Annealing plate, method for producing annealing plate, and method for producing substrate

LAP732AUndetermined Publication Date: 2026-02-20HOYA CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP732
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-03-30
Filing Date
2019-03-28
Publication Date
2026-02-20

AI Technical Summary

Technical Problem

Conventional annealing methods for glass substrates often result in sticking issues during separation, leading to reduced productivity and increased risk of damage, such as cracks or scratches, which affects the quality and yield of glass substrates for magnetic disks.

Method used

A plate material for annealing treatment with through holes on its surface, designed to facilitate easy separation by allowing air flow and preventing sticking, is used to sandwich the glass blank material, with specific surface roughness and hole configurations to enhance separation efficiency.

Benefits of technology

The plate material with through holes effectively prevents sticking and facilitates easy separation of the glass blank material, improving productivity and reducing damage, thereby enhancing the quality and yield of glass substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0001_ABST
    Figure 00000000_0001_ABST
  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

An annealing plate is one of several plates used in the annealing process to anneal a workpiece (a plate) in the form of a hot plate and is stacked to hold the workpiece (a plate) from both sides. An annealing plate includes a pair of main surfaces, at least one of which is in contact with the workpiece (a plate), and one or more through-holes that open in the main surface and pass through the plate.
Need to check novelty before this filing date? Find Prior Art

Description

Annealing treatment plate material, manufacturing method of annealing treatment plate material, and manufacturing method of substrate

[0001] The present invention relates to a plate material for annealing treatment used in annealing a blank material, a method for manufacturing the plate material for annealing treatment, and a method for manufacturing a substrate.

[0002] Nowadays, personal computers, DVD (Digital Versatile Disc) recording devices, and the like are equipped with hard disk drives (HDDs) for data recording. Hard disk drives use a magnetic disk having a magnetic layer provided on a substrate, and magnetically recorded information is recorded on or read from the magnetic layer by a magnetic head slightly levitated above the surface of the magnetic disk. Metal substrates (aluminum substrates) or glass substrates, which are less susceptible to plastic deformation than metal substrates, are preferably used as the substrate for this magnetic disk.

[0003] For example, a magnetic disk glass substrate is produced by subjecting a plate-shaped glass blank to machining, such as grinding and polishing. Before machining, the glass blank may be annealed to remove distortion. A conventional annealing method is known, which involves heat treatment of a laminate consisting of alternately stacked plate materials called setters and glass blanks (see Patent Document 1). This annealing not only removes distortion but also reduces the flatness of the glass blank, improving the surface quality of the glass blank.

[0004] Patent No. 6238282

[0005] In the conventional method described above, after the annealing treatment, the glass blanks are recovered by alternately removing the setter and the glass blank from the laminate. However, when the setter is removed, the glass blank may adhere to the underside of the setter and be removed from the laminate together with the setter. In this case, in order to recover the glass blank, it is necessary to separate (remove) the glass blank from the setter, which reduces work efficiency and reduces the productivity of glass substrates. Furthermore, the glass blank that is lifted while adhering to the underside of the setter may fall and crack, chip, or become scratched. Such damaged glass blanks are unsuitable as raw materials for glass substrates, which may reduce the yield of glass substrates.

[0006] An object of the present invention is to provide a plate material for annealing treatment that can easily separate stacked plate materials for annealing treatment from a blank material, a method for manufacturing such a plate material for annealing treatment, and a method for manufacturing a magnetic disk substrate using such a plate material for annealing treatment.

[0007] One aspect of the present invention is a plate material for annealing treatment, which is used in the annealing treatment of a plate-shaped blank material, and is one of a plurality of plate materials stacked so as to sandwich the blank material from both sides, characterized in that it has a pair of main surfaces, at least one of which is in contact with the blank material, and has one or more through holes that open on the main surface and penetrate the plate material.

[0008] The main surfaces preferably have an arithmetic mean roughness adjusted to allow air to flow between the laminated plate materials and the blank material.

[0009] It is preferable that the sum of the arithmetic mean roughness of the main surface of the plate material and the main surface of the blank material in contact with the main surface is 0.2 μm or more.

[0010] The arithmetic mean roughness of the main surface of the plate material is preferably greater than the arithmetic mean roughness of the main surface of the blank material that is in contact with the main surface.

[0011] The arithmetic mean roughness of the main surface of the plate material is preferably 0.2 to 1.0 μm.

[0012] At least one of the through holes preferably opens to a main surface of the plate material such that an edge of the plate material surrounding the at least one through hole abuts against a main surface of the blank piece.

[0013] It is preferable that the through holes opening in the main surface of the plate material have a circular shape and a diameter of 1 to 6 mm.

[0014] It is preferable that a plurality of the through holes are provided and open in a dispersed manner within the main surface of the plate material.

[0015] When the main surface of the plate is divided into a plurality of regions having equal areas, the plurality of through holes are preferably arranged in equal numbers in each of the regions.

[0016] It is preferable that a position where a circular hole is to be formed is set in the blank material, and that the through hole opens in an area of ​​the main surface of the plate material that contacts the part of the blank material where the position is set.

[0017] It is preferable that the sidewall of the plate surrounding the through hole is chamfered so that the cross-sectional area of ​​the through hole along a direction parallel to the main surface of the plate increases as it approaches the main surface of the plate.

[0018] Another aspect of the present invention is a method for manufacturing a plate material for annealing treatment, which is used for annealing a plate-shaped blank material and is one of a plurality of plate materials stacked so as to sandwich the blank material from both sides, the plate material having a pair of main surfaces, at least one of which is in contact with the blank material, and one or more through holes opening on the main surfaces and penetrating the plate material, the manufacturing method comprising a molding process for molding raw material powder of the plate material filled in a molding die, the molding die having a protrusion protruding from an inner wall surface of the molding die so as to form the through hole in the plate material.

[0019] Another aspect of the present invention is a method for manufacturing a substrate, characterized in that it includes an annealing treatment in which a stack of at least two plate materials, which are the plate materials for annealing treatment or plate materials for annealing treatment manufactured by the method for manufacturing a plate material for annealing treatment, sandwiches a plate-shaped blank material from both sides, is heated, and the blank material is annealed.

[0020] According to the present invention, the stacked plate material to be annealed and the blank material can be easily separated.

[0021] 1 is a perspective view showing an example of a plate material for annealing treatment; FIG. 2 is a cross-sectional view showing the outer shape of the plate material; (a) and (b) are views showing the state in which the plate material has been removed from the stack; (a) to (d) are views explaining the flow of air passing through the through holes; (a) to (c) are views explaining another example of the flow of air passing through the through holes; FIG. 3 is a view showing a jig for loading and unloading the plate material from the stack; FIG. 4 is a view showing a cross-section of the plate material near the through holes; FIG. 5 is a view showing a modified example of the plate material; FIG. 6 is a view showing another modified example of the plate material; and FIG. 7 is a view explaining the annealing treatment performed using the plate material of FIG. 1.

[0022] Hereinafter, a plate material for annealing treatment, a method for manufacturing a plate material for annealing treatment, and a method for manufacturing a magnetic disk substrate according to embodiments of the present invention will be described in detail.

[0023] (Plate material for annealing treatment) The plate material for annealing treatment (hereinafter referred to as plate material) of this embodiment will be described. This embodiment includes various embodiments described below. FIG. 1 shows a plate material 10 of this embodiment. The plate material 10 is one of a plurality of plate materials used in the annealing treatment of a glass blank material, which is an example of a blank material. When performing the annealing treatment, the plate material 10 is stacked so as to sandwich the plate-shaped glass blank material from both sides.

[0024] The sheet 10 has a pair of main surfaces 1a, 1b, at least one of which is in contact with the glass blank. The main surfaces 1a, 1b of the sheet 10 are substantially circular. In this specification, the term "substantially circular" includes a perfect circle and an ellipse, and the outer periphery of the sheet 10 may be formed by an arc with a single radius of curvature or by multiple arcs with different radii of curvature.

[0025] The diameter of the sheet material 10 is, for example, 1.05 to 1.5 times the diameter of the glass blank material. If the diameter of the sheet material 10 is smaller than the diameter of the glass blank material, the outer periphery of the glass blank material laminated on the sheet material 10 may deform along the outer edge of the sheet material 10 during the annealing treatment, and the outer shape of the sheet material 10 may be transferred to the glass blank material 20, resulting in a mark (transfer mark) on the main surface of the glass blank material, which may reduce the flatness of the glass blank material. On the other hand, if the diameter of the sheet material 10 is too large, the number of laminates that can be placed in a heating furnace (described below) during the annealing treatment may be reduced, which may reduce the productivity of the glass blank material. Furthermore, when the glass blank material and the sheet material 10 are laminated, the deviation in their respective centers may increase, causing the center of gravity of the laminate to shift, resulting in poor stability and causing the laminate to tip over or tilt during transport. From this perspective, the diameter of the sheet material 10 is preferably 1.05 to 1.2 times the diameter of the glass blank material 20.

[0026] The main surfaces 1a and 1b of the sheet material 10 are preferably larger than the main surfaces of the glass blank material so that the glass blank material laminated on the sheet material 10 does not protrude from the main surfaces 1a and 1b. This reduces the flatness across the entire glass blank material, reducing the amount of glass blank material to be removed in the grinding and polishing processes, or even eliminating the grinding or polishing processes. This improves the productivity of magnetic disk glass substrates.

[0027] The flatness of the plate material 10 is preferably smaller than that of the glass blank material in order to reduce the flatness of the glass blank material. The flatness of the plate material 10 is, for example, 10 μm or less. The flatness is measured using a flatness measuring device.

[0028] It is preferable that the difference between the thermal expansion coefficient of the material of the sheet material 10 and the thermal expansion coefficient of the material of the glass blank material is close to that of the material of the glass blank material. If the difference in the thermal expansion coefficients of the sheet material 10 and the glass blank material is large, large stresses may be generated in the glass blank material during annealing due to the difference in the amounts of thermal expansion and thermal contraction between the two, and these stresses may remain in the glass blank material after annealing. For this reason, in the temperature range from room temperature to the annealing temperature, it is preferable that the ratio of the thermal expansion coefficient of the sheet material 10 to the thermal expansion coefficient of the glass blank material is 0.9 to 1.1. The thermal expansion coefficient refers to the linear expansion coefficient measured by thermomechanical analysis in accordance with JIS R1618:2002. When the material of the glass blank material 20 is aluminosilicate glass, the thermal expansion coefficient of the sheet material 10 is, for example, 3 to 10 x 10 in the temperature range from 100°C to 300°C. -6 / ℃.

[0029] The thermal conductivity of the material of the plate 10 is preferably greater than the thermal conductivity of the material of the glass blank 20. The high thermal conductivity of the plate 10 allows sufficient heat transfer to the glass blank laminated with the plate 10 during annealing. The thermal conductivity is a value calculated in accordance with JIS R1611:2010. The thermal conductivity of the plate 10 is, for example, 1 to 150 W / m·K at room temperature to 300°C.

[0030] Examples of materials for the plate 10 include metal oxides, metal carbides, metal nitrides, metal borides, and materials containing two or more of these. Specific examples of these materials include alumina (Al2O3), silicon carbide (SiC), silicon nitride (Si3N4), zirconia (ZrO2), sialon (Si3N4·Al2O3), steatite, spinel, cordierite, etc. Among these, alumina (Al2O3) and silicon carbide (SiC) are preferably used.

[0031] The thickness of the plate material 10 is, for example, 1 to 3 mm. A specific example of the thickness of the plate material 10 is 1.5 mm.

[0032] The end face shape of the plate material 10 may be a shape extending linearly so as to be perpendicular to the main surfaces 1a, 1b, or may be a shape in which the end intersecting with the main surfaces 1a, 1b is chamfered. An example of the shape of the chamfered end face is the cross-sectional shape shown in FIG. 2. FIG. 2 is a cross-sectional view showing the shape of the outer periphery of the plate material 10. In the example shown in FIG. 2, the chamfered end has a shape that is convexly curved toward the interior of the plate material 10, and the length L1 of the chamfered end in a direction parallel to the main surfaces 1a, 1b is, for example, 0.2 to 0.4 mm, preferably 0.3 mm. The length L2 of the chamfered end in a direction perpendicular to the main surfaces 1a, 1b (plate thickness direction) is, for example, 0.05 to 0.2 mm, preferably 0.1 mm.

[0033] As shown in FIG. 1 , the sheet material 10 has one or more through holes 2 that open on the main surfaces 1 a, 1 b and penetrate the sheet material 10. Specifically, the through holes 2 open at positions on the main surfaces 1 a, 1 b that allow air to flow into the gap between the laminated sheet material 10 and the glass blank material. By providing such through holes 2 in the sheet material 10, when the sheet material 10 is removed from the laminate 30 (see FIG. 10 ) after annealing, as will be described below, air flows between the sheet material 10 and the glass blank material 20 (see FIG. 10 ), preventing the glass blank material 20 from sticking to the sheet material 10. From this perspective, at least one of the through holes 2 is provided so that an edge of the sheet material 10 surrounding the open end of the at least one through hole 2 abuts against the main surface of the glass blank material 20.

[0034] 3( a) and 3(b) are diagrams showing the state of a plate removed from the stack, where FIG. 3(a) shows the case where a conventional plate 100 is used, and FIG. 3(b) shows the case where the plate 10 of this embodiment is used. The conventional plate 100 does not have a through-hole penetrating the plate 100, and when the plate 100 is lifted from the stack after annealing, as shown in FIG. 3(a), the glass blank 20 sticks to the underside of the plate 100 and is lifted together with the plate 100. This is thought to be because the small gap between the underside of the plate 100 and the upper surface of the glass blank 20 tries to widen due to the weight of the glass blank 20, and the pressure in this gap becomes lower than the ambient pressure (atmospheric pressure). This sticking of the glass blank 20 occurs more noticeably the faster the plate 100 is unloaded in order to increase the efficiency of the work of recovering the glass blank 20. On the other hand, as shown in FIG. 3( b), the sheet material 10 of this embodiment has a through hole 2. This allows air to flow into the gap between the sheet material 10 and the glass blank 20 through the through hole 2 when the sheet material 10 is lifted. Therefore, the glass blank 20 does not stick to the sheet material 10, and only the sheet material 10 is lifted. In the example shown in FIG. 3( b), the through hole 2 is open to the atmosphere. Therefore, when the sheet material 10 is lifted, air above the sheet material 10 can flow downward through the through hole 2. As described above, this embodiment can prevent the glass blank 20 from sticking to the sheet material 10, facilitating separation of the sheet material 10 and the glass blank 20. This allows the glass blank 20 to be efficiently recovered. Furthermore, the glass blank 20 stuck to the sheet material 10 can be prevented from falling.

[0035] Here, the flow of air through the through holes 2 will be described with reference to FIG. 4 . In FIGS. 4( a) to 4(d), the flow of air through the through holes 2 is indicated by arrows using an example of a laminate in which sheets 10A, 10B, and 10C and glass blanks 20A and 20B are alternately stacked on a base 60. Each of the sheets 10A to 10C has two through holes 2. In FIGS. 4( a) to 4(d), the surface roughness of the main surfaces of the glass blanks 20A and 20B is exaggerated. In this specification, surface roughness refers to the arithmetic mean roughness Ra (JIS B0601:2001). A gap exists between the main surfaces of the sheet and the glass blank facing each other, due to the surface roughness of the sheet and the glass blank, and this gap communicates with the through holes 2 of the sheet. Therefore, air can flow between the sheet material 10A and the glass blank material 20A, as shown by the double-headed arrows in Figure 4(a). When the sheet material 10A is lifted, air can flow from above the sheet material 10A through the through-hole 2 into the gap between the sheet material 10A and the glass blank material 20A. At this time, a flow of air is also formed that flows from the side of the glass blank material 20A through the gap between the sheet material 10A and the glass blank material 20A and into the through-hole 2. In this way, when the sheet material 10A is lifted, air flows between the sheet material 10A and the glass blank material 20A, preventing the glass blank material 20A from sticking to the sheet material 10A.

[0036] Furthermore, because the through-hole 2 in the sheet 10B communicates with the gap between the glass blank 20A and the sheet 10B and with the gap between the glass blank 20B and the sheet 10B, air can flow as shown by the double-headed arrows in Fig. 4(b) when the sheet 10A is removed from the stack. Therefore, when the glass blank 20A is lifted, the glass blank 20A can be removed without the glass blank 20B sticking to the glass blank 20A. Furthermore, when the glass blank 20A is removed from the stack, air can flow as shown by the double-headed arrows in Fig. 4(c), which prevents the glass blank 20B from sticking to the sheet 10B when the sheet 10B is lifted.

[0037] Although the through-hole 2 of the sheet 10C communicates with the gap between the glass blank 20B and the sheet 10C, if there is no gap between the sheet 10C and the base 60, no air flow will be formed through the gap and the through-hole 2. Therefore, it is preferable to take measures to allow air to flow between the sheet 10C located at the bottom of the stack and the base 60, as shown in FIGS. 5( a ) to 5( c ). In the example shown in FIG. 5( a ), the main surface of the sheet 10C facing the base 60 has a high surface roughness, and a gap exists between the sheet 10C and the base 60, allowing air to flow as indicated by the double-headed arrow in FIG. 5( a ). Therefore, when the glass blank 20B is lifted, the sheet 10C does not stick to the glass blank 20B, and the glass blank 20B can be removed. In the example shown in FIG. 5( b), the surface of the base 60 has a high surface roughness, and a gap exists between the sheet material 10C and the base 60, allowing air to flow as indicated by the double-headed arrow in FIG. 5( b). Therefore, when the glass blank 20B is lifted, the sheet material 10C does not stick to the glass blank 20B, and the glass blank 20B can be removed. In the example shown in FIG. 5( c), a hollow region S is formed in a portion including the surface of the base 60. The hollow region S communicates with the through-hole 2 of the sheet material 10C and with the space on the outer periphery of the sheet material 10C. Therefore, air can flow as indicated by the double-headed arrow in FIG. 5( c). Therefore, when the glass blank 20B is lifted, the sheet material 10C does not stick to the glass blank 20B, and the glass blank 20B can be removed.

[0038] The air flowing through the gap and through hole 2 described above is not limited to atmospheric air communicating with the gap and through hole 2, but may be air supplied from outside separately from the atmosphere. Such air can be supplied, for example, using a jig 50 (see FIG. 6 ) for loading and unloading the sheet material 10. FIG. 6 is a diagram showing the jig 50 for removing the sheet material 10 and the glass blank material from the stack. The jig 50 is equipped with suction cups 51 and a suction mechanism (not shown), and can transport the sheet material 10 while sucking the main surface of the sheet material 10 against the suction cups 51. The jig 50 also has a supply mechanism (not shown) that supplies air toward the through hole 2. By supplying air from the jig 50 toward the through hole 2, air flows through the through hole 2 between the sheet material 10 and the glass blank material 20 in contact with the sheet material 10. This prevents the glass blank material 20 from sticking to the sheet material 10 when the suctioned sheet material 10 is lifted, facilitating separation of the sheet material 10 and the glass blank material 20.

[0039] According to one embodiment, the sum of the arithmetic mean roughness Ra1 of the main surface of the sheet material 10 and the arithmetic mean roughness Ra2 of the main surface of the glass blank material 20 in contact with the main surface is preferably 0.2 μm or more. When the sum of the arithmetic mean roughnesses is 0.2 μm or more, a sufficient gap is secured between the laminated sheet material 10 and the glass blank material 20, allowing air to flow into the gap between the sheet material 10 and the glass blank material 20 through the through holes 2, thereby suppressing sticking of the glass blank material 20 to the sheet material 10. The arithmetic mean roughness Ra is measured using a stylus-type roughness meter (contact roughness measuring device) using a stylus (contact needle). In this embodiment, and according to another embodiment, it is preferable to satisfy the relationship Ra1 > Ra2. By satisfying this relationship, the effect of suppressing sticking of the glass blank material 20 to the sheet material 10 is enhanced.

[0040] According to one embodiment, the arithmetic mean roughness Ra1 of the main surface of the sheet material 10 is preferably 0.2 to 1.0 μm. If Ra1 is less than 0.2 μm, air is less able to pass between the sheet material 10 and the glass blank material 20, and the glass blank material 20 is more likely to stick to the sheet material 10. This makes it time-consuming to remove the glass blank material 20 from the sheet material 10, which reduces work efficiency. Furthermore, if Ra1 is less than 0.2 μm, the manufacturing cost of the sheet material 10 increases in order to reduce the arithmetic mean roughness. On the other hand, if Ra1 exceeds 1.0 μm, contact between the glass blank material 20 and the sheet material 10 may cause fine particles to detach from the sheet material 10 and generate dust. The fine particles detached from the sheet material may adhere to the surface of the glass blank material 20, contaminating the glass blank material 20 and damaging the surface of the glass blank material 20. Furthermore, when Ra1 exceeds 1.0 μm, particularly when it is 1.3 μm or more, a special process is required to increase the arithmetic mean roughness, which increases the manufacturing cost of the sheet material 10. A preferable arithmetic mean roughness Ra1 of the main surface of the sheet material 10 is, for example, 0.6 μm.

[0041] The arithmetic mean roughness Ra2 of the main surface of the glass blank 20 is, for example, 0.001 to 1.3 μm. A preferred example of the arithmetic mean roughness Ra2 is 0.7 μm.

[0042] According to one embodiment, the through holes 2 opening on the main surfaces 1a and 1b of the sheet material 10 are preferably circular, and the diameter of the through holes 2 is preferably 1 to 6 mm. If the diameter of the through holes 2 exceeds 6 mm, the glass blank material 20 laminated to the sheet material 10 may deform slightly into the through holes 2 during the annealing treatment, transferring the opening shape of the through holes 2 to the glass blank material 20 and leaving marks (transfer marks) on the main surfaces of the glass blank material 20. This may result in a deterioration in the flatness of the glass blank material 20. A glass blank material 20 with such marks is likely to be unsuitable as a raw plate for a magnetic disk glass substrate. Furthermore, if the diameter of the through holes 2 is less than 1 mm, air is less likely to flow between the sheet material 10 and the glass blank material 20, resulting in poor airflow. Therefore, it may take a long time to separate the glass blank material 20 from the sheet material 10, potentially reducing work efficiency. Furthermore, if the diameter of the through holes 2 is less than 1 mm, the manufacturing cost of the through holes 2 increases. The diameter of the through-hole 2 is more preferably 2 to 5 mm.

[0043] According to one embodiment, the glass blank 20 has a position (circular hole formation position) set for forming a circular hole. The circular hole is, for example, a circular hole concentric with the outer periphery of the glass blank 20. In this case, the through hole 2 is preferably provided in a region of the main surfaces 1a, 1b of the sheet material 10 that contacts the portion of the glass blank 20 where the circular hole formation position is set. If the through hole 2 is provided in such a region, even if a transfer mark is left on the glass blank 20, it is removed from the glass blank 20, so there is no influence of the transfer mark on the glass blank 20. The circular hole formation position is set in a portion including the center of the main surface of the glass blank 20.

[0044] According to one embodiment, as shown in FIG. 7 , the sidewall 3 of the plate 10 surrounding the through hole 2 is preferably chamfered so that the cross-sectional area of ​​the through hole 2 along a direction parallel to the main surface 1a or 1b of the plate 10 (the left-right direction in FIG. 7 ) increases toward the main surface 1a or 1b of the plate 10. FIG. 7 is a diagram showing a cross section of the plate 10 near the through hole 2. In the example shown in FIG. 7 , the chamfered portion of the sidewall 3 of the plate 10 has an inclined wall surface 3a inclined with respect to the thickness direction of the plate 10. By chamfering the sidewall 3 of the plate 10 in this manner, when the glass blank 20 deforms during the annealing process so as to leave the above-mentioned transfer mark, the amount of deformation can be reduced, and deterioration of the flatness of the glass blank 20 can be suppressed. Such an inclined wall surface 3a is effective when the through hole 2 is provided in the region of the main surface 1a, 1b of the plate 10 that contacts the portion of the glass blank 20 excluding the circular hole formation position. The angle of inclination of the inclined wall surface 3a with respect to the direction of extension of the wall surface of the side wall 3 excluding the inclined wall surface 3a (the wall surface between the inclined wall surfaces 3a on both sides) is preferably 30 to 60°, for example 45°. The cross-sectional shape of the side wall 3 portion of the chamfered plate material 10 is not limited to a linear shape as shown in Fig. 7, and may be a bent or curved shape that is convex or concave toward the inside of the through hole 2.

[0045] According to one embodiment, it is preferable that a plurality of through holes 2 are provided and are distributed throughout the main surfaces 1a and 1b. This enhances the effect of suppressing adhesion of the glass blank 20 to the sheet material 10. The number of through holes 2 may be, for example, one, two, three, four, five, or more. As shown in FIG. 8 , when the main surfaces 1a and 1b of the sheet material 10 are divided into multiple regions of equal area, it is preferable that the same number of through holes 2 are arranged in each of the multiple regions. For example, it is preferable that one through hole 2 is arranged in each of the multiple regions. FIG. 8 is a diagram showing a modified example of the sheet material 10. In the example shown in FIG. 8 , the main surfaces 1a and 1b of the sheet material 10 are each divided into four regions by two virtual lines (dashed lines) that intersect at right angles at the center of the main surfaces 1a and 1b, and one through hole 2 is arranged in each region. On the other hand, if the number of through holes 2 is large, the possibility of transfer marks occurring on the glass blank 20 increases. For this reason, the preferred number of through holes 2 provided in sheet material 10 is 1 to 4. In this embodiment, as described above, it is also preferred to provide through holes 2 in regions of main surfaces 1a and 1b that contact the portions of glass blank material 20 where the circular hole formation positions are set. It is also preferred to reduce the opening area of ​​each of through holes 2, or to reduce the total opening area of ​​through holes 2.

[0046] The opening shape of the through hole 2 in the plate material 10 is not limited to a substantially circular shape, but may be a polygon, a shape extending in one direction or multiple directions along the extension direction of the plate material 10, or the like. An example of a shape extending in one direction is a shape extending along the circumferential direction of the plate material 10, as shown in FIG. 9 . FIG. 9 is a diagram showing another modified example of the plate material 10. Furthermore, an example of a shape extending in multiple directions is a shape extending in three or more directions (e.g., a Y-shape or a cross shape). Furthermore, the extension direction of the through hole 2 is not limited to a direction parallel to the plate thickness direction, but may be a direction inclined relative to the plate thickness direction. Furthermore, the through hole 2 may extend in a curved or bent manner between both sides of the extension direction of the through hole 2.

[0047] The above-described plate material 10 can also be used for annealing blank materials other than glass blank materials, such as aluminum blank materials.

[0048] (Method for Manufacturing a Sheet Material) Next, a method for manufacturing a sheet material according to this embodiment will be described. This embodiment includes various embodiments described below. The method for manufacturing a sheet material is used in the annealing treatment of a glass blank material and is a method for manufacturing one of multiple sheet materials stacked so as to sandwich a plate-shaped glass blank material from both sides. The sheet material has a pair of main surfaces, at least one of which contacts the glass blank material, and has one or more through holes opening on the main surfaces and penetrating the sheet material. That is, the sheet material is similar to the sheet material 10 described above. This manufacturing method includes a molding process for molding raw material powder for the sheet material filled into a molding die. The molding die has a protrusion protruding from the inner wall surface of the molding die so as to form a through hole in the sheet material. According to this manufacturing method, a sheet material with a through hole can be manufactured by the molding process, and can be manufactured at a lower cost than drilling a raw sheet of sheet material without a through hole to provide a through hole. For example, a sheet material made of the above-mentioned metal compound material is hard, and drilling holes using a tool such as a drill or a laser is costly.

[0049] In the molding process, for example, cold isostatic pressing (CIP) can be used for molding, followed by debinding and sintering. Sintering can be performed by atmospheric sintering, but gas pressure sintering or hot isostatic pressing (HIP) after sintering is preferred for compaction. The above-mentioned plate manufacturing method can also be used to manufacture plate materials used in the annealing of blank materials other than glass blank materials, such as aluminum blank materials.

[0050] (Magnetic Disk Substrate) Next, the magnetic disk substrate of this embodiment will be described. Note that this embodiment is suitable for producing a magnetic disk glass substrate having a nominal size of 2.5 to 3.5 inches (diameter 65 to 95 mm) and a plate thickness of 0.1 to 1.5 mm, preferably a plate thickness of 0.3 to 0.9 mm. The magnetic disk glass substrate is disk-shaped. Note that the magnetic disk glass substrate may also be ring-shaped with a central hole bored out that is concentric with the outer periphery of the magnetic disk glass substrate. A magnetic disk is formed by forming magnetic layers (recording regions) in annular regions on both sides of the magnetic disk glass substrate.

[0051] (Magnetic Disk Blank) A magnetic disk glass blank (hereinafter simply referred to as a glass blank), which is an example of a magnetic disk blank, is a glass plate produced by a press molding process before the grinding process described below. The glass blank is not limited to glass blanks produced by a press molding process, but may also be glass blanks produced using a float process, a fusion process, or the like. The glass blank has a substantially circular shape. The glass blank may also have a circular hole formed by a circular hole forming process described below. Aluminosilicate glass, soda-lime glass, borosilicate glass, or the like can be used as the material for the glass blank. Aluminosilicate glass is particularly suitable because it can be chemically strengthened and allows the production of a magnetic disk glass substrate with excellent main surface flatness and substrate strength.

[0052] (Method for Manufacturing a Magnetic Disk Substrate) Next, a method for manufacturing a magnetic disk substrate according to this embodiment will be described. This embodiment includes various embodiments described below. First, a glass blank is produced by press-molding a molten glass mass, which will be the material for a plate-shaped magnetic disk glass substrate having a pair of main surfaces (press-molding process). Next, a heat treatment is performed to remove distortion from the glass blank (annealing process). After the annealing process, a circular hole is formed in the center of the glass blank to form a ring shape (circular hole forming process). Next, the glass blank is shaped by edge grinding (shaping process). This produces a ring-shaped (annular) glass substrate. Next, the main surfaces are ground using fixed abrasive grains (grinding process), and the flattened glass substrate is edge-polished (edge-polishing process). Next, a first polishing is performed on the main surfaces of the glass substrate (first polishing process). Next, the glass substrate is chemically strengthened as needed (chemical strengthening process). Next, the chemically strengthened glass substrate is second-polished (second polishing process). Through these processes, a magnetic disk glass substrate is obtained. Each process will be described in detail below.

[0053] (a) Press molding process: The molten glass flow is cut by a cutter, and the cut molten glass gob is sandwiched between the press surfaces of a pair of molds and pressed to form a glass blank. In this embodiment, as described below, the leading end of the molten glass flow is dropped onto the upper surface of the lower mold, and then the molten glass flow is cut at a position upstream from the upper mold to form a molten glass gob. This molten glass gob is then pressed downward from above by the upper mold to form a glass blank. After pressing for a predetermined time, the molds are opened and the glass blank is removed.

[0054] (b) Annealing Treatment In the annealing treatment, a laminate formed by stacking a plurality of plate materials so as to sandwich a glass blank material from both sides is heated to anneal the glass blank material. The plate material 10 described above is used as the plate material. Specifically, as shown in FIG. 10, the laminate is formed by alternately stacking plate materials 10 and glass blank materials 20. The number of plate materials 10 is one more than the number of glass blank materials 20 (for example, 10 to 30), and they are arranged in positions including the top and bottom layers of the laminate 30. The annealing treatment is performed by applying a load to the top layer of the laminate 30 and keeping it warm in a heating furnace 40.

[0055] (c) Circular Hole Forming Treatment A circular hole (circular hole) is formed in the glass blank by coring, scribing, or the like, to obtain a disk-shaped glass blank with a circular hole.

[0056] Coring is a method of cutting a glass blank from one main surface using a cylindrical core drill with an open end, thereby removing the circumferential portion of a circular hole and hollowing out the glass at the center (core) to form a through hole. In addition to removing the circumferential portion (inner circle) of the circular hole, the core drill may also be used to cut a circular cutting line (outer circle) that defines the outer contour of the glass blank. The glass blank is then removed from the outer and inner parts of the outer and inner circles to obtain a disk-shaped glass blank.

[0057] Scribing is a method in which a circular cutting line is made on one main surface of a glass blank using a cutter (scriber) made of cemented carbide or diamond particles, and then the glass blank is heated to extend the circular cutting line in the thickness direction of the glass blank and press the inside of the circular cutting line to separate it. Note that a circular cutting line that will define the outline of the hole may be simultaneously formed with a circular cutting line that will define the outer outline of the glass blank. In this case, the circular cutting line that will define the outer outline of the glass blank (outer circle) and the circular cutting line that will define the outline of the hole (inner circle) are formed concentrically. The glass blank is then partially heated, and due to the difference in thermal expansion of the glass blank, the portion of the glass blank outside the outer circle and the portion inside the inner circle are removed, resulting in a disk-shaped glass blank.

[0058] (d) Shape Processing In the shape processing, the outer peripheral edge of the glass blank is chamfered. If a circular hole is formed in the glass blank, the inner peripheral edge of the circular hole is also chamfered.

[0059] (e) Grinding Process: In the grinding process, a double-side grinding machine equipped with a planetary gear mechanism is used to grind the main surfaces of the glass blank. Specifically, both main surfaces of the glass blank are ground while the outer peripheral end face of the glass blank is held in a holding hole provided in a holding member of the double-side grinding machine. The double-side grinding machine has a pair of upper and lower surface plates (upper and lower surface plates), and a glass substrate is sandwiched between the upper and lower surface plates. Either the upper or lower surface plate, or both, can be moved to move the glass blank relative to each other, thereby grinding both main surfaces of the glass blank, thereby adjusting the plate thickness and further improving flatness.

[0060] (f) Edge Polishing In the edge polishing process, the outer edge of the glass substrate obtained by grinding the glass blank is polished to a mirror finish by brush polishing. If a circular hole is formed in the glass substrate, the inner edge of the circular hole is also polished to a mirror finish. In this process, an abrasive slurry containing fine particles such as cerium oxide as free abrasive grains is used.

[0061] (g) First Polishing Process The first polishing process is intended to remove scratches or distortions remaining on the main surfaces when grinding is performed using a fixed abrasive, for example, or to adjust minute surface irregularities (microwaviness, roughness). Specifically, both main surfaces of the glass substrate are polished while the outer peripheral end face of the glass substrate is held in a holding hole provided in a polishing carrier of a double-side polishing machine.

[0062] In the first polishing process, a glass substrate is polished while applying a polishing slurry using a double-sided polishing machine having a configuration similar to that of a double-sided polishing machine used in a grinding process using a fixed abrasive. In the first polishing process, unlike grinding using a fixed abrasive, a polishing slurry containing loose abrasive grains is used instead of the fixed abrasive grains.

[0063] Similar to a double-sided grinding machine, a double-sided polishing machine has a pair of upper and lower surface plates (upper and lower surface plates), and a glass substrate is sandwiched between the upper and lower surface plates. Annular, flat polishing pads (e.g., resin polishers) are attached to the top and bottom surfaces of the lower surface plate. By moving either the upper or lower surface plate, or both, the glass substrate and the surface plates are moved relative to each other, thereby polishing both main surfaces of the glass substrate.

[0064] The glass substrate after the first polishing treatment may be chemically strengthened by immersing it in a chemical strengthening liquid (chemical strengthening treatment). As the chemical strengthening liquid, for example, a mixed molten liquid of potassium nitrate and sodium sulfate can be used.

[0065] (h) Second Polishing (Final Polishing) Process: The second polishing process aims to mirror-polish the main surfaces. A double-sided polishing machine with the same configuration as the double-sided polishing machine used in the first polishing process is also used for the second polishing process. Specifically, the outer peripheral edge of the glass substrate is held in a holding hole provided in a polishing carrier of the double-sided polishing machine, while polishing both main surfaces of the glass substrate. The second polishing process differs from the first polishing process in the type and size of free abrasive particles and the hardness of the resin polisher. Specifically, a polishing solution containing colloidal silica with a particle size of approximately 5 to 100 nm as free abrasive particles is supplied between the polishing pad of the double-sided polishing machine and the main surfaces of the glass substrate, polishing the main surfaces of the glass substrate. The polished glass substrate is then washed with a neutral detergent, pure water, isopropyl alcohol, or the like to obtain a glass substrate for magnetic disks.

[0066] In the method for manufacturing a magnetic-disk glass substrate of this embodiment, the annealing treatment is performed using the plate material 10 having the through-holes 2, so that the plate material 10 and the glass blank material 20 can be easily separated after the annealing treatment, and the glass blank material 20 can be efficiently recovered. This also improves the productivity of magnetic-disk glass substrates. Furthermore, it is possible to prevent the glass blank material 20 from falling when removing the plate material 10 after the annealing treatment. This makes it possible to prevent the glass blank material 20 from becoming unsuitable as a raw material for magnetic-disk glass substrates, and to prevent a decrease in the yield of magnetic-disk glass substrates.

[0067] The above-described method for manufacturing a substrate can also be used to manufacture substrates other than glass substrates for magnetic disks, such as aluminum substrates for magnetic disks.

[0068] Experimental Example: To investigate the effects of the plate material of this embodiment, annealing was performed using plate materials and glass blanks of various specifications. The annealing was performed by assembling stacks of the plate materials and glass blanks of the specifications shown in Tables 1 to 3 below. For each sample, a stack was constructed by alternately arranging 61 plate materials and 60 glass blanks of the same specifications on a base. A 500 g weight was placed on the top plate material, and the stack was annealed in the heating furnace 40 shown in FIG. 10 at 500 to 550°C for 30 to 120 minutes. The plate material and base arranged on the bottom layer were in the form shown in FIG. 5(b).

[0069] The plates used for samples 1 to 25 were made of alumina and had a roughly circular shape with a diameter of 110 mm. The through holes on the main surfaces of the plates were concentric with the outer periphery of the plate and were located inside a circle whose diameter was half the diameter of the plate. The through holes had a cylindrical shape extending in the plate thickness direction. The glass blanks used were made of aluminosilicate glass and had a roughly circular shape with a diameter of 100 mm. The glass blanks used for samples 21 to 23 were produced by the float method, while the glass blanks used for the other samples were produced by a press molding process.

[0070] After the annealing treatment, the number of sticking occurrences, the number of sheets with transfer marks, and the number of contaminated glass blanks were counted as follows: (1) Number of sticking occurrences When the plate materials were loaded and unloaded one by one starting from the top shelf, if the number of times sticking of the glass blank materials occurred out of 60 times was rated A, if it occurred 3 to 10 times, B, and if it occurred 10 or more times, C. A and B were evaluated as having been able to suppress sticking, and C was evaluated as having not been able to suppress sticking. The loading and unloading of the plate materials was carried out in half the time normally required. (2) Number of sheets on which transfer marks occurred The main surfaces on both sides of 60 glass blanks were visually observed, and if the number of sheets on which transfer marks caused by through holes occurred was less than 3 out of 60, it was given an A+, if it was 3 or more but less than 5, it was given an A, if it was 5 or more but less than 10, it was given a B, if it was 10 or more but less than 15, it was given a C, and if it was 15 or more, it was given a D. A+ to C were evaluated as meaning that transfer marks could be suppressed, and D was evaluated as meaning that transfer marks could not be suppressed. (3) Number of contaminated glass blanks The main surfaces and end faces on both sides of 60 glass blanks were observed using a grazing incidence interferometric flatness tester (FT-17 manufactured by Nidek Co., Ltd.). If the number of glass blanks to which particles having a size of 1 to 100 μm that had been emitted from the plate material adhered was less than 5 out of 60, it was rated as A, if it was 5 to 10, it was rated as B, and if it was 10 or more, it was rated as C. A and B were evaluated as indicating that contamination of the glass blanks had been suppressed, and C was evaluated as indicating that contamination of the glass blanks had not been suppressed. The results are shown in Tables 1 to 3.

[0071]

[0072]

[0073]

[0074] A comparison of Samples 6 to 25 with Samples 1 to 5 shows that the plate materials having through holes can suppress sticking. When experiments were conducted under the same conditions except that loading and unloading of the plate materials took approximately twice as long (the time normally required) for Samples 22, 23, and 25, the number of times sticking occurred was evaluated as B, indicating that sticking could be suppressed. On the other hand, when experiments were conducted under the same conditions except that loading and unloading of the plate materials took approximately twice as long for Samples 4 and 5, the number of times sticking occurred was evaluated as C, indicating that sticking could not be suppressed.

[0075] As can be seen from the results of Samples 6 to 10, the fewer the number of through holes and the smaller the diameter of the through holes, the greater the effect of suppressing transfer marks. In particular, when the number of through holes is two or less or when the diameter of the through holes is 6 mm or less, the effect of suppressing transfer marks is particularly great. The same can be seen from the results of Samples 11 to 15 and Samples 16 to 20.

[0076] Furthermore, a comparison of Samples 1 to 3 with Samples 4 and 5 reveals that a small arithmetic mean roughness Ra1 of the main surface of the plate material reduces the number of contaminated glass blanks.

[0077] In samples 9, 14, and 19, the diameter of the plate material was changed to 95 mm, 95 mm, and 90 mm, respectively, and annealing was performed. In each sample, transfer marks caused by the outer edge of the plate material occurred in 15 or more out of 60 samples.

[0078] The above has described in detail the plate material for annealing treatment, the method for manufacturing the plate material for annealing treatment, and the method for manufacturing a substrate of the present invention, but the present invention is not limited to the above-mentioned embodiments, and various improvements and modifications may be made within the scope of the present invention.

[0079] 1a, 1b Main surface 2 Through hole 3 Side wall 3a Inclined wall surface 10, 10A, 10B, 10C Annealing treatment plate material 20, 20a, 20B Glass blank material 30 Laminated body 40 Heating furnace 50 Jig 60 Base

Claims

1. A plate material for annealing treatment, which is used in the annealing treatment of a plate-shaped blank material and is one of multiple plate materials stacked so as to sandwich the blank material from both sides, characterized in that it has a pair of main surfaces, at least one of which is in contact with the blank material, and has one or more through holes that open on the main surface and penetrate the plate material.

2. A plate material for annealing treatment according to claim 1, wherein the main surfaces have an arithmetic mean roughness adjusted to allow air to flow between the laminated plate material and the blank material.

3. A plate material for annealing treatment according to claim 1 or 2, wherein the sum of the arithmetic mean roughness of the main surface of the plate material and the main surface of the blank material in contact with the main surface is 0.2 μm or more.

4. A plate material for annealing treatment according to any one of claims 1 to 3, wherein the arithmetic mean roughness of the main surface of the plate material is greater than the arithmetic mean roughness of the main surface of the blank material in contact with the main surface.

5. A plate material for annealing treatment according to any one of claims 1 to 4, wherein the arithmetic mean roughness of the main surfaces of the plate material is 0.2 to 1.0 μm.

6. A plate material for annealing treatment according to any one of claims 1 to 5, wherein at least one of the through holes opens into a main surface of the plate material so that an edge of the plate material surrounding the at least one through hole abuts against a main surface of the blank material.

7. A plate material for annealing treatment according to any one of claims 1 to 6, wherein the through holes opening on the main surfaces of the plate material are circular and have a diameter of 1 to 6 mm.

8. A plate material for annealing treatment according to any one of claims 1 to 7, wherein a plurality of the through holes are provided and are open in a dispersed manner within the main surface of the plate material.

9. A plate material for annealing treatment according to claim 8, wherein when the main surface of the plate material is divided into a plurality of regions of equal area, the plurality of through holes are arranged in equal numbers in each of the regions.

10. A plate material for annealing treatment according to any one of claims 1 to 9, wherein a position where a circular hole is to be formed is set in the blank material, and the through hole opens in an area of ​​the main surface of the plate material that contacts the part of the blank material where the position is set.

11. A plate material for annealing treatment according to any one of claims 1 to 10, wherein the sidewall of the plate material surrounding the through hole is chamfered so that the cross-sectional area of ​​the through hole along a direction parallel to the main surface of the plate material increases as it approaches the main surface of the plate material.

12. A method for manufacturing one of a plurality of plate materials used in the annealing treatment of a plate-shaped blank, stacked so as to sandwich the blank material from both sides, wherein the plate material has a pair of main surfaces, at least one of which is in contact with the blank material, and has one or more through holes that open on the main surfaces and penetrate the plate material, the manufacturing method comprising a molding process for molding raw material powder of the plate material filled in a molding die, and the molding die having a protrusion that protrudes from the inner wall surface of the molding die so as to form the through hole in the plate material.

13. A method for manufacturing a substrate, comprising an annealing treatment in which at least two annealing treatment plate materials described in any one of claims 1 to 11 or annealing treatment plate materials manufactured by the manufacturing method described in claim 12 are stacked on top of each other with a plate-shaped blank material sandwiched between them, and the stack is heated to anneal the blank material.