Coating composition having high solid content

The high solids coating composition, featuring a polyaspartic acid ester, polyisocyanate, epoxy group-containing silane coupling agent, and polyol, addresses the challenges of weather resistance, corrosion resistance, and VOC reduction, enabling effective application on metal materials with enhanced performance and regulatory compliance.

WO2024202850A1PCT designated stage expired Publication Date: 2024-10-03KANSAI PAINT CO LTD

Patent Information

Application Number
PCT/JP2024/007239
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-19
Filing Date
2024-02-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional high solids coating compositions for metal materials face limitations in achieving excellent weather resistance, corrosion resistance, and coating hardness while also being difficult to handle and having low VOC reduction, which hinders their practical application on construction and industrial machinery.

Method used

A high solids coating composition comprising a polyaspartic acid ester, a polyisocyanate compound, an epoxy group-containing silane coupling agent, and a polyol with specific molecular weight and hydroxyl value ranges, which improves crosslinking density and adhesion to metal surfaces, enhancing weather resistance, corrosion resistance, and coating hardness.

Benefits of technology

The composition achieves excellent weather resistance, corrosion resistance, and coating hardness, allowing for direct application on metal materials while reducing VOC emissions, thus meeting stringent regulatory requirements and improving handling and application efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

This coating composition having a high solid content contains a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D) having a weight-average molecular weight of 250-2300 and a hydroxyl value of 50-800.
Need to check novelty before this filing date? Find Prior Art

Description

High solids coating composition

[0001] The present invention relates to a high-solids coating composition that has excellent weather resistance and corrosion resistance and can be applied directly to metal substrates.

[0002] Conventionally, acrylic lacquer, acrylic urethane paint, amino acrylic resin paint, etc. have been used when painting industrial machinery, buildings, automobiles, structures, furniture (including steel), etc. In particular, when painting construction machinery or industrial machinery such as bulldozers, hydraulic excavators, wheel loaders, etc., acrylic urethane paint containing a hydroxyl group-containing acrylic resin and a polyisocyanate compound is mainly used because of its room temperature drying property, durability, etc. Furthermore, in recent years, from the standpoint of ESG (Environmental, Social, and Corporate Governance), there has been a demand for a reduction in volatile organic compounds (VOCs) in paints due to their impact on the environment, and VOC regulations, including the establishment of legislation, are being strengthened worldwide.

[0003] In one-coat coatings applied directly to metal materials for construction machinery and other applications, paint compositions containing acrylic resins and isocyanate compounds have been used to ensure weather resistance and corrosion resistance, but the paint solids concentration is generally low, and there are limits to the VOC reduction that can be achieved.

[0004] In general, coating compositions containing polyamine compounds and isocyanate compounds have excellent coating film properties such as high corrosion resistance and chemical resistance, but their high reactivity results in a fast curing rate and a short pot life, making them difficult to handle, such as for coating workability. Furthermore, coating compositions containing acrylic resins and isocyanate compounds have low coating film hardness from application to the next day after application. For this reason, they have not been widely used for coating construction machinery, etc.

[0005] Patent Document 1 discloses a high-solids coating composition characterized by using a polyisocyanate composition that uses as raw materials a base polyol containing a low-molecular-weight acrylic polyol or polyester polyol, an aliphatic diisocyanate, and an alicyclic diisocyanate, the content of components with a molecular weight of 700 or less being 20 to 60 mass%, a ratio of weight-average molecular weight to number-average molecular weight being 1.2 to 5.0, and a ratio of viscosity (unit: mPa s) of the polyisocyanate composition at 25°C to the number-average functionality of isocyanate groups being represented by a specific formula.

[0006] However, the high-solids coating composition described in Patent Document 1 is insufficient to satisfy the VOC regulation levels that have been strengthened in recent years, and there are cases in which the coating workability is insufficient.

[0007] Patent Document 2 discloses a polyaspartic acid ester-based coating composition in which the dialkyl fumarate content is significantly reduced as a coating composition for producing a gloss-stable colored top coat.

[0008] However, the coating composition described in Patent Document 2 has insufficient corrosion resistance and weather resistance, and in some cases has insufficient adhesion to metal materials, which is required particularly when applying coating directly to metal materials.

[0009] Japanese Patent Publication No. 2003-128989 Japanese Special Publication No. 2022-521250

[0010] The problem to be solved by the present invention is to provide a high solids coating composition which has excellent weather resistance, corrosion resistance and coating film hardness and can be applied directly to metal substrates.

[0011] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by a high solids coating composition containing a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D) having a weight average molecular weight and a hydroxyl value within a specific range, and have thus completed the present invention.

[0012] That is, the present invention provides: 1. A high solids coating composition containing a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D) having a weight average molecular weight of 250 to 2,300 and a hydroxyl value in the range of 50 to 800.

[0013] 2. A high solids coating composition according to item 1, wherein the polyaspartic acid ester (A) contains a polyaspartic acid ester having a secondary amino group represented by the following formula (1):

[0014]

[0015] (wherein X is an n-valent cyclic or chain aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue having a number average molecular weight of 25 to 5000, and R 1 and R 2 are each independently an organic group inactive to an isocyanate group, and n is an integer of 2 or greater.

[0016] 3. A high solids coating composition according to item 1 or 2, wherein the polyol (D) contains a polyester polyol and / or a polyether polyol.

[0017] 4. The high solids coating composition according to any one of items 1 to 3, having a solids concentration of 70% by mass or more.

[0018] 5. The high solids coating composition according to any one of items 1 to 4, further comprising a pigment.

[0019] 6. The high solids coating composition according to any one of items 1 to 5, wherein the polyisocyanate compound (B) contains a silyl group-containing modified polyisocyanate.

[0020] 7. The high solids coating composition according to item 6, wherein the silyl group-containing modified polyisocyanate is a reaction product of raw materials containing an alkoxysilane (x1) having a primary amino group, a carboxylic acid alkyl ester (x2), and a polyisocyanate (x3).

[0021] 8. The high solids coating composition according to any one of items 1 to 7, further comprising a zeolite.

[0022] 9. The high solids coating composition according to any one of items 1 to 8, which is a high solids coating composition for one-coat application.

[0023] 10. A coating method comprising coating a substrate with the high solids coating composition according to any one of items 1 to 8 above.

[0024] 11. Construction machinery or industrial machinery coated with the high solids coating composition according to any one of items 1 to 8.

[0025] The coating composition of the present invention comprises, as its constituent components, a polyaspartic acid ester, a polyisocyanate compound, an epoxy group-containing silane coupling agent, and a low-molecular-weight, high-hydroxyl value polyol, and therefore has low viscosity, a high VOC reduction effect, and excellent curing properties, and the resulting urea crosslinked coating film has excellent weather resistance and corrosion resistance.

[0026] Furthermore, the improved corrosion resistance of the epoxy group-containing silane coupling agent leads to improved adhesion to metal, making the coating composition of the present invention suitable for direct application to metal substrates. It is presumed that the improved crosslink density of the low-molecular-weight polyol significantly improves the weather resistance, corrosion resistance, and coating hardness of the coating composition.

[0027] Therefore, the coating composition of the present invention has the effect of being able to be directly applied to metal substrates due to its excellent weather resistance, corrosion resistance and coating film hardness, as well as its high metal adhesion.

[0028] In this specification, the term "comprise" is a concept that encompasses "consist essentially of" and "consist only of."

[0029] In this specification, the term "one-coat specification" refers to a paint that can be finished with one coat of paint, and may also be expressed as "one-coat specification."

[0030] The high solids coating composition of the present disclosure (hereinafter sometimes simply referred to as the present coating composition) is a composition containing a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D). It will be described in detail below.

[0031] <Polyaspartic acid ester (A)> As the polyaspartic acid ester, a polyaspartic acid ester having a secondary amino group is preferred from the viewpoints of reactivity and coating workability.

[0032] Specifically, the following formula (1)

[0033]

[0034] (wherein X is an n-valent cyclic or chain aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue having a number average molecular weight of 25 to 5000, and R 1 and R 2 are each independently an organic group inactive to an isocyanate group, and n is an integer of 2 or more.

[0035] In formula (1), X is an n-valent cyclic or chain aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue having a number average molecular weight of 25 to 5,000.

[0036] X is an n-valent group having a number average molecular weight of 25 to 5,000, and the number average molecular weight is preferably 50 to 3,000, and more preferably 100 to 2,000.

[0037] X is an aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue.

[0038] The aliphatic hydrocarbon group may be an alicyclic hydrocarbon group, a chain hydrocarbon group, or a group having both an alicyclic portion and a chain portion.

[0039] The alicyclic hydrocarbon group may have a side chain. The chain hydrocarbon group may be a straight-chain hydrocarbon group or a branched hydrocarbon group.

[0040] X is preferably a divalent aliphatic hydrocarbon group. Examples of the divalent aliphatic hydrocarbon group include alkylene, cycloalkylene, cycloalkylalkylene, alkylcycloalkylene, alkylenebiscycloalkylene, alkylenebis(alkylcycloalkylene), and cycloalkylenebisalkylene.

[0041] Here, alkylene is preferably alkylene having 1 to 8 carbon atoms, cycloalkylene is preferably cycloalkylene having 5 to 6 carbon atoms, alkyl is preferably alkyl having 1 to 8 carbon atoms, and cycloalkyl is preferably cycloalkyl having 5 to 6 carbon atoms.

[0042] The polyoxyalkylene polyamine residue refers to a group obtained by removing two or more terminal, preferably both terminal, primary amino groups from a polyoxyalkylene polyamine. The polyoxyalkylene polyamine residue may have a side chain. The polyoxyalkylene polyamine residue is preferably a polyoxyethylene polyamine residue, a polyoxypropylene polyamine residue, a polyoxybutylene polyamine residue, or a polyoxyethylene polyoxypropylene polyamine residue. The polyoxyalkylene polyamine residue is more preferably a -(CH(CH 3 )-CH 2 —O)x—CH 2 -CH(CH 3 ) - (where x is an integer from 3 to 6).

[0043] In formula (1), R 1 and R 2 R is each independently an organic group that is inert to an isocyanate group. 1 and R 2 is preferably alkyl having 1 to 15 carbon atoms, more preferably alkyl having 1 to 8 carbon atoms, even more preferably methyl or ethyl, and most preferably ethyl.

[0044] In formula (1), n ​​is an integer of 2 or more. n is preferably an integer of 2 to 6, more preferably an integer of 2 to 4, and most preferably 2.

[0045] Compounds of formula (1) can be synthesized, for example, by reacting an optionally substituted maleic or fumaric acid ester with a polyamine.

[0046] Specific examples of the compound represented by formula (1) include, but are not limited to, tetraethyl N,N'-[methylenebis(cyclohexane-4,1-diyl)]bisaspartate, tetraethyl N,N'-(hexane-1,6-diyl)bisaspartate, tetrabutyl N,N'-(2-methylpentane-1,5-diyl)bisaspartate, tetraethyl N,N'-[methylenebis(3-methylcyclohexane-4,1-diyl)]bisaspartate, tetraethyl N,N and at least one selected from the group consisting of tetraethyl N,N'-(bis-2-propyl)polypropylene glycol 300-O,O'-diylbisaspartate, tetraethyl N,N'-(butane-1,4-diyl)bisaspartate, tetraethyl N,N'-(2,2-dimethylpropane-1,3-diyl)bisaspartate, tetraethyl N,N'-(2,4-dimethylhexane-1,6-diyl)bisaspartate, and mixtures thereof. Among these, tetraethyl N,N'-[methylenebis(cyclohexane-4,1-diyl)]bisaspartate, tetrabutyl N,N'-(2-methylpentane-1,5-diyl)bisaspartate, and tetraethyl N,N'-[methylenebis(3-methylcyclohexane-4,1-diyl)]bisaspartate are preferred.

[0047] Commercially available polyaspartic acid esters (A) include "Desmophen NH1420," "Desmophen NH1423LF," "Desmophen NH 1520," and "Desmophen NH 1220" (all trade names, manufactured by Sumika Bayer Co., Ltd.), "FEISOARTIC F420," "FEISOARTIC F220," and "FEISOARTIC F520" (all trade names, manufactured by Feiyang Chemical Industry Co., Ltd.), and the like.

[0048] <Polyisocyanate Compound (B)> As the polyisocyanate compound, any compound that has been conventionally used in polyurethane production can be used.

[0049] Specific examples of the polyisocyanate compound include aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, aromatic aliphatic polyisocyanate compounds, aromatic polyisocyanate compounds, crude products thereof, and modified products of these polyisocyanate compounds.

[0050] Examples of the modified product include biuret modified products, isocyanurate modified products, and mixtures of two or more of these.

[0051] Among the above, aliphatic polyisocyanate compounds can be preferably used from the viewpoint of high solid content.

[0052] The aliphatic polyisocyanate compound is a compound having a straight chain or a chain containing branched carbon skeleton and having two or more free isocyanate groups in one molecule.

[0053] Specific examples of the aliphatic polyisocyanate compound include ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl)fumarate, bis(2-isocyanatoethyl)carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate.

[0054] Specific examples of modified aliphatic polyisocyanate compounds include biuret-modified HDI and isocyanurate-modified HDI.

[0055] As the aliphatic polyisocyanate compound, from the viewpoints of curability and finished appearance, hexamethylene diisocyanate (HDI) and modified products of HDI can be preferably used.

[0056] Commercially available aliphatic polyisocyanate compounds (B) include, for example, TUL-100 (manufactured by Asahi Kasei Chemicals Corporation), Desmodur N3900 (manufactured by Sumika Covestro Urethanes Co., Ltd.), Desmodur N3600 (manufactured by Sumika Covestro Urethanes Co., Ltd.), Desmodur N3200 (manufactured by Sumika Covestro Urethanes Co., Ltd.), TOLONATE XF-800 (manufactured by Vencolex), and TOLONATE XF-450 (manufactured by Vencolex).

[0057] Specific examples of the alicyclic polyisocyanate compound include isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, and 2,5- and / or 2,6-norbornane diisocyanate.

[0058] Specific examples of the aromatic aliphatic polyisocyanate compound include m- and / or p-xylylene diisocyanate (XDI), α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI), and the like.

[0059] Specific examples of the aromatic polyisocyanate compound include 1,3- and / or 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate (TDI), crude TDI, 2,4'- and / or 4,4'-biphenylmethane diisocyanate (MDI), 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, crude MDI, 1,5-naphthylene diisocyanate, 4,4',4"-triphenylmethane triisocyanate, m- and p-isocyanatophenylsulfonyl isocyanate, and the like.

[0060] Specific examples of modified polyisocyanate compounds other than the above-mentioned aliphatic polyisocyanate compounds include modified polyisocyanate compounds such as modified MDI (urethane-modified MDI, carbodiimide-modified MDI, trihydrocarbyl phosphate-modified MDI), urethane-modified TDI, and isocyanurate-modified IPDI; and mixtures of two or more of these [for example, a mixture of modified MDI and urethane-modified TDI].

[0061] Furthermore, as a modified polyisocyanate compound, a silyl group-containing modified polyisocyanate can be used for the purpose of improving corrosion resistance.

[0062] The silyl group-containing modified polyisocyanate can further improve the corrosion resistance of the resulting coating film without reducing the gloss.

[0063] The silyl group-containing modified polyisocyanate is not particularly limited, and any modified polyisocyanate containing a silyl group can be used without limitation. In particular, a silyl group-containing modified polyisocyanate (X) which is a reaction product of raw materials containing an alkoxysilane (x1) having a primary amino group, a carboxylic acid alkyl ester (x2), and a polyisocyanate (x3) can be preferably used.

[0064] The silyl group-containing modified polyisocyanate (X) is synthesized using a carboxylic acid alkyl ester (x2) as a modifier, and is a modified polyisocyanate that can be stably diluted in an organic solvent and has excellent storage stability.

[0065] Specific examples of compound (x1) include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyl-methyldiethoxysilane, 3-aminopropyl-methyldimethoxysilane, 3-aminopropyl-ethyleneglycoloxymethoxysilane, 4-amino-3,3-dimethylbutyltrimethoxysilane, 4-amino-3,3-dimethylbutyltriethoxysilane, and combinations thereof. 3-Aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane are particularly preferred.

[0066] The carboxylic acid alkyl ester (x2) is preferably a saturated carboxylic acid alkyl ester.

[0067] Specific examples of saturated carboxylic acid alkyl esters include methyl acetate, ethyl acetate, n-propyl acetate, i-propyl acetate, n-butyl acetate, i-butyl acetate, n-pentyl acetate, i-pentyl acetate, cyclohexyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, 1-methylpentyl acetate (also known as sec-hexyl acetate), 2-methoxyethyl acetate, 2-ethoxyethyl acetate, 3-methoxybutyl acetate, 3-ethoxybutyl acetate, methyl propionate, ethyl propionate, n-propyl propionate, i-propyl propionate, n-butyl propionate, i-butyl propionate, n-pentyl propionate, i-pentyl propionate, methyl butyrate, ethyl butyrate, n-propyl butyrate propyl, i-propyl butyrate, n-butyl butyrate, i-butyl butyrate, t-butyl butyrate, methyl valerate, ethyl valerate, methyl octanoate, methyl laurate, methoxypropyl acetate, ethyl 3-ethoxypropionate, butyl glycol acetate, butyl diglycol acetate, methyl isovalerate, ethyl isovalerate, methyl 3,3,5-trimethylhexanoate, methyl isobutyrate, ethyl isobutyrate, i-butyl isobutyrate, n-butyl i-butyrate, t-butyl i-butyrate, methyl 2-ethylhexanoate, methyl pivalate, ethyl 2-hydroxy-2-methylpropionate, methyl neodecanoate, di-i-propyl fumarate, isobornyl acrylate, and combinations thereof.

[0068] Examples of the polyisocyanate (x3) include the polyisocyanate compounds described above as the polyisocyanate compound (B).

[0069] The method for producing the silyl group-containing modified polyisocyanate (X) may be a method of simultaneously reacting an alkoxysilane (x1) having a primary amino group, an alkyl carboxylic acid ester (x2), and a polyisocyanate (x3). However, a preferred method is a method of previously reacting an alkoxysilane (x1) with an alkyl carboxylic acid ester (x2) to obtain an N-position-modified alkoxysilane having a secondary amino group or a secondary amide group, and then reacting this with a polyisocyanate (x3).

[0070] The amount of isocyanate groups in the silyl group-containing modified polyisocyanate is preferably within a range of, for example, 1.0 mmol or more, 2.0 mmol or more, 5.5 mmol or less, or 5.0 mmol or less per gram of nonvolatile content of the modified polyisocyanate from the viewpoints of corrosion resistance, drying property, etc.

[0071] The amount of isocyanate groups in the modified polyisocyanate can be determined, for example, by adding 10 ml of a 0.1 mol / L dibutylamine solution to 0.1 g of a sample to react with the NCO groups, and then titrating the remaining dibutylamine with an aqueous hydrochloric acid solution using bromophenol blue as a titration indicator.

[0072] The polyisocyanate compounds (B) may be used alone or in combination of two or more.

[0073] From the viewpoints of curability and dryness to touch, the ratio of the amino group of the polyaspartic acid ester (A) to the isocyanate group of the polyisocyanate compound (B) is preferably within a range of 0.5 to 2.0 equivalents, particularly 0.8 to 1.5 equivalents, and more particularly 1.0 to 1.3 equivalents of isocyanate group per equivalent of amino group.

[0074] From the viewpoint of corrosion resistance and weather resistance, it is preferable that the polyaspartic acid ester (A) is contained in an amount of 20 to 70 mass %, particularly 30 to 50 mass %, and the polyisocyanate compound (B) is contained in an amount of 30 to 80 mass %, particularly 50 to 70 mass %, based on the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B).

[0075] Furthermore, when a silyl group-containing modified polyisocyanate is contained as the polyisocyanate compound (B), from the viewpoints of corrosion resistance and dryness to touch, the solid content of the silyl group-containing modified polyisocyanate is preferably within the range of 1 to 100 mass%, particularly 5 to 70 mass%, and more particularly 5 to 50 mass%, relative to the total solid content of the polyisocyanate compound (B).

[0076] <Epoxy Group-Containing Silane Coupling Agent (C)> In the present disclosure, the epoxy group-containing silane coupling agent (C) is a component that contributes to improving the adhesion to metal materials, and thereby particularly the corrosion resistance of the coating composition of the present disclosure.

[0077] The epoxy group-containing silane coupling agent (C) is a compound having both an alkoxysilyl group and an epoxy group in the molecule, and specific examples thereof include glycidoxymethyltrimethoxysilane, glycidoxymethyltriethoxysilane, β-glycidoxyethyltrimethoxysilane, β-glycidoxyethyltriethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropyl(methyl)dimethoxysilane, γ-glycidoxypropyl(dimethyl)methoxysilane, γ-glycidoxypropyl(ethyl)dimethoxysilane, (3,4-epoxycyclohexyl)methyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0078] As the epoxy group-containing silane coupling agent (C), γ-glycidoxypropyltrimethoxysilane and γ-glycidoxypropylmethyldiethoxysilane can be preferably used from the viewpoints of corrosion resistance and finished appearance.

[0079] From the viewpoint of the appearance of the coating film, the epoxy equivalent of the epoxy group-containing silane coupling agent (C) is preferably in the range of 100 to 1000 g / eq, particularly 100 to 500 g / eq.

[0080] The epoxy group-containing silane coupling agent (C) may be used alone or in combination of two or more kinds.

[0081] In the coating composition of the present disclosure, from the viewpoints of water resistance and coating film appearance, the amount of the epoxy group-containing silane coupling agent (C) is preferably 0.1 to 50 mass%, particularly 0.5 to 30 mass%, and even more particularly 0.5 to 15 mass%, relative to the total solid content of the polyaspartic acid ester (A) and the polyisocyanate compound (B).

[0082] <Polyol (D)> Specific examples of the polyol (D) include polyester polyols, polyether polyols, acrylic polyols, polyolefin polyols, fluorine polyols, polycarbonate polyols, polyurethane polyols, etc. The polyol (D) may be contained alone or in combination of two or more.

[0083] Among these, as the polyol (D), from the viewpoints of dryness to the touch and weather resistance, polyether polyols and polyether polyols are preferred.

[0084] 1. Polyester Polyol Polyester polyol can be obtained, for example, by subjecting a dibasic acid and a polyhydric alcohol to a condensation reaction.

[0085] Examples of the dibasic acid include succinic acid, adipic acid, dimer acid, maleic anhydride, phthalic anhydride, isophthalic acid, terephthalic acid, 1,4-cyclohexanedicarboxylic acid, and other carboxylic acids.

[0086] Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, trimethylpentanediol, cyclohexanediol, trimethylolpropane, glycerin, pentaerythritol, 2-methylolpropanediol, and ethoxylated trimethylolpropane.

[0087] In addition, polycaprolactones obtained by ring-opening polymerization of lactones such as ε-caprolactone with polyhydric alcohols can also be used as polyester polyols.

[0088] Furthermore, alcohol components other than the above polyhydric alcohols can also be used.

[0089] Specific examples of such an alcohol include monoalcohols such as methanol, ethanol, propyl alcohol, butyl alcohol, stearyl alcohol, and 2-phenoxyethanol; alcohol compounds obtained by reacting a monoepoxy compound such as propylene oxide, butylene oxide, or neodecanoic acid glycidyl ester (commercially available as "Cardura E 10P" (trade name, manufactured by HEXION, a glycidyl ester of synthetic highly branched saturated fatty acid)) with an acid; and esters of glycol and monobasic acid.

[0090] 2. Polyether Polyols Polyether polyols are not particularly limited, but examples thereof include the following (1) to (3).

[0091] (1) Polyether polyols obtained by random or block addition of a single or mixture of alkylene oxides to a single or mixture of polyhydric hydroxy compounds using a catalyst.

[0092] Examples of the catalyst include hydroxides (lithium, sodium, potassium, etc.), strongly basic catalysts (alcoholates, alkylamines, etc.), and composite metal cyanide complexes (metalloporphyrins, zinc hexacyanocobaltate complexes, etc.).

[0093] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, cyclohexene oxide, and styrene oxide.

[0094] (2) Polyether polyols obtained by reacting a polyamine compound with an alkylene oxide.

[0095] Examples of the polyamine compound include ethylenediamines.

[0096] Examples of the alkylene oxide include the same ones as those exemplified in (1).

[0097] (3) Polymer polyols obtained by polymerizing acrylamide or the like using the polyether polyols obtained in (1) or (2) as a medium.

[0098] Examples of the polyvalent hydroxy compound include the following compounds (i) to (vi).

[0099] (i) Diglycerin, ditrimethylolpropane, pentaerythritol, dipentaerythritol, etc.

[0100] (ii) Sugar alcohol compounds such as erythritol, D-threitol, L-arabinitol, ribitol, xylitol, sorbitol, mannitol, galactitol, and rhamnitol.

[0101] (iii) Monosaccharides such as arabinose, ribose, xylose, glucose, mannose, galactose, fructose, sorbose, rhamnose, fucose, and ribonucleotides.

[0102] (iv) Disaccharides such as trehalose, sucrose, maltose, cellobiose, gentiobiose, lactose, and melibiose.

[0103] (v) Trisaccharides such as raffinose, gentianose, and melezitose.

[0104] (vi) Tetrasaccharides such as stachyose.

[0105] 3. Acrylic Polyol The acrylic polyol is not particularly limited, but examples thereof include those obtained by copolymerizing a single or mixture of ethylenically unsaturated bond-containing monomers having a hydroxy group with a single or mixture of other ethylenically unsaturated bond-containing monomers copolymerizable therewith.

[0106] The ethylenically unsaturated bond-containing monomer having a hydroxy group is not particularly limited, but examples thereof include hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate. These may be used alone or in combination of two or more. Among these, hydroxyethyl acrylate or hydroxyethyl methacrylate is preferred.

[0107] Examples of other ethylenically unsaturated bond-containing monomers copolymerizable with the above-mentioned monomers include the following (1) to (6), which may be used alone or in combination of two or more.

[0108] (1) Acrylic acid esters such as methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, benzyl acrylate, and phenyl acrylate.

[0109] (2) Methacrylate esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, benzyl methacrylate, and phenyl methacrylate.

[0110] (3) Unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, and itaconic acid.

[0111] (4) Unsaturated amides such as acrylamide, methacrylamide, N,N-methylenebisacrylamide, diacetone acrylamide, diacetone methacrylamide, maleic acid amide, and maleimide.

[0112] (5) Vinyl monomers such as glycidyl methacrylate, styrene, vinyltoluene, vinyl acetate, acrylonitrile, and dibutyl fumarate.

[0113] (6) Vinyl monomers having a hydrolyzable silyl group, such as vinyltrimethoxysilane, vinylmethyldimethoxysilane, and γ-(meth)acryloxypropyltrimethoxysilane.

[0114] 4. Polyolefin Polyol The polyolefin polyol is not particularly limited, but examples thereof include polybutadiene having two or more hydroxyl groups, hydrogenated polybutadiene, polyisoprene, and hydrogenated polyisoprene.

[0115] 5. Fluorine Polyol In this specification, the term "fluorine polyol" refers to a polyol containing fluorine in the molecule. Specific examples of the fluorine polyol include copolymers of fluoroolefins, cyclovinyl ethers, hydroxyalkyl vinyl ethers, and monocarboxylic acid vinyl esters, as disclosed in JP-A-57-34107 (Reference 1) and JP-A-61-275311 (Reference 2).

[0116] From the viewpoint of ESG, it is preferable not to use fluorine polyol.

[0117] 6. Polycarbonate Polyol The polycarbonate polyol is not particularly limited, but examples thereof include the following (1) to (4).

[0118] (1) Dialkyl carbonates such as dimethyl carbonate; (2) Alkylene carbonates such as ethylene carbonate; (3) Diaryl carbonates such as diphenyl carbonate; (4) Those obtained by condensation polymerization of low molecular weight carbonate compounds such as those listed in (1) to (3) above.

[0119] 7. Polyurethane Polyol The polyurethane polyol is not particularly limited, but can be obtained, for example, by reacting a polyol with an isocyanate component in a conventional manner.

[0120] Examples of the polyol include low molecular weight polyols such as ethylene glycol and propylene glycol, and high molecular weight polyols such as acrylic polyols, polyester polyols, and polyether polyols.

[0121] The hydroxyl value of the polyol (D) is preferably in the range of 50 to 800, particularly 100 to 700, and more particularly 150 to 600, from the viewpoints of drying properties, crosslink density, and weather resistance.

[0122] In the present disclosure, the hydroxyl value can be measured in accordance with JIS K1557.

[0123] From the viewpoints of drying properties, crosslink density, weather resistance, corrosion resistance, and finished appearance, the weight-average molecular weight of the polyol (D) is preferably within the range of 250 to 2300, particularly 250 to 1500, and more particularly 250 to 1000. If the weight-average molecular weight of the polyol (D) exceeds 2300, the corrosion resistance and finished appearance may be impaired.

[0124] In the present disclosure, the "weight average molecular weight" is a value calculated based on the molecular weight of standard polystyrene from a chromatogram measured by gel permeation chromatography in accordance with the method described in JIS K 0124-2011.

[0125] The gel permeation chromatograph used was "HLC8120GPC" (manufactured by Tosoh Corporation). Four columns, "TSKgel G-4000HXL," "TSKgel G-3000HXL," "TSKgel G-2500HXL," and "TSKgel G-2000HXL" (all manufactured by Tosoh Corporation, trade names), were used, and measurements were performed under the following conditions: mobile phase: tetrahydrofuran, measurement temperature: 40°C, flow rate: 1 ml / min, detector: RI.

[0126] In the coating composition of the present disclosure, from the viewpoints of drying property and crosslink density, the amount of polyol (D) is preferably 1 to 20 mass%, particularly 1 to 10 mass%, and further particularly 3 to 10 mass%, based on the total amount of solids of the polyaspartic acid ester (A) and the polyisocyanate compound (B).

[0127] In the coating composition of the present disclosure, the molar ratio of hydroxyl groups in the polyol (D) to the isocyanate groups in the polyisocyanate composition (B) (hydroxyl groups / isocyanate groups) is preferably within the range of 0.5 to 2.0 equivalents, particularly 0.8 to 1.5 equivalents, and more particularly 1.0 to 1.3 equivalents.

[0128] It is believed that the polyol (D) improves the crosslink density, and in particular the weather resistance of the coating film.

[0129] The coating composition of the present disclosure may contain a curing catalyst, if necessary, for the purpose of promoting the reaction between the polyisocyanate compound (B) and the polyol (D). Examples of the curing catalyst include known urethane curing catalysts such as organometallic compounds, tertiary amines, and phosphoric acid compounds.

[0130] Examples of organometallic compounds include tin octylate, dibutyltin di(2-ethylhexanoate), dioctyltin di(2-ethylhexanoate), dioctyltin diacetate, dibutyltin dilaurate, dibutyltin oxide, dioctyltin oxide, dibutyltin fatty acid salts, lead 2-ethylhexanoate, zinc octylate, zinc naphthenate, zinc fatty acids, cobalt naphthenate, calcium octylate, copper naphthenate, and tetra(2-ethylhexyl)titanate.

[0131] The above curing catalysts can be used alone or in combination of two or more. A coloring pigment can be used in the coating composition of the present disclosure to achieve a desired color. Specific examples of coloring pigments include titanium white, zinc molybdate, calcium molybdate, carbon black, graphite, iron black, Prussian blue, ultramarine, cobalt blue, copper phthalocyanine blue, indanthrone blue, yellow lead, synthetic yellow iron oxide, red iron oxide, transparent red iron oxide, bismuth vanadate, titanium yellow, zinc yellow, monoazo yellow, ochre, disazo, isoindolinone yellow, metal complex azo yellow, and quinophthalone. Yellow, benzimidazolone yellow, monoazo red, unsubstituted quinacridone red, azo lake (Mn salt), quinacridone magenta, anthanthrone orange, dianthraquinonyl red, perylene maroon, perylene red, diketopyrrolopyrrole chrome vermilion, chlorinated phthalocyanine green, brominated phthalocyanine green, pyrazolone orange, benzimidazolone orange, dioxazine violet, perylene violet, and the like.

[0132] When a color pigment is used in the coating composition of the present disclosure, the amount used is preferably 5 to 100 mass %, particularly 10 to 60 mass %, based on the total amount of solids of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of coating film appearance, weather resistance, and base hiding ability.

[0133] The coating composition of the present disclosure may contain an extender pigment as needed.

[0134] Examples of the extender pigment include clay, silica, barium sulfate, talc, calcium carbonate, white carbon, diatomaceous earth, magnesium carbonate, etc. Among the extender pigments, barium sulfate or calcium carbonate having an average particle size of 0.01 to 5 μm, preferably 0.05 to 4 μm, and more preferably 0.05 to 3 μm, can be suitably used from the viewpoints of reducing the viscosity of the paint, ease of application, and the finished appearance. Commercially available products of such extender pigments include, for example, barium sulfate, such as Varifine BF-20 (manufactured by Sakai Chemical Industry Co., Ltd., trade name, barium sulfate having an average particle size of 0.03 μm), Variace B-33 (manufactured by Sakai Chemical Industry Co., Ltd., trade name, barium sulfate having an average particle size of 0.3 μm), SPARWITE W-5HB (manufactured by Sino-Can, trade name, barium sulfate powder, average particle size: 1.6 μm), and BLANC FIXE MICRO (manufactured by Venator Materials, trade name, barium sulfate having an average particle size of 0.7 μm); and calcium carbonate, such as Neolite SA-200 (manufactured by Takehara Chemical Industry Co., Ltd., trade name, calcium carbonate having an average particle size of 0.08 μm), and MicroPOWDER Examples of suitable calcium carbonate include 3N (trade name, manufactured by Bihoku Funka Kogyo Co., Ltd., calcium carbonate having an average particle size of 1.1 μm) and Sunlight SL1500 (trade name, manufactured by Takehara Chemical Industry Co., Ltd., calcium carbonate having an average particle size of 2.5 μm).

[0135] In this specification, the average particle size is a value obtained by measuring particle size distribution by dynamic light scattering.

[0136] Specifically, this is a value measured using, for example, UPA-EX250 (trade name, particle size distribution analyzer using dynamic light scattering, manufactured by Nikkiso Co., Ltd.) When a body pigment is used in the coating composition of the present disclosure, the amount used is preferably 10 to 200 mass %, particularly 15 to 150 mass %, based on the total solids content of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of finished appearance and coating workability.

[0137] Furthermore, in the coating composition of the present disclosure, the amount of pigments (coloring pigments, extender pigments, and other pigments) used is preferably within the range of 5 to 250 mass %, particularly 20 to 200 mass %, and even more particularly 25 to 150 mass %, based on the total solids content of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of finished appearance and coating workability.

[0138] The coating composition of the present disclosure may further contain zeolite for the purpose of improving the pot life. Zeolite is a general term for crystalline aluminosilicate, and its constituent elements are Al, Si, O, and cations (positive ions), and SiO 4 and AlO 4 A tetrahedral structure formed from (Si 4+ or Al 3+ Zeolite is a compound with a basic structure of a tetrahedron (a tetrahedron formed around a center). These tetrahedrons are connected in a complex and regular pattern, forming one-, two-, or three-dimensional regular pores with diameters roughly the same size as small molecules, with diameters ranging from a few Å to a dozen Å. This is the characteristic of zeolites.

[0139] Cations exist within the pores of zeolites, and the various functions of zeolites are based on these cations. Because only molecules smaller than the diameter of the pores of zeolites can enter, and they can be screened out from larger molecules, some zeolites are called molecular sieves.

[0140] There are two types of zeolite: natural zeolite, which is mainly composed of hydrated aluminosilicate, and Na 2 O.Al 2 O 3 xSiO 2 ・yH 2 There is a synthetic zeolite whose main component is O. Synthetic zeolite, also known as palmitite, is produced by a dry process in which sodium carbonate, silica, alumina, or kaolin are eutecticed together, or by a wet process in which sodium silicate and sodium aluminate are combined to precipitate a gel.

[0141] Both natural and synthetic zeolites have ion exchange capacity, their crystalline structure remains unchanged upon dehydration, and molecular-sized pores are obtained after dehydration, resulting in high adsorption capacity. Furthermore, zeolites obtained by hydrothermal synthesis, where sodium aluminosilicate gel is crystallized and dehydrated to produce pores of a certain size, are generally called molecular sieves. Zeolites generally known as molecular sieves are suitable for use from the viewpoints of pot life and corrosion resistance. Zeolites molded into powder or pellet form are commercially available, and depending on the type of raw zeolite, molecular sieve 3A, molecular sieve 4A, molecular sieve 5A, molecular sieve 13X, etc., are commercially available. The numbers indicate the approximate pore diameter (angstroms), and the capital letters indicate the type of zeolite, with A representing LTA zeolite and X representing FAU zeolite.

[0142] Of the above molecular sieves, molecular sieve 3A, molecular sieve 4A, and molecular sieve 5A are preferred from the viewpoint of finished appearance, with molecular sieve 5A being particularly preferred.

[0143] The effective diameter of the pores in the molecular sieve crystal varies depending on the location and size of the metal cations near the pores. For example, molecular sieve 5A is molecular sieve 4A in which the sodium ions are replaced with calcium ions.

[0144] From the viewpoint of the finished appearance, the pore diameter (effective diameter of the pores) of the zeolite is preferably in the range of 0.50 nm or less, particularly preferably in the range of 0.10 to 0.50 nm, and even more particularly preferably in the range of 0.20 to 0.50 nm. The pore diameter of the zeolite can be measured by a nitrogen gas adsorption method.

[0145] When a zeolite is used in the coating composition of the present disclosure, the amount used is preferably within the range of 0.1 to 30 mass%, particularly 3 to 30 mass%, and more particularly 5 to 20 mass%, based on the total amount of solids of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoints of pot life and finished appearance.

[0146] A rheology control agent can be used in the coating composition of the present disclosure for the purpose of controlling the fluidity of the coating to improve the finished appearance and coating workability.

[0147] Specific examples of the rheology control agent include clay minerals (e.g., metal silicates, montmorillonite), acrylic resins (e.g., those containing a structure consisting of an acrylic acid ester or methacrylic acid ester polymer or oligomer in the molecule), polyolefins (e.g., polyethylene, polypropylene, etc.), amides (higher fatty acid amides, polyamides, oligomers, etc.), polycarboxylic acids (including derivatives having at least two carboxyl groups in the molecule), cellulose (including various derivatives such as nitrocellulose, acetyl cellulose, cellulose ether, etc.), urethanes (polymers, oligomers, etc. containing a urethane structure in the molecule), ureas (polymers, oligomers, etc. containing a urea structure in the molecule), and urethane ureas (polymers, oligomers, etc. containing a urethane structure and a urea structure in the molecule).

[0148] Of the above, from the viewpoint of finished appearance, acrylic resin, urea and urethane urea are preferably used.

[0149] The rheology control agent is a substance different from the crosslinked product of the polyaspartic acid ester (A) and the isocyanate compound (B) and the polyol (D).

[0150] Commercially available rheology control agents include, for example, amide waxes such as Disparlon 6900 (manufactured by Kusumoto Chemicals Co., Ltd.), Disparlon A603 (manufactured by Kusumoto Chemicals Co., Ltd.), and Thixol W300 (Kyoeisha Chemical Co., Ltd.); polyethylene waxes such as Disparlon 4200 (manufactured by Kusumoto Chemicals Co., Ltd.); CAB (cellulose acetate butyrate, manufactured by Eastman Chemical Products Co.), HEC (hydroxyethyl cellulose), hydrophobized HEC, and CMC (carboxymethyl cellulose). cellulose-based rheology control agents such as BYK-410, BYK-411, BYK-420, and BYK-425 (all manufactured by BYK-Chemie Co., Ltd.); polyolefin-based rheology control agents such as Floon SA-345HF (Kyoeisha Chemical Co., Ltd.); and higher fatty acid amide-based rheology control agents such as Floon HR-4AF (Kyoeisha Chemical Co., Ltd.).

[0151] When a rheology control agent is used in the coating composition of the present disclosure, the amount used is preferably within the range of 0.1 to 20 mass%, particularly 0.5 to 15 mass%, and more particularly 0.8 to 10 mass%, based on the total solids content of the polyaspartic acid ester (A) and the polyisocyanate compound (B), from the viewpoint of finished appearance and coating workability. The coating composition of the present disclosure may further contain, as necessary, pigment dispersants, surface conditioners, surfactants, antifoaming agents, resins other than the polyaspartic acid ester (A) (e.g., epoxy resins), curing agents (excluding the polyisocyanate compound (B)), preservatives, antifreeze agents, etc.

[0152] The coating composition of the present disclosure contains a polyisocyanate compound (B) having free isocyanate groups as a constituent component, and therefore undergoes a crosslinking reaction with the base resin polyaspartic acid ester (A) at room temperature, making it a two-component coating composition consisting of a base component containing the polyaspartic acid ester (A) and a curing agent containing the polyisocyanate compound (B). The base component and curing agent are usually mixed immediately before application, and a solvent such as an organic solvent is added as necessary to adjust the viscosity, making it suitable for use.

[0153] In this case, it is generally preferable that the components used as needed are contained in the main agent side. Mixing can be carried out using a mixer such as a disper or a homogenizer.

[0154] The coating composition of the present disclosure is a high-solids coating composition, which can reduce the amount of volatile substances such as VOCs emitted during coating. Specifically, the coating solids (non-volatile content) concentration during coating can be 70% by mass or more, particularly 80% by mass or more.

[0155] In this specification, the concentration of paint solids (non-volatile content) at the time of painting can be determined by weighing 1.0 g of a sample immediately before painting, which has been adjusted to a viscosity suitable for painting under conditions of a temperature of 20°C and a humidity of 60%, into a tin dish, heating it at a temperature of 105°C for 3 hours to remove the volatile components, and calculating the remaining amount as a mass percentage.

[0156] The coating composition of the present disclosure can be applied by a coating method such as, for example, dip coating, brush coating, roll brush coating, spray coating, roll coating, spin coating, dip coating, bar coating, flow coating, electrostatic coating, airless coating, electrodeposition coating, or die coating.

[0157] Examples of substrates include cold-rolled steel sheets, black steel sheets, alloyed galvanized steel sheets, electro-galvanized steel sheets, etc., and construction or industrial machinery made from these materials, such as bulldozers, hydraulic excavators, wheel loaders, etc. These may be subjected to shot blasting, surface conditioning, surface treatment, etc., and may also be subjected to a primer coating, if necessary.

[0158] The coating composition of the present disclosure is a high-solids coating composition that has excellent weather resistance and corrosion resistance and can be applied directly to metal substrates. Therefore, it can be suitably used as a topcoat coating that complies with VOC regulations from an ESG perspective for the above-mentioned substrate applications, particularly as a one-coat topcoat coating that is applied directly to metal substrates.

[0159] The present invention will be described in more detail below with reference to Production Examples, Examples, and Comparative Examples, but the present invention is not limited thereto. In each example, "parts" means parts by mass, and "%" means % by mass.

[0160] Preparation of Coating Compositions Example 1 Preparation of Coating Composition No. 1 Coating composition No. 1 was obtained by the following steps 1 and 2.

[0161] Step 1: 49.5 parts (solids) of aspartic acid ester resin (A-1), 5.5 parts (solids) of polyol compound (D-1), 18 parts of Variace B-33 (Note 1), 8 parts of Typec CR-95 (Note 2), 1 part of Carbon MA-100 (Note 3), 3 parts of BYK-161 (Note 4), 2 parts of TINUVIN 400 (Note 5), 2 parts of TINUVIN 123 (Note 6), 0.01 parts of BYK-052N (Note 7), and 0.05 parts of BYK-300 (Note 8) were mixed and stirred, and the solids concentration was adjusted with a solvent to obtain a base material for coating composition No. 1 with a solids content of 80% by mass.

[0162] In the above, the extender pigment and color pigment were added and mixed as a pigment dispersion paste prepared using 20 parts of the aspartic acid ester resin (A-1).

[0163] Step 2: To the base resin obtained in Step 1 above, 45.1 parts of polyisocyanate compound (D-1) and 7.0 parts of epoxy group-containing silane coupling agent (C-1) were added, and the solids concentration was adjusted with a solvent to obtain coating composition No. 1 with a solids content of 80% by mass.

[0164] Examples 2 to 26 and Comparative Examples 1 to 4: Preparation of Coating Compositions No. 2 to 30 Coating compositions No. 2 to 30 were obtained in the same manner as in Example 1, except for using the formulations shown in Table 1. Coating compositions No. 27 to 30 are comparative examples.

[0165] The raw material compositions (values) in Table 1 are solid content masses.

[0166]

[0167]

[0168]

[0169]

[0170]

[0171] The raw materials in the table are as follows:

[0172] Polyaspartic acid ester compounds (A) Polyaspartic acid ester (A-1): Desmophen NH-1420: Trade name, manufactured by Covestro, polyaspartic acid ester, amine value 201, molecular weight 554.7, viscosity 1000 mPa·s Polyaspartic acid ester (A-2): Desmophen NH-1423LF: Trade name, manufactured by Covestro, polyaspartic acid ester, amine value 230, molecular weight 554.7, viscosity 1500 mPa·s Polyaspartic acid ester (A-3): Desmophen NH-1220: Trade name, manufactured by Covestro, polyaspartic acid ester, amine value 206, molecular weight 460.6, viscosity 100 mPa·s

[0173] Polyisocyanate Compounds (B) Polyisocyanate Compound (B-1): Desmodur N 3900: Trade name, manufactured by Covestro, low viscosity HDI isocyanurate, NCO group content 23.5%, Viscosity at 23°C 700 mPa·s Polyisocyanate Compound (B-2): Desmodur N 3600: Trade name, manufactured by Covestro, HDI isocyanurate, NCO group content 23%, Viscosity at 23°C 1200 mPa·s Polyisocyanate Compound (B-3): Desmodur N 3200: Trade name, manufactured by Covestro, HDI biuret type isocyanate, NCO group content 23%. Viscosity at 23°C: 2500 mPa·s Polyisocyanate compound (B-4): TOLONATE XF-800: trade name, manufactured by VENCOLEX, HDI-modified aliphatic polyisocyanate, NCO group content: 20.1%. Viscosity at 23°C: 900 mPa·s

[0174] Epoxy group-containing silane coupling agent (C) Epoxy group-containing silane coupling agent (C-1): "KBM-403": Trade name, manufactured by Shin-Etsu Chemical Co., Ltd., γ-glycidoxypropyltrimethoxysilane, epoxy equivalent 236, molecular weight 236. Epoxy group-containing silane coupling agent (C-2): "KBE-402": Trade name, manufactured by Shin-Etsu Chemical Co., Ltd., γ-glycidoxypropylmethyldiethoxysilane, epoxy equivalent 248, molecular weight 248. Epoxy group-containing silane coupling agent (C-3): "MP-200": Trade name, manufactured by Momentive Corporation, γ-glycidoxypropyltrimethoxysilane condensate, epoxy equivalent 205.

[0175] Epoxy resin (1): "JER-828": trade name, manufactured by Mitsubishi Chemical Corporation, bisphenol A type liquid epoxy resin, epoxy equivalent 188.

[0176] Polyol Compounds (D) Polyol compound (D-1): "Desmophen XP-2488": trade name, manufactured by Covestro, polyester polyol, hydroxyl value 528, molecular weight 1400. Polyol compound (D-2): "EXCENOL 750ED": trade name, manufactured by AGC, polyester polyol, hydroxyl value 760, molecular weight 300. Polyol compound (D-3): "Joncryl 507": trade name, manufactured by BASF, hydroxyl group-containing acrylic resin, hydroxyl value 140, molecular weight 2200. Polyol compound (D-4): "TA22-981": trade name, manufactured by Resonac Corporation, polyester polyol, hydroxyl value 55, molecular weight 2000. Polyol compound (D-5): "Sannyx GP-3000": trade name, manufactured by Sanyo Chemical Industries, Ltd., polyether polyol, hydroxyl value 56, molecular weight 3000.

[0177] (Note 1) Variace B-33: Sakai Chemical Industry Co., Ltd., trade name, barium sulfate, average particle size 0.3 μm (Note 2) Typec CR-95: Ishihara Sangyo Kaisha, Ltd., trade name, titanium dioxide (Note 3) Carbon MA-100: Mitsubishi Chemical Corporation, trade name, carbon black (Note 4) BYK-161: BYK-Chemie Co., Ltd., trade name, wetting and dispersing agent (Note 5) TINUVIN 400: B.A.S.F., trade name, hydroxyphenyltriazine ultraviolet absorber (Note 6) TINUVIN 123: B.A.S.F. (Note 7) BYK-052N: BYK Corporation, trade name, defoamer, alkyl vinyl ether copolymer (Note 8) BYK-300: BYK Corporation, trade name, silicone surface conditioner (Note 9) Neostan U-100: Nitto Kasei Co., Ltd., trade name, dibutyltin dilaurate, urethane curing catalyst (Note 10) Silyl group-containing modified polyisocyanate X1: 89.5 parts of 3-aminopropyltrimethoxysilane and 0.04 parts of methoquinone were placed in a flask, heated to 80°C, and air was introduced into the liquid to bubble and stir. To this was added 110 parts of di-i-propyl fumarate dropwise over 2 hours, followed by holding at 80°C for 1 hour and then aging at 50°C for 1 week, yielding 199 parts of a mixture containing 95% 3-(N-(1,2-bis(i-propoxycarbonyl)ethyl)amino)propyltrimethoxysilane. Into a separate flask were placed 280 parts of mineral spirits, 224 parts of "Swasol 1000" (naphtha-based solvent, manufactured by Maruzen Petrochemical Co., Ltd., trade name), and 550 parts of "Duranate TSA-100" (hexamethylene diisocyanate-modified isocyanurate polyisocyanate, manufactured by Asahi Kasei Corporation, trade name, isocyanate group content 20.6 wt%), and the mixture was stirred at room temperature. To this was added dropwise 108 parts of a mixture containing 95% 3-(N-(1,2-bis(i-propoxycarbonyl)ethyl)amino)propyltrimethoxysilane over 2 hours, and the mixture was then maintained at 60°C for 1 hour and cooled to room temperature to obtain a silyl group-containing modified polyisocyanate X1 solution with a non-volatile content of 56%. The concentration of isocyanate groups contained in 1 g of this solution was 2.09 mmol / g (3.72 mmol / g in terms of non-volatile content).

[0178] (Note 11) Silyl group-containing modified polyisocyanate X2: 89.5 parts of 3-aminopropyltrimethoxysilane, 0.04 parts of methoquinone, and 4 parts of "Swasol 1000" (naphtha-based solvent, product name, manufactured by Maruzen Petrochemical Co., Ltd.) were placed in a flask, and air was introduced into the liquid while bubbling and stirring. 104 parts of isobornyl acrylate was added dropwise over 2 hours, and the mixture was then maintained at 50°C for 1 hour. This mixture was then further aged at 50°C for 1 week, yielding 198 parts of a mixture containing 3-(N-(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane / 3-aminopropyltrimethoxysilane / 3-(N,N-di(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane in a molar ratio of 74 / 13 / 13. The total amount of (primary amino groups + secondary amino groups) per gram of the mixture was 2.20 mmol. Into a separate flask were placed 273 parts of mineral spirits, 223 parts of "Swasol 1000" (a naphtha-based solvent, manufactured by Maruzen Petrochemical Co., Ltd., trade name), and 500 parts of "Duranate TSA-100," and the mixture was stirred at room temperature. To this mixture, 111 parts of a mixture containing 3-(N-(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane / 3-aminopropyltrimethoxysilane / 3-(N,N-di(2-(isobornyloxycarbonyl)ethyl)amino)propyltrimethoxysilane in a molar ratio of 74 / 13 / 13 was added dropwise over 2 hours, followed by holding at 60°C for 2 hours and cooling to room temperature to obtain a silyl group-containing modified polyisocyanate X2 solution with a nonvolatile content of 55%. The concentration of isocyanate groups per gram of this solution was 1.99 mmol / g (3.62 mmol / g in terms of nonvolatile content).

[0179] (Note 12) Silyl Group-Containing Modified Polyisocyanate X3: 89 parts of methyl acetate (a linear saturated ester) and 179 parts of 3-aminopropyltrimethoxysilane were placed in a flask under a nitrogen atmosphere and stirred at room temperature. 0.58 parts of a 28% methanol solution of sodium methoxide was added as a catalyst, and the mixture was stirred. The temperature was raised to 70°C and aged for one day. The reaction rate of 3-aminopropyltrimethoxysilane was 97%, and methanol was by-produced in an amount roughly equimolar to the reacted 3-aminopropyltrimethoxysilane. Subsequently, 1.1 parts of bis(2-ethylhexyl)phosphoric acid was added as an acidic compound, and the mixture was concentrated under reduced pressure at 50°C to 70°C to remove methanol and remaining methyl acetate. As a result, 222 parts of crude 3-acetamidopropyltrimethoxysilane containing catalyst-derived residue was obtained as an N-acyl-modified intermediate. 62 parts of butyl acetate and 500 parts of "Duranate TSA-100" were placed in a separate flask under a nitrogen atmosphere and stirred at room temperature. To this was added 55 parts of crude 3-acetamidopropyltrimethoxysilane, and the mixture was heated at 110°C for 7 hours to adduct the secondary amide groups with isocyanate groups, yielding a solution of silyl group-containing modified polyisocyanate X3 with a nonvolatile content of 90%. The concentration of isocyanate groups contained in 1 g of this solution was 3.49 mmol / g (3.88 mmol / g in terms of nonvolatile content).

[0180] (Note 13) Molecular sieve 3A: Union Showa Co., Ltd., trade name, sodium calcium amino silicate, pore size 0.25 nm (Note 14) Molecular sieve 5A: Union Showa Co., Ltd., trade name, sodium calcium amino silicate, pore size 0.42 nm (Note 15) Molecular sieve 13X: Union Showa Co., Ltd., trade name, sodium calcium amino silicate, pore size 1.0 nm. The test plates were prepared and the performance evaluation was carried out as follows. The results obtained by the test are shown in Table 1.

[0181] Preparation of Test Plates Each of Coating Compositions No. 1 to 30 was air spray coated (pressure 0.4 MPa) onto shot-blasted general structural rolled steel material SS-400 (size 2.3 × 150 × 300 mm, Ra: 3.9 μm, Ry: 34 μm, Rz: 23 μm) so that the dry film thickness was 80 μm, and after setting at 20°C for 10 minutes, it was heated and dried at 60°C for 30 minutes using an electric hot air dryer, and further aged at 20°C for 168 hours to obtain test plates of each of Coating Compositions No. 1 to 30.

[0182] Performance Evaluation Each of the coating compositions Nos. 1 to 30 and the test panels of each coating composition were subjected to performance tests for the following test items, and performance evaluation was carried out according to the following evaluation criteria. The performance evaluation results are also shown in Table 1.

[0183] (1) Finished appearance The appearance of the coated surface of each test panel was evaluated visually and by gloss value. A: Good smoothness, and a 60-degree gloss value of 80 or more. B: Good smoothness, and a 60-degree gloss value of 70 or more but less than 80. C: Slight deterioration in at least one type of finished appearance selected from sidewalls, undulations, matte marks and chipped areas was observed, or a 60-degree gloss value of 60 or more but less than 70. D: Significant deterioration in at least one type of finished appearance selected from sidewalls, undulations, matte marks and chipped areas was observed, or a 60-degree gloss value of less than 60.

[0184] (2) Pencil Hardness In accordance with JIS K 5600-5-4:1999, each test plate was placed with a pencil lead at an angle of approximately 45° to the test plate surface, and the lead was pressed firmly against the test plate surface without breaking, while being moved forward at a uniform speed for approximately 10 mm. The hardness symbol of the hardest pencil that did not break the coating film was taken as the pencil hardness. The pencil hardness symbols are in accordance with JIS S6006 (2020). A: 2H or more B: H or more and less than 2H C: F or more and less than H D: Less than F

[0185] (3) Touch-drying property Each coating composition was spray-painted onto a tin plate in a constant temperature and humidity chamber at a temperature of 20°C and a humidity of 50% so as to give a dry film thickness of 60 μm, and the touch-drying time until the paint no longer sticks to the finger was measured. A: Drying time less than 20 minutes B: Drying time 20 minutes or more but less than 30 minutes C: Drying time 30 minutes or more but less than 45 minutes D: 45 minutes or more

[0186] (4) Corrosion resistance According to JIS K 5600-7-1, each test coated plate was given a cross cut on the test coated surface reaching the substrate, and was sprayed with a 5% aqueous solution of sodium chloride adjusted to a pH of 7.0 in an atmosphere of 35°C for 168 hours, and then the width of the blister on one side from the cut was evaluated. A: Less than 1.0 mm B: 1.0 mm or more and less than 2.0 mm C: 2.0 mm or more and less than 3.0 mm D: 3.0 mm or more

[0187] (5) Weather Resistance A Super Xenon Weatherometer (trade name, manufactured by Suga Test Instruments Co., Ltd.) specified in JIS B 7754 was used for each test panel. One cycle consisted of 1 hour 42 minutes of irradiation with a xenon arc lamp and 18 minutes of irradiation with the same lamp under rainfall conditions for 2 hours. After a 1,500-hour (750 cycle) repeated test, the 60-degree gloss retention (GR%) and color difference (ΔE) of each countercoated panel (initial coated panel) were measured and evaluated according to the following criteria: A: 60-degree gloss retention (GR%) of 80 or more and color difference (ΔE) of less than 2.0; B: 60-degree gloss retention (GR%) of 70 or more and less than 80, or color difference (ΔE) of 2.0 or more and less than 3.0; C: 60-degree gloss retention (GR%) of 50 or more and less than 70, or color difference (ΔE) of 3.0 or more and less than 5.0. D: 60 degree gloss retention (GR%) is less than 50 or color difference (ΔE) is 5.0 or more.

[0188] (6) Pot Life The pot life of coating compositions Nos. 23 to 26 containing zeolite (molecular sieve) was evaluated in terms of the viscosity increase rate in comparison with coating composition No. 16. When the viscosity of each coating composition was measured using an Iwata Cup (ANEST IWATA Viscosity Cup NK-2), the viscosity increase rate after 1 hour (Iwata Cup viscosity after 1 hour (seconds) / initial Iwata Cup viscosity (seconds)) was 4.0 for No. 16, while it was 1.4 for No. 23, 1.3 for No. 24, 1.1 for No. 25, and 1.2 for No. 26.

Claims

1. A high solids coating composition containing a polyaspartic acid ester (A), a polyisocyanate compound (B), an epoxy group-containing silane coupling agent (C), and a polyol (D) having a weight average molecular weight of 250 to 2,300 and a hydroxyl value in the range of 50 to 800.

2. A high solids coating composition according to claim 1, wherein the polyaspartic acid ester (A) contains a polyaspartic acid ester having a secondary amino group represented by the following formula (1): (In the formula, X is an n-valent cyclic or chain aliphatic hydrocarbon group or a polyoxyalkylene polyamine residue having a number average molecular weight of 25 to 5,000, and R 1 and R 2 are each independently an organic group inactive to an isocyanate group, and n is an integer of 2 or more.

3. A high solids coating composition according to claim 1 or 2, wherein the polyol (D) contains a polyester polyol and / or a polyether polyol.

4. A high solids coating composition according to any one of claims 1 to 3, having a solids concentration of 70 mass% or more.

5. The high solids coating composition according to any one of claims 1 to 4, further comprising a pigment.

6. A high solids coating composition according to any one of claims 1 to 5, wherein the polyisocyanate compound (B) contains a silyl group-containing modified polyisocyanate.

7. The high solids coating composition according to claim 6, wherein the silyl group-containing modified polyisocyanate is a reaction product of raw materials including an alkoxysilane (x1) having a primary amino group, an alkyl carboxylate (x2) and a polyisocyanate (x3).

8. The high solids coating composition according to any one of claims 1 to 7, further comprising zeolite.

9. A high solids coating composition according to any one of claims 1 to 8, which is a high solids coating composition for one-coat application.

10. A coating method comprising coating a substrate with the high solids coating composition according to any one of claims 1 to 8.

11. A construction machine or industrial machine coated with the high solids coating composition according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • High-functional polyisocyanate containing allophanate group and silane group

    JP2011074390A

  • Printing ink, method for producing polyurethane polyurea resin, and printed matter

    JP2017149858A

  • High solid coating composition

    JP7409757B1

  • Modified polyaspartic acid ester and curable resin composition

    WO2016063884A1

  • Polyaspartic coating composition, coating film, and coated article

    WO2018163953A1

Cited By

  • Multi-layer coating

    JP2026133833A

  • Multi-layer coating

    JP7811810B1