8% or more. Furthermore, from the viewpoint of maintaining chemical durability, the MgO content in the glass is 28% or less, preferably 26% or less, more preferably 23% or less, even more preferably 20% or less, even more preferably 17% or less, and even more preferably 15% or less.

[0023] The CaO content in the above glass is 0% or more. CaO also has the effect of increasing the Young's modulus and specific modulus of the glass, increasing the coefficient of thermal expansion, and improving the meltability and formability of the glass. From the viewpoint of obtaining these effects well, the CaO content in the above glass is preferably 1% or more, more preferably 2% or more, even more preferably 3% or more, even more preferably 4% or more, and even more preferably 5% or more. Furthermore, from the viewpoint of maintaining chemical durability, the CaO content in the above glass is 18% or less, preferably 15% or less, more preferably 13% or less, and even more preferably 12% or less.

[0024] SrO improves the meltability, formability, and stability of glass, and increases the coefficient of thermal expansion. From the viewpoint of maintaining chemical durability, reducing specific gravity, and lowering raw material costs, the SrO content in the glass is preferably 0 to 2%. A more preferable range for the SrO content is 0 to 1%, an even more preferable range is 0 to 0.5%, and it is most preferable that there is no SrO content, i.e., the SrO content is 0%.

[0025] Both BaO and SrO are components that increase the specific gravity of glass. From the viewpoint of lowering the specific gravity of glass, the total content of BaO and SrO (BaO + SrO) in the glass is preferably 0 to 2%, more preferably 0 to 1%, more preferably 0 to 0.5%, and most preferably no BaO or SrO is present, i.e., the total content of BaO and SrO (BaO + SrO) is 0%.

[0026] BaO also improves the melting properties, formability, and stability of the glass, and increases the coefficient of thermal expansion. From the viewpoint of maintaining chemical durability, reducing specific gravity, and lowering raw material costs, the BaO content in the above glass is preferably 0 to 2%, more preferably 0 to 1%, even more preferably 0 to 0.5%, and most preferably no BaO content, i.e., a BaO content of 0%.

[0027] The total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) in the above glass is 12% or more, preferably 14% or more, more preferably 15% or more, and even more preferably 16% or more, from the viewpoint of the melting properties and stability of the glass. Furthermore, from the viewpoint of the chemical durability of the glass, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) in the above glass is 30% or less, preferably 28% or less, more preferably 26% or less, and even more preferably 25% or less.

[0028] Among alkaline earth metal oxides, MgO has the effect of increasing the Young's modulus and specific modulus of glass, and is also a component that contributes to suppressing the increase in specific gravity. Therefore, MgO is a very useful component for increasing the Young's modulus, specific modulus, and specific gravity of glass, and is particularly effective for increasing the Young's modulus and specific gravity. CaO also has the effect of increasing the Young's modulus and specific modulus of glass, is a component that contributes to suppressing the increase in specific gravity, and is also an effective component for increasing the coefficient of thermal expansion of glass. On the other hand, SrO and BaO increase the specific gravity and raw material costs. From the above viewpoint, in the above glass, the molar ratio of the total content of MgO and CaO to the total content of alkaline earth metal oxides {(MgO + CaO) / (MgO + CaO + SrO + BaO)} is preferably 0.75 to 1.00. The lower limit of the above molar ratio is more preferably 0.80 or higher, even more preferably 0.85 or higher, even more preferably 0.90 or higher, and even more preferably 0.95 or higher.

[0029] Li 2 O is an alkali metal oxide that strongly improves the meltability and formability of glass, and is also a suitable component for increasing Young's modulus and imparting suitable rigidity to magnetic recording medium substrates. 2 O is also a component that increases the coefficient of thermal expansion. Furthermore, when the above glass is used as chemically strengthened glass, it is also a component that plays a role in ion exchange during chemical strengthening. On the other hand, Li 2 O is also a component that lowers the glass transition temperature. Considering the above functions, Li in the above glass 2 The O content is preferably 0-10%. 2 Regarding the lower limit of the O content, it is more preferable that it be 0.5% or more, even more preferable that it be 1.0% or more, and even more preferable that it be 2.0% or more. Also, Li 2 Regarding the upper limit of the O content, it is more preferable that it be 8% or less, even more preferable that it be 7% or less, and even more preferable that it be 6% or less.

[0030] Na 2O is a component that improves the melting and moldability of glass, increases the coefficient of thermal expansion, and reduces the viscosity of glass during clarification, thereby promoting bubble removal. Furthermore, when the above glass is used for chemical strengthening, it is also a component that plays a role in ion exchange during chemical strengthening. Considering the above functions, the Na in the above glass 2 The O content is preferably 0-10%. 2 Regarding the lower limit of the O content, it is more preferable that it be 0.5% or more, even more preferable that it be 1.0% or more, and even more preferable that it be 2.0% or more. Also, Na 2 Regarding the upper limit of the O content, it is more preferable that it be 8% or less, even more preferable that it be 7% or less, and even more preferable that it be 6% or less.

[0031] K 2 O is a component that improves the meltability and moldability of glass and also increases the coefficient of thermal expansion. However, if introduced in excess, it reduces chemical durability, especially acid resistance, and increases alkali leaching from the substrate surface when used as a glass substrate, and the precipitated alkali may affect the film properties of magnetic recording layers, etc. Considering the above points, K in the above glass 2 The O content is preferably 0-5%, more preferably 0-3%, even more preferably 0-2%, and even more preferably 0-1%, and K 2 It is most preferable that the product does not contain oxygen.

[0032] Li 2 O, Na 2 O and K 2 O is a component that improves the meltability and moldability of the glass and increases the coefficient of thermal expansion, as described above. From the viewpoint of obtaining the effects of these components well, the total content of alkali metal oxides (Li) in the above glass is 2 O + Na 2 O+K 2 O) is 3.5% or more, and more preferably 4% or more. On the other hand, from the viewpoint of maintaining the heat resistance and chemical durability of the glass, the total content of alkali metal oxides in the above glass (Li 2 O + Na 2 O+K2 O) is 15% or less, preferably 13% or less, more preferably 12% or less, and still more preferably 11% or less. When the glass contains two or more kinds of alkali metal oxides, the effect of reducing or preventing the elution of alkali from the glass surface can be obtained due to the mixed alkali effect.

[0033] Li 2 O is a component that more effectively contributes to increasing the Young's modulus of the glass and increasing the coefficient of thermal expansion among the alkali metal oxides. Therefore, in one aspect, from the viewpoint of increasing the Young's modulus and improving the coefficient of thermal expansion, the molar ratio of the Li 2 O content to the total content of alkali metal oxides {Li 2 O / (Li 2 O + Na 2 O + K 2 O)} is preferably 0.4 to 1. In one aspect of the glass where the molar ratio {Li 2 O / (Li 2 O + Na 2 O + K 2 O)} is within the above range, a Young's modulus of 90 GPa or more can be obtained. In one aspect, for the lower limit of the molar ratio {Li 2 O / (Li 2 O + Na 2 O + K 2 O)}, it is more preferably 0.5 or more, still more preferably 0.6 or more, even more preferably 0.7 or more, and even more preferably 0.8 or more.

[0034] Na 2 O is a component that improves the melting property and formability of the glass and more effectively contributes to increasing the coefficient of thermal expansion among the alkali metal oxides. Further, Na 2 O has a smaller effect of lowering the glass transition temperature compared to Li 2 O. Therefore, in one aspect, from the viewpoint of improving heat resistance and the coefficient of thermal expansion, the molar ratio of the Na 2 O content to the total content of alkali metal oxides {Na 2 O / (Li 2 O + Na 2 O + K2 O)} is preferably from 0.4 to 1. The molar ratio {Na 2 O / (Li 2 O + Na 2 O + K 2 O)} in the above range, in one embodiment of the above glass, the glass transition temperature can be 690 °C or higher. In one embodiment, the molar ratio {Na 2 O / (Li 2 O + Na 2 O + K 2 O)} is more preferably 0.5 or higher, still more preferably 0.6 or higher, even more preferably 0.7 or higher, and yet more preferably 0.8 or higher.

[0035] TiO 2 improves glass stability and chemical durability and has the function of increasing Young's modulus. However, if introduced excessively, the liquidus temperature of the glass may increase, leading to deterioration of devitrification resistance and an increase in specific gravity. Therefore, the content of TiO 2 in the above glass is preferably from 0 to 8%, more preferably from 0 to 6%, still more preferably from 0 to 5%, even more preferably from 0 to 4%, yet more preferably from 0 to 3%, and still yet more preferably from 0 to 2%.

[0036] HfO 2 、Nb 2 O 5 、Ta 2 O 5 、La 2 O 3 and Y 2 O 3 have the function of improving chemical durability, particularly alkali resistance. However, excessive introduction may deteriorate the melting property and increase the specific gravity. Therefore, from the viewpoint of maintaining the melting property and improving chemical durability, particularly alkali resistance, HfO 2 、Nb 2 O 5 、Ta 2 O 5 、La 2 O 3 and Y 2 O 3 The total content of (HfO2 +Nb 2 O 5 +Ta 2 O 5 +La 2 O 3 +Y 2 O 3 The amount of (of) is preferably 0 to 5%. The lower limit is preferably 0.3% or more, more preferably 0.5% or more, and even more preferably 1.0% or more. The upper limit is preferably 5% or less, more preferably 3% or less, and even more preferably 2% or less.

[0037] ZrO 2 It has the effect of improving chemical durability and also increasing Young's modulus. However, excessive introduction may reduce the melting properties of the glass and result in residual molten raw material. Therefore, ZrO in the above glass 2 The content is preferably 0-5%, more preferably 0-3%, even more preferably 0-2%, and even more preferably 0-1%.

[0038] ZnO improves fusion properties and increases Young's modulus, but excessive introduction raises the liquidus temperature. Therefore, the ZnO content in the glass is preferably 0-3%. The ZnO content is more preferably 0-2%, even more preferably 0-1%, and may even be 0%.

[0039] P 2 O 5 Although it can be introduced in small amounts, excessive introduction tends to reduce chemical durability, therefore, P in the above glass 2 O 5 The content of P is preferably 0-2%. 2 O 5 The content of is more preferably 0 to 1%, P 2 O 5 It does not contain P 2 O 5 It is even more preferable that the content of [the substance] is 0%.

[0040] The above glass contains at least one selected from the group consisting of Sn oxide and Ce oxide, from the viewpoint of obtaining a clarification effect, and the total content of Sn oxide and Ce oxide is 0.05% to 2.00%. By having a total content of Sn oxide and Ce oxide of 0.05% or more, a sufficient clarification effect can be obtained, and the remaining bubbles can be reduced or suppressed. Furthermore, by having a total content of 2.00% or less, it is possible to prevent the molten glass from blowing up during glass melting, which reduces productivity. The lower limit of the total content of Sn oxide and Ce oxide is preferably 0.10% or more, more preferably 0.15% or more, and even more preferably 0.20% or more. Furthermore, the upper limit of the total content of Sn oxide and Ce oxide is preferably 1.50% or less, more preferably 1.20% or less, and even more preferably 1.00% or less.

[0041] Sn oxides promote clarification of glass at relatively high melting temperatures (around 1400-1600°C). 2 O 3 With the use of environmentally harmful clarifying agents such as arsenous acid being restricted, in order to remove bubbles from glass with a high glass transition temperature, Sn oxide (for example, SnO) is applied to the glass. 2 It is preferable to introduce ). From the viewpoint of obtaining a clarifying effect, the content of Sn oxide is preferably 0.01% or more, more preferably 0.05% or more, even more preferably 0.10% or more, even more preferably 0.15% or more, and even more preferably 0.20% or more. Furthermore, the content of Sn oxide is preferably 2.00% or less, more preferably 1.50% or less, even more preferably 1.00% or less, and even more preferably 0.80% or less.

[0042] Ce oxides, like Sn oxides, are components that exhibit a clarifying effect on glass. Ce oxides have the function of incorporating oxygen and fixing it as a glass component when the melting temperature of the glass is relatively low (temperature range of about 1200 to 1400°C), and as a clarifying agent, Ce oxides (for example, CeO) are added to the glass.2 It is preferable to introduce ). From the viewpoint of obtaining a clarifying effect, the Ce oxide content is preferably 0.01% or more, more preferably 0.05% or more, even more preferably 0.10% or more, and even more preferably 0.20% or more. Furthermore, the Ce oxide content is preferably 1.00% or less, more preferably 0.80% or less, even more preferably 0.50% or less, and even more preferably 0.40% or less.

[0043] The above glass contains at least one selected from the group consisting of Sn oxide and Ce oxide, and in one embodiment it contains only Sn oxide, in another embodiment it contains only Ce oxide, and in yet another embodiment it contains both Sn oxide and Ce oxide. In particular, by having Sn oxide and Ce oxide coexist in the above glass, a clarifying effect can be obtained over a wide temperature range, so it is preferable that the above glass contains both Sn oxide and Ce oxide.

[0044] Sb, which has been widely used as a clarifying agent 2 O 3 From the perspective of reducing environmental impact, it is desirable to refrain from using Sb in the above glass. 2 O 3 The content of is preferably in the range of 0 to 0.5%. 2 O 3 The content of is more preferably 0.2% or less, even more preferably 0.1% or less, even more preferably 0.05% or less, and even more preferably 0.02% or less, Sb 2 O 3 It is especially preferable that it does not contain [the specified ingredient].

[0045] The above glass contains Fe, Fe 2 O 3 Converted to this, it can contain approximately 0.5% or less. The Fe content is Fe 2 O 3 When converted to an amount, it is preferably 0.2% or less, more preferably 0.1% or less, even more preferably 0.05% or less, and even more preferably does not contain Fe.

[0046] Since Pb, Cd, As, etc., are substances that have adverse effects on the environment, it is preferable to avoid introducing them.

[0047] The above-mentioned glass can be produced by weighing and mixing glass raw materials such as oxides, carbonates, nitrates, sulfates, and hydroxides to obtain a predetermined glass composition, thoroughly mixing them, heating and melting them in a melting vessel at, for example, a range of 1400 to 1600°C, clarifying and stirring to form homogenized molten glass that has been thoroughly de-bubbled. For example, it is preferable to heat and melt the glass raw materials in a melting tank at 1400 to 1550°C, raise the temperature of the obtained molten glass in a clarifying tank and maintain it at 1450 to 1600°C, then cool it down to 1200 to 1400°C to pour out and form the glass.

[0048] <Glass Properties> The above glass can have the following glass properties by performing the compositional adjustments described above.

[0049] (Glass Transition Temperature) As mentioned earlier, magnetic recording medium substrates are typically subjected to high-temperature processing during the process of forming a magnetic recording layer on the substrate. For example, in order to form a magnetic recording layer containing a magnetic material with high magnetic anisotropy energy, which has been developed in recent years for high-density recording of magnetic recording mediums, the film is usually deposited at a high temperature, or heat-treated at a high temperature after film deposition. If the magnetic recording medium substrate does not have sufficient heat resistance to withstand such high-temperature processing, the flatness of the substrate will be impaired by exposure to high temperatures during the high-temperature processing. In contrast, the above-mentioned glass has a glass transition temperature (hereinafter also referred to as "Tg") of 625°C or higher, which is an indicator of heat resistance. If the substrate is made of glass with high heat resistance, having a glass transition temperature of 625°C or higher, it can maintain excellent flatness even after high-temperature processing. However, the above-mentioned glass is not limited to glass for substrates of magnetic recording mediums having a magnetic recording layer containing a magnetic material that requires high-temperature processing, but can be used in the manufacture of magnetic recording mediums equipped with various magnetic materials. The glass transition temperature is preferably 630°C or higher, more preferably 640°C or higher, even more preferably 650°C or higher, even more preferably 660°C or higher, even more preferably 670°C or higher, even more preferably 675°C or higher, and even more preferably 680°C or higher. The upper limit of the glass transition temperature is, for example, around 770°C, but is not particularly limited as a higher glass transition temperature is preferable from the viewpoint of heat resistance.

[0050] (Young's Modulus) In order to meet the demand for improved rigidity of magnetic recording media as described above, it is desirable that the glass for magnetic recording media substrates have high rigidity. In this regard, the glass has a Young's modulus of 83 G or higher, which is an indicator of rigidity. By using a glass for magnetic recording media substrates with high rigidity exhibiting a Young's modulus of 83 G or higher, substrate deformation during rotation of the spindle motor can be suppressed, and thus warping and deflection of the magnetic recording media due to substrate deformation can also be suppressed. The Young's modulus of the glass is preferably 85 GPa or higher, more preferably 86 GPa or higher, even more preferably 88 GPa or higher, and even more preferably 90 GPa or higher. The upper limit of the Young's modulus is, for example, around 120 GPa, but it is not particularly limited as a higher Young's modulus is preferable because the higher the Young's modulus, the higher the rigidity.

[0051] (Specific Gravity) The specific gravity of the glass is 2.85 or less, preferably 2.80 or less, more preferably 2.75 or less, even more preferably 2.70 or less, and most preferably 2.65 or less. Lowering the specific gravity of the glass for the magnetic recording medium substrate makes it possible to lighten the magnetic recording medium substrate, and further lighten the magnetic recording medium, thereby reducing the power consumption of the HDD. The lower limit of the specific gravity is, for example, around 2.40, but it is not particularly limited as a lower specific gravity is preferable.

[0052] (Specific Modulus) The specific modulus is the Young's modulus of glass divided by its density. Here, density is the specific gravity of the glass multiplied by g / cm³. 3 This can be considered a value with the unit 'm' attached. From the viewpoint of providing a substrate that is less prone to deformation, the specific modulus of elasticity of the glass is preferably 31 MNm / kg or more, more preferably 33 MNm / kg or more, and even more preferably 34 MNm / kg or more. The upper limit of the specific modulus is, for example, about 40 MNm / kg, but it is not particularly limited as a higher specific modulus is preferable.

[0053] (Coefficient of Thermal Expansion) From the viewpoint of improving the reliability of magnetic recording media, as mentioned above, it is desirable for the glass for magnetic recording media substrates to have an appropriate coefficient of thermal expansion. Generally, the spindle material of HDDs has a coefficient of thermal expansion of 70 × 10 in the temperature range of 100 to 300°C. -7 It has an average linear expansion coefficient (thermal expansion coefficient) of 1 / °C or higher, and the average linear expansion coefficient of the glass for magnetic recording medium substrates at 100 to 300°C is 48 × 10⁻⁶. -7 If the temperature is above 1 / °C, the difference in thermal expansion coefficient with the spindle material is small, which can contribute to improving the reliability of the magnetic recording medium. The average linear expansion coefficient of the above glass at 100 to 300°C (hereinafter also referred to as "α") is 48 × 10⁻⁶. -7 / ℃ or higher, 50 × 10 -7 It is more preferable that the temperature be above / ℃, 51 × 10 -7 It is even more preferable that the temperature is above / °C. Furthermore, the average coefficient of linear expansion (α) of the above glass at 100 to 300°C is 90 × 10⁻⁶. -7 It is preferable that the temperature is below / ℃.

[0054] (Glass Stability) The above glass can exhibit high glass stability. Methods for evaluating glass stability include the 1300°C for 16 hours holding test and the 1250°C for 16 hours holding test, which will be described in detail later. It is preferable that the evaluation result is A in the 1300°C for 16 hours holding test, it is more preferable that the evaluation result is A in the 1300°C for 16 hours holding test and that the evaluation result is A or B in the 1250°C for 16 hours holding test, and it is even more preferable that the evaluation result is A in both holding tests.

[0055] (Bubble Density) The above glass can also have its bubbles reduced by the composition adjustment described above. With respect to bubbles in the glass, the bubble density per unit mass, as observed with an optical microscope (magnification 40 to 100 times) and having a diameter of more than 0.03 mm, is preferably less than 50 bubbles / kg, more preferably less than 20 bubbles / kg, even more preferably less than 10 bubbles / kg, even more preferably 2 bubbles / kg or less, and most preferably 0 bubbles / kg.

[0056] [Magnetic recording medium substrate] A magnetic recording medium substrate according to one aspect of the present invention is made of the above-mentioned glass for magnetic recording medium substrates.

[0057] Magnetic recording medium substrates can be manufactured by preparing molten glass by heating glass raw materials, forming this molten glass into a plate shape using one of the following methods: press molding, down-draw, or float molding, and then processing the resulting plate-shaped glass. For example, in the press molding method, molten glass flowing out of a glass outflow pipe is cut to a predetermined volume to obtain the required amount of molten glass, which is then press-molded in a press molding die to produce a thin-walled disc-shaped substrate blank. Next, a central hole is made in the obtained substrate blank, and the inner and outer periphery are processed, and both main surfaces are lapped and polished. Then, a cleaning process including acid cleaning and alkaline cleaning is performed to obtain a disc-shaped substrate.

[0058] In one embodiment, the magnetic recording medium substrate described above has a homogeneous surface and internal composition. Here, a homogeneous surface and internal composition means that ion exchange is not performed (i.e., it does not have an ion exchange layer). For example, a magnetic recording medium substrate without an ion exchange layer can be used when an HDD (hard disk drive) incorporating a magnetic recording medium is used in an environment where it is less susceptible to external shocks. Furthermore, since a magnetic recording medium substrate without an ion exchange layer does not undergo ion exchange treatment, manufacturing costs can be significantly reduced.

[0059] Furthermore, in one embodiment, the magnetic recording medium substrate has an ion exchange layer on part or all of its surface. Since the ion exchange layer exhibits compressive stress, the presence or absence of the ion exchange layer can be confirmed by fracturing the substrate perpendicular to the main surface and obtaining a stress profile on the fracture surface using the Babinet method. The "main surface" is the surface of the substrate on which the magnetic recording layer is provided or has been provided. This surface is called the main surface because it is the surface with the largest area among the surfaces of the magnetic recording medium substrate, and in the case of a disk-shaped magnetic recording medium, it corresponds to the circular surface of the disk (excluding the central hole if there is one). The presence or absence of the ion exchange layer can also be confirmed by methods such as measuring the concentration distribution of alkali metal ions in the depth direction from the substrate surface.

[0060] An ion exchange layer can be formed by contacting an alkali salt with the substrate surface at a high temperature and exchanging alkali metal ions in the alkali salt with alkali metal ions in the substrate. For ion exchange (also called "strengthening treatment" or "chemical strengthening"), known techniques can be applied, and for example, paragraphs 0068-0069 of WO2011 / 019010A1 can be seen.

[0061] The magnetic recording medium substrate described above has a thickness of, for example, 1.5 mm or less, preferably 1.2 mm or less, more preferably 1 mm or less, and the lower limit of the thickness is preferably 0.3 mm. Furthermore, the magnetic recording medium substrate is preferably in the shape of a disk having a central hole.

[0062] The magnetic recording medium substrate described above is made of amorphous glass. Compared to crystallized glass, amorphous glass can achieve superior surface smoothness when processed into a substrate.

[0063] [Magnetic recording medium] One aspect of the present invention relates to a magnetic recording medium having a magnetic recording layer on a magnetic recording medium substrate.

[0064] Magnetic recording media are also called magnetic disks or hard disks, and are suitable for various magnetic recording and playback devices, such as internal storage devices (fixed disks, etc.) in desktop computers, server computers, notebook computers, and mobile computers, internal storage devices in portable recording and playback devices that record and / or play back images and / or sound, and recording and playback devices in car audio systems. In the present invention and this specification, "magnetic recording and playback device" means a device capable of recording information magnetically, or recording information magnetically, or both.

[0065] A magnetic recording medium has a structure in which, for example, at least an adhesion layer, an underlayer, a magnetic layer (magnetic recording layer), a protective layer, and a lubricating layer are laminated on the main surface of a magnetic recording medium substrate, in order from the side closest to the main surface. For example, the magnetic recording medium substrate is introduced into a vacuum deposition apparatus, and films are sequentially deposited on the main surface of the magnetic recording medium substrate from the adhesion layer to the magnetic layer in an Ar atmosphere using DC (Direct Current) magnetron sputtering. For example, CrTi can be used as the adhesion layer, and for example, CrRu can be used as the underlayer. After the above film deposition, for example, C is deposited by CVD (Chemical Vapor Deposition). 2 H 4 A magnetic recording medium can be formed by depositing a protective layer using [a specific method] and then performing a nitriding treatment in which nitrogen is introduced to the surface within the same chamber. Subsequently, a lubricating layer can be formed by applying, for example, PFPE (polyfluoropolyether) onto the protective layer using a dip-coating method.

[0066] To achieve even higher density recording in magnetic recording media, it is preferable that the magnetic recording layer contains a magnetic material with high magnetic anisotropy energy. From this point of view, preferred magnetic materials include Fe-Pt-based magnetic materials or Co-Pt-based magnetic materials. Here, "system" means containing. That is, it is preferable that the above-mentioned magnetic recording media has a magnetic recording layer containing Fe and Pt, or Co and Pt, as the magnetic recording layer. For details on a magnetic recording layer containing such magnetic materials and a method for forming such a film, refer to paragraph 0074 of WO2011 / 019010A1 and the examples described in the same publication. Furthermore, it is preferable that a magnetic recording media having such a magnetic recording layer be applied to a magnetic recording device using a recording method called energy-assisted recording. Among energy-assisted recording methods, a recording method that assists magnetization reversal by irradiation with laser light or the like is called a thermal-assisted recording method, and a recording method that assists with microwaves is called a microwave-assisted recording method. For details on these, refer to paragraph 0075 of WO2011 / 019010A1.

[0067] In recent years, the Dynamic Flying Height (DFH) mechanism has been incorporated into magnetic heads to significantly reduce the gap between the recording / reproduction element of the magnetic head and the surface of the magnetic recording medium (reduced levitation), thereby achieving even higher recording densities. The DFH mechanism is a function that provides a heating element, such as a tiny heater, near the recording / reproduction element of the magnetic head, causing only the area around the element to protrude towards the surface of the medium. This reduces the distance between the magnetic head and the magnetic recording layer of the medium (flying height), making it possible to pick up signals from smaller magnetic particles and achieve even higher recording densities. However, on the other hand, the gap between the element of the magnetic head and the surface of the medium (flying height) becomes extremely small. If there are irregularities on the surface of the magnetic recording medium substrate caused by bubbles, these irregularities will be reflected on the surface of the magnetic recording medium, reducing the surface smoothness of the magnetic recording medium. When a magnetic head is brought close to a magnetic recording medium surface with poor surface smoothness, there is a risk that the magnetic head may come into contact with the magnetic recording medium surface and be damaged. Therefore, a certain amount of flying height must be ensured to prevent contact. From this point of view, it is desirable to reduce bubbles in the magnetic recording medium substrate in order to produce a magnetic recording medium with high surface smoothness. Reducing bubbles in the substrate makes it possible to narrow the flying height. Since the above magnetic recording medium substrate preferably has reduced bubbles, the magnetic recording medium equipped with such a substrate is also suitable for magnetic recording devices equipped with a DFH mechanism that has an extremely narrow flying height.

[0068] There are no particular restrictions on the dimensions of the magnetic recording medium substrate (e.g., magnetic disk substrate) and the magnetic recording medium (e.g., magnetic disk) mentioned above. However, it is possible to miniaturize the medium and substrate, for example, because high recording density is possible. For example, in addition to the nominal diameter of 2.5 inches, even smaller diameters (e.g., 1 inch, 1.8 inches), or dimensions such as 3 inches, 3.5 inches, etc., are possible.

[0069] [Glass spacer for magnetic recording and playback device] One aspect of the present invention is a spacer containing SiO2 in mol%. 2 The content is 45-68%, Al 2 O3 The content is 5-20%, SiO 2 and Al 2 O 3 Total content (SiO 2 +Al 2 O 3 ) is 60-80%, B 2 O 3 The content of is 0-5%, the content of MgO is 3-28%, the content of CaO is 0-18%, the total content of BaO and SrO (BaO + SrO) is 0-2%, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is 12-30%, the total content of alkali metal oxides (Li 2 O + Na 2 O+K 2 The O) is 3.5 to 15%, and contains at least one selected from the group consisting of Sn oxide and Ce oxide, with a total content of Sn oxide and Ce oxide of 0.05 to 2.00%, a glass transition temperature of 625°C or higher, a Young's modulus of 83 GPa or higher, a specific gravity of 2.85 or lower, and an average coefficient of linear expansion of 48 × 10⁻¹⁰ at 100 to 300°C. -7 This relates to a glass spacer for a magnetic recording and playback device, made of amorphous oxide glass with a temperature of 2°C or higher.

[0070] Magnetic recording media can be used in magnetic recording and / or reproducing information magnetically in a magnetic recording and reproducing device. Magnetic recording and reproducing devices typically include spacers to fix the magnetic recording media to the spindle of a spindle motor and / or to maintain distance between multiple magnetic recording media. In recent years, the use of glass spacers has been proposed as such spacers. For similar reasons as those previously detailed for glass for magnetic recording media substrates, it is desirable for these glass spacers to have excellent heat resistance, rigidity, and glass stability, a low specific gravity, and a moderate coefficient of thermal expansion. In this regard, as previously detailed for glass for magnetic recording media substrates according to one aspect of the present invention, the above-mentioned glass can have excellent heat resistance, rigidity, and glass stability, a low specific gravity, and a moderate coefficient of thermal expansion, making it suitable as a glass spacer for a magnetic recording and reproducing device.

[0071] Spacers for magnetic recording and playback devices are ring-shaped members, and details such as the structure and manufacturing method of glass spacers are publicly known. Furthermore, for the manufacturing method of glass spacers, refer to the above-mentioned descriptions concerning the manufacturing method of glass for magnetic recording medium substrates and the manufacturing method of magnetic recording medium substrates. For other details such as the glass composition and glass properties of the glass spacer for magnetic recording and playback devices according to one aspect of the present invention, refer to the above-mentioned descriptions concerning glass for magnetic recording medium substrates, magnetic recording medium substrates, and magnetic recording media according to one aspect of the present invention. In addition, a conductive film can be formed on the surface of the glass spacer by immersion, vapor deposition, sputtering, etc., to remove static electricity generated when the magnetic recording medium rotates. Furthermore, the surface smoothness of the glass spacer can be increased by polishing (for example, an average surface roughness of 1 μm or less), thereby strengthening the adhesion between the magnetic recording medium and the spacer and suppressing the occurrence of misalignment.

[0072] [Magnetic recording and playback apparatus] One aspect of the present invention relates to a magnetic recording and playback apparatus comprising at least one of a magnetic recording medium according to one aspect of the present invention and a glass spacer according to one aspect of the present invention.

[0073] A magnetic recording and reproducing apparatus includes at least one magnetic recording medium and at least one spacer, and typically further includes a spindle motor for rotating the magnetic recording medium and at least one magnetic head for recording and / or reproducing information on the magnetic recording medium. The magnetic recording and reproducing apparatus according to one aspect of the present invention described above may include a magnetic recording medium according to one aspect of the present invention as at least one magnetic recording medium, and may also include a plurality of magnetic recording media according to one aspect of the present invention. The magnetic recording and reproducing apparatus according to one aspect of the present invention described above may include a glass spacer according to one aspect of the present invention as at least one spacer, and may also include a plurality of glass spacers according to one aspect of the present invention. A small difference between the thermal expansion coefficient of the magnetic recording medium and the thermal expansion coefficient of the spacer is preferable from the viewpoint of suppressing phenomena that may occur due to the difference in their thermal expansion coefficients, such as distortion of the magnetic recording medium and a decrease in rotational stability due to misalignment of the magnetic recording medium. From this viewpoint, it is preferable that the magnetic recording and reproducing apparatus according to one aspect of the present invention includes a magnetic recording medium according to one aspect of the present invention as at least one magnetic recording medium, and more magnetic recording media if a plurality of magnetic recording media are included, and includes a glass spacer according to one aspect of the present invention as at least one spacer, and more spacers if a plurality of spacers are included. Furthermore, for example, in one embodiment of the present invention, the magnetic recording and playback apparatus may have the same glass composition as the glass constituting the magnetic recording medium substrate included in the magnetic recording medium and the glass constituting the glass spacer.

[0074] A magnetic recording and reproducing apparatus according to one aspect of the present invention may include at least one of a magnetic recording medium according to one aspect of the present invention and a glass spacer according to one aspect of the present invention, and prior art relating to magnetic recording and reproducing apparatuses may be applied to other aspects. In one aspect, an energy-assisted magnetic recording head can be used as the magnetic head, having an energy source (e.g., a heat source such as a laser light source, microwaves, etc.) for assisting magnetization reversal (assisting the writing of magnetic signals), a recording element section, and a reproducing element section. A magnetic recording and reproducing apparatus using an energy-assisted recording method that includes such an energy-assisted magnetic recording head is useful as a magnetic recording and reproducing apparatus with high recording density and high reliability. Furthermore, when manufacturing a magnetic recording medium used in an energy-assisted recording apparatus such as a heat-assisted recording method equipped with a heat-assisted magnetic recording head having a laser light source, etc., a magnetic recording layer containing a magnetic material with high magnetic anisotropy energy may be formed on the magnetic recording medium substrate. To form such a magnetic recording layer, film deposition is usually performed at a high temperature, or heat treatment is performed at a high temperature after film deposition. As a magnetic recording medium substrate that can withstand such high-temperature processing, the magnetic recording medium substrate according to one aspect of the present invention is preferred. However, the magnetic recording and playback device according to one aspect of the present invention is not limited to an energy-assisted magnetic recording and playback device.

[0075] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the embodiments shown in the examples.

[0076] [Examples No. 1 to No. 47, Comparative Examples 1 to 5, Reference Example 1] Raw materials such as oxides, carbonates, nitrates, and hydroxides were weighed and mixed to obtain a blended raw material so that glass with the composition shown in Table 1 could be obtained. This blended raw material was placed in a melting tank and heated and melted in the range of 1400 to 1600°C. The molten glass obtained was held in a clarification tank at 1400 to 1550°C for 6 hours, then the temperature was lowered (cooled) and held in the range of 1200 to 1400°C for 1 hour before the molten glass was molded to obtain glass (amorphous oxide glass) for the evaluation described below.

[0077] [Evaluation Method] (1) Glass transition temperature (Tg), mean linear expansion coefficient (α) The glass transition temperature Tg and mean linear expansion coefficient α at 100 to 300°C were measured for each glass using a thermomechanical analyzer (TMA).

[0078] (2) Young's modulus The Young's modulus of each glass was measured using the ultrasonic method.

[0079] (3) Specific gravity The specific gravity of each glass was measured using the Archimedes method.

[0080] (4) Specific modulus The specific modulus was calculated from the Young's modulus obtained in (2) and the specific gravity obtained in (3) above.

[0081] (5) Glass Stability 100g of each glass was placed in a platinum crucible, and each crucible was placed in a heating furnace set to a temperature of 1250°C or 1300°C, and left for 16 hours while maintaining the furnace temperature (holding test). After 16 hours, the crucible was removed from the heating furnace, the glass inside the crucible was transferred to a refractory material and cooled to room temperature, and the presence or absence of crystals in each glass was observed with an optical microscope and evaluated according to the following criteria: A: No crystals were observed under magnification with an optical microscope (magnification 40 to 100 times). B: Crystals were observed under magnification with an optical microscope (magnification 40 to 100 times), but no crystals were observed by visual inspection. C: Crystals were observed by visual inspection.

[0082] (6) Evaluation of bubble density rank A glass plate (substrate blank) with a thickness of approximately 1.2 mm was prepared from the molten glass obtained above. The surface of this glass plate was polished to be flat and smooth, and the inside of the glass was observed under magnification (magnification 40 to 100 times) from the polished surface using an optical microscope, and the number of bubbles with a diameter greater than 0.03 mm (hereinafter simply referred to as "bubbles") was counted. The bubble density was determined by dividing the number of counted bubbles by the mass of the glass corresponding to the area observed under magnification. The bubble density rank was evaluated from S rank to F rank according to the bubble density obtained by the above method. Specifically, a bubble density of 0 bubbles / kg was ranked S, bubbles present with a bubble density of 2 bubbles / kg or less were ranked A, bubbles with a bubble density of more than 2 bubbles / kg but less than 10 bubbles / kg were ranked B, bubbles with a bubble density of 10 bubbles / kg or more but less than 20 bubbles / kg were ranked C, bubbles with a bubble density of 20 bubbles / kg or more but less than 50 bubbles / kg were ranked D, bubbles with a bubble density of 50 bubbles / kg or more but less than 80 bubbles were ranked E, and bubbles with a bubble density of 80 bubbles / kg or more were ranked F.

[0083] The results are shown in Table 1 (Tables 1-1 to 1-6).

[0084]

[0085]

[0086]

[0087]

[0088]

[0089]

[0090] As shown in Table 1, the glass for magnetic recording medium substrates in the examples all exhibited excellent heat resistance and rigidity, low specific gravity, a moderate coefficient of thermal expansion, and excellent glass stability. Regarding glass stability, in the holding test performed by the above method, the lower the evaluation result at a lower temperature, the less likely crystals are to precipitate in the molten state, and the lower the molding temperature. Lowering the molding temperature extends the lifespan of components of the molding apparatus such as heating elements, furnace bodies, and pipes. In particular, when manufacturing substrate blanks by press molding, a lower molding temperature is preferable. Furthermore, lowering the molding temperature allows for increased glass viscosity during molding, thereby suppressing volatilization, striations, and the generation of molding bubbles. On the other hand, the glass for the magnetic recording medium substrate of Comparative Example 1 has the composition of Example 9 of Japanese Patent Application Publication No. 2010-64921 (Patent Document 1), the glass for the magnetic recording medium substrate of Comparative Example 2 has the composition of Example 18 of the same publication, the glass for the magnetic recording medium substrate of Comparative Example 3 has the composition of Example 27 of the same publication, the glass for the magnetic recording medium substrate of Comparative Example 4 has the composition of Example 29 of the same publication, and the glass for the magnetic recording medium substrate of Comparative Example 5 has the composition of Example 30 of the same publication. The glass for the magnetic recording medium substrate of Comparative Example 1 is composed of SiO 2 and Al 2 O 3 The total content of is excessive, and the glass for magnetic recording medium substrates of Comparative Examples 4 and 5 contains SiO 2 The content and SiO 2 and Al 2 O 3 The total content of these substances is excessive. Furthermore, the magnetic recording medium substrate glass of Comparative Examples 4 and 5 has a low total content of alkaline earth oxides. Also, the magnetic recording medium substrate glass of Comparative Examples 1 to 3 either does not contain alkali metal oxides or has a low content of alkali metal oxides. All of these magnetic recording medium substrate glass of Comparative Examples 1 to 5 had low coefficients of thermal expansion and poor glass stability. In addition, the glass of the examples shown in Table 1 all had a bubble density rank of S, A, or B, confirming that bubble generation was suppressed. In contrast, the magnetic recording medium substrate glass of Reference Example 1, in which the total content of Sn oxide and Ce oxide was less than 0.05% by mass, showed significant bubble generation (bubble density rank E).

[0091] [Fabrication of Magnetic Recording Medium Substrate] (1) Fabrication of Substrate Blank Next, a disc-shaped substrate blank was fabricated by method A or B below. A glass blank for fabricating a glass spacer for a magnetic recording and playback device can also be obtained by the same method. (Method A) The clarified and homogenized molten glass of the above embodiment was flowed out of the outflow pipe at a constant flow rate and received in a lower die for press molding. The flowed molten glass was cut with a cutting blade so that a predetermined amount of molten glass lumps were obtained on the lower die. The lower die with the molten glass lumps was then immediately removed from the bottom of the pipe and press-molded into a thin-walled disc shape with a diameter of 66 mm and a thickness of 1.2 mm using an upper die and a body die facing the lower die. After the press-molded product was cooled to a temperature at which it would not deform, it was removed from the mold and annealed to obtain a substrate blank. In the above molding process, multiple lower dies were used to successively mold the flowing molten glass into disc-shaped substrate blanks. (Method B) The clarified and homogenized molten glass of the above embodiment was continuously poured from above into the through-hole of a heat-resistant mold provided with a cylindrical through-hole, formed into a cylindrical shape, and removed from the bottom of the through-hole. After annealing the removed glass, the glass was sliced ​​at regular intervals perpendicular to the cylindrical axis using a multi-wire saw to produce a disc-shaped substrate blank. Although methods A and B above were used in this embodiment, methods C and D below are also suitable as manufacturing methods for disc-shaped substrate blanks. Furthermore, methods C and D below are also suitable as manufacturing methods for glass blanks for producing glass spacers for magnetic recording and playback devices. (Method C) The molten glass of the above embodiment can also be poured onto a float bath and formed into a sheet of glass (forming by the float method), then annealed, and a disc-shaped glass can be cut out from the sheet glass to obtain a substrate blank. (Method D) The molten glass of the above embodiment can also be formed into a sheet of glass by the overflow downdraw method (fusion method), annealed, and then a disc-shaped piece of glass can be cut out from the sheet of glass to obtain a substrate blank.

[0092] (2) Preparation of glass substrates A through hole was drilled in the center of the substrate blank obtained by the above methods, the outer and inner circumferences were ground, and the main surface of the disk was lapped and polished (mirror polished) to finish it as a glass substrate for magnetic disks with a diameter of 65 mm and a thickness of 0.8 mm. Similarly, a glass blank for the production of a glass spacer for a magnetic recording and playback device can be finished into a glass spacer for a magnetic recording and playback device using the same method. The glass substrate obtained above was washed with a 1.7 mass% silicic acid (H2SiF) aqueous solution, then with a 1 mass% potassium hydroxide aqueous solution, then rinsed with pure water and dried. When the surface of the substrate made from the glass of the example was observed under magnification, no surface roughness was observed, and the surface was smooth.

[0093] [Fabrication of Magnetic Recording Medium (Magnetic Disk)] A magnetic disk was obtained by forming an adhesion layer, an underlayer, a magnetic recording layer, a protective layer, and a lubricating layer in that order on the main surface of a glass substrate obtained from the glass of the example using the following method.

[0094] First, using a vacuum deposition apparatus, the adhesion layer, underlayer, and magnetic recording layer were sequentially deposited in an Ar atmosphere using the DC magnetron sputtering method.

[0095] At this time, the attached layer was deposited using a CrTi target to form an amorphous CrTi layer with a thickness of 20 nm. Subsequently, a 10 nm thick layer of CrRu was formed as the underlayer using a single-wafer, stationary opposing deposition apparatus in an Ar atmosphere by DC magnetron sputtering. The magnetic recording layer was deposited using an FePt or CoPt target at a deposition temperature of 400°C to form a 10 nm thick FePt or CoPt layer.

[0096] After the magnetic recording layer was formed, the magnetic disk was moved from the deposition apparatus into a heating furnace for annealing. The temperature inside the heating furnace during annealing was set to a range of 650 to 700°C.

[0097] Next, a 3 nm protective layer made of hydrogenated carbon was formed using a CVD method with ethylene as the material gas. After this, a lubricating layer made of PFPE (perfluoropolyether) was formed by a dip-coating method. The thickness of the lubricating layer was 1 nm. A magnetic disk was obtained through the above manufacturing process. The obtained magnetic disk was mounted in a hard disk drive (flying height: 8 nm) equipped with a DFH mechanism, and a magnetic signal was recorded on the recording area on the main surface of the magnetic disk at a recording density of 20 gigabits per square inch. No collisions between the magnetic head and the magnetic disk surface (crash failures) were observed.

[0098] According to one aspect of the present invention, a magnetic recording medium optimized for high-density recording can be provided.

[0099] Finally, we will summarize each of the aforementioned aspects.

[0100] According to one embodiment, SiO is expressed in mole percent. 2 The content is 45-68%, Al 2 O 3 The content is 5-20%, SiO 2 and Al 2 O 3 Total content (SiO 2 +Al 2 O 3 ) is 60-80%, B 2 O 3 The content of is 0-5%, the content of MgO is 3-28%, the content of CaO is 0-18%, the total content of BaO and SrO (BaO + SrO) is 0-2%, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is 12-30%, the total content of alkali metal oxides (Li 2 O + Na 2 O+K 2 The O) is 3.5 to 15%, contains at least one selected from the group consisting of Sn oxide and Ce oxide, the total content of Sn oxide and Ce oxide is 0.05 to 2.00%, the glass transition temperature is 625°C or higher, the Young's modulus is 83 GPa or higher, the specific gravity is 2.85 or lower, and the average coefficient of linear expansion at 100 to 300°C is 48 × 10⁻⁶. -7A glass for magnetic recording medium substrates, which is an amorphous oxide glass with a temperature of 2°C or higher, is provided.

[0101] Furthermore, according to one embodiment, SiO is expressed in mole percent. 2 The content is 45-68%, Al 2 O 3 The content is 5-20%, SiO 2 and Al 2 O 3 Total content (SiO 2 +Al 2 O 3 ) is 60-80%, B 2 O 3 The content of is 0-5%, the content of MgO is 3-28%, the content of CaO is 0-18%, the total content of BaO and SrO (BaO + SrO) is 0-2%, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is 12-30%, the total content of alkali metal oxides (Li 2 O + Na 2 O+K 2 The O) is 3.5 to 15%, contains at least one selected from the group consisting of Sn oxide and Ce oxide, the total content of Sn oxide and Ce oxide is 0.05 to 2.00%, the glass transition temperature is 625°C or higher, the Young's modulus is 83 GPa or higher, the specific gravity is 2.85 or lower, and the average coefficient of linear expansion at 100 to 300°C is 48 × 10⁻⁶. -7 A glass spacer for a magnetic recording and playback device is provided, which is an amorphous oxide glass with a temperature of 2°C or higher.

[0102] The glass for the magnetic recording medium substrate described above has excellent heat resistance and rigidity, a low specific gravity, a moderate coefficient of thermal expansion, and exhibits excellent glass stability. The same applies to the glass spacer for the magnetic recording and playback device described above.

[0103] In one embodiment, the Li of the oxide glass 2 The O content is 0-8 mol%, and Na 2 The O content is 0 to 10 mol%, and K 2 The oxygen content is 0-5 mol%.

[0104] In one embodiment, the oxide glass contains Sn oxide and Ce oxide.

[0105] In one embodiment, the molar ratio of the total content of MgO and CaO to the total content of alkaline earth metal oxides in the oxide glass {(MgO + CaO) / (MgO + CaO + SrO + BaO)} is 0.75 to 1.00.

[0106] In one embodiment, Li is added to the total alkali metal oxide content of the oxide glass. 2 Molar ratio of O content {Li 2 O / (Li 2 O + Na 2 O+K 2 O)} is between 0.4 and 1.

[0107] In one embodiment, Na is a component of the total alkali metal oxide content of the oxide glass. 2 Molar ratio of O content {Na 2 O / (Li 2 O + Na 2 O+K 2 O)} is between 0.4 and 1.

[0108] In one embodiment, the CaO content of the oxide glass is 2 to 15%.

[0109] According to one embodiment, a magnetic recording medium substrate made of the above-mentioned magnetic recording medium is provided.

[0110] In one embodiment, the magnetic recording medium substrate has a homogeneous surface and internal composition.

[0111] In one embodiment, the magnetic recording medium substrate has an ion exchange layer on part or all of its surface.

[0112] According to one embodiment, a magnetic recording medium having a magnetic recording layer on the magnetic recording medium substrate is provided.

[0113] The embodiments disclosed herein should be considered in all respects as illustrative and not restrictive. The scope of the present invention is indicated by the claims rather than by the foregoing description, and all modifications within the meaning and scope of the claims are intended to be included. For example, by making the compositional adjustments described in the specification to the glass compositions exemplified above, a glass for a magnetic recording medium substrate and a glass spacer for a magnetic recording and reproducing apparatus according to one aspect of the present invention can be produced. Furthermore, it is of course possible to arbitrarily combine two or more of the items described as illustrative or preferred in the specification.

Claims

1. In terms of mol%, the content of SiO 2 is 45 - 68%, the content of Al 2 O 3 is 5 - 20%, the total content of SiO 2 and Al 2 O 3 (SiO 2 + Al 2 O 3 ) is 60 - 80%, the content of B 2 O 3 is 0 - 5%, the content of MgO is 3 - 28%, the content of CaO is 0 - 18%, the total content of BaO and SrO (BaO + SrO) is 0 - 2%, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is 12 - 30%, the total content of alkali metal oxides (Li 2 O + Na 2 O + K 2 O) is 3.5 - 15%, and it contains at least one selected from the group consisting of Sn oxide and Ce oxide, the total content of Sn oxide and Ce oxide is 0.05 - 2.00%, the glass transition temperature is 625 °C or higher, the Young's modulus is 83 GPa or higher, the specific gravity is 2.85 or lower, and the average linear expansion coefficient at 100 - 300 °C is 48×10 -7 / °C or higher. It is an amorphous oxide glass for a magnetic recording medium substrate.

2. The glass for a magnetic recording medium substrate according to claim 1, wherein the content of Li 2 O is 0 - 8 mol%, the content of Na 2 O is 0 - 10 mol%, and the content of K 2 O is 0 - 5 mol%.

3. The glass for a magnetic recording medium substrate according to claim 1 or 2, which contains Sn oxide and Ce oxide.

4. The glass for a magnetic recording medium substrate according to any one of claims 1 - 3, wherein the molar ratio of the total content of MgO and CaO to the total content of alkaline earth metal oxides {(MgO + CaO) / (MgO + CaO + SrO + BaO)} is 0.75 - 1.

00.

5. A magnetic recording medium substrate made of the glass for a magnetic recording medium substrate according to any one of claims 1 - 4.

6. A magnetic recording medium having a magnetic recording layer on the magnetic recording medium substrate according to claim 5.

7. In terms of mol%, the content of SiO 2 is 45 to 68%, the content of Al 2 O 3 is 5 to 20%, the total content of SiO 2 and Al 2 O 3 (SiO 2 + Al 2 O 3 ) is 60 to 80%, the content of B 2 O 3 is 0 to 5%, the content of MgO is 3 to 28%, the content of CaO is 0 to 18%, the total content of BaO and SrO (BaO + SrO) is 0 to 2%, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is 12 to 30%, the total content of alkali metal oxides (Li 2 O + Na 2 O + K 2 O) is 3.5 to 15%, and it contains at least one selected from the group consisting of Sn oxide and Ce oxide, the total content of Sn oxide and Ce oxide is 0.05 to 2.00%, the glass transition temperature is 625 °C or higher, the Young's modulus is 83 GPa or higher, the specific gravity is 2.85 or lower, and the average linear expansion coefficient at 100 to 300 °C is 48×10 -7 / °C or higher, and it is an amorphous oxide glass for a magnetic recording and reproducing device.