High-efficiency method for producing lithium hydroxide from lithium carbonate through process improvement

The method of mixing lithium carbonate with calcium hydroxide, followed by filtration and crystallization, addresses the inefficiencies in lithium hydroxide production by enhancing recovery rates and reducing environmental impacts, achieving efficient and sustainable lithium hydroxide production.

WO2024215014A1PCT designated stage expired Publication Date: 2024-10-17KOREA INSTITUTE OF GEOSCIENCE AND MINERAL RESOURCES

Patent Information

Application Number
PCT/KR2024/004472
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-13
Filing Date
2024-04-05
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Conventional methods for producing lithium hydroxide from lithium carbonate face challenges such as low recovery rates, environmental burdens due to wastewater and waste landfill issues, and inefficiencies in lithium ion separation, particularly with lithium sulfate and chloride processes, and moisture-related losses with calcium carbonate methods.

Method used

A method involving the mixing of lithium carbonate with calcium hydroxide in a slurry, followed by filtration, concentration, and crystallization under controlled temperature and pressure conditions to enhance lithium hydroxide recovery and purity, utilizing a Membrane Captive Deionization process for ion recovery and recycling of wastewater and sludge.

Benefits of technology

This method improves lithium hydroxide recovery rates, reduces calcium ion concentration, recycles waste materials, and minimizes wastewater generation, resulting in a more efficient and environmentally friendly lithium hydroxide production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004472_17102024_PF_FP_ABST
    Figure KR2024004472_17102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing lithium hydroxide (LiOH) with high efficiency from lithium carbonate (Li2CO3) through process improvement, whereby lithium hydroxide can be produced from lithium carbonate with high efficiency in an environmentally friendly manner by improving the final lithium ion concentration and the lithium ion recovery rate and reusing wastes.
Need to check novelty before this filing date? Find Prior Art

Description

High-efficiency method for producing lithium hydroxide from lithium carbonate through process improvement

[0001] The present invention relates to a method for producing lithium hydroxide from lithium carbonate with high efficiency through process improvement.

[0002] Conventionally, methods for converting lithium compounds such as lithium sulfate (Li2SO4), lithium chloride (LiCl), and lithium carbonate (Li2CO3) into lithium hydroxide (LiOH) have been proposed, and the method for converting lithium hydroxide varies depending on the type of lithium compound, and the conversion efficiency and recovery rate also vary accordingly.

[0003] Among the methods for converting lithium sulfate (Li2SO4) into lithium hydroxide (LiOH), a method is being used in which a lithium sulfate (Li2SO4) solution, an intermediate material recovered in the recycling process of spent lithium secondary batteries, is mixed with caustic soda, and the lithium hydroxide solution is recovered by precipitating and separating the byproduct sodium sulfate (Na2SO4) through a soda cooling method. However, the sodium sulfate (Na2SO4) generated as a byproduct has a somewhat high environmental burden due to wastewater treatment or landfill issues.

[0004] In addition, a method of separating lithium hydroxide (LiOH) solution and hydrochloric acid (HCl) solution using lithium chloride (LiCl) as a raw material through a bipolar electrodialysis process by converting lithium chloride (LiCl) into lithium hydroxide (LiOH) has been proposed, but the separation efficiency is somewhat low and there is a burden of maintenance due to the low alkaline resistance of the membrane material, which is a component of the electrodialysis system.

[0005] Therefore, a method of converting lithium carbonate (Li2CO3) into lithium hydroxide (LiOH) is commonly applied.

[0006] In the conventional method of converting lithium carbonate (Li2CO3) to lithium hydroxide (LiOH), calcium carbonate (CaCO3) is discharged in the form of a cake, and since the lithium hydroxide solution content is high due to the moisture content, there is a problem of loss of lithium hydroxide solution if it is not reused.

[0007] The purpose of the present invention is to provide a method for producing lithium hydroxide from lithium carbonate with a high recovery rate.

[0008] Another object of the present invention is to reduce the amount of wastewater generated in the process by recycling sludge generated in the process of producing lithium hydroxide from lithium carbonate.

[0009] Another object of the present invention is to reduce the amount of wastewater generated in the process by recycling steam generated in the process of producing lithium hydroxide from lithium carbonate.

[0010] Another object of the present invention is to provide a manufacturing method for selecting a crystal form of lithium hydroxide by controlling crystallization pressure and temperature conditions.

[0011] In order to solve the above-mentioned conventional problems, the present invention provides a method for producing lithium hydroxide, comprising the steps of: (a) preparing a mixture by adding calcium hydroxide (Ca(OH)2) to a lithium carbonate (Li2CO3) slurry; (b) separating a filtrate from the mixture prepared in step (a); (c) concentrating the filtrate separated in step (b); and (d) crystallizing lithium hydroxide (LiOH) from the filtrate concentrated in step (c).

[0012] In addition, in the step (a), the lithium carbonate slurry is mixed with lithium carbonate (Li2CO3) and an aqueous solution at a high-liquid ratio of 40 to 80 (g / L), and the hydroxide ions (OH) of the mixture in the step (a) - ) and lithium ion (Li +) can be characterized by a molar ratio of 1:1 to 1.5:1.

[0013] In addition, the step (a) may be characterized in that it is performed at 20 to 100°C for 1 hour or more.

[0014] In addition, the method may further include: (b-1) a step of separating the filtrate in step (b) and washing the remaining sludge with water while stirring; (b-2) a step of separating the solution after washing the sludge with water in step (b-1) and producing a concentrated lithium ion aqueous solution through an electric adsorption process; and (b-3) a step of adding the concentrated lithium ion aqueous solution in step (b-2) to the mixture in step (a).

[0015] In addition, the above electric adsorption process may be characterized as an MCDI (Membrance Captive Deionization) process.

[0016] In addition, it may be characterized by repeating the electric adsorption process of step (c-1) above.

[0017] In addition, it can be characterized in that the desalination liquid generated through the above electric adsorption process is used for sludge washing.

[0018] In addition, when a calcium compound is precipitated through the concentration in step (c), the purity of lithium hydroxide (LiOH) can be increased by removing the precipitated calcium compound from the filtrate.

[0019] In addition, when lithium hydroxide and calcium compounds are precipitated through the concentration in step (c), it may be characterized in that the calcium compound is removed from the solution of precipitated lithium hydroxide and calcium compounds and then the lithium hydroxide aqueous solution is added to the mixture in step (a).

[0020] In addition, the crystallization of lithium hydroxide (LiOH) performed in the above step (d) may be characterized in that it is performed by evaporating the filtrate.

[0021] In addition, the crystallization of lithium hydroxide (LiOH) performed in the above step (d) may be characterized as occurring at 20 to 50 mbar and 40°C or lower.

[0022] In addition, the crystallization of lithium hydroxide (LiOH) performed in the above step (d) may be characterized by being performed at 50°C or higher at 20 to 50 mbar.

[0023] In addition, it can be characterized by condensing the vapor generated by the evaporation in the above step (d) and using the condensed solution for sludge water washing.

[0024] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of improving the recovery rate of lithium hydroxide.

[0025] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of reducing the calcium ion concentration of the final product.

[0026] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of recycling waste sludge and waste water produced by the reaction of lithium carbonate and calcium hydroxide.

[0027] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of reducing the amount of wastewater produced in the process by recycling steam generated in the process of producing lithium hydroxide from lithium carbonate.

[0028] Figure 1 is a process diagram showing a method for producing lithium hydroxide from lithium carbonate according to one embodiment of the present invention.

[0029] FIG. 2 is a graph comparing the thermodynamic stability of each lithium hydroxide (LiOH) conversion reaction when lithium carbonate (Li2CO3) according to one embodiment of the present invention reacts with a hydroxide of alkaline earth metal group 2.

[0030] Figure 3 shows the final lithium ion (Li) contained in the filtrate after the reaction of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to the reaction temperature according to one embodiment of the present invention. + ) is a graph showing the concentration distribution.

[0031] Figure 4 shows the high-liquid ratio of lithium carbonate (Li2CO3) slurry and OH of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to one embodiment of the present invention. - / Li + Final lithium ion (Li) contained in the filtrate according to the molar ratio + ) is a graph showing the concentration distribution.

[0032] Figure 5 shows the high-liquid ratio of lithium carbonate (Li2CO3) slurry and the OH ratio of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to one embodiment of the present invention. - / Li + This is a graph showing the recovery rate (%) of lithium hydroxide (LiOH) according to the molar ratio.

[0033] Figure 6 shows the final lithium ion (Li) contained in the filtrate after the reaction of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to the reaction temperature according to one embodiment of the present invention. + ) is a graph showing the concentration distribution (solid-liquid ratio of lithium carbonate (Li2CO3) slurry: 108.4, OH of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) - / Li + Molar ratio: 2).

[0034] Figure 7 is a graph showing the recovery rate of lithium hydroxide (LiOH) after the reaction of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to the reaction temperature according to one embodiment of the present invention (solid-liquid ratio of lithium carbonate (Li2CO3) slurry: 108.4, OH of the mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) - / Li + Molar ratio: 2).

[0035] FIG. 8 shows the final lithium ions (Li) contained in the filtrate after the reaction of the lithium carbonate (Li2CO3) slurry according to the high-liquid ratio when the mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to one embodiment of the present invention is mixed using a homogenizer. + ) is a graph showing the concentration and recovery rate (%).

[0036] FIG. 9 shows the final lithium ions (Li) contained in the filtrate according to the number of repetitions of the hydroxide reaction when a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) was repeatedly added to the separated filtrate after the reaction according to one embodiment of the present invention and mixed and reacted using a homogenizer. + ) is a graph showing the concentration and recovery rate (%) of lithium carbonate (Li2CO3) slurry (solid-liquid ratio: 27, OH of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) - / Li + Molar ratio: 1.2).

[0037] Figure 10 shows a graph of a solution separated after a water washing process of sludge discharged after a hydration reaction of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to one embodiment of the present invention, after repeatedly applying an electrosorption process, and then lithium ions (Li) + ) is a graph showing the separated and concentrated concentration.

[0038] FIG. 11 is a graph showing the XRD pattern of the final product according to the crystallization conditions of the filtrate after the hydration reaction of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to one embodiment of the present invention (solid-liquid ratio of lithium carbonate (Li2CO3) slurry: 60, reaction time: 3 to 8 hours, reaction temperature: 40 to 80°C, pressure conditions: 37 mbar).

[0039] FIG. 12 is a graph showing the XRD pattern of the final product according to the crystallization temperature of the filtrate after the hydroxide reaction of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to another embodiment of the present invention (solid-liquid ratio of lithium carbonate (Li2CO3) slurry: 60, reaction time: 3 hours, reaction temperature 80°C, pressure conditions: 37 mbar).

[0040] FIG. 13 is a graph showing the XRD pattern of the final product according to the crystallization temperature of the filtrate after the hydroxide reaction of a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (Ca(OH)2) according to another embodiment of the present invention (solid-liquid ratio of lithium carbonate (Li2CO3) slurry: 60, reaction time: 8 hours, reaction temperature: 40°C, pressure conditions: 37 mbar).

[0041] Figure 14 shows the lithium ion (Li) contained in the filtrate according to the concentration ratio of the lithium hydroxide (LiOH) solution according to one embodiment of the present invention. + ) is a graph showing the content distribution.

[0042] Figure 15 shows the calcium (Ca) contained in the filtrate according to the concentration ratio of lithium hydroxide (LiOH) solution according to one embodiment of the present invention. 2+ ) is a graph showing the distribution of ion content.

[0043] The purpose of the present invention is to provide a method for producing lithium hydroxide from lithium carbonate with a high recovery rate.

[0044] Another object of the present invention is to reduce the amount of wastewater generated in the process by recycling sludge generated in the process of producing lithium hydroxide from lithium carbonate.

[0045] Another object of the present invention is to reduce the amount of wastewater generated in the process by recycling steam generated in the process of producing lithium hydroxide from lithium carbonate.

[0046] Another object of the present invention is to provide a manufacturing method for selecting a crystal form of lithium hydroxide by controlling crystallization pressure and temperature conditions.

[0047] Before describing the present invention in detail, it should be understood that the terms or words used in this specification should not be interpreted as being unconditionally limited to their usual or dictionary meanings, and that the inventor of the present invention may appropriately define and use the concepts of various terms in order to explain his or her invention in the best possible manner, and further, that these terms or words should be interpreted as meanings and concepts that are consistent with the technical idea of ​​the present invention.

[0048]

[0049] Method for producing lithium hydroxide from lithium carbonate

[0050] The present invention provides a method for producing lithium hydroxide, comprising the steps of: (a) preparing a mixture by adding calcium hydroxide (Ca(OH)2) to a lithium carbonate (Li2CO3) slurry; (b) separating a filtrate from the mixture prepared in step (a); (c) concentrating the filtrate separated in step (b); and (d) crystallizing lithium hydroxide (LiOH) from the filtrate concentrated in step (c).

[0051]

[0052] (a) A step of preparing a mixture by adding calcium hydroxide (Ca(OH)2) to lithium carbonate (Li2CO3) slurry.

[0053] [Chemical Formula 1] Li2CO3+ Ca(OH)2+ H2O → LiOH(aq) + CaCO3

[0054] Lithium hydroxide can be produced by reacting lithium carbonate (Li2CO3) with calcium hydroxide (Ca(OH)2) according to chemical formula 1.

[0055] At this time, it is preferable to use lithium carbonate (Li2CO3) by adding it to an aqueous solution to prepare a lithium carbonate (Li2CO3) slurry. The aqueous solution may be water, distilled water, purified water, etc., but is not limited thereto, and any solution commonly used in the technical field of the present invention may be added.

[0056] A slurry is a suspension of fine solid particles in an aqueous solution, or a mixture of solids and liquids. In other words, when the amount of solids is below the solubility value, it exists in an aqueous solution, and when the amount of solids is above the solubility value, it exists in a powdered state.

[0057] Sludge refers to the precipitate formed when the suspension is separated into solid and liquid after a reaction. In other words, it refers to solid substances such as cake produced during a wet conversion reaction.

[0058] When lithium carbonate is subjected to a hydration reaction in a slurry state, the mixing uniformity increases, thereby improving the reaction speed and reaction efficiency. After the hydration reaction of lithium carbonate (Li2CO3), the filtrate is separated, and the unreacted lithium carbonate contained in the remaining sludge is subjected to additional reaction and washing to recover lithium hydroxide, and the burden of treating calcium carbonate with strong alkaline properties and the amount of wastewater can be reduced.

[0059] In the hydroxide reaction process of lithium carbonate (Li2CO3), alkaline earth metal hydroxides, such as Ca(OH)2, Sr(OH)2, Ba(OH)2, and Ra(OH)2, can be used.

[0060] Among alkaline earth metal hydroxides (e.g., Ca(OH)2, Sr(OH)2, Ba(OH)2, Ra(OH)2), calcium hydroxide (Ca(OH)2) shows the lowest thermodynamic reaction stability, which means that the hydroxide reaction conversion efficiency is low (see Fig. 2). However, since calcium hydroxide (Ca(OH)2) has an economic advantage over other alkaline earth metal hydroxides, a method for producing lithium hydroxide was developed that increases the final lithium ion concentration and lithium ion recovery rate in the process of producing lithium hydroxide by reacting calcium hydroxide (Ca(OH)2) with lithium carbonate.

[0061] In the above step (a), the lithium carbonate (Li2CO3) slurry is prepared by mixing lithium carbonate (Li2CO3) and an aqueous solution at a high-liquid ratio of 40 to 80 (g / L), and in the above step (a), hydroxide ions (OH - ) and lithium ion (Li + ) may have a molar ratio of 1:1 to 1.5:1.

[0062] The above high-liquid ratio range and hydroxide ion (OH - ) and lithium ion (Li + ) The recovery rate of lithium ions is high at 80% or more within the molar ratio range.

[0063] The above step (a) can be performed at 20 to 100°C for 1 hour or more.

[0064] It was confirmed that as the reaction temperature increases during the hydration reaction of lithium carbonate, the final lithium ion concentration and the recovery rate of lithium ions increase, and the time to reach chemical equilibrium decreases. If the step of adding calcium hydroxide (Ca(OH)2) to the lithium carbonate (Li2CO3) slurry and mixing it is performed at less than 20℃, the final lithium ion concentration and the recovery rate of lithium ions decrease, and the time to reach chemical equilibrium increases, and if the step of adding calcium hydroxide (Ca(OH)2) to the lithium carbonate (Li2CO3) slurry and mixing it is performed at more than 100℃, there is a problem that a lot of energy is consumed in the hydration reaction of the lithium carbonate (Li2CO3) slurry. If the mixing time is less than 1 hour, there is a problem that the final lithium ion concentration and the recovery rate are low because the chemical equilibrium is not reached (see Table 1 and Fig. 3).

[0065] The mixture of step (a) can be obtained as a lithium hydroxide solution by stirring. Preferably, the mixture can be stirred at 5000 to 9000 rpm.

[0066] Referring to Table 3 and Table 9 below, when preparing a mixture, a homogenizer of 5000 to 9000 rpm is used to stir at high speed, which has the effect of increasing the lithium ion recovery rate.

[0067]

[0068] (b) A step of separating the filtrate from the prepared mixture.

[0069] In this step (b), the filtrate is separated from the mixture produced through the hydroxide reaction in the step (a) and the sludge is discharged.

[0070] For the above sludge, the method may further include: (b-1) a step of separating the filtrate in step (b) and washing the remaining sludge with water while stirring; (b-2) a step of separating the solution after washing the sludge with water in step (b-1) and producing a concentrated lithium ion aqueous solution through an electric adsorption process; and (b-3) a step of adding the concentrated lithium ion aqueous solution in step (b-2) to the mixture in step (a).

[0071] Through the above step (b-1), the hydration reaction of unreacted lithium carbonate (Li2CO3) can be carried out, and the lithium hydroxide (LiOH) solution attached and adsorbed on the surface of calcium carbonate (CaCO3) due to the moisture content of calcium carbonate (CaCO3) can be separated from calcium carbonate (CaCO3), thereby obtaining a low-concentration lithium hydroxide aqueous solution. Referring to Example 7 below, it can be confirmed that the lithium ion solution obtained through water washing can be recycled for the production of lithium carbonate (Li2CO3) slurry (see Fig. 1).

[0072] The lithium ion concentration of a lithium hydroxide solution obtained by washing sludge using an electrochemical adsorption process can be increased. When the lithium ion concentration of a lithium hydroxide solution obtained by washing sludge using an electrochemical adsorption process is increased and then used as an aqueous solution for subsequent lithium carbonate (Li2CO3) slurry production, the lithium ion recovery rate is significantly higher.

[0073] The above electric adsorption process may be an MCDI (Membrance Captive Deionization) process.

[0074] The MCDI (Membrance Captive Deionization) process is an electrochemical adsorption process that combines anion and cation exchange membranes with carbon-based electrodes, allowing ions to selectively pass through and be adsorbed and desorbed. Using the MCDI (Membrance Captive Deionization) process as an electrochemical adsorption process offers the advantages of high ion recovery rates and ease of regeneration and maintenance.

[0075] The above electric adsorption process can be repeated.

[0076] By repeatedly performing the electric adsorption process, a more concentrated lithium ion aqueous solution can be produced, and the more concentrated lithium ion aqueous solution can be added to the mixture of step (a) to increase the lithium ion recovery rate.

[0077] Additionally, the filtrate generated through the above-described electric adsorption process can be used for sludge washing. Preferably, it can be used for sludge washing in the above-described step (b-1).

[0078] By reusing the filtrate generated during the electric adsorption process by adding it to sludge washing water, the wastewater generated during the process can be reduced, allowing lithium hydroxide to be manufactured in an environmentally friendly manner.

[0079]

[0080] (c) Step of concentrating the separated filtrate

[0081] Step (c) is a process for increasing the concentration of lithium hydroxide in the filtrate separated in step (b), which can be performed by evaporating water from the filtrate. The evaporation can be performed under reduced pressure conditions.

[0082] In the case where a calcium compound is precipitated through the concentration in step (c), the purity of the lithium hydroxide (LiOH) in the filtrate can be increased by removing the precipitated calcium compound from the filtrate. Preferably, the removal of the calcium compound may be by filtering the calcium compound from the filtrate. The calcium compound may be calcium carbonate (CaCO3) or calcium hydroxide (Ca(OH)2).

[0083] If the amount of calcium contained in the concentrate is higher than the solubility through the concentration in step (c), it can be precipitated as calcium carbonate (CaCO3).

[0084] For example, the solubility of calcium carbonate (CaCO3) is about 0.013 g / L at 25°C, but the solubility of lithium hydroxide (LiOH) is about 128 g / L at 20°C. Therefore, it can be seen that the solubility of calcium carbonate (CaCO3) is much lower than that of lithium hydroxide (LiOH) under similar temperature conditions. Therefore, as the filtrate is concentrated, the concentration of calcium carbonate (CaCO3) increases, and the amount of precipitated calcium carbonate (CaCO3) increases. Therefore, by removing the precipitated calcium carbonate, the concentration of lithium hydroxide (LiOH) in the filtrate can be increased, thereby improving the purity of lithium hydroxide (LiOH) (see FIGS. 14 and 15).

[0085] Carbonate ions (CO3) in the residue 2- ) remains, calcium carbonate is precipitated during the concentration process, and carbonate ions (CO3) are present in the filtrate. 2- ) does not exist, the filtrate becomes strongly alkaline, so calcium ions (Ca 2+ ) is a hydroxide ion (OH - ) can react with calcium hydroxide (Ca(OH)2) to be precipitated.

[0086] In addition, when lithium hydroxide and calcium compounds are precipitated through the concentration in step (c), the calcium compound may be removed from the solution of the precipitated lithium hydroxide and calcium compound, and then the lithium hydroxide aqueous solution may be added to the mixture in step (a). Preferably, the removal of the calcium compound may be by filtering the calcium compound from the solution of lithium hydroxide and calcium compound. Water, distilled water, purified water, etc. may be used as the aqueous solution, but is not limited thereto, and a solution commonly used in the technical field of the present invention may be added.

[0087] When the amount of lithium hydroxide contained in the concentrate through the concentration in step (c) is higher than the solubility of lithium hydroxide, not only calcium compounds but also lithium hydroxide (LiOH) may be precipitated together.

[0088] In the process of concentrating the filtrate, if not only calcium compounds but also lithium hydroxide (LiOH) are precipitated, when the precipitated lithium hydroxide (LiOH) and calcium compounds are mixed with an aqueous solution, the calcium compounds exist as solids because their solubility is lower than that of lithium hydroxide (LiOH). Therefore, the calcium compounds existing as solids can be easily filtered.

[0089] By adding the remaining lithium hydroxide aqueous solution after filtering the above calcium compound to the mixture of step (a), the precipitated lithium hydroxide (LiOH) can be effectively reused, thereby increasing the purity of the lithium hydroxide (LiOH) (see Table 13).

[0090]

[0091] (d) A step of crystallizing lithium hydroxide (LiOH) from the separated filtrate.

[0092] In this step (d), lithium hydroxide is crystallized from the concentrated filtrate in step (c). Crystallization refers to forming crystals of a substance in a liquid or solution. The crystallization of lithium hydroxide (LiOH) provided by the present invention can be performed by evaporating the filtrate.

[0093] Figures 11 to 13 show XRD patterns of lithium hydroxide crystallized by evaporating an aqueous solution at a temperature of 40 to 80°C under a reduced pressure condition of 37 mbar.

[0094] At temperatures above 50°C and a pressure of 37 mbar, lithium hydroxide anhydride was observed. Lithium hydroxide anhydride refers to lithium hydroxide that is not bound to water molecules.

[0095] Lithium hydroxide monohydrate was observed at a temperature of 40°C under a reduced pressure of 37 mbar. Lithium hydroxide monohydrate refers to lithium hydroxide combined with one water molecule.

[0096] The solution obtained by condensing the vapor generated by the above evaporation can be used for sludge washing. Preferably, it can be used for sludge washing in the step (b-1).

[0097] By cooling the vapor generated through evaporation and using it in the sludge washing process, the amount of process water and wastewater used in the process can be reduced, allowing lithium hydroxide to be manufactured in an environmentally friendly manner.

[0098]

[0099] Example

[0100] Hereinafter, the present invention will be described in detail with examples to specifically illustrate it. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention should not be construed as being limited to the examples described below. These examples are provided to more fully explain the present invention to those of average skill in the art.

[0101]

[0102] Experimental Example 1: Hydroxylation reaction rate and lithium recovery rate of lithium carbonate according to reaction temperature

[0103] The concentration of lithium ions contained in the filtrate was analyzed according to the reaction temperature in the hydration reaction of lithium carbonate (Li2CO3) using calcium hydroxide (Ca(OH)2) (see Fig. 3).

[0104] First, 54.2 g of lithium carbonate (Li2CO3) powder (purity 98.5%) was mixed with 1 L of distilled water (H2O) and then OH - / Li + 56.07 g of calcium hydroxide (Ca(OH)2) powder (purity 95%) was mixed so that the molar ratio was 1, and the reaction was carried out for 12 hours under stirring conditions of 300 RPM using a mechanical stirrer.

[0105] Second, in order to suppress the loss and concentration change due to vaporization of the solution as the reaction temperature increases during the hydroxide reaction of lithium carbonate (Li2CO3), a reflux reactor equipped with a condenser that can circulate cooling water to condense and recirculate the vaporized solution was used, and the temperature inside the reactor was controlled by supplying heated water according to temperature into the double-jacketed reactor.

[0106]

[0107] Table 1 shows the results of the analysis of the conversion efficiency of lithium carbonate (Li2CO3) hydroxide reaction by reaction temperature.

[0108] Sample Reaction Time (min) 25℃ 40℃ 60℃ 80℃ Analysis Concentration (ppm) Recovery Rate (%) Analysis Concentration (ppm) Recovery Rate (%) Analysis Concentration (ppm) Recovery Rate (%) Analysis Concentration (ppm) Recovery Rate (%) Li2CO3: 54.20g / 1L H2OCa(OH)2: 56.07g(OH - / Li +Molar ratio = 1)300RPM, RefluxInitial23881998169814385463846.2529252.8721271.9754875.310568256.6598859.7776477.4822682.0206660 66.4721872.0832883.0851484.940781877.9820281.8865886.3931892.960834683.2853885.1919291.6940893.8120877 287.5900689.8935493.3955295.2180910890.8925292.2952294.9963096.0240916891.4941493.9957095.4961295.8360914491.2945694.3958895.6963696.1480923492.1944494.2959495.7960695.8720921691.9943894.1960695.8962496.0

[0109]

[0110] As a result of the experiment, it was observed that the reaction equilibrium was reached in about 4 hours at reaction temperatures of 25℃ and 40℃, and as the reaction temperature increased to 80℃, the time to reach equilibrium was confirmed to decrease and be reached within about 1 hour.

[0111] [Formula 1]

[0112]

[0113] The target lithium concentration is a value indicating the lithium content contained in the lithium carbonate added relative to the volume of the solution used in manufacturing the lithium carbonate slurry, and refers to the expected lithium concentration when the hydroxide reaction of lithium carbonate (Li2CO3) proceeds at a conversion rate of 100% according to the chemical formula 1 above.

[0114] [Formula 2]

[0115]

[0116] The recovery rate is a value that represents the lithium content contained in the conversion solution compared to the lithium content contained in the lithium carbonate injected.

[0117] According to Equation 1, the target lithium concentration is 10,030 ppm (mg / L), and when analyzing the recovery rate (%) according to Equation 2, it was observed to reach approximately 92% at 25°C and approximately 96% when the reaction temperature increased to 80°C.

[0118] Therefore, it was confirmed that when the target lithium concentration is approximately 10,000 to 12,000 ppm, as the reaction temperature increases, the time to reach reaction equilibrium decreases and the recovery rate increases.

[0119]

[0120] Experimental Example 2: High-liquid ratio and OH of lithium carbonate (Li2CO3) slurry solution - / Li + Lithium concentration and recovery rate in the filtrate after hydroxide reaction according to the molar ratio

[0121] High-liquid ratio and OH of lithium carbonate (Li2CO3) slurry - / Li + The lithium concentration and recovery rate in the filtrate after hydroxide reaction according to the molar ratio were measured.

[0122] First, for lithium carbonate (Li2CO3) slurry, the solid (lithium carbonate, g) / liquid (H2O, L) ratio is adjusted to the range of 6 to 100, and OH - / Li + Calcium hydroxide (Ca(OH)2) powder was mixed at molar ratios of 1, 1.25, 1.5, and 2, and then stirred at 25°C for 24 hours to carry out a hydration reaction.

[0123] Second, the volume of the slurry solution used in the reaction was fixed at 50 mL, and after preparing lithium carbonate (Li2CO3) slurry, calcium hydroxide (Ca(OH)2) powder was added and the reaction was carried out by stirring at 300 RPM using a magnetic bar.

[0124]

[0125] Table 2 shows OH - / Li +This shows the reaction efficiency according to the high-liquid ratio of lithium carbonate (Li2CO3) slurry when the molar ratio is 1.

[0126] Li2CO3+ Ca(OH)2(OH - / Li + Molar ratio = 1) Lithium carbonate solid-liquid ratio (g / L)Lithium carbonate weight (g)Initial lithium concentration (ppm)Final lithium concentration (ppm)Lithium Recovery Rate (%)Calcium Concentration (ppm)60.31019.575864.83077.888N.D.120.61973.1511812.06581.599N.D.150.752034.1762273.66281.908N.D.180.92058.4682727.91581.893N.D.211.052069.9753180.55081.842N.D.241.22028.3053519.95679.253N.D.271.352039.6414010.90680.273N.D.301.5 2069.7564481.31280.719N.D.4022091.3525999.26681.046ND502.5204 0.8097271.56478.58713.2896032063.4188479.21976.36520.573703.52 078.1099158.93970.70327.2908042078.7679254.02762.50728.448904.52040.1419381.47756.32729.43710052014.7729340.53950.47329.198

[0127]

[0128] Table 3 shows OH - / Li + This shows the reaction efficiency according to the high-liquid ratio of lithium carbonate (Li2CO3) slurry when the molar ratio is 1.25.

[0129] Li2CO3+ Ca(OH)2(OH - / Li +Molar ratio = 1.25) Lithium carbonate solid-liquid ratio (g / L)Lithium carbonate weight (g)Final lithium concentration (ppm)Lithium recovery rate (%)Calcium concentration (ppm)60.31030.67392.824138.058120.61966.75988.56591.629150.752496.34989.930106.234180.93018.80890.62665.626211.053573.27791.94757.082241.24055.68191.31554.315271.354519.11790.44449 .360301.54826.65286.93967.3664026561.84988.64647.538502.58012.66686.59633.4976039516.11185.70429.705703.510634.89682.09731.03180410726.79072.45566.537904.510512.92063.12128.529100510862.49858.69828.907

[0130]

[0131] Table 4 shows OH - / Li + This shows the reaction efficiency according to the high-liquid ratio of lithium carbonate (Li2CO3) slurry when the molar ratio is 1.5.

[0132] Li2CO3+ Ca(OH)2(OH - / Li +Molar ratio = 1.5) Lithium carbonate solid-liquid ratio (g / L)Lithium carbonate weight (g)Final lithium concentration (ppm)Lithium recovery rate (%)Calcium concentration (ppm)60.31002.37590.275151.264120.62023.86891.1363.358150.752462.31988.7043.752180.93008.46090.3163.522211.053582.02692.1723.643241.24045.86691.0943.637271.354747.79795.0214.5 89301.55237.70994.3434.4334027050.71595.2505.943502.58349.26090.2347.88460310014.55390.19314.731703.510426.54280.48818.63380410488.78570.84819.130904.510513.43463.12419.528100510665.89757.63520.079

[0133]

[0134] Table 5 shows OH - / Li + This shows the reaction efficiency according to the high-liquid ratio of lithium carbonate (Li2CO3) slurry when the molar ratio is 2.

[0135] Li2CO3+ Ca(OH)2(OH - / Li +Molar ratio = 2) Lithium carbonate solid-liquid ratio (g / L)Lithium carbonate weight (g)Final lithium concentration (ppm)Lithium recovery rate (%)Calcium concentration (ppm)60.31126.85199.949177.264120.62193.90598.79387.409150.752533.26291.26073.163180.93035.07691.11562.767211.053486.57989.71656.192241.23944.82788.81948.577271.354409.06788.24245 .210301.54864.82787.62741.6734026395.92386.40434.914502.58114.78587.70033.0226039552.67286.03329.999703.510866.40983.88427.53280410962.59074.04829.929904.510970.46465.86828.445100510988.19459.37728.459

[0136]

[0137] The experimental results confirmed that the final lithium ion concentration value contained in the filtrate increased as the solid-liquid ratio of the lithium carbonate (Li2CO3) slurry solution increased (see Fig. 4). In addition, the OH of the lithium carbonate (Li2CO3) slurry solution - / Li + It was confirmed that the final lithium ion concentration value contained in the filtrate increased as the molar ratio increased (see Fig. 4).

[0138] In addition, OH of lithium carbonate (Li2CO3) slurry solution - / Li + It was confirmed that the recovery rate of lithium ions contained in the filtrate increased as the molar ratio increased (see Fig. 5).

[0139] In addition, the high-liquid ratio of lithium carbonate (Li2CO3) slurry solution is 100 g / L, OH - / Li + Under the condition of a molar ratio of 2, the maximum lithium concentration was confirmed to be 10988.194 ppm, and the lithium ion recovery rate was confirmed to be 59.377% (see Table 5).

[0140] Therefore, the high-liquid ratio of lithium carbonate (Li2CO3) slurry solution or the OH of lithium carbonate (Li2CO3) slurry solution - / Li + It was confirmed that it was difficult to increase the maximum lithium concentration to more than about 12,000 ppm even if the molar ratio was increased (see Fig. 4).

[0141] In addition, it was confirmed that the recovery rate of lithium ions contained in the filtrate decreased as the solid-liquid ratio of the lithium carbonate (Li2CO3) slurry solution increased (see Fig. 5).

[0142] In addition, it was confirmed that the recovery rate rapidly decreased when the target concentration was 60 g / L or higher (see Figure 5).

[0143]

[0144] Experimental Example 3: Hydroxylation reaction rate and lithium recovery rate of lithium carbonate according to reaction temperature (target lithium concentration: 20060 ppm)

[0145] The solid-liquid ratio of lithium carbonate (Li2CO3) slurry solution is 108.4 g / L, OH - / Li + The lithium ion concentration and recovery rate of the filtrate after the hydroxide reaction were evaluated according to the reaction temperature (40°C, 60°C, and 80°C) and reaction time (0 to 1440 minutes) at a molar ratio of 2.

[0146]

[0147] Table 6 shows the distribution of lithium and calcium ion concentrations and lithium recovery rates in the filtrate after the hydroxide reaction of lithium carbonate (Li2CO3) when the solid-liquid ratio of the lithium carbonate (Li2CO3) slurry solution is 108.4 g / L and the reaction temperature is 40°C.

[0148] Li2CO3+ Ca(OH)2_Temperature (40℃)Lithium carbonate solid-liquid ratio (g / L)Reaction time (min)Final Lithium concentration (ppm)Lithium recovery rate (%)Calcium concentration (ppm)108.4g / 1L108829.2544.0133.96208940.3544.5732.38409447.8247.1036.96609629.7748.0031.4612010026.1849.9829.471809965.8749.6828.9424010250.0651.1029.9336010234.4851.0232.0348010611.4552.9027.72144010964.2454.6626.37

[0149]

[0150] Table 7 shows the distribution of lithium and calcium ion concentrations and lithium recovery rates in the filtrate after the hydroxide reaction of lithium carbonate when the solid-liquid ratio of lithium carbonate (Li2CO3) slurry solution is 108.4 g / L and the reaction temperature is 60°C.

[0151] Li2CO3+ Ca(OH)2_Temperature (60℃)Lithium carbonate solid-liquid ratio (g / L)Reaction time (min)Final Lithium concentration (ppm)Lithium recovery rate (%)Calcium concentration (ppm)108.4g / 1L108720.6243.4733.30208941.6044.5731.25409315.3146.4431.42609491.6347.3229.121209695.5848.3327.591809867.0149.1928.1724010429.0051.9934.2336010497.6652.3329.5148010637.4053.0327.78144011135.4155.5126.54

[0152]

[0153] Table 8 shows the distribution of lithium and calcium ion concentrations and lithium recovery rates in the filtrate after the hydroxide reaction of lithium carbonate when the solid-liquid ratio of lithium carbonate (Li2CO3) slurry solution is 108.4 g / L and the reaction temperature is 80°C.

[0154] Li2CO3+ Ca(OH)2_Temperature (80℃)Lithium carbonate solid-liquid ratio (g / L)Reaction time (min)Final Lithium concentration (ppm)Lithium recovery rate (%)Calcium concentration (ppm)108.4g / 1L108773.9943.7430.80209138.8145.5627.73409458.6647.1530.05609592.6347.8227.391209767.9548.6927.2518010034.2250.0226.5224010029.3850.0029.7036010234.3851.0227.7948010299.3151.3429.31144010438.1552.0330.65

[0155]

[0156] Experimental results confirmed that equilibrium was reached within 4 hours at temperatures of 40°C, 60°C, and 80°C. Furthermore, the lithium ion concentration reached after the completion of the hydroxide reaction was highest at 60°C, at approximately 11,135 ppm.

[0157] In addition, in order to increase the lithium ion concentration contained in the mixture, OH was added under the condition of a high-liquid ratio of 100 g / L or more of lithium carbonate (Li2CO3) slurry solution. - / Li + When the molar ratio increases to 2 or more, the slurry viscosity is limited, so stirring is not smooth, and the recovery rate is also low at less than 60%. In addition, it was confirmed that the moisture content of the sludge is high during lithium solution separation, so the solution recovery loss is high.

[0158] Therefore, it was confirmed that when the target lithium concentration is about 20,000 ppm, it is difficult to increase the maximum lithium concentration to more than about 12,000 ppm even if the reaction temperature is increased (see Fig. 6).

[0159] In addition, it was confirmed that it was difficult to increase the recovery rate of lithium ions contained in the mixture even if the reaction temperature was increased when the target lithium concentration was approximately 20,000 ppm (see Fig. 7).

[0160]

[0161] Experimental Example 4: Lithium ion (Li) content in filtrate according to the solid-liquid ratio of lithium carbonate (Li2CO3) slurry solution by applying a homogenizer + ) Concentration and recovery rate

[0162] The purpose of this study was to evaluate the conversion reaction efficiency according to the stirring conditions during the hydroxide reaction of lithium carbonate (Li2CO3), and to analyze the lithium ion concentration in the filtrate after the reaction according to the solid-liquid ratio of lithium carbonate (Li2CO3) slurry using a lab scale homogenizer.

[0163] OH as reaction condition - / Li + Under the condition of a molar ratio of 1.2, the solid-liquid ratio of 50 mL of lithium carbonate (Li2CO3) slurry was adjusted to 27 to 108 (g / L), and the stirring speed was maintained at 7000 RPM to carry out the reaction at 25°C for 4 hours.

[0164] And the recovery rate of hydroxide reaction was analyzed through analysis of recovered lithium ion concentration compared to target lithium ion concentration.

[0165]

[0166] Table 9 shows the concentrations of lithium and calcium in the recovered filtrate after the hydroxide reaction of lithium carbonate (Li2CO3) slurry at different solid-liquid ratios using a homogenizer.

[0167] Li2CO3+ Ca(OH)2_Slurry Homogenizer Conditions Lithium carbonate solid-liquid ratio (g / L) Reaction temperature (℃) Stirring speed (RPM) Reaction time (hr) Final lithium concentration (ppm) Target lithium concentration (ppm) Lithium recovery rate (%) Calcium concentration (ppm) Li2CO3+ Ca(OH)2OH - / Li + Molar ratio: 1.22725℃700044986.654996.5899.80ND549269.639993.1692.7623.928110249.1514989.7568.3725.2010810727.0819986.3353.6726.69

[0168]

[0169] Referring to Table 9, the target lithium concentration was set to 9993.16 ppm, and OH at 25℃ - / Li + The molar ratio was adjusted to 1.2 and the solid-liquid ratio of lithium carbonate (Li2CO3) slurry was 54 g / L, and the maximum lithium ion concentration reached using a homogenizer was 9269.63 ppm, the lithium recovery rate was 92.76%, and the calcium concentration was 23.92 ppm. In addition, the target lithium concentration was set to 19986 ppm, and the OH - / Li + The molar ratio was adjusted to 1.2 and the solid-liquid ratio of lithium carbonate (Li2CO3) slurry was adjusted to 108 g / L. The maximum lithium ion concentration reached using a homogenizer was 10727.08 ppm, the lithium recovery rate was 53.67%, and the calcium concentration was 26.69 ppm.

[0170] Referring to Table 3, the target lithium concentration was set to 9252.9 ppm, and OH at 25°C - / Li + The molar ratio was adjusted to 1.25 and the solid-liquid ratio of lithium carbonate (Li2CO3) slurry was adjusted to 50 g / L. The maximum lithium ion concentration reached using a magnetic bar was 8012.666 ppm, the lithium recovery rate was 86.596%, and the calcium concentration was 33.497 ppm.

[0171] In addition, the target lithium concentration was set to 18505.8 ppm, and OH at 25℃ - / Li + The molar ratio was adjusted to 1.25 and the solid-liquid ratio of lithium carbonate (Li2CO3) slurry was adjusted to 100 g / L, and the maximum lithium ion concentration reached using a magnetic bar was 10862.498 ppm, the lithium recovery rate was 58.6987%, and the calcium concentration was 28.907 ppm.

[0172] Therefore, when the solid-liquid ratio of lithium carbonate slurry is adjusted so that the target lithium concentration is 10,000 to 12,000 ppm and a homogenizer is used, the lithium ion recovery rate increases somewhat compared to the case where a magnetic bar is used for stirring. However, when the target lithium concentration is approximately 20,000 ppm, the difference in the lithium recovery rate achieved after the hydroxide reaction between the case where a homogenizer is used for stirring and the case where a magnetic bar is used for stirring was found to be insignificant.

[0173]

[0174] Experimental Example 5: Lithium concentration and recovery rate in the filtrate after repeated hydroxide reactions using a homogenizer

[0175] First, the first filtrate is separated after the first hydroxide reaction so that the lithium carbonate (Li2CO3) slurry solid-liquid ratio becomes 27 g / L.

[0176] Second, a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (OH) was added to the primary filtrate so that the high-liquid ratio was 27 g / L. - / Li + After the secondary hydroxylation reaction is performed by adding (molar ratio: 1.2) and stirring with a mechanical stirrer (300 RPM) or homogenizer (7000 RPM) for 4 hours, the secondary filtrate is separated.

[0177] Third, a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (OH) is added to the secondary filtrate so that the high-liquid ratio becomes 27 g / L. - / Li + After the third hydroxylation reaction, the third filtrate is separated by adding (molar ratio: 1.2) and stirring with a mechanical stirrer (300 RPM) or homogenizer (7000 RPM) for 4 hours.

[0178] Fourth, a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (OH) is added to the above 3rd filtrate so that the high-liquid ratio becomes 27 g / L.- / Li + After the fourth hydroxylation reaction by adding (molar ratio: 1.2) and stirring with a mechanical stirrer (300 RPM) or homogenizer (7000 RPM) for 4 hours, the fourth filtrate is separated.

[0179] Fifth, the lithium ion concentration and lithium recovery rate contained in the first to fourth filtrates were analyzed.

[0180]

[0181] Table 10 shows the lithium concentration and hydroxide recovery rate of the lithium solution recovered after repeated hydroxide reactions of lithium carbonate slurry stirred with a mechanical stirrer.

[0182] Li2CO3+ Ca(OH)2_ Mechanical stirrer stirring - Solid-liquid ratio by repetition number (g / L) Ca addition amount (g) Stirring speed (RPM) Number of repetitions Final lithium ion concentration (ppm) Maximum lithium concentration (ppm) Lithium recovery rate (%) Final calcium concentration (ppm) 2734.20 300 145 46.73 4996.589 1.00 N.D. 2734.20 288 57.6 295 43.31 92.81 11.64 2734.20 39 603.73 138 54.20 69.32 21.33

[0183]

[0184] Table 11 shows the lithium concentration and hydroxide recovery rate of the lithium solution recovered after repeated hydroxide reactions of lithium carbonate slurry stirred with a homogenizer.

[0185] Li2CO3+ Ca(OH)2_Homogenizer Stirring Repetition - Solid-liquid ratio by number of times (g / L) Ca addition amount (g) Stirring speed (RPM) Number of repetitions Final lithium ion concentration (ppm) Maximum lithium concentration (ppm) Lithium recovery rate (%) Final calcium concentration (ppm) 2734.20 7000 14757.44 4996.58 95.21 21.76 2734.20 29 194.9 19754.0 294.27 25.29 2734.20 310656.27 14191.50 75.09 30.93 2734.20 411778.34 15652.85 75.25 32.57

[0186]

[0187] As shown in Tables 11 and 12, it can be confirmed that the concentration of lithium ions in the filtrate increases as the number of hydroxide reactions increases. In addition, it was confirmed that the final lithium ion concentration and lithium recovery rate increased when stirring was performed using a homogenizer compared to when stirring was performed using a mechanical stirrer. Referring to Table 9, the final lithium concentration after the reaction was observed as 10727.08 ppm and the lithium recovery rate was 53.67% in the hydroxide reaction in which the solid-liquid ratio of lithium carbonate (Li2CO3) slurry was stirred for 4 hours using a homogenizer (7000 RPM) at a solid-liquid ratio of 108 (g / L).

[0188] Referring to Table 11, after the hydroxide reaction in which the lithium carbonate (Li2CO3) slurry solid-liquid ratio was 27 (g / L) and stirred with a homogenizer (7000 RPM) for 4 hours, a mixture of lithium carbonate (Li2CO3) and calcium hydroxide (OH) was added to the filtrate so that the solid-liquid ratio became 27 g / L. - / Li + After repeating the hydroxide reaction by adding (molar ratio: 1.2) four times, the final lithium ion concentration after the reaction was observed to be 11778.34 ppm and the lithium recovery rate was observed to be 75.25%.

[0189] Therefore, referring to Table 9 and Table 11, it was observed that the final lithium ion concentration slightly increased when lithium carbonate (Li2CO3) was divided into small amounts and the hydroxide reaction was repeated under the same stirring conditions.

[0190] However, even when lithium carbonate (Li2CO3) is divided into small amounts and the hydroxide reaction is repeated, it was confirmed that the final lithium ion concentration and lithium recovery rate are still less than about 80% when the target lithium concentration is about 15,000 ppm.

[0191]

[0192] Experimental Example 6: Lithium concentration in the filtrate after additional washing of sludge discharged from the hydroxide reaction

[0193] In the process of separating the filtrate from the mixture, a volume loss (less than 30 vol%) of the recovered lithium hydroxide (LiOH) solution occurs due to the moisture content of the calcium carbonate (CaCO3) cake formed. Therefore, in order to improve the recovery rate of the lithium hydroxide (LiOH) solution, an attempt was made to separate the lithium hydroxide (LiOH) solution by additionally washing the formed calcium carbonate (CaCO3) cake.

[0194] First, lithium carbonate (Li2CO3) slurry high-liquid ratio 54 g / L (Li2CO3-53.7g / H2O-1000mL), OH - / Li + A mixture of lithium carbonate (Li2CO3) slurry and calcium hydroxide (Ca(OH)2) was added under the condition of a molar ratio of 1.1, and the slurry was reacted at 20°C for 12 hours to carry out a hydration reaction. The formed sludge (calcium carbonate, unreacted Li2CO3, Ca(OH)2) was separated from the lithium hydroxide (LiOH) solution.

[0195] Second, 1000 mL of water was added to the separated sludge, and washing was performed for 1 hour using a mechanical stirrer, and then the filtrate was separated.

[0196] Third, the above washing process was repeated twice.

[0197] Fourth, the lithium and calcium concentrations contained in the recovered solution were measured for each number of washings.

[0198]

[0199] Table 12 shows the lithium and calcium concentrations in the recovered solution by repeated washing of the hydroxide reaction sludge.

[0200] Li2CO3+ Ca(OH)2(High-liquid ratio: 54 g / L, OH - / Li + Molar ratio: 1.1) Experimental conditions Addition amount (mL) Reaction time (20℃) Stirring speed (RPM) OH - / Li + Molar ratioLithium carbonate added (g)Calcium hydroxide added (g)Final lithium ion concentration (ppm)Lithium recovery rate (%)Final calcium concentration (ppm)Raw 1000 12 hours 300 1.15 3.77 0 6 1.80 0 9 5 9 7.20 9 5.11 22.12 1 st Suse10001hour3001468.8678.302 nd Water 10001 hours 300219.9736.93

[0201]

[0202] Referring to Table 12, the lithium concentration contained in the solution recovered from the hydroxide reaction was confirmed to be 9597.2 ppm, and the calcium content was confirmed to be 22.12 ppm. The lithium concentration contained in the solution recovered through the first washing of the sludge was 1468.86 ppm, and the lithium concentration contained in the solution recovered through the second washing was 219.97 ppm, indicating that the lithium concentration decreased as the number of sludge washes increased. Therefore, it is believed that it is possible to recover the unrecovered residual lithium hydroxide (LiOH) component as a solution through additional washing of the sludge generated after the hydroxide reaction of lithium carbonate (Li2CO3) and utilize it as an aqueous solution for the subsequent production of lithium carbonate (Li2CO3) slurry.

[0203]

[0204] Experimental Example 7: Lithium concentration and recovery rate in the filtrate after hydroxide reaction according to initial lithium ion concentration

[0205] As confirmed in the above Example 6, it was observed that additional recovery of residual lithium hydroxide (LiOH) solution was possible from the sludge generated after the hydration reaction of lithium carbonate (Li2CO3). This was circulated as an aqueous solution for subsequent lithium carbonate (Li2CO3) slurry production, and the recovery efficiency of lithium components after the hydration reaction of lithium carbonate (Li2CO3) according to the target lithium concentration was evaluated.

[0206] First, the solution was prepared so that the initial lithium ion concentration contained in the lithium hydroxide (LiOH) solution was approximately 1000 to 5000 ppm.

[0207] Second, the lithium carbonate and calcium hydroxide mixture was dissolved in OH until the target lithium concentration was approximately 10000 and approximately 15000 ppm. - / Li + The hydroxylation reaction was carried out at 25°C for 4 hours under the condition that the molar ratio was 1.

[0208]

[0209] Table 13 shows the distribution of lithium and calcium contents in the filtrate after the reaction according to the initial lithium ion concentration contained in the lithium hydroxide (LiOH) solution when the target lithium concentration is approximately 10,000 ppm.

[0210] LiOH sol. + (Li2CO3+ Ca(OH)2)Volume (mL)Reaction time (room temperature)Stirring speed (RPM)OH - / Li +Molar ratioLithium carbonate added (g)Calcium hydroxide added (g)Initial lithium ion concentration (ppm)Final lithium ion concentration (ppm)Lithium recovery rate (%)Final calcium concentration (ppm)50430012.4312.5281097.3310058.7999.6419.3050430012.1612.2472140.59101 19.7399.8120.0050430011.8911.9663169.7510130.8999.6321.0550430011.6211.6854121.0410112.6099.9228.3350430011.3511.4045119.4310108.8199.8933.12

[0211]

[0212] Table 14 shows the distribution of lithium and calcium contents in the filtrate after the reaction according to the initial lithium ion concentration contained in the lithium hydroxide (LiOH) solution when the target lithium concentration is approximately 15,000 ppm.

[0213] LiOH sol. + (Li2CO3+ Ca(OH)2)Volume (mL)Reaction time (room temperature)Stirring speed (RPM)OH - / Li + Molar ratioLithium carbonate added (g)Calcium hydroxide added (g)Initial lithium ion concentration (ppm)Final lithium ion concentration (ppm)Lithium recovery rate (%)Final calcium concentration (ppm)100430017.5657.8651042.1310299.7068.4727.67100430017.0257.3032086.4910386 .2368.8529.28100430016.4846.7413060.2010481.3469.6028.48100430015.9446.1804032.6910667.4670.9644.19100430015.4045.6185034.0810366.3668.9545.89

[0214]

[0215] Referring to Table 13, when the target concentration is about 10,000 ppm and the initial lithium ion concentration is about 1,000 to 5,000 ppm, a lithium recovery rate of about 99% is observed. Therefore, it can be confirmed that the lithium recovery rate will be as high as about 99% if the solution obtained by washing the sludge obtained through Example 6 is used as an aqueous solution for producing a subsequent lithium carbonate (Li2CO3) slurry with a target lithium concentration of about 10,000 ppm.

[0216] Referring to Table 14, a lithium recovery rate of about 70% is observed when the target concentration is about 15000 ppm and the initial lithium ion concentration is about 1000 to 5000 ppm.

[0217] Therefore, it can be confirmed that the lithium recovery rate will not be high when the solution obtained by washing the sludge through Example 6 is used as an aqueous solution for producing a subsequent lithium carbonate (Li2CO3) slurry with a target lithium concentration of about 15,000 ppm.

[0218]

[0219] Experimental Example 8: Separation and concentration of lithium ions from sludge washing solution from hydroxide reaction using an electric adsorption process

[0220] In Experimental Example 6, it was determined that the unrecovered residual lithium hydroxide (LiOH) component could be recovered as a solution through additional water washing of the sludge generated after the hydration reaction of lithium carbonate (Li2CO3) and used as an aqueous solution for subsequent production of lithium carbonate (Li2CO3) slurry.

[0221] In addition, it can be confirmed that the lithium recovery rate will be high if the solution obtained by washing the sludge in Experimental Example 7 is used as an aqueous solution for producing a subsequent lithium carbonate (Li2CO3) slurry with a target lithium concentration of approximately 10,000 ppm.

[0222] However, since the amount of water used to improve the lithium recovery rate is large, in order to improve this, low-concentration lithium ions with a final lithium concentration of approximately 1000 ppm or less were recovered and converted into an aqueous solution with a lithium concentration of approximately 3000 ppm or more by applying an electric adsorption technology, which is a low-energy concentration technology.

[0223] Figure 10 shows that the MCDI (Membrane Capacitive Deionization) process, which is an electrical adsorption technology, can be applied to a lithium hydroxide solution having a lithium ion concentration of about 1032 ppm to separate lithium ions from the lithium hydroxide solution and concentrate it, thereby converting it into an aqueous solution having a lithium ion concentration of about 3022 ppm.

[0224] First, the electric adsorption module applied for separation and concentration of lithium ions used electrodes composed of conductive activated carbon, and the adsorption module was assembled into 200 sets of unit cells composed of (+) electrode / anion exchange membrane / spacer / cation exchange membrane / (-) electrode.

[0225] Second, the operating potential for adsorption and concentration of lithium ions was applied at ±1.3 V each.

[0226] Third, 10 L of lithium hydroxide (LiOH) aqueous solution with a lithium ion concentration of approximately 1032 ppm was circulated through the electric adsorption module at a flow rate of 2 L / min for 5 minutes to adsorb lithium ions.

[0227] Fourth, after lithium ions were adsorbed onto the electric adsorption module, the solvent was removed from the inside of the electrode by an air flushing process while maintaining the potential at 1.3 V before desorption of lithium ions.

[0228] Fifth, after removing the solvent, apply a reverse potential (-1.3 V) and use 1 L of distilled water as a desorption solution to separate and concentrate lithium ions for 8 minutes.

[0229]

[0230] Sixth, the solution from which lithium ions have been desorbed is repeatedly used as a desorption liquid in the above-described electric adsorption process, and the above-described electric adsorption and desorption processes are repeated.

[0231] Seventh, the lithium ion concentration of the lithium hydroxide aqueous solution and desorption solution is measured as the electric adsorption process is repeated.

[0232] When the electric adsorption process was repeated 7 times, it was confirmed that almost no lithium ions existed in the lithium hydroxide aqueous solution with a lithium ion concentration of approximately 1032 ppm, and the lithium ion concentration of the desorbed solution was approximately 3000 ppm.

[0233] Therefore, it was confirmed that the solution obtained by washing sludge with water can be concentrated using an electro-adsorption process and then used as an aqueous solution for subsequent production of lithium carbonate (Li2CO3) slurry.

[0234] In addition, it is expected to have the advantage of significantly reducing the amount of wastewater (low-concentration lithium solution) generated from the hydroxide reaction and reducing the strong alkaline characteristics of waste calcium carbonate sludge, thereby reducing the environmental burden when discharged.

[0235]

[0236] Example 9: Analysis of product composition according to crystallization conditions of hydroxylation reaction filtrate

[0237] The composition of the final product was analyzed according to the crystallization conditions (temperature) of lithium hydroxide (LiOH) solution manufactured by hydroxide reaction from lithium carbonate (Li2CO3).

[0238] The lithium hydroxide (LiOH) solution used in the crystallization reaction was a solution of lithium carbonate (Li2CO3) with a high-liquid ratio of 60 and OH - / Li + Li2CO3 / Ca(OH)2 slurry was reacted at 25℃ under the condition of a molar ratio of 1.5 to produce a lithium ion concentration of approximately 10014 ppm in the filtrate.

[0239] Figures 11 to 13 show XRD patterns of products manufactured at different crystallization temperatures under reduced pressure conditions of 37 mbar.

[0240] In the case of lithium hydroxide (LiOH) powder recovered at a crystallization temperature of 50℃ or higher, anhydride was observed, and at 40℃ or lower, the castability was confirmed to be lithium hydroxide (LiOH) monohydrate.

[0241]

[0242] Experimental Example 10: Separation of impurities contained in the filtrate of the hydroxide reaction

[0243] It was confirmed that some calcium content remained in the filtrate due to the solubility of calcium carbonate (CaCO3) formed after the hydroxide reaction of lithium carbonate (Li2CO3) and unreacted calcium hydroxide (Ca(OH)2). In this experiment, the calcium ions (Ca) contained in the filtrate 2+ ) was controlled to increase the content of lithium hydroxide (LiOH) after crystallization.

[0244] The purpose of this study was to analyze the changes in the lithium concentration and calcium concentration components contained in the filtrate according to the concentration ratio of lithium hydroxide (LiOH) solution.

[0245] First, Li2CO3 / Ca(OH)2 slurry (lithium carbonate (Li2CO3) high-liquid ratio: 54.2 g / L, OH - / Li + Molar ratio: 1) After reacting at 25℃ for 24 hours, the lithium hydroxide (LiOH) filtrate was separated. At this time, the lithium concentration contained in the lithium hydroxide (LiOH) solution was confirmed to be approximately 9200 ppm, and the calcium concentration was confirmed to be approximately 17.4 ppm.

[0246] Second, a concentration experiment was conducted using 100 mL of lithium hydroxide (LiOH) filtrate at a temperature of 80°C and a pressure of 37 mbar. When the volume of the solution was reduced to approximately 63 mL, approximately 54 mL, and approximately 34 mL, the precipitated lithium hydroxide (LiOH) and calcium carbonate (CaCO3) were separated from the filtrate by filtration.

[0247] Third, lithium ions (Li) contained in the lithium hydroxide (LiOH) filtrate by volume after concentrating the filtrate + ) and calcium ions (Ca 2+ ) measure the concentration.

[0248] After concentrating the solution, the results of analysis of lithium and calcium concentrations in the filtrate by volume showed that lithium ions (Li + ) increases similarly to the theoretical concentration prediction value, but calcium ions (Ca 2+ ) It was observed that the concentration increase rate was somewhat lower than the theoretical concentration prediction value. At this time, when the volume of the lithium hydroxide solution was reduced to approximately 34 mL, the lithium and calcium contents in the filtrate showed values ​​of approximately 27784.6 ppm and approximately 30.5 ppm, respectively.

[0249] It is believed that the purity of lithium hydroxide powder can be improved by separating calcium precipitated during the filtrate concentration process from the filtrate.

[0250]

[0251] So far, specific examples of a method for producing lithium hydroxide from lithium carbonate with high efficiency through process improvement according to one embodiment of the present invention have been described, but it is obvious that various modifications are possible within the scope of the present invention.

[0252] Therefore, the scope of the present invention should not be limited to the described embodiments, but should be defined not only by the claims described below but also by equivalents of the claims.

[0253] That is, it should be understood that the above-described embodiments are exemplary in all respects and not restrictive, and the scope of the present invention is indicated by the claims to be described later rather than the detailed description, and all changes or modified forms derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

[0254] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of improving the recovery rate of lithium hydroxide.

[0255] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of reducing the calcium ion concentration of the final product.

[0256] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of recycling waste sludge and waste water produced by the reaction of lithium carbonate and calcium hydroxide.

[0257] The method for producing lithium hydroxide from lithium carbonate with high efficiency according to the present invention has the effect of reducing the amount of wastewater produced in the process by recycling steam generated in the process of producing lithium hydroxide from lithium carbonate.

Claims

1. (a) A step of preparing a mixture by adding calcium hydroxide (Ca(OH)2) to lithium carbonate (Li2CO3) slurry; (b) a step of separating a filtrate from the mixture prepared in step (a); (c) a step of concentrating the filtrate separated in step (b); and (d) a step of crystallizing lithium hydroxide (LiOH) from the concentrated filtrate in step (c); Method for producing lithium hydroxide.

2. In paragraph 1, In the above step (a), the lithium carbonate slurry is prepared by mixing lithium carbonate (Li2CO3) and an aqueous solution at a high-liquid ratio of 40 to 80 (g / L), In the above step (a), the hydroxide ion (OH) of the mixture - ) and lithium ion (Li + ) is characterized by a molar ratio of 1:1 to 1.5:

1. Method for producing lithium hydroxide.

3. In paragraph 2, The above step (a) is characterized in that it is performed at 20 to 100 ℃ for 1 hour or more. Method for producing lithium hydroxide.

4. In paragraph 1, (b-1) A step of separating the residue in the above step (b) and washing the remaining sludge with water while stirring; (b-2) a step of separating the solution after washing the sludge in the step (b-1) and producing a concentrated lithium ion aqueous solution through an electric adsorption process; and (b-3) characterized in that it further includes a step of adding the concentrated lithium ion aqueous solution in the step (b-2) to the mixture in the step (a); Method for producing lithium hydroxide.

5. In paragraph 4, The above electric adsorption process is characterized by being an MCDI (Membrance Captive Deionization) process. Method for producing lithium hydroxide.

6. In paragraph 4, Characterized in that the electric adsorption process of step (b-1) is repeated, Method for producing lithium hydroxide.

7. In paragraph 4, It is characterized in that the desalination liquid generated through the above electric adsorption process is used for sludge washing. Method for producing lithium hydroxide.

8. In paragraph 1, In the case where a calcium compound is precipitated through the concentration in the above step (c), the purity of lithium hydroxide (LiOH) is increased by removing the precipitated calcium compound from the filtrate. Method for producing lithium hydroxide.

9. In paragraph 1, In the case where lithium hydroxide and calcium compounds are precipitated through the concentration of the above step (c), the calcium compound is removed from the solution of the precipitated lithium hydroxide and calcium compound, and then the lithium hydroxide aqueous solution is added to the mixture of the above step (a). Method for producing lithium hydroxide.

10. In paragraph 1, The crystallization of lithium hydroxide (LiOH) performed in the above step (d) is characterized in that it is performed by evaporating the filtrate. Method for producing lithium hydroxide.

11. In paragraph 10, The crystallization of lithium hydroxide (LiOH) performed in the above step (d) is characterized in that it is performed at 20 to 50 mbar and 40°C or lower. Method for producing lithium hydroxide.

12. In paragraph 10, The crystallization of lithium hydroxide (LiOH) performed in the above step (d) is characterized in that it is performed at 50°C or higher at 20 to 50 mbar. Method for producing lithium hydroxide.

13. In paragraph 10, Characterized in that the solution obtained by condensing the vapor generated by the evaporation in the above step (d) is used for sludge water washing. Method for producing lithium hydroxide.

Citation Information

Patent Citations

  • Manufacturing method of lithium hydroxide using lithium carbonate

    KR101873933B1

  • Batch type centrifugal classifier and activated carbon processing apparatus including the same

    KR102483271B1

  • KR20210066418A

Cited By

  • Method for recovering lithium from waste

    WO2026135109A1

  • Method for recovering lithium from waste

    WO2026135113A1